Binder, cement composition, and concrete composition
A concrete composition with moderate heat Portland cement and pulverized blast furnace slag, combined with a hardening accelerator, addresses self-shrinkage and temperature-dependent cracking by reducing heat of hydration, enhancing thermal resistance and lowering CO2 emissions.
Patent Information
- Application Number
- JP2023051533
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Concrete compositions with high pulverized blast furnace slag powder content exhibit significant self-shrinkage and temperature-dependent increases, leading to increased temperature cracking risk due to heat of hydration.
A concrete composition using a binder comprising moderate heat Portland cement and pulverized blast furnace slag within specific content ranges, along with a hardening accelerator, to reduce the temperature rise due to heat of hydration and enhance thermal cracking resistance.
The proposed composition effectively reduces the temperature rise and improves thermal cracking resistance, maintaining compressive strength while minimizing CO2 emissions.
Smart Images

Figure 2024140404000001 
Figure 2024140404000002 
Figure 2024140404000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to binders, cement compositions, and concrete compositions. [Background technology]
[0002] In recent years, the demand for measures against global warming has increased, and there is a demand for reducing the amount of CO2 generated in concrete production. As a method for reducing the amount of CO2 generated, a method of producing concrete by replacing part of cement clinker, which generates a large amount of CO2 during preparation, with an admixture has been widely considered. Among admixtures, steel slag such as ground granulated blast furnace slag is expected to increase the long-term strength of concrete and improve its salt shielding effect. Therefore, research is being conducted on concrete that uses steel slag as an admixture and has a higher mixing ratio. For example, Patent Document 1 discloses a concrete composition that uses a blast furnace slag composition as a binder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-285293 A Summary of the Invention [Problem to be solved by the invention]
[0004] Meanwhile, concrete compositions in which 60% by mass or more of cement is replaced with ground granulated blast furnace slag can suppress the temperature rise of concrete caused by the heat of hydration generated by the hydration reaction between the binder and water, and are known to have excellent thermal crack resistance. However, the autogenous shrinkage of concrete containing ground granulated blast furnace slag is highly temperature-dependent, and tends to increase as the temperature increases. The greater the autogenous shrinkage of concrete, the more detrimental it is to thermal crack resistance. Therefore, by suppressing the temperature rise of concrete as much as possible, the increase in autogenous shrinkage can be suppressed and the temperature of components can be further reduced, leading to improved thermal crack resistance.
[0005] Therefore, an object of the present disclosure is to provide a concrete composition capable of reducing the amount of temperature rise due to heat of hydration, and a main object of the present disclosure is to provide a binder and a cement composition useful for producing such a concrete composition. [Means for solving the problem]
[0006] In order to solve the above problem, the present inventors have studied changing the base cement in a concrete composition containing a high content of ground granulated blast furnace slag from the commonly used ordinary Portland cement to a specified cement such as moderate heat Portland cement. In this study, a concrete composition using ordinary Portland cement and a concrete composition using the specified cement were adjusted to have the same compressive strength, and it was found that the concrete composition using the specified cement has a larger unit binder amount (or unit cement amount) than the concrete composition using ordinary Portland cement. Usually, the amount of temperature rise due to heat of hydration tends to increase as the unit binder amount increases. Therefore, it is expected that the concrete composition using the specified cement will have a larger amount of temperature rise due to heat of hydration than the concrete composition using ordinary Portland cement, but it was found that the concrete composition using the specified cement has a smaller amount of temperature rise due to heat of hydration, and the present invention has been completed.
[0007] This disclosure includes [1] to
[12] . [1] A binder comprising cement and ground granulated blast furnace slag, The cement has a C3S content of 25.0 mass% or more and 45.0 mass% or less, a C3A content of 2.5 mass% or more and 6.5 mass% or less, and a SO3 content of 1.5 mass% or more and 3.0 mass% or less, The content of the cement in 100 parts by mass of the binder is 20.0 parts by mass or more and 40.0 parts by mass or less, A binder in which the content of the ground granulated blast furnace slag per 100 parts by mass of the binder is 60.0 parts by mass or more and 80.0 parts by mass or less. [2] Further containing gypsum, The binder according to [1], wherein the content of the gypsum in 100 parts by mass of the binder is greater than 0 parts by mass and less than or equal to 3.5 parts by mass. [3] The binder according to [2], wherein the gypsum comprises at least one selected from the group consisting of gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. [4] The binder according to any one of [1] to [3], wherein the content of aluminum oxide in the ground granulated blast furnace slag is 14.5 mass% or less. [5] A cement composition comprising the binder according to [1] and a hardening accelerator. [6] The cement composition according to [5], wherein the content of the hardening accelerator is 0.23 parts by mass or more and 3.60 parts by mass or less in terms of solid content per 100 parts by mass of the binder. [7] The cement composition according to [5] or [6], wherein the hardening accelerator comprises at least one selected from the group consisting of alkali metal salts and alkaline earth metal salts. [8] The cement composition according to any one of [5] to [7], wherein the hardening accelerator contains a calcium salt. [9] The cement composition according to any one of [5] to [8], wherein the hardening accelerator contains a salt having a monovalent anion.
