Composition and surface protection method

A silicone-modified (meth)acrylic copolymer composition with specific structural units improves adhesion to porous bodies like concrete, addressing the adhesion issues in existing technologies and enhancing the bond between layers.

JP2024140656APending Publication Date: 2024-10-10DENKA CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023051912
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing surface protection compositions for porous bodies, such as those described in Patent Document 1, suffer from inadequate adhesion to the surface and require improvements, particularly in terms of adhesion to concrete structures.

Method used

A composition comprising a silicone-modified (meth)acrylic copolymer with specific structural units, including a structural unit N with a silicon atom bonded to an alkoxy group, a structural unit O with a hydroxyl group, and a structural unit P with a fluoroalkyl group, which enhances adhesion to porous bodies, especially concrete, by improving both the adhesion to the surface and to upper layers.

Benefits of technology

The composition forms a coating film with excellent adhesion to porous bodies, particularly concrete, even in humid environments, and supports a strong bond between the primer layer and upper layers, while being environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140656000021
    Figure 2024140656000021
  • Figure 2024140656000001
    Figure 2024140656000001
  • Figure 2024140656000002
    Figure 2024140656000002
Patent Text Reader

Abstract

To provide a composition capable of forming a coating film excellent in adhesion to a porous body surface.SOLUTION: A composition of the invention is one which is used for application to a surface of a porous body. The composition includes a silicone-modified (meth)acrylic copolymer that has, in a molecule, a predetermined structural unit N having a silicon atom with an alkoxy group bonded thereto, and at least one of a predetermined structural unit O having a hydroxy group at a terminal and a predetermined structural unit P having a perfluoroalkyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition and a method for protecting a surface. [Background technology]

[0002] Various methods for protecting the surface of porous bodies have been developed so far. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a method of forming a primer layer containing a silane coupling agent and a urethane resin on the surface of a concrete structure, and then forming a main material layer containing a urethane resin on the primer layer (Table 1 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-017762 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of investigations by the present inventors, it was found that there is room for improvement in the adhesion to the surface of a porous body in the compositions such as the primer described in the above Patent Document 1. [Means for solving the problem]

[0005] After further investigation, the inventors found that by using a silicone-modified (meth)acrylic copolymer containing a structural unit N having a silicon atom bonded to an alkoxy group, and at least one of a structural unit O having a hydroxyl group at its terminal and a specific structural unit P having a perfluoroalkyl group, as a composition to be applied to the surface of a porous body, the adhesion of the composition to the surface of a porous body can be improved overall, and thus the present invention was completed.

[0006] According to one aspect of the present invention, the following composition and method for protecting a surface are provided. 1. A composition for use in applying to the surface of a porous body, comprising: Contains a silicone modified (meth)acrylic copolymer, The silicone-modified (meth)acrylic copolymer is A structural unit N represented by the following general formula (N), A composition comprising, in the molecule, at least one of a structural unit O represented by the following general formula (O) and a structural unit P represented by the following general formula (P): [ka] (In the above general formula (N), R 3 is a hydrogen atom or a methyl group, R 4 is an alkyl group having 1 to 3 carbon atoms, R 5 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, b is an integer of 1 to 6, and c is an integer of 1 to 3. [ka] (In the above general formula (O), R 6 is a hydrogen atom or a methyl group, and d is an integer of 1 to 8. [ka] (In the above general formula (P), R 7 is a hydrogen atom or a methyl group, Cf is -CF3 or CHF2, e is an integer of 1 to 6, and f is an integer of 0 to 10. 2. The composition according to 1., The content of the structural unit N contained in the silicone-modified (meth)acrylic copolymer is C N The content of the structural unit P is C p Then, C p / C N is greater than or equal to 0.001 and less than or equal to 1.0. 3. The composition according to 1. or 2., The content of the structural unit N contained in the silicone-modified (meth)acrylic copolymer is CN The content of the structural unit O is C O Then, C O / C N is greater than or equal to 0.05 and less than or equal to 5.0. 4. The composition according to any one of 1. to 3., The silicone-modified (meth)acrylic copolymer has a structural unit M represented by the following general formula (M): [ka] (In the above general formula (M), R 1 is a hydrogen atom or a methyl group, R 2 is an alkyl group having 1 to 3 carbon atoms, and a is an integer of 0 to 3. 5. The composition according to any one of 1. to 4., The silicone-modified (meth)acrylic copolymer has a weight average molecular weight (Mw) of 500 or more and 50,000 or less. 6. The composition according to any one of 1. to 5., A composition comprising a solvent. 7. The composition according to any one of 1. to 6., A composition that is substantially free of epoxy resins. 8. The composition according to any one of 1. to 7., The composition, wherein the porous body is a concrete structure. 9. The composition according to any one of 1. to 8., The composition is a primer composition. 10. A surface protection method comprising the steps of applying a composition according to any one of 1. to 9. to a surface of a porous body and drying the composition to form a layer. 11. A silicone-modified (meth)acrylic copolymer is included, The silicone-modified (meth)acrylic copolymer is A structural unit N represented by the above general formula (N), A composition comprising, in the molecule, at least one of a structural unit O represented by the above general formula (O) and a structural unit P represented by the above general formula (P). Effect of the Invention

