Selection method of modifier for improving fluidity of coal, modifier for improving fluidity of coal, method for modifying coal, and method for producing coke
By selecting modifiers based on solubility parameter and thermal stability criteria, low-caking coal is transformed into high-fluidity coal, addressing the scarcity and cost issues of high-caking coal in coke production, thereby enhancing coke strength and fluidity.
Patent Information
- Application Number
- JP2023052160
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
The challenge lies in improving the fluidity of low-caking coal to enhance its suitability as a raw material for producing high-strength coke, as high-caking coal is scarce and expensive, while low-caking coal is abundant but requires modification to meet the necessary fluidity and strength criteria for coke production.
A method for selecting a modifier using solubility parameter value δ and boiling point or decomposition start temperature T as indices, specifically compounds with 15.0≧δ≧11.0((cal/cm 3 ) 1/2 and T≧350(℃), such as nylon 66, to improve coal fluidity, which is then mixed with coal and carbonized at 350°C to enhance its fluidity and strength.
This approach allows for the efficient reforming of low-caking coal into high-fluidity coal, reducing production costs and enabling the production of high-strength coke with improved fluidity and strength, comparable to that produced using high-caking coal.
Smart Images

Figure 2024140816000004 
Figure 2024140816000005 
Figure 2024140816000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for selecting a modifier for improving the fluidity of coal, which improves the thermoplasticity and melting properties (hereinafter also referred to as "fluidity") of coal (including non- or slightly caking coal) used in coke production, a modifier selected by the selection method, a method for modifying coal using the modifier, and a method for producing coke. [Background technology]
[0002] Coke, which is charged into a blast furnace together with iron ore as a smelting raw material, is required to have high strength. In order to produce high-strength coke, it is desirable to use coal with high caking properties as the coke raw material. However, it is not the case that only coal with high caking properties is mined; coal with low caking properties is also mined. For this reason, it is common to blend multiple types (brands) of coal with different properties to produce a coal blend, and use the blended coal as the coke raw material.
[0003] Coal with high caking properties (also called "good quality caking coal" or "strong caking coal") is in short supply and generally expensive. On the other hand, coal with low caking properties is produced in large quantities and is relatively inexpensive. For this reason, using coal with low caking properties, so-called "non- or slightly caking coal," as a coke raw material is effective in making up for the shortage of good quality caking coal and reducing raw material costs. In order to increase the caking properties of non- or slightly caking coal so that it can be used as a coke raw material, an inexpensive and efficient modifier and modification process were needed.
[0004] Here, the caking property of coal refers to the property of coal melting and solidifying when carbonized, and is an essential property for producing coke. Caking property is determined by the characteristics of coal when it softens and melts (i.e., fluidity), so when evaluating the suitability of a certain brand of coal as a coke raw material, it is important to use the value (measured value or estimated value) related to the fluidity of that coal as an indicator.
[0005] As mentioned above, when producing coke for blast furnaces, etc., a coal blend consisting of multiple brands of coal is usually used, and various methods have been considered to estimate the strength of the coke produced from the coal blend. Among them, the "coke strength estimation method using matrix strength and fluidity as indicators" is commonly adopted. This method uses two indicators of coal properties, the vitrinite average maximum reflectance (Ro) and the Gieseler plastometer maximum fluidity (MF), as parameters to estimate the strength of coke made from the coal blend.
[0006] Specifically, two characteristics, the vitrinite average maximum reflectance (Ro) indicating the coalification degree of coal and the maximum fluidity (MF) indicating the caking property (particularly fluidity), are combined as factors when carbonizing coal to produce coke, and the strength of the produced coke is estimated based on this combination. In other words, in order to ensure the strength of the produced coke, raw coal is blended so that the vitrinite average maximum reflectance (Ro) and the maximum fluidity (MF) of the blended coal are within a predetermined range. Note that the maximum fluidity (MF), which indicates the fluidity of coal, is expressed as the number of rotations of the test stirrer (ddpm) or its common logarithm (logMF=log[ddpm]) due to the characteristics of the test method. Here, "ddpm" is an abbreviation for Dial Division per Minute, and the measurement method is specified in JIS M8801:2008.
[0007] In general, various coals are blended so that the logarithm of the maximum fluidity (logMF) of the coal blend, i.e., the weighted average of the logarithm of the maximum fluidity (logMF) of each of the raw coals to be blended, is within the range of 1.0 to 4.0, and preferably within the range of 2.0 to 3.5 (Non-Patent Document 1). However, the optimal range of the logarithm of the maximum fluidity (logMF) for the coal blend used may be outside the above range because it differs depending on the characteristics of the coke oven used and the coke production conditions.
[0008] Therefore, in order to produce high-strength coke, the fluidity of coal is a very important factor, and it is necessary to combine several brands and optimize the maximum fluidity (MF) of the coal blend. If the fluidity of the coal blend is insufficient, the strength of the produced coke will decrease (Non-Patent Document 1).
[0009] As mentioned above, there is a shortage of high-quality caking coal for producing coke, and development is underway on technologies to modify non- or slightly caking coal to have properties equivalent to or similar to those of high-quality caking coal, as well as technologies to produce high-strength coke using non- or slightly caking coal.
[0010] For example, Patent Document 1 describes that waste plastics are added to a coke oven for processing in order to reuse and recycle them from an environmental perspective, and that this processing improves the strength of the coke.
[0011] Patent Document 2 describes a method for producing coke having the required strength by heating a part or all of a coal blend at a heating rate of 40 to 1000°C / min to a temperature range of 250 to 350°C, and then cooling from the end temperature of the heat treatment to at least 100°C at an average cooling rate of 10°C / min or more (hereinafter referred to as rapid heat treatment), and adding waste plastics to the coal blend.
[0012] Furthermore, Patent Document 3 proposes a method of adding and mixing a heavy tar fraction with raw coal, and carbonizing the raw coal mixed with the heavy tar fraction to produce high-strength coke.
