Thermoplastic elastomer compositions and articles

A thermoplastic elastomer composition with specific components enhances the compatibility and mechanical properties of polypropylene and acrylic rubber, resulting in improved oil resistance, compression set resistance, and appearance in molded articles.

JP2024140818APending Publication Date: 2024-10-10RIKEN TECHNOS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052163
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Polypropylene and acrylic rubber have different affinities, making it difficult to disperse them uniformly, resulting in thermoplastic elastomers with poor compatibility and low mechanical properties.

Method used

A thermoplastic elastomer composition comprising carboxyl group-containing acrylic rubber, polypropylene polymer, epoxy-modified polypropylene, a crosslinking agent, and an ester or epoxy plasticizer, with specific ratios and properties to enhance compatibility and mechanical properties.

Benefits of technology

The composition achieves excellent oil resistance, compression set resistance, and mechanical properties, along with improved appearance in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140818000001
    Figure 2024140818000001
  • Figure 2024140818000002
    Figure 2024140818000002
  • Figure 2024140818000003
    Figure 2024140818000003
Patent Text Reader

Abstract

To provide a thermoplastic elastomer composition that is excellent in oil resistance, compression set resistance, and mechanical properties, and that provides excellent appearance (molding appearance) when molded into an article.SOLUTION: Selected is a thermoplastic elastomer composition that comprises at least: (a) 100 pts.mass of a carboxyl group-containing acrylic rubber; (b) 10 to 50 pts.mass of a polypropylene-based polymer; (c) 5 to 50 pts.mass of an epoxy-modified polypropylene; (d) 0.5 to 10 pts.mass of a crosslinking agent; and (e) 1 to 150 pts.mass of an ester-based plasticizer and / or an epoxy-based plasticizer, where the component (b) does not include the component (c).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic elastomer composition and articles comprising the same. [Background technology]

[0002] Elastomers (elastic polymeric materials) used in various industrial products are required to have various physical properties such as hardness, strength, low-temperature characteristics, oil resistance, moldability, etc., depending on the application. In order to achieve the desired physical properties, elastomers made of multiple materials (polymers, etc.) are also commonly used. However, depending on the type of material, multiple materials may not dissolve in each other, making it difficult to disperse them uniformly.

[0003] In such cases, it is known that the addition of a compatibilizer makes it possible to make the materials compatible and disperse them uniformly. Note that compatibilization does not only mean that multiple materials melt together at the molecular level, but also includes the dispersion of micro- or nano-sized material particles in other raw materials.

[0004] For example, the elastomers described in Patent Documents 1 and 2 below contain a graft copolymer as a compatibilizer for compatibilizing olefin resin and acrylic rubber. Although the compatibility between olefin resin and acrylic rubber is low, it is said that the use of a graft copolymer allows the two to be sufficiently dispersed, improving physical properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-277571 A [Patent Document 2] JP 2004-002743 A Summary of the Invention [Problem to be solved by the invention]

[0006] A compatibilizer functions as a compatibilizer due to its high affinity for each material to be made compatible. In other words, a compatibilizer does not function as a compatibilizer for every material, and must have an appropriate structure depending on the type of material to be made compatible.

[0007] Polypropylene is a polymeric material with excellent moldability and oil resistance, and is widely used industrially. On the other hand, acrylic rubber has high strength and excellent heat resistance. Therefore, it is believed that by thoroughly dispersing both polypropylene and acrylic rubber, it is possible to obtain an elastomer with excellent physical properties.

[0008] However, polypropylene and acrylic rubber have different affinities (compatibility parameters), making it difficult to disperse the two materials sufficiently as is. For this reason, thermoplastic elastomers consisting of polypropylene and acrylic rubber have poor compatibility and very low mechanical properties (tensile strength and tensile elongation). On the other hand, the reality is that no compatibilizer capable of sufficiently compatibilizing the two materials is known to date.

[0009] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a thermoplastic elastomer composition which is excellent in oil resistance, compression set resistance, and mechanical properties, and which gives an excellent appearance (molded appearance) when molded into an article, a crosslinked product thereof, and an article containing the crosslinked product. [Means for solving the problem]

[0010] As a result of extensive investigations, the present inventors have found that the above object can be achieved by using a specific thermoplastic elastomer composition.