[0007] According to the present invention, there are provided a composition capable of forming a coating film having excellent adhesion to the surface of a porous body, and a surface protection method using the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram for explaining an adhesion test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The composition of the present embodiment will be described.

[0010] The composition of the present embodiment contains a silicone-modified (meth)acrylic copolymer, and the silicone-modified (meth)acrylic copolymer contains, in the molecule, a structural unit N represented by the following general formula (N) and at least one of a structural unit O represented by the following general formula (O) and a structural unit P represented by the following general formula (P).

[0011] This composition is a composition for coating a porous body used to coat the surface of a porous body, and may be any of a primer composition, an undercoat paint, or a topcoat paint, with a primer composition being preferred.

[0012] According to the findings of the present inventors, it has been found that the use of a silicone-modified (meth)acrylic copolymer having a structural unit N having a silicon atom bonded to an alkoxy group, and at least one of a structural unit O represented by the following general formula (O) and a structural unit P represented by the following general formula (P) can improve the overall adhesion of a composition to the surface of a porous body. Furthermore, when used as a primer composition, it was found that the adhesion between the concrete / primer layer and the adhesion between the primer layer / intercoat layer (the layer above the primer layer) was improved, resulting in an overall improvement in adhesive strength.

[0013] Although the detailed mechanism is unclear, it is presumed that the structural unit N described below improves adhesion to concrete, and the structural unit P improves the ability to impregnate concrete in a wet environment, and therefore, by using a silicone-modified (meth)acrylic copolymer having at least the structural units N and P, the adhesion of the composition to the surface of a porous body is improved overall. In addition, although the detailed mechanism is unclear, it is presumed that the structural unit N described below improves adhesion to concrete, and the structural unit O improves adhesion to upper layers such as an undercoat layer, and therefore, by using a silicone-modified (meth)acrylic copolymer having at least the structural unit N and the structural unit O, the adhesion of the composition to the surface of a porous body is improved overall.

[0014] In addition, silicone-modified (meth)acrylic copolymers are also known as materials that have a low environmental impact, making it possible to realize primer compositions with excellent low toxicity.

[0015] The porous body is preferably a concrete structure, but is not limited thereto. The porous body may be a member having independent pores and / or continuous pores formed on the surface. At least the surface of such a member may be made of an inorganic material. Furthermore, examples of concrete structures include, but are not limited to, parts of viaduct structures and the like, and include those used outdoors.

[0016] [ka]

[0017] In the above general formula (N), R 3 is a hydrogen atom or a methyl group, R 4 is an alkyl group having 1 to 3 carbon atoms, R 5 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, b represents an integer of 1 to 6, and c represents an integer of 1 to 3. In the above general formula (N), R 3 is preferably a methyl group. In the above general formula (N), R4 and R 5 may each be a methyl group or an ethyl group, and is preferably a methyl group. In the above general formula (N), b is preferably 2 to 5, and more preferably 3 to 4. In the above general formula (N), c is preferably 2 to 3, and more preferably 3.