[0013] Patent Document 4 proposes a method for pre-treating raw coal as a method for improving and utilizing coal with low caking properties, in which non- or slightly caking coal is crushed and dried more finely than good-quality caking coal, and then mixed with binders such as tar, heavy oil, and pitches to form pseudo-particles. Patent Document 5 proposes a method for improving non-caking coal, in which non-caking coal is mixed with a non-hydrogen donor solvent to form a slurry, the slurry is heated to 300 to 420°C to perform solvent extraction, the heated slurry is separated into a liquid portion and a non-liquid portion, the solvent is separated from the liquid portion to obtain extracted coal, and non-extracted coal is obtained from the non-liquid portion, and the extracted coal, which has excellent softening fluidity, is appropriately blended with the non-extracted coal to obtain a coke raw material. In addition, Patent Document 6 and Patent Document 7 describe a method of efficiently modifying low-grade coal into artificial caking coal by heating low-grade coal containing a large amount of oxygen atoms together with heavy oils at a predetermined temperature, adhering decomposition products of heavy oils to the surface of the low-grade coal, and not generating a large amount of water during the treatment process. In addition, Patent Document 8 describes a method of modifying coal by adding a primary or secondary amine compound having an aromatic ring such as phenothiazine or carbazole. Furthermore, Patent Document 9 describes a technology of mixing a thermosetting composition with coal to obtain molded coke. In addition, Patent Document 10 describes a method of calculating the molecular surface area, molecular volume, and polarizability based on the molecular structure of the material to be selected, using a molecular orbital method, and selecting a compound having a value equal to or greater than a specific threshold value as a modifier.
[0014] In the coke manufacturing industry, the boundary between good quality caking coal and non- or slightly caking coal is not clearly defined. However, as described above, when manufacturing coke to be used in blast furnaces, etc., coal is often blended so that the logarithm of the maximum fluidity (logMF) is within the range of 1.0 to 4.0. Considering this, coal with a logarithm of the maximum fluidity (logMF) of 1.0 or less can be said to be a low-grade coal that is unsuitable for use alone as coke to be used in blast furnaces, etc. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] Japanese Unexamined Patent Publication No. 48-34901 [Patent Document 2] JP 2016-210866 A [Patent Document 3] Japanese Patent Application Publication No. 11-43675 [Patent Document 4] Japanese Patent Application Publication No. 10-183136 [Patent Document 5] JP 2006-70182 A [Patent Document 6] JP 2009-13222 A [Patent Document 7] JP 2009-13221 A [Patent Document 8] JP 2014-43545 A [Patent Document 9] JP 2016-56335 A [Patent Document 10] Patent Publication No. 2022-032852 [Non-patent literature]
[0016] [Non-Patent Document 1] Takashi Miyatsu et al., Nippon Kokan Giho, 67 (1975), p.125 [Non-Patent Document 2] Nomura, Seiji et al., Journal of the Japan Institute of Energy, 81 (2002), p.728 [Non-Patent Document 3] Yuzo Sanada, Fuel Association Journal, 57(1978), 1, p.5 [Non-Patent Document 4] James E. Mark, Physical Properties of Polymers Handbook 2nd ed., Springer, (2006), p.292-293 [Non-Patent Document 5] Chemical Society of Japan, 5th Edition, Experimental Chemistry Course 4: Basics IV Organic, Polymer, and Biochemistry, (2003), p.31 [Non-Patent Document 6] A. Miyakawa et al., Journal of the Fuel Association, 54 (1975), p.983 Summary of the Invention [Problem to be solved by the invention]
[0017] When low-rank coal is modified and the modified low-rank coal is used as a part or all of the raw coal to produce coke for use in blast furnaces, etc., it is desirable to carry out the modification process of the low-rank coal and the coke production process simultaneously from the viewpoint of improving productivity. In addition, a simple method is to mix or add a solid substance similar to coal, preferably a powder, as a modifier for coal to the coal.
[0018] On the other hand, from the viewpoint of using less expensive modifiers, a technology is conceivable in which low-rank coal is modified by adding waste plastic, which is a polymer compound, to a coke oven. This would make it possible to carry out the aforementioned low-rank coal modification process and coke production process simultaneously and inexpensively. However, in the past, the mainstream method for selecting solid modifiers was empirical, and there were few methods for selecting modifiers by taking into account specific physical property conditions. If it were possible to select modifiers by taking into account specific physical property conditions, it would be possible to select modifiers that meet the necessary addition conditions in the addition process in a short time, which would be advantageous in terms of cost and production time.
[0019] When the above-mentioned conventional techniques are examined from the above-mentioned viewpoints, Patent Document 1 describes that the strength of the obtained coke is increased by selecting a plastic that leaves fixed carbon when vaporized as an additive, and adding polyvinyl chloride or bakelite selected by the selection method to coal and carbonizing it. However, Non-Patent Document 2 reports that the fluidity of coal is reduced by adding polyvinyl chloride, and it is difficult to imagine that the coke strength is increased. Patent Document 9 describes that the coke strength is not increased by adding bakelite (phenolic resin) disclosed in Patent Document 1 to coal in a solid state, but is improved by the addition method of solidifying it from a liquid. In other words, it is impossible to select an additive that increases the coke strength by the selection method described in Patent Document 1. Also, Non-Patent Document 2, which investigated the effect of fluidity by adding various plastics to coal, reports that the addition of plastics to coal does not have the effect of improving the fluidity of coal.
[0020] Patent Document 2 describes a method for producing coke with a required strength by adding waste plastics to coal that has been subjected to rapid heat treatment. As reported in Non-Patent Document 2, adding plastics to coal reduces the strength of the coke. Patent Document 2 describes a coke production method in which the reduction in coke strength caused by the addition of such plastics is compensated for by increasing the fluidity of the coal in advance through rapid heat treatment. Therefore, it cannot be said that the increase in coke strength is due to the addition of plastics.
[0021] In Patent Document 3, a heavy tar fraction is added to raw coal and mixed, and the raw coal mixed with the heavy tar fraction is carbonized. Although it is a simple process, since liquid tar is used as a modifier, a mixing process using a dedicated mixing vessel is necessary. Patent Documents 4, 5, 6, 7, and 9 require treatment of coal before producing coke. Patent Document 8 is a technology for blending a solid substance with coal, but in order to use a large amount of modifier, it is necessary to manufacture (synthesize) it, which is expensive, and many problems remain for industrial practical use. Furthermore, the modifiers in Patent Documents 3 to 9 are empirically selected, and there is no description of a selection method based on physical property conditions, and the description is limited to compounds. As such, there are many points to be improved in the above conventional technology.