[10] The cement composition according to any one of [5] to [9], wherein the hardening accelerator comprises at least one selected from the group consisting of nitrites, nitrates, and chlorides.
[11] A cement composition according to any one of [5] to
[10] , water, fine aggregate, coarse aggregate, and a water-reducing agent, The content of the binder is 1 m of the concrete composition. 3 Based on the standard, 250kg / m 3 More than 600kg / m 3 is as follows: A concrete composition, wherein the water content is 25 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the binder.
[12] The concrete composition according to
[11] , wherein the water reducing agent comprises a high performance air entraining water reducing agent. Effect of the Invention
[0008] According to the present disclosure, a concrete composition capable of reducing the amount of temperature rise due to heat of hydration is provided. Such a concrete composition is also excellent in thermal crack resistance. The present disclosure also provides a binder and a cement composition useful for producing such a concrete composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments.
[0010] In the numerical ranges described in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in another numerical range. In the numerical ranges described in this specification, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0011] In this specification, unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more within the range corresponding to the conditions. When multiple substances corresponding to each component exist, the content of each component means the total amount of the multiple substances unless otherwise specified.
[0012] [Binding material] The binder includes cement and ground granulated blast furnace slag.
[0013] <Cement> The cement contains cement clinker and gypsum (hereinafter, may be referred to as "gypsum A"). The cement clinker may be, for example, a moderate-heat Portland cement clinker as defined in JIS R 5210:2009 "Portland cement". The cement may be a moderate-heat Portland cement containing moderate-heat Portland cement clinker and gypsum A, since the amount of temperature rise caused by heat of hydration during hardening of the concrete composition can be reduced.
[0014] Examples of gypsum A include gypsum dihydrate (CaSO4·2H2O), gypsum hemihydrate (CaSO4·1 / 2H2O), and anhydrous gypsum (CaSO4).
[0015] The C3S content in the cement is 25.0% by mass or more and 45.0% by mass or less, the C3A content is 2.5% by mass or more and 6.5% by mass or less, and the SO3 content is 1.5% by mass or more and 3.0% by mass or less. Moderate-heat Portland cement can satisfy these content conditions.
[0016] The mineral composition in cement can be calculated using the Bogue formula. The Bogue formula is a widely used formula for calculating the content of major minerals in cement from the content of chemical components in the cement. By using the Bogue formula shown below, the content of C3S (tricalcium silicate (3CaO·SiO2)), C2S (dicalcium silicate (2CaO·SiO2)), C3A (tricalcium aluminate (3CaO·Al2O3)), and C4AF (tetracalcium aluminate ferroferrate (4CaO·Al2O3·Fe2O3)) in cement can be calculated. In addition, the chemical formulas represented by CaO (aluminum oxide), SiO2 (silicon dioxide), Al2O3 (aluminum oxide), Fe2O3 (iron oxide), and SO3 (sulfur trioxide) in the following formulas represent the content (mass%) of each chemical component in the cement measured in accordance with JIS R 5202:2015 "Methods for chemical analysis of cement" or JIS R 5204:2019 "Methods for fluorescent X-ray analysis of cement." In addition, "%" in the following formulas represents "mass%."
[0017] ·Bogue style C3S[%]=(4.07×CaO[%])-(7.60×SiO2[%])-(6.72×Al2O3[%])-(1.43×Fe2O3[%])-(2.85×SO3[%]) C2S[%]=(2.87×SiO2[%])-(0.754×C3S[%]) C3A[%]=(2.65×Al2O3[%])-(1.69×Fe2O3[%]) C4AF[%]=3.04×Fe2O3[%]
[0018] The C3S content in the cement is 25.0% by mass or more, and may be 28.0% by mass or more, or 30.0% by mass or more. When the C3S content in the cement is 25.0% by mass or more, it is possible to ensure the development of compressive strength at an early age (age of 7 days or less). The C3S content in the cement is 45.0% by mass or less, and may be 42.0% by mass or less, or 40.0% by mass or less. When the C3S content in the cement is 45.0% by mass or less, it is possible to reduce the amount of temperature rise due to heat of hydration while ensuring the development of compressive strength at an age of 28 days.