[0011] That is, the present invention has the following aspects. [1] (a) 100 parts by mass of a carboxyl group-containing acrylic rubber; (b) 10 to 50 parts by mass of a polypropylene-based polymer; (c) epoxy-modified polypropylene, 5 to 50 parts by mass; (d) 0.5 to 10 parts by mass of a crosslinking agent; and (e) 1 to 150 parts by mass of ester plasticizer and / or epoxy plasticizer A thermoplastic elastomer composition comprising at least one of the following: However, the component (b) does not include the component (c). [2] The thermoplastic elastomer composition according to [1], wherein the acid value of the component (a) is 0.1 to 5 KOHmg / g. [3] The thermoplastic elastomer composition according to [1] or [2], wherein the component (d) is an epoxy group-containing acrylic resin. [4] The thermoplastic elastomer composition according to [3], wherein the epoxy group-containing acrylic resin has an epoxy index of 0.2 to 6 meq. / g. [5] The thermoplastic elastomer composition according to any one of [1] to [4], wherein the component (e) is a polyether ester plasticizer. [6] The thermoplastic elastomer composition according to any one of [1] to [5], further comprising (f) an antioxidant. [7] A crosslinked product of the thermoplastic elastomer composition according to any one of [1] to [6]. [8] An article comprising the crosslinked material described in [7]. Effect of the Invention

[0012] The thermoplastic elastomer composition of the present invention can give articles having excellent oil resistance, compression set resistance and mechanical properties, and the articles also have excellent appearance (molded appearance). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In the present invention, the numerical range expressed using "~" includes the numerical values ​​at both ends.

[0014] The present invention relates to a thermoplastic elastomer composition comprising at least (a) 100 parts by mass of a carboxyl group-containing acrylic rubber; (b) 10 to 50 parts by mass of a polypropylene-based polymer; (c) 5 to 50 parts by mass of an epoxy-modified polypropylene; (d) 0.5 to 10 parts by mass of a crosslinking agent; and (e) 1 to 150 parts by mass of an ester-based plasticizer and / or an epoxy-based plasticizer; and, as necessary, further comprising (f) an antioxidant, and an article comprising the thermoplastic elastomer composition. The components constituting the present invention are described in detail below.

[0015] <Thermoplastic elastomer composition> (a) Carboxyl group-containing acrylic rubber The component (a) contains a (meth)acrylic acid ester as a main monomer and a structural unit derived from a carboxyl group-containing monomer in an amount such that the acid value measured in accordance with JIS K0070-1992 is preferably 0.1 to 5 KOHmg / g, more preferably 0.2 to 2 KOHmg / g, and the Mooney viscosity (ML 1+4 150° C.) is preferably 15 to 40. Here, the term "main monomer" means that the content of structural units derived from the monomer is usually 50% by mass or more, preferably 60% by mass or more, and more preferably 65% ​​by mass or more. The term "(meth)acrylic acid ester" means "acrylic acid ester or methacrylic acid ester".

[0016] Examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl esters and (meth)acrylic acid alkoxyalkyl esters.

[0017] The (meth)acrylic acid alkyl ester is preferably an ester of an alkyl alcohol having 1 to 8 carbon atoms and (meth)acrylic acid. For example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate can be mentioned. Among these, ethyl (meth)acrylate and n-butyl (meth)acrylate are more preferable.

[0018] The above-mentioned (meth)acrylic acid alkoxyalkyl ester is preferably an ester of an alkoxyalkanol having 2 to 8 carbon atoms and (meth)acrylic acid. For example, methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, and 4-methoxybutyl (meth)acrylate can be mentioned. Among these, 2-ethoxyethyl (meth)acrylate and 2-methoxyethyl (meth)acrylate are more preferable, and 2-ethoxyethyl acrylate and 2-methoxyethyl acrylate are even more preferable.

[0019] As the (meth)acrylic acid ester, one or more of these can be used.