[0022] The method of Patent Document 10 has the advantage that it is highly accurate and can be performed in a short time because specific physical property values are calculated and used for selection. In addition, highly accurate selection results can be expected for compounds whose molecular weight can be accurately specified. On the other hand, when calculating a compound whose molecular weight is extremely large and generally expressed using an average molecular weight, for example, when selecting a modifier from polymer compounds, the physical property values obtained by calculation may exceed a threshold value depending on the molecular structure model used in the calculation, and there is a limit to obtaining highly accurate evaluation results.
[0023] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a method for selecting a modifier capable of improving the fluidity of coal, which is a necessary property for producing high-strength coke, from a wide range of compounds in a simple manner, and the modifier, and further to provide a method for modifying coal using the modifier. [Means for solving the problem]
[0024] As a result of intensive research, the present inventors have found specific physical property conditions for selecting a modifier to be added to coal or a coal blend that is a coke raw material to improve the fluidity of the coal, and a modifier having the specific physical property conditions, and have completed the present invention. The gist of the present invention for solving the above problems is as follows.
[0025] [1] A method for selecting a modifier for improving coal fluidity, comprising the steps of: selecting, as a modifier for improving the fluidity of coal, a compound whose solubility parameter value δ and the lower temperature T of either the boiling point or the decomposition onset temperature simultaneously satisfy the ranges of predetermined threshold values.
[0026] [2] The solubility parameter value δ and the lower temperature T of the boiling point or the decomposition onset temperature under a pressure of 1013 hPa are expressed by the following formula, 15.0 ≥ δ ≥ 11.0 ((cal / cm 3 ) 1 / 2 ) T≧350(℃) The method for selecting the modifier according to [1], wherein a compound that simultaneously satisfies the above requirements is selected as the modifier.
[0027] [3] The solubility parameter value δ and the lower temperature T of the boiling point or the decomposition temperature at a pressure of 1013 hPa are expressed by the following formula: 15.0 ≥ δ ≥ 11.0 ((cal / cm 3 ) 1 / 2 ) T≧350(℃) A coal fluidity improving modifier comprising a compound which simultaneously satisfies the above requirements.
[0028] [4] A method for modifying coal, comprising mixing the modifying agent according to [3] with coal and heating the mixture obtained to 350°C or higher.
[0029] [5] The method for modifying a blast furnace coke according to [4], wherein the mixture is used as a raw material for blast furnace coke.
[0030] [6] The method for modifying a fiber according to [4] or [5], wherein the modifier is nylon 66.
[0031] [7] A method for producing coke, comprising carbonizing a mixture of coal and the modifier described in [3] to produce coke.
[0032] [8] The method according to [7], wherein the mixture contains 30% by mass or less of the modifier relative to 100% by mass of the coal.
[0033] [9] The method according to [7] or [8], wherein the modifier is nylon 66. Effect of the Invention
[0034] According to the present invention, it is possible to select a modifier that improves the fluidity of coal in an extremely simple manner from compounds with a wide range of molecular weights, from low to high, using the solubility parameter value δ of the compound and the lower temperature T of either the boiling point or the decomposition start temperature as indicators. In addition, the coal used as a raw material for coke can be modified to have a higher maximum fluidity (MF) than that at the time of acquisition. Furthermore, when producing coke in a coke oven, it is possible to simultaneously modify the coal, and compared to the conventional technology, it is possible to realize the modification of coal simply and efficiently. This modification produces the same effect as securing coal with a high maximum fluidity (MF), and increases the degree of freedom in the blend design of multiple brands required for the production of high-strength coke. In addition, even if low-grade coal with poor fluidity is used, coke of the same quality as that produced using high-grade coal in the past can be produced, and the production cost of coke can be reduced. [Brief description of the drawings]
[0035] [Figure 1] 1 is a graph showing the relationship between the amount of modifier MA-2 added and the logarithm of maximum fluidity (logMF). [Diagram 2] 1 is a graph showing the relationship between the amount of modifier MA-2 added and the indirect tensile strength of cylindrical coke. [Diagram 3] 1 is a cross-sectional micrograph of coke with and without the addition of modifier MA-2. [Figure 4] 1 is a graph showing the strength (DI150 15) of coke obtained by carbonizing coal to which modifier MA-2 has been added. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The present invention will be described in detail below.
[0037] The present inventors have investigated a method for selecting a modifier and a method for modifying coal by adding various solids to the coal, in order to improve the fluidity of coal, that is, to increase the maximum fluidity (MF) in the Gieseler Plastometer, which is necessary for obtaining high-strength coke. As mentioned above, the maximum fluidity (MF) in the Gieseler Plastometer is generally adopted as one of the evaluation indexes of important coal properties that affect the quality of coke.
[0038] [How to select a modifier] The method for selecting a modifier for improving coal fluidity of the present invention is characterized in that a compound whose solubility parameter value δ (SP value) and the lower temperature T of either the boiling point or the decomposition onset temperature simultaneously satisfy the ranges of each of the predetermined threshold values is selected as a modifier for improving coal fluidity.
[0039] The reason why the selection method of the present invention can select a compound that can be used as a modifier based on the solubility parameter value δ (SP value) and the lower temperature T of the boiling point or the decomposition onset temperature is presumed to be as follows.
[0040] It is presumed that compounds that can be used as modifiers penetrate into coal constituent molecules when melted, and have the effect of widening the bond distance between coal constituent molecules. Therefore, it is considered that the greater the affinity between the modifier and coal when they soften and melt, the easier it is for the modifier molecules to penetrate into the coal constituent molecules, resulting in a more homogeneous mixture. A feature of the present invention is that the solubility parameter value δ (SP value) is used as an index for determining this affinity, and a modifier is selected that provides a close solubility parameter value δ (SP value) for the coal and modifier. In fact, the solubility parameter value δ (SP value) of practical coal is 11.0 (cal / cm) according to Van Krevelen's formula. 3 ) 1 / 2 Above, 15.0(cal / cm 3 ) 1 / 2 It is considered that if a compound has a solubility parameter value δ (SP value) within this range, it can be selected as a modifier that has a high affinity with coal and can be mixed homogeneously.