[0018] [ka]

[0019] In the above general formula (O), R 6 is a hydrogen atom or a methyl group. In the above general formula (O), d is preferably 1 to 8, and more preferably 2 to 5. By making it equal to or less than the above upper limit, the hydrophilicity can be adjusted, and by making it equal to or more than the above lower limit, the hydrophobicity can be adjusted.

[0020] The silicone-modified (meth)acrylic copolymer may contain a structural unit P represented by the following general formula (P), which can improve the adhesive strength in a wet environment.

[0021] [ka]

[0022] In the above general formula (P), R 7 is a hydrogen atom or a methyl group, Cf is -CF3 or CHF2, e is an integer of 1 to 6, and f is an integer of 0 to 10. In the above general formula (P), e is preferably 1 to 4, and more preferably 1 to 3. In the above general formula (P), f is preferably 0 to 7, and more preferably 0 to 6. By making it equal to or less than the above upper limit, it is possible to suppress a decrease in impregnation into wet concrete. By making it equal to or more than the above lower limit, it is possible to improve impregnation into wet concrete. Although the detailed mechanism is unclear, it is believed that since the surface tension of the composition can be appropriately adjusted by the amount of perfluoroalkyl groups in general formula (P), it is possible to improve impregnation into swollen concrete.

[0023] The content of the structural unit N contained in the silicone modified (meth)acrylic copolymer is C N The content of the structural unit P is C p , the content of the structural unit O is C O Let us assume that. In this embodiment, the content of each structural unit contained in the silicone-modified (meth)acrylic copolymer refers to the proportion (mol %) of each structural unit measured by NMR based on the constituent compound information obtained by pyrolysis GC-MS. The GC-MS conditions were as follows: Equipment: JMS Q1500GC&PY 3030E Pyrolysis furnace temperature: 600℃ GC inlet temperature: 280℃ Ion source temperature: 260℃ GC-IF temperature: 280℃ Ionization method: EI Column: ZB-5MS (20 m x inner diameter: 0.18 mm x film thickness: 0.18 μm) The NMR conditions were as follows: Equipment: Bruker AVANCE NEO Probe: CPBBO Deuterated solvent: CDCl3 As a pretreatment, add 0.4 mL of deuterated chloroform to dissolve.

[0024] The C calculated above p , C N C required from p / C N is, for example, 0.001 or more and 1.0 or less, preferably 0.005 or more and 0.5 or less, more preferably 0.01 or more and 0.2 or less. By making it equal to or more than the lower limit, it is possible to improve the impregnation into concrete in a humid environment. On the other hand, by making it equal to or less than the upper limit, it is possible to achieve a balance between the impregnation into concrete and the adhesion to concrete.

[0025] In addition, the C calculated above O , C N C required from O / C N is, for example, 0.05 to 5.0, preferably 0.1 to 3.0, and more preferably 0.2 to 1.5. By making it equal to or more than the lower limit, the adhesion to the upper layer such as the intermediate coat layer can be improved. By making it equal to or less than the upper limit, the adhesion to the upper layer and the adhesion to concrete can be balanced.

[0026] The silicone-modified (meth)acrylic copolymer may contain a structural unit M represented by the following general formula (M).

[0027] [ka]

[0028] In the above general formula (M), R 1 is a hydrogen atom or a methyl group, R 2 is an alkyl group having 1 to 3 carbon atoms, and a is an integer of 0 to 3. In addition, in the above general formula (M), R 1 is preferably a methyl group. In the above general formula (M), R 2 is preferably a methyl group or an ethyl group, and more preferably a methyl group. In the above general formula (M), a is preferably 2 or less, more preferably 1 or less, and even more preferably 0.

[0029] The silicone-modified (meth)acrylic copolymer may contain a structural unit L represented by the following general formula (L).