[0019] The content of C3A in the cement is 2.5% by mass or more, and may be 3.0% by mass or more, or 3.5% by mass or more. When the content of C3A in the cement is 2.5% by mass or more, it is possible to further suppress a decrease in initial strength development when the concrete composition is hardened. The content of C3A in the cement is 6.5% by mass or less, and may be 6.0% by mass or less, or 5.5% by mass or less. When the content of C3A in the cement is 6.5% by mass or less, it is possible to suppress the formation of ettringite and reduce the amount of temperature rise due to heat of hydration.
[0020] The content of SO3 in the cement is 1.5% by mass or more, and may be 1.8% by mass or more, or 2.0% by mass or more. When the content of SO3 in the cement is 1.5% by mass or more, it is possible to reduce autogenous shrinkage to a certain extent. The content of SO3 in the cement is 3.0% by mass or less, and may be 2.9% by mass or less, or 2.8% by mass or less. When the content of SO3 in the cement is 3.0% by mass or less, it is possible to further suppress a decrease in long-term strength development when the concrete composition is hardened.
[0021] The Blaine specific surface area of cement is, for example, 2800 cm 2 / g or more or 3000cm 2 / g or more. The Blaine specific surface area of the cement may be 2800 cm 2 / g or more, the hydration reaction with ground granulated blast furnace slag can be further promoted. The Blaine specific surface area of cement is, for example, 10,000 cm 2 / g or less, 5000cm 2 / g or less, 4000cm 2 / g or less, or 3500cm 2 / g or less. The Blaine specific surface area of the cement may be 10,000 cm 2 / g or less, production costs can be reduced, and CO2 emissions in the production of cement can be further reduced.
[0022] In this specification, the Blaine specific surface area means a value measured in accordance with JIS R 5201:2015 "Physical testing methods for cement".
[0023] The content of cement in 100 parts by mass of the binder is 20.0 parts by mass or more and 40.0 parts by mass or less. The content of cement in 100 parts by mass of the binder may be 22.0 parts by mass or more or 25.0 parts by mass or more, and may be 38.0 parts by mass or less or 36.0 parts by mass or less. When the content of cement in 100 parts by mass of the binder is in such a range, the proportion of cement that generates a large amount of CO2 in the binder is reduced, and therefore the amount of CO2 generated in the production of the concrete composition can be suppressed.
[0024] <Grained blast furnace slag> The ground granulated blast furnace slag may be, for example, commercially available, or slag equivalent to the ground granulated blast furnace slag may be prepared by oneself and used.
[0025] The content of Al2O3 (aluminum oxide) in the ground granulated blast furnace slag may be, for example, 14.5% by mass or less, 14.0% by mass or less, 13.5% by mass or less, or 13.0% by mass or less. By having the content of Al2O3 in the ground granulated blast furnace slag be 14.5% by mass or less, it is possible to further suppress the deterioration of the long-term strength development when the obtained concrete composition is hardened. The content of Al2O3 in the ground granulated blast furnace slag may be, for example, 8% by mass or more, 10% by mass or more, or 12% by mass or more. By having the content of Al2O3 in the ground granulated blast furnace slag be 8% by mass or more, it is possible to more fully exhibit the latent hydraulic properties of the ground granulated blast furnace slag.
[0026] The content of SiO2 (silicon dioxide) in the ground granulated blast furnace slag may be, for example, 30.0 mass% or more, 31.0 mass% or more, or 32.0 mass% or more. By having the content of SiO2 in the ground granulated blast furnace slag be 30.0 mass% or more, the initial and long-term strength development can be further suppressed from decreasing. The content of SiO2 in the ground granulated blast furnace slag may be, for example, 40.0 mass% or less, 38.0 mass% or less, 36.0 mass% or less, or 35.0 mass% or less. By having the content of SiO2 in the ground granulated blast furnace slag be 40.0 mass% or less, the initial strength development can be further suppressed from decreasing.