[0041] On the other hand, the carbonization temperature when producing coke is generally high, 1000 to 1300 ° C., but the effect of improving the fluidity of coal by the modifier is expressed in the temperature range of 350 ° C. or more and 550 ° C. or less. Therefore, a compound that can be used as a modifier needs to have a boiling point or decomposition start temperature of at least 350 ° C. or more at an atmospheric pressure of 1013 hPa. If the boiling point or decomposition start temperature of the modifier is lower than 350 ° C., the compound will be vaporized or decomposed to a lower molecular weight, and it is considered that the compound cannot enter the coal constituent molecules, or even if it can enter, the effect of widening the bond distance between the coal constituent molecules will be extremely lost. In addition, when both the boiling point and the decomposition start temperature of the compound are determined, the lower temperature is set as T, and the temperature T may be 350 ° C. or more. When either the boiling point or the decomposition start temperature of the compound is not determined, the temperature that is determined may be set as the temperature T.
[0042] From the above perspective, we selected a modifier with a focus on the solubility parameter value δ (SP value) and the boiling point or decomposition onset temperature T, and found that a compound that satisfies the following conditions is effective for improving the fluidity of coal. It was not previously known that a compound having the following properties has a coal-modifying effect, and the present invention provides a new method for selecting such a compound and a modifier.
[0043] <boiling point> An example of the method for measuring the boiling point in the present invention is a method for optically detecting bubbles using a boiling point measuring device and measuring the boiling point. The general procedure for measuring the boiling point using this device is as follows. To measure the boiling point (the temperature at which a phase transition from liquid to gas occurs), about 100 μL of the compound to be measured is weighed out and sealed in a glass tube. Next, in order to prevent measurement errors due to excessive heating of the measured object, a smaller capillary is inserted into the glass tube containing the measured object, and the glass tube is then installed in the measuring device to perform the measurement. In the measuring device, the glass tube is heated, and the generation of bubbles is observed as the temperature increases. The generated bubbles reflect the light of the built-in light source of the measuring device and are measured as the frequency of bubble generation, and the temperature at the time of bubble generation is defined as the boiling point. It should be noted that for high boiling point compounds, it is common to measure the air pressure inside the measuring device at a low pressure, in which case the air pressure is measured with a barometer built into the measuring device and converted into a value converted to atmospheric pressure (1013 hPa) to calculate the boiling point. In the present invention, the measurement method is not limited to the above-mentioned method, and any known method for measuring boiling point, such as differential analysis, differential scanning calorimetry, Siwoloboff method, distillation method, dynamic method (method of measuring recondensation temperature using a reflux condenser), may be used for measurement. In addition, the boiling point at atmospheric pressure (1013 hPa) described in known documents may be used, and if the boiling point at an atmospheric pressure different from atmospheric pressure is known, it may be converted to the boiling point at atmospheric pressure (1013 hPa) and used. The conversion method for this purpose is not limited to a specific method, but in the present invention, the boiling point conversion chart described in Non-Patent Document 5 was used to convert to the boiling point at atmospheric pressure (1013 hPa).
[0044] <Decomposition start temperature> In the selection method of the present invention, when a polymeric material or the like is used as a candidate modifier, the boiling point may not be clearly measured even if the above-mentioned boiling point measurement method is used. In that case, the decomposition start temperature may be measured instead of the boiling point, and the measured temperature may be used. One example of the method for measuring the decomposition start temperature in the present invention is a measurement method using pyrolysis gas chromatography / mass spectrometry (Pyro-GC-MS). In this measurement method, a measurement device consisting of a pyrolysis device, a gas chromatograph (GC), and a mass spectrometer (MS) is used, and the polymeric material is decomposed into small molecules while increasing the temperature in the pyrolysis device, and various types of decomposed small molecules are separated in a column by GC, and each separated component is detected by MS to identify the decomposition products associated with the increase in temperature. In addition, the measurement of the decomposition start temperature in the present invention is not limited to the above-mentioned method, and the decomposition start temperature may be measured using any known measurement method for the decomposition start temperature, such as a measurement method using an evolved gas analysis method (EGA-MS) or a measurement method using a simultaneous differential thermal-thermogravimetry (TG-DTA). In addition, the gas generated in the early stage after the start of the temperature rise is impurities such as solvent molecules and polymerization initiators attached during the synthesis of the polymer material. Therefore, in the present invention, the temperature at which a weight loss of 10% of the total weight loss when heated from room temperature to 800°C at a heating rate of 3 to 10°C / min using a thermobalance is observed is defined as the decomposition starting temperature.
[0045] <Solubility parameter value> The solubility parameter value δ (SP value) is a value defined by the regular solution theory introduced by Hildebrand, and is expressed as the square root of the cohesive energy density of the solvent and solute, and is a guide to the solubility of a two-component solution. Methods for calculating the solubility parameter value δ (SP value) include a method of calculating from the heat of evaporation, a method of calculating from the chemical composition, and a method of actually measuring from the compatibility with a substance whose solubility parameter value δ (SP value) is known. In the present invention, a value calculated by the group contribution method described in Non-Patent Document 4, which is an example of a method of calculating from the chemical composition, can be suitably used. In the calculation, Van Krevelen's parameters are used, and when some Van Krevelen's parameters cannot be obtained, Small's parameters are used for calculation. The density required for the calculation can be a value measured by a known method or a literature value. Note that the upper and lower limit values of the numerical range in the present invention are included in the equivalent range of the present invention even if they are slightly out of the numerical range specified by the present invention, as long as they have the same action and effect as those within the numerical range.
[0046] The solubility parameter value δ (SP value) of the compound selected as the modifier is, for example, 11.0 (cal / cm 3 ) taking into consideration the solubility parameter value δ (SP value) of coal by Van Krevelen described in Non-Patent Document 3. 3 ) 1 / 2 More than 15.0(cal / cm 3 ) 1 / 2 From the viewpoint of improving viscosity and fluidity, it is preferable that the viscosity is 11.2 (cal / cm 3 ) 1 / 2 More than 15.0(cal / cm 3 ) 1 / 2 Less than 11.3 (cal / cm 3 ) 1 / 2 More than 15.0(cal / cm 3 ) 1 / 2 More preferably, the solubility parameter value δ (SP value) is 11.0 (cal / cm 3 ) 1 / 2 Less than or equal to 15.0 (cal / cm 3 ) 1 / 2If it is larger, the affinity between the coal and the compound is small, making it impossible for the compound molecules to penetrate into the coal constituent molecules, and a sufficient effect of the addition cannot be obtained.