[0030] [ka]

[0031] In the above general formula (L), R 7 is a hydrogen atom or a methyl group, R 8 is an alkyl group having 1 to 3 carbon atoms, and g is an integer of 4 to 16. In the above general formula (L), R 8may be a methyl group or an ethyl group, and is preferably a methyl group. In the above general formula (L), g is preferably 4 to 15, more preferably 4 to 10, and even more preferably 4 to 6. By adjusting it to the upper limit or less, hydrophilicity is improved, and adhesion to concrete can be improved even in a wet environment.

[0032] The weight average molecular weight (Mw) of the silicone modified (meth)acrylic copolymer is, for example, 500 or more and 50,000 or less, preferably 1,000 or more and 45,000 or less, and more preferably 1,500 or more and 40,000 or less. By setting the thickness to be equal to or greater than the lower limit, the adhesion and film-forming properties of the primer layer can be improved, whereas by setting the thickness to be equal to or less than the upper limit, the maximum displacement in a push-out test can be increased. In the present embodiment, the weight average molecular weight is, for example, a weight average molecular weight measured by gel permeation chromatography (GPC) (solvent: tetrahydrofuran (THF)) and converted into standard polystyrene.

[0033] The silicone-modified (meth)acrylic copolymer can be obtained, for example, by blending raw material components from which the respective structural units are derived and reacting them in a predetermined solvent in the presence of a catalyst. In this specification, the term "(meth)acrylic" means at least one of acrylic and methacrylic.

[0034] The composition of the present embodiment may contain a solvent, if necessary. The solvent may include, for example, a polar organic solvent. Examples of polar organic solvents include, but are not limited to, ether-based solvents, alcohol-based solvents, ketone-based solvents, ester-based solvents, etc. These may be used alone or in combination of two or more.

[0035] The solvent may contain, for example, a solvent having a boiling point of 50° C. or higher, preferably 100° C. or higher, more preferably 120° C. or higher. This can improve the film formation stability. The upper limit of the boiling point of the solvent is not particularly limited, but may be, for example, 300° C. or lower, or 250° C. or lower.

[0036] The composition may contain additives other than the above components as long as the effects of the present invention are not impaired. Examples of additives include silicone resins other than silicone-modified (meth)acrylic copolymers, (meth)acrylic resins, fillers, pigments, ultraviolet absorbers, light stabilizers, antioxidants, silane coupling agents, thickeners, and the like.

[0037] The composition may be substantially free of epoxy resin, for example, may be configured to contain no epoxy resin or to have an epoxy resin content of 3 mass% or less in 100 mass% of the primer composition. That is, the composition is configured to contain substantially no epoxy resin that reacts with the silicone-modified (meth)acrylic copolymer. This allows the formation of an uncured primer layer.

[0038] The viscosity of the composition at a liquid temperature of 25° C. is, for example, 50 mPa·s to 3000 mPa·s, preferably 200 mPa·s to 2000 mPa·s, and more preferably 700 mPa·s to 900 mPa·s. By setting the viscosity to be equal to or greater than the lower limit, film-forming properties can be improved. By setting the viscosity to be equal to or less than the upper limit, in-plane thickness variations can be suppressed. The viscosity in this embodiment can be measured by a standard method using a Brookfield viscometer (B-type rotational viscometer) at 25° C. and a rotation speed of 10 rpm. In addition, in this specification, the symbol "to" indicates that the upper and lower limits are included, unless otherwise specified.

[0039] The content of the non-volatile components in the composition is, for example, 20% by mass to 100% by mass, preferably 30% by mass to 70% by mass, and more preferably 40% by mass to 60% by mass. Within such ranges, film-forming properties and handling properties can be improved.

[0040] The surface protection method of this embodiment will be described.

[0041] An example of a surface protection method includes a step of applying the above-mentioned composition to the surface of a porous body such as a concrete structure and drying it to form a layer. When the composition is a primer composition, a primer layer can be formed on the surface of the porous body. The surface protection method may also include a step of applying a surface protection composition onto the primer layer and drying the composition to form a surface protection layer.