[0027] The content of CaO (calcium oxide) in the ground granulated blast furnace slag may be, for example, 38.0 mass% or more, 40.0 mass% or more, or 42.0 mass% or more. When the content of CaO in the ground granulated blast furnace slag is 38.0 mass% or more, the initial strength development can be further improved. The content of CaO in the ground granulated blast furnace slag may be, for example, 50.0 mass% or less, 48.0 mass% or less, or 46.0 mass% or less. When the content of CaO in the ground granulated blast furnace slag is 50.0 mass% or less, the decrease in long-term strength development can be further suppressed.
[0028] The content of MgO (magnesium oxide) in the ground granulated blast furnace slag may be, for example, 3.0% by mass or more, 4.0% by mass or more, or 4.5% by mass or more. When the content of MgO in the ground granulated blast furnace slag is 3.0% by mass or more, the decrease in initial and long-term strength development when the concrete composition is hardened can be further suppressed. The content of MgO in the ground granulated blast furnace slag may be, for example, 10.0% by mass or less, 8.0% by mass or less, or 6.0% by mass or less. When the content of MgO in the ground granulated blast furnace slag is 10.0% by mass or less, the decrease in initial strength development when the concrete composition is hardened can be further suppressed.
[0029] The ground granulated blast furnace slag may contain, as other components, for example, SO3 (sulfur trioxide), NaO2 (sodium oxide), K2O (potassium oxide), TiO2 (titanium oxide), and the like.
[0030] In this specification, the chemical composition of the ground granulated blast furnace slag means a value measured in accordance with the description of JIS R 5202:2015 "Method of chemical analysis of cement".
[0031] The Blaine specific surface area of ground granulated blast furnace slag is, for example, 2500 cm 2 / g or more 10000cm 2 / g, 2500cm 2 / g or more 8000cm 2 / g, 2500cm 2 / g or more 6000cm 2 / g, 2500cm2 / g or more 5000cm 2 / g, 3000cm 2 / g or more 5000cm 2 / g, or 4000 cm 2 / g or more 5000cm 2 / g.
[0032] The content of ground granulated blast furnace slag in 100 parts by mass of the binder is 60.0 parts by mass or more and 80.0 parts by mass or less. The content of ground granulated blast furnace slag in 100 parts by mass of the binder may be 62.0 parts by mass or more or 64.0 parts by mass or more, and may be 75.0 parts by mass or less or 70.0 parts by mass or less. When the content of ground granulated blast furnace slag in 100 parts by mass of the binder is in such a range, the proportion of cement that generates a large amount of CO2 in the binder is reduced, and therefore the amount of CO2 generated in the production of the concrete composition can be suppressed.
[0033] <Gypsum> The binder may further contain gypsum (hereinafter, sometimes referred to as "gypsum B"). Note that gypsum B does not include gypsum A contained in the above-mentioned cement. In other words, gypsum B here means gypsum added as a component separate from gypsum A contained in cement, and for example, gypsum added to ground granulated blast furnace slag is included in gypsum B. Also, the content of gypsum B means the content of gypsum added as a component separate from gypsum A contained in cement.
[0034] The gypsum B may contain at least one selected from the group consisting of gypsum dihydrate (CaSO4·2H2O), hemihydrate (CaSO4·1 / 2H2O), and anhydrous gypsum (CaSO4). Examples of the dihydrate gypsum include dehydrated gypsum dihydrate, gypsum phosphate dihydrate, gypsum hydrofluoride dihydrate, and natural gypsum dihydrate. Examples of the hemihydrate gypsum include α-type hemihydrate gypsum and β-type hemihydrate. Examples of the anhydrous gypsum include natural anhydrous gypsum and hydrofluoric anhydrous gypsum. The content of SO3 in the anhydrous gypsum may be, for example, 54% by mass or more and 60% by mass or less.
[0035] When the binder further contains gypsum B, the content of gypsum B in 100 parts by mass of the binder may be more than 0 parts by mass and not more than 3.5 parts by mass. The content of gypsum B in 100 parts by mass of the binder may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1.0 parts by mass or more, or 1.5 parts by mass or more, and may be 3.3 parts by mass or less, or 3.1 parts by mass or less. By having the content of gypsum B in such a range, it is possible to reduce the action of inhibiting the effect of the hardening accelerator in improving the compressive strength of the concrete composition as it hardens, while exerting the effect of the gypsum in improving the compressive strength of the concrete composition as it hardens.
[0036] The method for producing the binder is not particularly limited, and the binder can be prepared by blending the above-mentioned components and mixing and kneading them by a known method.
[0037] [Cement composition] The cement composition contains the above-mentioned binder and a hardening accelerator.