[0047] <Modifier> An example of a polymer compound that can be a modifier that satisfies the above parameters of the present invention is a polymer compound having a solubility parameter value δ (SP value) of 11.0 to 15.0 (cal / cm) calculated using a calculation formula based on the group contribution method (Non-Patent Document 4). 3 ) 1 / 2 Examples of suitable polyamide resins include polyamide resins having a solubility parameter δ (SP value) and a decomposition temperature of 350 (°C, 1013 hPa) or higher. The term "polyamide resin" refers to a resin formed by bonding a large number of monomers through amide bonds. In general, polyamides containing an aliphatic skeleton are collectively called "nylons," and polyamides consisting of only an aromatic skeleton are collectively called "aramids." Among these, nylon 6, nylon 66, nylon 11, nylon 12, nylon 610, nylon 612, nylon 46, nylon 6 / 66, nylon 6 / 66 / 12, nylon 6 / 66 / 610, nylon MXD6, nylon 6T, nylon 6 / 6T, nylon 6I, and nylon 9T have a high fluidity improving effect and are preferred as modifiers. As long as the solubility parameter value δ (SP value) and the decomposition temperature are within the numerical range specified by the present invention, the polyamide resins are not limited to those listed here, and any known compound may be used.
[0048] Another example of a polymer compound that can be a modifier that satisfies the above parameters of the present invention is a polymer compound having a solubility parameter value δ (SP value) of 12.39 (cal / cm) calculated using a formula based on the group contribution method (Non-Patent Document 4). 3 ) 1 / 2and a polyacetal resin (polyoxymethylene resin) having a decomposition onset temperature of 400 (℃, 1013 hPa). Polyacetal resin is a polymer having CHO (oxymethylene or formaldehyde) as a unit structure (monomer). Among them, a homopolymer of formaldehyde only, a copolymer in which (CHO) and (CHCHO) are copolymerized at a constant ratio, and the like, in which about 10 mol% of CHCHO (oxyethylene) is added as a monomer, and the like can be mentioned. Note that, as long as the solubility parameter value δ (SP value) and the decomposition onset temperature are within the numerical range specified by the present invention, the polyacetal resin is not limited to the polyacetal resins listed here, and any known compound may be used.
[0049] An example of the structure of a low molecular weight compound that can be a modifier that satisfies the above parameters of the present invention is a compound having a solubility parameter value δ (SP value) of 11.0 to 15.0 (cal / cm) calculated using a formula based on the group contribution method (Non-Patent Document 4). 3 ) 1 / 2 Examples of the compound include primary or secondary amine compound derivatives, phenothiazine derivatives, carbazole derivatives, indole derivatives, imidazole derivatives, pyrazole derivatives, and other heterocyclic compounds, aniline derivatives, hydrazone derivatives, aromatic amine derivatives, arylamine derivatives, and compounds in which a plurality of these compounds are bonded, or polymers having groups consisting of these compounds in the main chain or side chain, which are within the range of 100°C and have a boiling point of 350°C, 1013hPa or more. In particular, compounds having an aromatic amine skeleton, such as 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, N,N'-diphenyl-1,4-phenylenediamine, N,N',N''-triphenyl-1,3,5-benzenetriamine, N,N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-1,4-phenylenediamine (abbreviation: DNPD), and N-phenyl-1-naphthylamine (abbreviation: NPN), have a high fluidity improving effect and are preferred as modifiers. Phenothiazine, carbazole, etc. are also preferred. However, as long as the solubility parameter value δ (SP value) and boiling point are within the numerical ranges specified in the present invention, the compounds are not limited to those listed here, and any known low molecular weight compounds may be used.
[0050] In general, coal used as a raw material for coke used in blast furnaces and the like is said to begin to soften and melt at around 350° C. when heated, and the softening and melting temperature range is from 350° C. to 550° C. Therefore, it is believed that polyamide resins with relatively high melting points can melt into coal when the coal softens and melts.
[0051] In addition, polyamide resins such as nylon 66, nylon 6, and nylon 6T are used in various fields due to their excellent mechanical properties, heat resistance, chemical resistance, and other characteristics, and are also collected as waste plastics. Therefore, such waste polyamide resins discharged in large quantities as industrial waste or general waste may be recycled and used.
[0052] [Methods for improving coal and manufacturing coke] Hereinafter, an embodiment of the method for modifying coal (method for improving fluidity) by adding a modifier and the method for producing coke according to the present invention will be described.
[0053] The coal to be subjected to fluidity improvement (modification) is crushed to a particle size of 5.0 mm or less (undersize that passed through a sieve with a mesh size of 5.0 mm), preferably to a particle size of 5.0 mm or less, and further crushed so that at least 70 mass % of the coal has a particle size of 3.0 mm or less (undersize that passed through a sieve with a mesh size of 3.0 mm), and the powder of the modifier (including granular form) is mixed with this crushed coal. At this time, multiple modifiers may be added.
[0054] The mixture of this coal and the modifier powder is carbonized at a temperature of 350° C. or higher. Coal for coke used in blast furnaces and the like exhibits a fluidity phenomenon when heated to 350° C. or higher, and this fluidity is improved by the addition of the modifier.
[0055] When the modifier is added as a solid substance, for example, a powder, its particle size is not particularly limited, but if efficient modification is desired, the particle size is preferably small, for example, 10 mm or less, and more preferably 3 mm or less.
[0056] Furthermore, when a coal blend containing a plurality of brands is charged into a coke oven to produce coke, one or more types of modifier powder may be added to one or more brands of coal and then mixed, and the mixture of the modifier and coal may be used as the coal constituting the coal blend in the production of coke. When the mixture of the modifier powder and coal is heated and heated during carbonization in the coke oven, the fluidity of the mixture is improved by the modifier, and the mixture reacts with the other brands of coal to produce coke.