[0042] First, in the process of forming a primer layer, silanol groups and terminal hydroxyl groups formed by hydrolysis of reactive silyl groups (groups containing silicon atoms bonded to alkoxy groups) in the silicone-modified (meth)acrylic copolymer form hydrogen bonds, chemical bonds, etc. between the primer layer and a surface composed of an inorganic material such as concrete.

[0043] The primer composition may be configured so that it does not contain a crosslinking agent and / or a curing catalyst, or the content of the crosslinking agent and / or the curing catalyst is 10% by mass or less, preferably 3% by mass or less, based on 100% by mass of the primer composition. In other words, the primer composition is configured so that it does not substantially contain a crosslinking agent that reacts with the silicone-modified (meth)acrylic copolymer. This makes it possible to suppress the crosslinking reaction of the silicone-modified (meth)acrylic copolymer during the film formation process of the primer layer.

[0044] On the other hand, when the surface protection composition contains a modified silicone resin and a crosslinking agent that reacts with silanol groups, the crosslinking agent penetrates from the surface protection layer toward the uncured primer layer during the film formation process of the surface protection layer, and the silicone-modified (meth)acrylic copolymer in the primer layer, the crosslinking agent, and the modified silicone resin in the surface protection layer can form a three-dimensional network structure, thereby improving the adhesion between the surface protection layer and the primer layer. When the modified silicone resin in the surface protective layer contains a polyol in its main chain that has low adhesion to the (meth)acrylic main chain in the silicone modified (meth)acrylic copolymer, the crosslinking mechanism described above is effective in improving the adhesion between the two. Furthermore, if the surface protective layer contains a curing catalyst, this curing catalyst also permeates the uncured primer layer and accelerates the curing reaction of the silicone-modified (meth)acrylic copolymer itself, resulting in a primer layer with excellent mechanical strength.

[0045] Here, an example of the surface protecting composition will be described.

[0046] The modified silicone resin refers to a polymer having a reactive silyl group, and includes those in which a reactive silyl group is added to a polymer that serves as the main chain. The polymer to which the reactive silyl group is added is not particularly limited, but examples thereof include polyether polymers such as polyoxyethylene, polyoxypropylene, and polyoxybutylene; aliphatic hydrocarbon polymers such as polyisoprene, polyisobutylene, and polybutadiene; (meth)acrylic polymers such as poly(meth)acrylic acid and poly(meth)acrylate; and polyester polymers. These may be used alone or in combination of two or more.

[0047] As the crosslinking agent, for example, a silane coupling agent is used. Examples of silane coupling agents include aminosilane compounds such as 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; epoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane; vinylsilane compounds such as γ-(meth)acryloxypropyltrimethoxysilane; cationic silane compounds such as N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride; and phenylsilane compounds. The content of the crosslinking agent is preferably 0.1 to 7.5 mass %, more preferably 0.5 to 5.0 mass %, and further preferably 1.0 to 3.0 mass %, of the total amount of the resin composition.

[0048] In addition to the above components, the surface protection composition may contain one or more selected from the group consisting of a silicone resin other than the above modified silicone, a filler, a curing catalyst, an organic pigment, an inorganic pigment, an ultraviolet absorber, and a light stabilizer.

[0049] The filler may be an inorganic filler or an organic filler. The inorganic filler is not particularly limited, but examples thereof include silica; oxides such as alumina, titanium oxide, and magnesium oxide; carbonates such as calcium carbonate and magnesium carbonate; hydroxides such as aluminum hydroxide and magnesium hydroxide; and inorganic fibers such as glass fibers.

[0050] Among these, it is preferable to use one or more selected from the group consisting of silica particles, aluminum particles, and calcium carbonate particles. By using such a filler, dripping tends to be suppressed.

[0051] The average particle size of the filler is preferably 400 nm or less, more preferably 1 to 200 nm, even more preferably 1 to 100 nm, and even more preferably 1 to 50 nm. When the average particle size is within the above range, dripping tends to be suppressed. In this embodiment, the average particle size refers to the primary particle size on a volume basis. The primary particle size can be measured by a laser diffraction scattering method.