[0038] <Binding material> The binder is a main component of the cement composition. The content of the binder in the cement composition may be, for example, 90% by mass or more, 95% by mass or more, 98% by mass or more, or 99% by mass or more.
[0039] <Curing accelerator> The hardening accelerator is a compound that accelerates the reaction of ground granulated blast furnace slag and improves its early strength. The hardening accelerator may contain at least one selected from the group consisting of alkali metal salts and alkaline earth metal salts. When the hardening accelerator contains an alkali metal salt or an alkaline earth metal salt, the reactivity of the ground granulated blast furnace slag can be further improved. Examples of the alkali metal include sodium and potassium. Examples of the alkaline earth metal include magnesium and calcium. From the viewpoint of accelerating the formation of hydrates and improving the compressive strength, the alkaline earth metal preferably contains calcium, and more preferably is calcium. The hardening accelerator may contain a calcium salt.
[0040] The hardening accelerator may contain a salt having a monovalent anion. The hardening accelerator may contain at least one selected from the group consisting of nitrites, nitrates, and chlorides, and preferably contains nitrites. By containing a nitrite in the hardening accelerator, the early strength of the concrete composition when hardened can be further improved, and the amount of heat generated by hydration when the concrete composition is hardened can also be reduced.
[0041] Specific examples of the hardening accelerator include calcium nitrite, calcium nitrate, calcium chloride, calcium hydroxide, sodium nitrite, potassium nitrite, sodium nitrate, potassium nitrate, sodium chloride, potassium chloride, etc. Among these, the hardening accelerator preferably contains an alkaline earth metal nitrite, more preferably contains calcium nitrite, and further preferably is calcium nitrite.
[0042] The content of the hardening accelerator may be 0.23 parts by mass or more and 3.60 parts by mass or less in terms of solid content relative to 100 parts by mass of the binder. The content of the hardening accelerator may be 0.23 parts by mass or more, 0.30 parts by mass or more, 0.35 parts by mass or more, or 0.40 parts by mass or more. By having the content of the hardening accelerator be 0.23 parts by mass or more, the reaction of the ground granulated blast furnace slag can be further promoted. The content of the hardening accelerator may be 3.30 parts by mass or less, 3.00 parts by mass or less, 2.80 parts by mass or less, or 2.50 parts by mass or less. By having the content of the hardening accelerator be 3.60 parts by mass or less, the reaction of the ground granulated blast furnace slag can be further promoted, while the occurrence of abnormal setting in the case where the reaction of the ground granulated blast furnace slag or the like is excessively promoted can be more reliably suppressed.
[0043] The method for producing the cement composition is not particularly limited, and the cement composition can be prepared by blending the above-mentioned components and mixing and kneading them by a known method.
[0044] [Concrete composition] In one embodiment, the concrete composition includes the above-mentioned cement composition, water, fine aggregate, coarse aggregate, and a water reducing agent. The concrete composition may be a composition equivalent to blast furnace cement type C.
[0045] <Cement composition (binding material)> The content of the binder in the concrete composition (the binder contained in the above cement composition) is 1 m of the concrete composition. 3 Based on the standard, 250kg / m 3 More than 600kg / m 3 The content of the binder in the concrete composition (the binder contained in the cement composition) is 1 / m of the concrete composition. 3 Based on the standard, 300kg / m 3 or more than 350kg / m 3 or more, 550 kg / m 3 Below 500kg / m 3 or less than 450kg / m 3 It may be the following.
[0046] <Water> Examples of water include tap water, distilled water, and deionized water. The water content is 25 parts by mass or more and 60 parts by mass or less with respect to 100 parts by mass of the binder (the binder contained in the cement composition). The water content may be 30 parts by mass or more, 35 parts by mass or more, or 40 parts by mass or more. By having a water content of 25 parts by mass or more, the fluidity of fresh concrete can be further improved, and the workability in concrete construction can be further improved. The water content may be 55 parts by mass or less, 52 parts by mass or less, or 50 parts by mass or less. By having a water content of 60 parts by mass or less, the compressive strength when the concrete composition is hardened can be further improved.
[0047] The water / binder ratio (100 × water mass / binder mass, hereinafter sometimes referred to as "W / B") may be, for example, 60 mass% or less, 55 mass% or less, 52 mass% or less, or 50 mass% or less, or may be 25 mass% or more, 30 mass% or more, 35 mass% or more, or 40 mass% or more.