[0057] The carbonization temperature for producing coke is generally as high as 1000 to 1300°C, but the fluidity improving effect of the modifier is manifested in a temperature range of 350°C to 550°C, and the coal is sufficiently modified during the heating process during carbonization for producing coke. If the objective is to evaluate only the improvement in fluidity of coal by the modifier without carbonizing the coal into coke, a carbonization temperature of 350 to 550°C is sufficient. In this case, the carbonization time depends on the type of coal, etc., and can be appropriately determined by conducting an evaluation test using a small amount of the coal whose fluidity is to be improved in advance.
[0058] In addition, the modifier may be mixed with another compound within a range that does not impair the effect of the modifier, and the resulting mixture may be used as a flowability modifier. Furthermore, two or more different types of the modifier may be mixed and used.
[0059] The other compounds may be, for example, waste containing plastics or spare plastics discharged in large quantities as industrial waste or general waste. In this case, the plastics contained in the waste plastics are not particularly limited, but examples thereof include plastics such as polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC).
[0060] In the coal upgrading method according to the present invention, the coal to be upgraded is not limited, and can be any coal that is used as a raw material for coke used in blast furnaces, such as strong caking coal and non- or slightly caking coal. Note that in the present invention, it is practical to target a single non- or slightly caking coal having a small maximum fluidity (MF) value, or a blended coal containing several types of non- or slightly caking coal.
[0061] The amount of the modifier to be added to the coal to be modified does not need to have a lower limit because even a small amount is effective. However, since the effect of modifying tends to be greater when the amount added is large, the amount added is preferably 0.01% by mass or more relative to 100% by mass of the coal to be modified. Furthermore, since an amount exceeding 30% by mass increases the cost, the amount is preferably 0.01 to 30% by mass, and more preferably 0.2 to 30% by mass. When two or more different types of modifiers are mixed and used, the total amount of the modifiers should be within the above range.
[0062] As described above, the modifier may be added in a powder form, but the form in which it is added is not particularly limited. For example, the modifier may be added in a state in which it is formed into particles, may be added as a solution by dissolving it in a solvent, or may be added in a slurry form.
[0063] As described above, according to the present invention, the fluidity of coal used as a coke raw material can be modified to a different fluidity from that at the time of procurement, that is, to a coal having a larger maximum fluidity (MF) value than that at the time of procurement, by the simple method of adding the modifier to the coal. Furthermore, when producing coke in a coke oven, it is also possible to modify the coal simultaneously with the production of the coke, thereby realizing the improvement of coal fluidity and the production of high-strength coke more simply and efficiently than before. EXAMPLES
[0064] The present invention will be described in more detail below with reference to examples.
[0065] Table 1 below shows the compound names of MA-1 to MA-8, 17, and 18, which are examples of modifiers suitable for the present invention, and the comparative modifiers MA-9 to MA-16, as well as their solubility parameter values δ (SP values) calculated using the group contribution method (Non-Patent Document 4), and the lower temperature T of their boiling points or decomposition onset temperatures described in known documents, etc. The following compounds are exemplified to make the present invention more specific, and are not limited to the compounds shown in Table 1 as long as they do not deviate from the concept of the present invention, and any known compound may be used as long as it does not go against the spirit of the present invention.
[0066] [Table 1]
[0067] As shown in the following examples, the effect of improving Gieseler fluidity when the compounds shown in Table 1 were added to coal was measured, and it was confirmed that compounds that simultaneously satisfy the range of a predetermined solubility parameter value δ (SP value) and a temperature T, whichever is lower, of the boiling point or the decomposition onset temperature, have the effect of modifying coal.
[0068] [Example 1] An example of modifying the fluidity of coal by adding a modifier MA-1 (N,N'-diphenyl-1,4-phenylenediamine) is described below. The modifier MA-1 has a solubility parameter value δ (SP value) calculated using the group contribution method and the lower temperature T of either the boiling point or the decomposition onset temperature measured by experiment, whichever is lower, of 15.0 (cal / cm 3 ) 1 / 2 ≧δ≧11.0(cal / cm 3 ) 1 / 2 and T≧350(℃,1013hPa).
[0069] The fluidity-improving effect (modification effect) of adding modifier MA-1 to coal was confirmed by the following procedure. First, coal pulverized to a particle size of 425 μm or less according to JIS M8801 was mixed with commercially available MA-1 powder (hereinafter, for polymer, powder frozen and pulverized to 450 μm or less) to prepare a mixed sample of coal and MA-1. The amount of MA-1 powder mixed with coal was adjusted so that the mass ratio of MA-1 to 100 mass% of coal was 10 mass%.
[0070] This mixed powder was placed in a specified container specified by the Gieseler Plastometer method of JIS M8801, and this container was placed in a furnace preheated to 300°C based on JIS M8801, and the mixed powder was heated to 550°C at 3°C / min, thereby raising the temperature of the mixed powder to the softening and melting temperature range of coal. The maximum fluidity (MF) of coal was measured for this mixed sample in accordance with JIS M8801.
[0071] Additionally, the maximum fluidity (MF) of raw coal without MA-1 was also measured (in the present embodiment, one brand of coal alone, without a mixture of multiple brands, i.e., single coal, was used). The logarithm of the maximum fluidity (logMF) of the coal subjected to the upgrading test is shown in Table 2. As shown in Table 2 as "Logarithm of maximum fluidity (logMF) of raw coal," the logarithm of the maximum fluidity (logMF) of the coal subjected to the upgrading test was at most 1.26, and all raw coals were low-grade coals with low fluidity that made it impossible to produce high-strength coke as they were.
[0072] [Examples 2 to 10] The solubility parameter value δ (SP value) of the modifier MA-1 calculated using the group contribution method and the lower temperature T of the boiling point or decomposition onset temperature measured experimentally were 15.0 (cal / cm 3 ) 1 / 2 ≧δ≧11.0(cal / cm 3 ) 1 / 2 The maximum fluidity (MF) was measured in the same manner as in Example 1, except that the modifiers were changed to MA-2 to MA-8, 17, and 18 shown in Table 1, which simultaneously satisfied the conditions of T≧350 (° C., 1013 hPa).