[0052] The content of the filler in the total amount of the resin composition is preferably 1.0 to 15 mass%, more preferably 1.5 to 10 mass%, and even more preferably 2.0 to 8.0 mass%. When the content of the filler is within the above range, dripping tends to be suppressed.

[0053] The curing catalyst is not particularly limited as long as it catalyzes the reaction of a reactive silyl group, and examples thereof include tin-based catalysts, titanium-based catalysts, aluminum-based catalysts, zinc-based catalysts, iron-based catalysts, and phosphorus-based catalysts.

[0054] The surface protection method may include a step of forming a topcoat layer on the surface protection layer (intermediate coat layer), which can further improve weather resistance and the like. The topcoat layer is not particularly limited, but may contain, for example, one or more selected from the group consisting of fluororesin, (meth)acrylic resin, (meth)acrylic silicone resin, (meth)acrylic urethane resin, urethane resin, olefin resin, vinyl acetate resin, ethylene-vinyl acetate copolymer resin, silicone resin, and modified resins thereof.

[0055] The surface protecting composition set of the present embodiment includes the above-mentioned primer composition and a surface protecting composition containing a modified silicone resin and a crosslinking agent that reacts with a silanol group. By carrying out a surface protection method using such a surface protection composition set, it is possible to improve both the adhesion of the primer layer to the porous body and the adhesion of the primer layer to the surface protection layer.

[0056] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0057] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0058] <Synthesis of silicone-modified methacrylic copolymer> (Silicone modified methacrylic copolymer A) 94 g of methyl methacrylate, 106 g of 3-(trimethoxysilyl)propyl methacrylate, 2 g of azobisisobutyronitrile, and 200 g of methyl isobutyl ketone were placed in a flask equipped with a stirrer, a condenser, and a thermometer, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer A having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer A had a weight average molecular weight of 35,000 in terms of polystyrene as measured by GPC, and n was 47 mol % and m was 53 mol % when n+m was 100 mol %.

[0059] [ka]

[0060] (Silicone modified methacrylic copolymer B) A flask equipped with a stirrer, a condenser, and a thermometer was charged with 50 g of methyl methacrylate, 18 g of 3-(trimethoxysilyl)propyl methacrylate, 72 g of butyl methacrylate, 54 g of 2-hydroxyethyl methacrylate, 6 g of 2-propenoic acid, 2-methyl-,3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl ester, and 2 g of azobisisobutyronitrile, along with 200 g of methyl isobutyl ketone, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer B having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer B had a weight average molecular weight of 17,000 in terms of polystyrene as measured using GPC, and when n+m+L+X+Z was taken as 100 mol%, n was 25 mol%, m was 36 mol%, L was 9 mol%, X was 27 mol%, and Z was 3 mol%.

[0061] [ka]

[0062] (Silicone-modified methacrylic copolymer C) A flask equipped with a stirrer, a condenser, and a thermometer was charged with 52 g of methyl methacrylate, 20 g of 3-(trimethoxysilyl)propyl methacrylate, 74 g of butyl methacrylate, 54 g of 2-hydroxyethyl methacrylate, and 2 g of azobisisobutyronitrile, and 200 g of methyl isobutyl ketone, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer C having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer C had a weight average molecular weight of 19,000 in terms of polystyrene as measured using GPC, and when n+m+L+X was taken as 100 mol%, n was 26 mol%, m was 37 mol%, L was 10 mol%, and X was 27 mol%.

[0063] [ka]

[0064] The proportions of each component in the silicone-modified methacrylic copolymers A to C obtained above were measured by NMR based on the information on the constituent compounds obtained by pyrolysis GC-MS according to the following conditions. The GC-MS conditions were as follows: Equipment: JMS Q1500GC&PY 3030E Pyrolysis furnace temperature: 600℃ GC inlet temperature: 280℃ Ion source temperature: 260℃ GC-IF temperature: 280℃ Ionization method: EI Column: ZB-5MS (20 m x inner diameter: 0.18 mm x film thickness: 0.18 μm) The NMR conditions were as follows: Equipment: Bruker AVANCE NEO Probe: CPBBO Deuterated solvent: CDCl3 As a pretreatment, 0.4 mL of deuterated chloroform was added to dissolve the sample.