[0048] <Fine and coarse aggregate> The fine aggregate may be any of those specified in JIS A 5005:2020 "Crushed stone and crushed sand for concrete". Examples of fine aggregate include river sand, land sand, sea sand, crushed sand, silica sand, copper slag fine aggregate, and electric furnace oxidized slag fine aggregate. The content of the fine aggregate per 1 m of the concrete composition is 100%. 3 Based on this, for example, 650 kg / m 3 More than 1000kg / m 3 Below, 725kg / m 3 More than 950kg / m 3 or less than 800kg / m 3 More than 900kg / m 3 It may be the following:
[0049] The coarse aggregate may be any of those specified in JIS A 5005:2020 "Crushed stone and crushed sand for concrete." Examples of the coarse aggregate include gravel and crushed stone. The content of the coarse aggregate per 1 m of the concrete composition is 100%. 3 Based on this, for example, 750 kg / m 3 More than 1025kg / m 3 Below 800kg / m 3 More than 975kg / m 3 or less than 850kg / m 3 More than 900kg / m 3 It may be the following:
[0050] The fine aggregate and the coarse aggregate can be used in combination. In this case, the total content of the fine aggregate and the coarse aggregate may be 100 parts by mass or more and 300 parts by mass or less, or 200 parts by mass or more and 250 parts by mass or less, relative to 100 parts by mass of the binder (the binder contained in the above cement composition).
[0051] The bulk volume of coarse aggregate is 1 m3 of concrete composition. 3 Based on this, for example, 0.500m 3 / m 3 Above, 0.520m 3 / m 3 or more, or 0.540m 3 / m 3 The bulk volume of the coarse aggregate is 0.500 m 3 / m 3 By satisfying the above requirements, the fluidity of fresh concrete can be improved, and the workability of concrete construction can be improved. The bulk volume of the coarse aggregate is, for example, 0.620 m 3 / m 3 Below, 0.600m 3 / m 3 Less than or equal to 0.580m 3 / m 3 The bulk volume of the coarse aggregate may be less than 0.620 m 3 / m 3 By satisfying the above condition, the material separation resistance in fresh concrete can be improved.
[0052] <Water reducing agent> Examples of the water reducing agent include water reducing agents, AE (Air Entraining) water reducing agents, high performance water reducing agents, and high performance AE water reducing agents. As the AE water reducing agent and the high performance AE water reducing agent, any of the standard type, delayed type, and accelerated type can be used, but it is preferable to use the delayed type. As the AE water reducing agent and the high performance AE water reducing agent, any of the types I, II, and III can be used, but it is preferable to use the type I. The water reducing agent may include a high performance AE water reducing agent or may be a high performance AE water reducing agent.
[0053] The content of the water reducing agent is 0.5 parts by mass or more and 3.0 parts by mass or less with respect to 100 parts by mass of the binder (the binder contained in the above cement composition). The content of the water reducing agent may be, for example, 0.6 parts by mass or more, 0.7 parts by mass or more, or 0.8 parts by mass or more. By having the content of the water reducing agent be 0.5 parts by mass or more, the fluidity in fresh concrete can be further improved. The content of the water reducing agent may be 2.5 parts by mass or less, 2.0 parts by mass or less, 1.5 parts by mass or less, or 1.0 parts by mass or less. By having the content of the water reducing agent be 3.0 parts by mass or less, material separation resistance can be imparted without impairing the fluidity in fresh concrete.
[0054] <Other admixtures> The concrete composition may further contain other admixtures. Examples of the other admixtures include air-enhancing agents, fluidizing agents, defoamers, shrinkage reducing agents, setting accelerators, setting retarders, thickeners, silica powder, inorganic powders containing calcium, fly ash, inorganic minerals containing Si or Al, etc. The content of the other admixtures may be, for example, 0.01 parts by mass or more and 2 parts by mass or less with respect to 100 parts by mass of the binder (the binder contained in the above cement composition).
[0055] The method for producing the concrete composition is not particularly limited, and the concrete composition can be prepared by blending the above-mentioned components and mixing and kneading them by a known method.
[0056] In another embodiment, the concrete composition includes the above-mentioned binder, water, fine aggregate, coarse aggregate, and a water reducing agent. Each component is the same as each component of the cement composition of the above embodiment, and the preferred aspects, contents, etc. are also the same. Therefore, a duplicated description will be omitted here. EXAMPLES
[0057] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.