[0073] [Comparative Examples 1 to 8] As a comparative example, instead of MA-1, the solubility parameter value δ (SP value) of each compound calculated using the group contribution method was δ>15.0 (cal / cm 3 ) 1 / 2 Or 11.0 (cal / cm 3 ) 1 / 2 MA-9 to MA-16, which satisfy the condition > δ, were added to coal in an amount of 10 mass% relative to 100 mass% of coal, and the maximum fluidity (MF) of coal was measured in accordance with JIS M8801 for these mixed samples.
[0074] Additionally, the maximum fluidity (MF) of raw coal without any modifier mixed therein was also measured in the same manner as in Example 1. The measurement results are shown in Table 2 together with the "logarithm of maximum fluidity of raw coal (logMF)." If the difference in the logarithm of maximum fluidity before and after modification (ΔlogMF) is a positive number, it is marked as "effective," if it is 0, it is marked as "no effect," and otherwise it is marked as "deteriorating effect." Furthermore, if the result of the maximum fluidity after modification is "immeasurable," it means that no fluidity was shown at all (MF=0ddpm), in other words, fluidity was lost.
[0075] [Table 2]
[0076] As shown in Table 2, it was found that by adding MA-1 to MA-8, 17, and 18 of Examples 1 to 10 to coal, the fluidity was improved in all cases, and the logarithm of the maximum fluidity (logMF) increased. This shows that MA-1 to MA-8, 17, and 18 are effective in improving the logarithm of the maximum fluidity (logMF), regardless of the magnitude of the logarithm of the maximum fluidity (logMF) of the raw coal. In other words, the improvement in the logarithm of the maximum fluidity (logMF) shows that the addition of the modifier makes it easier for coal to melt, and it can be said that the coking ability is improved.
[0077] In contrast to this, the modifiers MA-9 to MA-16 of Comparative Examples 1 to 8 did not change the fluidity of the coal, or even worsened it.
[0078] From the above results, it is found that the solubility parameter value δ (SP value) calculated using the group contribution method and the experimentally measured boiling point or decomposition onset temperature, whichever is lower, T, are within the range of 15.0 ≥ δ ≥ 11.0 ((cal / cm 3 ) 1 / 2 It was found that a modifier that simultaneously satisfies the conditions of T≧350(°C) and T≧350(°C) has the effect of improving the logarithm of the maximum fluidity (logMF) of coal. This modification effect was also confirmed for coals having a logMF higher than the logarithm of the maximum fluidity (logMF) of raw coal, 0.48 to 1.26, shown in Table 2. Therefore, it can be said that the modifier and modification method of the present invention are effective for any coal, but in terms of modifying coal with low fluidity, it is particularly effective to add a modifier to coal with a logMF of about 2.3 or less.
[0079] [Example 11: Amount of modifier added and effect of improving coal fluidity] The solubility parameter value δ (SP value) calculated using the group contribution method and the experimentally measured boiling point or decomposition onset temperature, whichever is lower, are 15.0 (cal / cm 3 ) 1 / 2 ≧δ≧11.0(cal / cm 3 ) 1 / 2The following describes examples (Examples 12 and 13) in which the maximum fluidity (logMF) was measured by changing the amount of modifier MA-2 (nylon 66) added, which simultaneously satisfies the conditions of 0°C and T≧350 (℃, 1013 hPa), and in which coke strength was measured. For the modification tests, coal was used that had a low maximum fluidity (logMF) of 0.3 or less, and from which it is difficult to produce high-strength coke by itself.
[0080] The effect of adding MA-2 on improving the fluidity of coal was confirmed by the following procedure. First, coal pulverized to a particle size of 425 μm or less according to JIS M8801 was mixed with MA-2 to prepare a mixed sample of coal and MA-2. The amount of MA-2 powder mixed with coal was adjusted so that the mass ratio of MA-2 to 100 mass% of coal was 0 (no addition), 0.2, 1, 5, 10, 20, or 30 mass%. The coals used were coal A with an MF of 2 ddpm (logMF=0.3) and coal B with an MF of 0 ddpm.
[0081] This mixed powder was charged into a specified container specified by the Gieseler Plastometer method of JIS M8801, and the container containing this mixed powder was charged into a furnace preheated to 300°C based on JIS M8801, and the mixed powder was heated to 550°C at 3°C / min, thereby raising the temperature of the mixed powder to the softening and melting temperature range of coal. The maximum fluidity (MF) of this mixed sample was measured in accordance with JIS M8801. The maximum fluidity (MF) of raw coal alone without mixing MA-2 was also measured.
[0082] FIG. 1 shows the relationship between the amount of MA-2 added and the logarithm of the maximum fluidity (logMF). In FIG. 1, when the MF is 0 ddpm, the logarithm of the maximum fluidity (logMF) cannot be shown, so for convenience, the position of 0 on the vertical axis is set to log0. In addition, in the measurement with an addition rate of 30% by mass, the maximum fluidity (MF) exceeded the upper measurement limit of 50,000 ddpm, so it could not be shown in FIG. 1, and the results were shown only in the range of addition rates of 0 to 20% by mass. In addition, in FIG. 1, logMF is shown as a constant value in the range where the amount of MA-2 added is small, but this is due to the fact that measurements are performed in 1 ddpm increments, and differences of less than 1 ddpm cannot be detected.
[0083] As shown in Figure 1, it was found that the fluidity of coal was improved significantly with increasing addition amount of MA-2.
[0084] In this way, it was found that application of the present invention makes it easy to select a modifier for improving the fluidity of coal, and that when the selected modifier is actually added to coal and heated, the flow characteristics of the coal are improved. In other words, the effectiveness of the method for selecting a modifier in the present invention was confirmed.
[0085] Furthermore, after producing coke using the modifier selected according to the present invention, its strength was confirmed by carrying out a simple carbonization test (Example 12) and a large-scale carbonization test (Example 13).
[0086] [Example 12: Measurement of coke strength by simple carbonization test] The simplified carbonization test was carried out as follows. Coal pulverized to a particle size of 500 μm or less was mixed with MA-2 to prepare a mixed sample of coal and MA-2. The amount of MA-2 powder mixed with coal was adjusted so that the mass ratio of MA-2 to 100 mass% of coal was 0 (no addition), 0.2, 1, 5, 10, 20, and 30 mass%. The same coals A and B as in Figure 1 were used.