[0065] <Adjustment of Composition> The obtained silicone-modified methacrylic copolymer A was added to and mixed with a solvent containing 50 mass % of methoxypropyl acetate (PGMAC, boiling point 146°C) to obtain composition A having a non-volatile component of 45% and a viscosity of 600 mPa·s. The obtained silicone-modified methacrylic copolymer B was added to the same solvent and mixed to obtain composition B having a non-volatile content of 50% and a viscosity of 800 mPa·s. The obtained silicone-modified methacrylic copolymer C was added to the same solvent and mixed to obtain composition C having a non-volatile content of 50% and a viscosity of 850 mPa·s.

[0066] [Table 1]

[0067] <Surface protection composition> 80 parts by mass of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502, viscosity at 25°C: 2000mPas, modified silicone resin having two or more silicon atoms bonded to methoxy groups at each end, having a polyoxypropylene structure as a polyether polymer, and having a dimethoxymethylsilyl group as a reactive silyl group), 20 parts by mass of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30, viscosity at 25°C: 30000mPas, modified silicone resin having one silicon atom bonded to a methoxy group at each end, having a polyoxypropylene structure as a polyether polymer, and having a dimethoxymethylsilyl group as a reactive silyl group), and 6 parts by mass of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18, average particle size: 10nm) were added and stirred for 5 minutes to obtain a base agent. The obtained base material and 3-aminopropyltrimethoxysilane, which is a crosslinking agent, were mixed in a mass ratio of 100:4 to prepare a surface protecting composition.

[0068] <Adhesion test> In accordance with JIS-A6909:2014, the adhesive strength (adhesion) of the above composition in the wet and dry states was measured according to the following procedure.

[0069] - Preparation of test boards Mortar prepared according to the method specified in JIS R 5201, 10.4 (How to prepare a test specimen) was molded using a metal formwork with inner dimensions of 70mm x 70mm x 20mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it was demolded and cured in water at 20±2°C for 6 days, and then left to stand in a curing room for a further 7 days or more.The bottom surface of the molded specimen was then polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface areas, and the surface was cleaned to prepare a test substrate.

[0070] -Preparation of test specimen The test substrate was immersed in water for one day, taken out of the water, and the water on the surface was wiped off (wet treatment). Immediately afterwards, any one of the compositions A to C obtained above was applied as a primer composition to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 ] and dried at 23°C and 50% relative humidity for 24 hours to form a primer layer. The surface protection composition obtained above was applied on the primer layer in a coating amount of 1.5 [kg / m 2 ] and left to stand at 23°C and 50% relative humidity for 7 days to form a surface protective layer, thereby preparing a wet test specimen. Furthermore, the composition and the surface protecting composition were similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment, to prepare a dry test specimen.

[0071] Adhesion strength measurement The wet test specimens were placed horizontally in a curing chamber and adhesive (solvent-free two-component epoxy resin adhesive, Konishi, Quickmender) was applied to the surface on which the primer layer was formed. A steel jig for upper tension was then gently placed on top and attached by lightly rubbing it, as shown in Figure 1(a), and any adhesive that had protruded out from the edges was wiped off. After leaving the specimens to rest for 24 hours, a tensile force was applied vertically to the surface of the specimen as shown in Figure 1(b), and the maximum tensile load (N) was determined for each of the three test specimens. The load rate until breakage was 1500 N / min. Adhesion strength (N / mm 2) is calculated using the formula "maximum tensile load (N) / 1600" and expressed as the average of three measured values. However, after making a 40 mm x 40 mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load was determined using the lower tensile steel jig and a steel backing plate.

[0072] From the results of the adhesion test described above, when the adhesion difference was calculated by dividing the "adhesion strength when dry" by the "adhesion strength when wet," if the adhesion difference exceeded 1.5, the adhesion to the porous body surface was judged to be poor, if it was between 1.2 and 1.5 or less, it was judged to be acceptable, and if it was 1.2 or less, it was judged to be excellent. In addition, when the fracture mode of the above adhesion test was confirmed, the fracture surface in Examples 1 and 2 was between the porous body surface and the primer layer, while the fracture surface in Comparative Example 1 was between the primer layer and the surface protection layer.