[0058] 1.Materials used The materials used are shown in Table 1, and the chemical composition of the cement and ground granulated blast furnace slag, as well as the mineral composition of the cement, are shown in Table 2. The chemical composition of the cement and ground granulated blast furnace slag was measured in accordance with the description in JIS R 5202:2015 "Methods for chemical analysis of cement" or JIS R 5204:2019 "Methods for fluorescent X-ray analysis of cement". The mineral composition of the cement was calculated using the Bogue formula. In Table 2, "ig.loss" means loss on ignition. The loss on ignition is the value measured at a heating temperature of 700°C in accordance with the method described in "5.2 Cases other than blast furnace cement and blast furnace slag" in "5. Methods for quantifying loss on ignition" of JIS R 5202:2010.
[0059] [Table 1]
[0060] [Table 2]
[0061] 2. Composition of binder and cement composition The formulations of the binder and cement composition are shown in Table 3. In Table 3, the numerical values of each component of the binder and the numerical values of the hardening accelerator refer to the content (unit: mass%) based on the total amount of the binder. The binders of Examples 1 to 4 and Comparative Examples 1 to 9 were prepared by kneading each component of the binder. In addition, the cement compositions of Examples 1 and 2 and Comparative Examples 3 to 9 were prepared by further kneading the binders and hardening accelerators of Examples 1 and 2 and Comparative Examples 3 to 9.
[0062] [Table 3]
[0063] 3. Mixing of concrete composition Concrete compositions were prepared using the binders of Examples 3 and 4 and Comparative Examples 1 and 2, and the cement compositions of Examples 1, 2 and Comparative Examples 3 to 9. The concrete composition mixes are shown in Table 4. The concrete compositions containing ground granulated blast furnace slag have a content of ground granulated blast furnace slag in the binder of 60% by mass or more and 70% by mass or less, and therefore can be said to be compositions equivalent to Class C blast furnace cement.
[0064] [Table 4] 4. Test Results (4-1) Various fresh properties and compressive strength test results The test results for various fresh properties and compressive strength are shown in Table 5. Slump, air content, concrete temperature, setting time, and compressive strength were measured in accordance with JIS A 1101:2020, JIS A 1128:2019, JIS A 1156:2014, JIS A 1147:2019, and JIS A 1108:2018, respectively. The environmental temperature was 20°C, and the compressive strength specimens were demolded after 1 day of age and then cured in water at 20°C until the test. The results are shown in Table 5.
[0065] [Table 5]
[0066] (4-2) Adiabatic temperature rise test results In the adiabatic temperature rise test, first, the conditions under which the compressive strength of each concrete composition at 28 days was the same were determined, and then the concrete compositions were mixed under those conditions and the adiabatic temperature rise test was carried out.
[0067] Nos. 0 and 13, 1 and 14, and 12 and 15 in Table 5 all have the same mix proportions, but different mix proportions (mass ratio of binder volume to unit water volume (B / W)). Based on the compressive strengths of these concretes at 28 days, the relationship between the mass ratio of binder volume to unit water volume (B / W) and the compressive strength at 28 days was determined. The relationship between the mass ratio of binder volume to unit water volume (B / W) and the compressive strength at 28 days for M(2.69), BC(2.04), and MBC(2.66)-GA3 and the compressive strength at 28 days is shown in Equations (1), (2), and (3), respectively.
[0068]
number
[0069] Assuming that the slope of the relationship between the mass ratio of binder to unit water (B / W) and the compressive strength at 28 days is as shown in equation (2) for BC based on ordinary Portland cement (N), and as shown in equation (3) for MBC based on moderate heat Portland cement (M), the compressive strength at 28 days is 42.0 N / mm 2 In addition, in the case of a mix with M (2.69), the compressive strength at 28 days was calculated using formula (1) as follows: 2 The W / B (mass%) was calculated when the above condition was satisfied. The W / B (mass%) is shown in Table 6.
[0070] Next, concrete compositions were mixed under the same conditions as in Table 4 for each calculated W / B (mass%) mix, and an adiabatic temperature rise test was performed. The adiabatic temperature rise test was performed using an air-circulating test device in accordance with JCI-SQA3 "Concrete Adiabatic Temperature Rise Test Method (Draft)". The sample container was cylindrical with an inner diameter of 400 mm and an inner height of 400 mm, and the amount of sample was approximately 50 L. The ambient temperature and the temperature of the mixed concrete were set to 20°C.
[0071] The actual measured values of the adiabatic temperature rise curve obtained by the adiabatic temperature rise test were approximated by the following formula (4) using the least squares method to obtain K, α, and β. The results are shown in Table 6.