[0087] A mixture of 1.0 g of dried coal and MA-2 (hereinafter, the unit is expressed as -dry) was filled into a mold with a diameter of 10 mm, and a pressure of 30 MPa was applied for 1 minute to obtain a cylindrical molded product. The molded product was heated to 900°C at a heating rate of 3°C / min in a N2 gas flow, and then held for 30 minutes to obtain a cylindrical coke. The strength of the obtained cylindrical coke was measured by applying a load from the side and measuring the pressure at which the coke broke as the indirect tensile strength, with reference to Non-Patent Document 6.
[0088] The test results are shown in Table 3 and Figure 2. Figure 2 shows the relationship between the amount of MA-2 added and the indirect tensile strength of the coke. As shown in Figure 2, the indirect tensile strength of both coal A and B improved from the addition of 0.2 mass%, and increased with the addition rate.
[0089] [Table 3]
[0090] In order to confirm the effect of MA-2 on coal, cross-sectional microscopic observations were performed on cylindrical cokes prepared with 0% and 30% MA-2 added. The microscopic photographs are shown in Figure 3. For both coal A and B, in the coke with 0% MA-2 added, melting between coal particles does not proceed easily, and most of the particles have an angular shape characteristic of coal. In contrast, in the coke with 30% MA-2 added, angular particles were hardly observed, and most of the particles had a structure in which the particles were fused together. Considering the amount of MA-2 added to the coal, it is thought that the amount added is too small to interpret that MA-2 remained between the coal particles after melting and bonded them together and solidified them. In other words, it is thought that the state shown in the microscopic photograph was formed because MA-2 penetrated into the coal molecules, modified the coal, and improved the fusibility of the coal itself.
[0091] [Example 13: Measurement of coke strength by large-scale carbonization test] The large-scale carbonization test was carried out as follows. Coal A (logMF=0.3) crushed to a particle size of 3 mm or less was mixed with MA-2 to prepare a mixed sample of coal and MA-2. The amount of MA-2 powder mixed with coal was adjusted so that the mass ratio of MA-2 to 100 mass% of coal was 0 (no addition), 2, 5 or 10 mass%. 12.2 kg-dry of the mixture of coal and MA-2 was poured into a SUS container at 750 kg-dry / m 3 The mixture was packed to a density of 1000g, carbonized at 1050℃ for 6 hours, and cooled in nitrogen to produce coke. The strength of the obtained coke was measured by the 150 rpm 15mm index (DI) specified in JIS K2151:2004. 150 15 ) was used for evaluation.
[0092] The test results are shown in Figure 4. Figure 4 shows the relationship between the amount of MA-2 added and coke strength (DI 150 15 ) is shown. As shown in Figure 4, coke strength increased with an increase in the addition rate of MA-2. The decomposition temperature of MA-2 is 450°C, and it is thought that most of it has decomposed at the carbonization processing temperature of 1050°C, but the addition of MA-2 increased coke strength. Therefore, from these results, it is thought that the action of MA-2 is not that it melts and remains between the coal particles, bonding them together, but that MA-2 reacts with the coal to modify it, increasing the fluidity of the coal, and as a result, improving the strength of the coke.
[0093] As described above, it was confirmed that the application of the present invention makes it easy to select a modifier for improving the fluidity of coal, and that the modifier actually selected has the effect of improving the fluidity of coal. In other words, the validity of the method for selecting a modifier in the present invention was confirmed. [Industrial Applicability]
[0094] According to the present invention, it is possible to very simply select a modifier for improving the fluidity of coal using the solubility parameter value δ (SP value) of the compound and the lower temperature T of either the boiling point or the decomposition initiation temperature as indicators. Furthermore, by the simple method of adding the selected modifier to coal, it is possible to improve the fluidity of coal used as a coke raw material to a fluidity different from that at the time of acquisition, that is, to coal having a higher logarithm of the maximum fluidity (logMF) compared to that at the time of acquisition. Furthermore, it is also possible to modify the coal in accordance with the production of coke in a coke oven, and it is possible to improve the fluidity of coal more simply and efficiently than before and produce high-strength coke.
Claims
1. A method for selecting a modifier for improving coal fluidity, comprising the steps of: selecting, as a modifier for improving coal fluidity, a compound whose solubility parameter value δ and the lower temperature T of either the boiling point or the decomposition onset temperature simultaneously satisfy the ranges of predetermined threshold values.
2. The solubility parameter value δ and the lower temperature T of the boiling point or the decomposition onset temperature under a pressure of 1013 hPa are expressed by the following formulas, respectively. 15.0≧δ≧11.0 ((cal / cm 3 ) 1/2 ) T≧350 (° C.) The method according to claim 1, wherein a compound that simultaneously satisfies the above is selected as the modifier.
3. The solubility parameter value δ and the lower temperature T of the boiling point or the decomposition onset temperature under a pressure of 1013 hPa are expressed by the following formulas, respectively. 15.0≧δ≧11.0 ((cal / cm 3 ) 1/2 ) T≧350 (° C.) A coal fluidity improving modifier comprising a compound which simultaneously satisfies the above requirements.
4. A method for modifying coal, comprising mixing the modifying agent according to claim 3 with coal and heating the resulting mixture to 350° C. or higher.
5. The method according to claim 4, wherein the mixture is used as a raw material for blast furnace coke.
6. 6. The method according to claim 4, wherein the modifier is nylon 66.
7. A method for producing coke, comprising carbonizing a mixture of coal and the modifier according to claim 3 to produce coke.
8. The method according to claim 7, wherein the mixture contains 30% by mass or less of the modifier relative to 100% by mass of the coal.
9. The method according to claim 7 or 8, wherein the modifier is nylon 66.
Citation Information
Patent Citations
Swelling agent screening method based on coal thermodynamic parameters
CN107121528A
Method for producing coke
JP2004168893A
Method for producing agglomerate including carbonaceous material for iron-making process
JP2005325435A
Method for reforming coal and method for producing coke
JP2014043545A
Method for producing coke, coke, modified coal, modified blended coal, and method for modifying coal or blended coal
JP2015040270A