[0073] The compositions of Examples 1 and 2, as compared with Comparative Example 1, showed good adhesion to the porous body surface in adhesion tests under dry and wet conditions.

Claims

1. A composition for use in applying to a surface of a porous body, comprising: Contains a silicone modified (meth)acrylic copolymer, The silicone-modified (meth)acrylic copolymer is A structural unit N represented by the following general formula (N): A composition comprising, in a molecule, at least one of a structural unit O represented by the following general formula (O) and a structural unit P represented by the following general formula (P): [Formula 1] (In the above general formula (N), R 3 is a hydrogen atom or a methyl group, R 4 is an alkyl group having 1 to 3 carbon atoms, R 5 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, b is an integer of 1 to 6, and c is an integer of 1 to 3. [chemical 2] (In the above general formula (O), R 6 is a hydrogen atom or a methyl group, and d is an integer from 1 to 8. [C3] (In the above general formula (P), R 7 is a hydrogen atom or a methyl group, and Cf is -CF 3 or CHF 2 where e is an integer from 1 to 6, and f is an integer from 0 to 10.

2. 2. The composition of claim 1 , The content of the structural unit N contained in the silicone-modified (meth)acrylic copolymer is C N The content of the structural unit P is C p Then, C p / C N is greater than or equal to 0.001 and less than or equal to 1.

0.

3. 3. The composition according to claim 1 or 2, The content of the structural unit N contained in the silicone-modified (meth)acrylic copolymer is C N The content of the structural unit O is C O Then, C O / C N is 0.05 or greater and 5.0 or less.

4. 3. The composition according to claim 1 or 2, The silicone-modified (meth)acrylic copolymer has a structural unit M represented by the following general formula (M): [C4] (In the above general formula (M), R 1 is a hydrogen atom or a methyl group, R 2 is an alkyl group having 1 to 3 carbon atoms, and a is an integer from 0 to 3.

5. 3. The composition according to claim 1 or 2, The silicone-modified (meth)acrylic copolymer has a weight average molecular weight (Mw) of 500 or more and 50,000 or less.

6. 3. The composition according to claim 1 or 2, A composition comprising a solvent.

7. 3. The composition according to claim 1 or 2, A composition that is substantially free of epoxy resins.

8. 3. The composition according to claim 1 or 2, The composition, wherein the porous body is a concrete structure.

9. 3. The composition according to claim 1 or 2, The composition is a primer composition.

10. A surface protection method comprising the steps of applying the composition according to claim 1 or 2 to a surface of a porous body and drying the composition to form a layer.

11. Contains a silicone modified (meth)acrylic copolymer, The silicone-modified (meth)acrylic copolymer is A structural unit N represented by the following general formula (N): A composition comprising, in a molecule, at least one of a structural unit O represented by the following general formula (O) and a structural unit P represented by the following general formula (P): [C5] (In the above general formula (N), R 3 is a hydrogen atom or a methyl group, R 4 is an alkyl group having 1 to 3 carbon atoms, R 5 is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, b is an integer of 1 to 6, and c is an integer of 1 to 3. [C6] (In the above general formula (O), R 6 is a hydrogen atom or a methyl group, and d is an integer from 1 to 8. [C7] (In the above general formula (P), R 7 is a hydrogen atom or a methyl group, and Cf is -CF 3 or CHF 2 where e is an integer from 1 to 6, and f is an integer from 0 to 10.

Citation Information

Patent Citations

  • Method of enhancing deposition of organo polysiloxane elastomer

    JP1976149324A

  • Coating composition for building material

    JP1981057860A

  • Hard coat

    JP1996192097A

  • Primer for porous inorganic substrate

    JP1998195337A

  • Aqueous curable sealer and in-line coating process of ceramic base

    JP1999222586A