[0072]
number
[0073] [Table 6]
[0074] 5. Temperature Stress Analysis Using temperature stress analysis software (ASTEA MACS, manufactured by Computational Mechanics Research Center, Inc.), adiabatic temperature rise curves (equation (4)) with K, α, and β shown in Table 6 substituted were used as input values for levels No. 17 to 23 and 28 shown in Table 6, and temperature stress analysis was performed for each level to determine the maximum component temperature and minimum crack index. The results are shown in Table 7. Note that the maximum component temperature refers to the maximum temperature that occurs in the concrete component of the model, and the minimum crack index refers to the minimum value of the ratio of the tensile strength of the concrete to the tensile stress that occurs in the concrete at the point where the maximum component temperature occurs, and the smaller this value is, the higher the probability of crack occurrence.
[0075] [Table 7]
[0076] 6. Evaluation The compressive strength at 28 days for the same W / B was smaller for the MBC mix based on moderate heat Portland cement than for the BC mix based on normal Portland cement, regardless of whether or not a hardening accelerator was used. Therefore, the compressive strength at 28 days was 42.0 N / mm 2When the strength was the same, the W / B (mass%) was smaller for the MBC mix, and the unit binder volume was larger. Normally, as the unit binder volume increases, the temperature rise due to heat of hydration tends to increase. However, even in this case, the final adiabatic temperature rise K for the MBC mix was smaller than that of the BC mix, and also smaller than that of the M mix containing only moderate-heat Portland cement. In other words, when comparing compressive strengths at the same age of 28 days, the MBC mix had a smaller temperature rise and was found to be advantageous in terms of thermal crack resistance.
[0077] In addition, as a result of conducting temperature stress analysis at some of the levels shown in Table 7, it was found that No. 28, which is an MBC mix, had a lower maximum component temperature than Nos. 17 to 23, which are BC mixes, resulting in a larger minimum crack index and superior thermal crack resistance.
Claims
1. A binder comprising cement and ground granulated blast furnace slag, In the cement, 3 The content of S is 25.0 mass% or more and 45.0 mass% or less, and C 3 The content of A is 2.5 mass% or more and 6.5 mass% or less, and SO 3 The content is 1.5 mass% or more and 3.0 mass% or less, The content of the cement in 100 parts by mass of the binder is 20.0 parts by mass or more and 40.0 parts by mass or less, A binder, wherein the content of the ground granulated blast furnace slag per 100 parts by mass of the binder is 60.0 parts by mass or more and 80.0 parts by mass or less.
2. Further comprising gypsum, The binder according to claim 1, wherein the content of the gypsum in 100 parts by mass of the binder is greater than 0 parts by mass and is not more than 3.5 parts by mass.
3. The binder according to claim 2 , wherein the gypsum comprises at least one selected from the group consisting of gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum.
4. The binder according to claim 1, wherein the content of aluminum oxide in the ground granulated blast furnace slag is 14.5 mass% or less.
5. A cement composition comprising the binder of claim 1 and a hardening accelerator.
6. The cement composition according to claim 5, wherein the content of the hardening accelerator is 0.23 parts by mass or more and 3.60 parts by mass or less in terms of solid content per 100 parts by mass of the binder.
7. 7. The cement composition according to claim 5, wherein the hardening accelerator comprises at least one selected from the group consisting of alkali metal salts and alkaline earth metal salts.
8. 7. The cement composition of claim 5 or 6, wherein the hardening accelerator comprises a calcium salt.
9. 7. The cement composition of claim 5 or 6, wherein the accelerator comprises a salt having a monovalent anion.
10. 7. The cement composition according to claim 5, wherein the hardening accelerator comprises at least one selected from the group consisting of nitrites, nitrates, and chlorides.
11. A cement composition comprising the cement composition according to claim 5, water, fine aggregate, coarse aggregate, and a water reducing agent, The content of the binder is 1 m of the concrete composition. 3 Based on this, 250 kg / m 3 More than 600kg / m 3 is as follows: The concrete composition, wherein the water content is 25 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the binder.
12. 12. The concrete composition of claim 11, wherein the water reducing admixture comprises a high-range water reducing admixture.
Citation Information
Patent Citations
Mixed cement
JP1990097441A
Low heat cement composition
JP1990120261A
Ultralow exotherm type b-type blast furnace cement
JP1994048789A
Concrete composition using blast-furnace slag composition
JP2010285293A
Method for producing cement hardened body
JP2011157242A