[0020] Examples of the carboxyl group-containing monomer include organic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and maleic acid; butenedioic acid monoalkyl esters such as maleic acid monobutyl ester and fumaric acid monobutyl ester; butenedioic acid monocycloalkyl esters such as maleic acid monocycloalkyl ester and fumaric acid monocycloalkyl ester; etc. One or more of these can be used as the carboxyl group-containing monomer.

[0021] The component (a) contains the structural unit derived from the carboxyl group-containing monomer in an amount such that the acid value measured by potentiometric titration in accordance with JIS K0070-1992 is preferably 0.1 to 5 KOHmg / g, more preferably 0.2 to 2 KOHmg / g. From the viewpoints of improving mechanical properties (tensile strength) and improving the appearance of molded articles, the acid value is preferably 0.1 KOHmg / g or more, more preferably 0.2 KOHmg / g or more. From the viewpoints of improving moldability and the appearance of molded articles, the acid value is preferably 5 KOHmg / g or less, more preferably 2 KOHmg / g or less.

[0022] Since the component (a) contains a carboxyl group derived from the carboxyl group-containing monomer, it reacts with the epoxy group of the component (c) to improve the heat resistance, oil resistance, compression set resistance, and mechanical properties.

[0023] In the polymerization of the above component (a), it is preferable to use a polyfunctional monomer having two or more vinyl groups as a monomer, which makes it possible to easily obtain a partially crosslinked product as described below.

[0024] Examples of the polyfunctional monomer having two or more vinyl groups include polyfunctional vinyl compounds such as divinylbenzene and 1,3,5-trivinylbenzene, diallyl compounds such as diallyl phthalate and diallyl fumarate, polyfunctional acrylates such as trimethylolpropane triacrylate and ethylene glycol dimethacrylate, etc. One or more of these can be used as the polyfunctional monomer having two or more vinyl groups.

[0025] The content of the structural unit derived from the polyfunctional monomer having two or more vinyl groups in the component (a) is preferably 1.5% by mass or less, more preferably 1% by mass or less, from the viewpoint of making the content of gel generated in the partially crosslinked product described below preferably 30% by mass or less, more preferably 25% by mass or less. Also, in order to easily obtain the partially crosslinked product, the content is usually 0.2% by mass or more, preferably 0.3% by mass or more.

[0026] In the polymerization of the above component (a), other monomers copolymerizable with the above-mentioned monomers (the above-mentioned (meth)acrylic acid esters, the above-mentioned carboxyl group-containing monomers, and the above-mentioned polyfunctional monomers having two or more vinyl groups) can be used as monomers in an amount such that the content of structural units derived from the monomers is usually 49.5 mass% or less, preferably 40 mass% or less, and more preferably 35 mass% or less.

[0027] Examples of the other monomers include conjugated diene monomers, non-conjugated diene monomers, aromatic vinyl monomers, α,β-ethylenically unsaturated nitrile monomers, amide group-containing (meth)acrylic monomers, polyfunctional di(meth)acrylic monomers, and α-olefin monomers.

[0028] Examples of the conjugated diene monomer include butadiene, chloroprene, and piperylene.

[0029] Examples of the non-conjugated diene monomer include 1,2-butadiene, 1,4-pentadiene, dicyclopentadiene, norbornene, ethylidenenorbornene, 1,4-hexadiene, and norbornadiene.

[0030] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, and divinylbenzene.

[0031] Examples of the α,β-ethylenically unsaturated nitrile monomer include acrylonitrile and methacrylonitrile.

[0032] Examples of the amide group-containing (meth)acrylic monomer include acrylamide and methacrylamide.

[0033] Examples of the α-olefin monomer include ethylene, propylene, 1-butene, 1-hexene, and 1-octene.

[0034] The other monomers may further include vinyl chloride, vinylidene chloride, vinyl acetate, ethyl vinyl ether, and butyl vinyl ether.

[0035] As the other monomer, one or more of these can be used.

[0036] The component (a) is preferably a partially crosslinked product of a polymer having the above-mentioned (meth)acrylic acid ester as a main monomer. This improves the miscibility with the component (b) and improves the mechanical properties and fatigue resistance. Furthermore, the partially crosslinked product is usually obtained as a powder (fine particles), which makes it easy to handle. The component (a) is more preferably the partially crosslinked product in which a gel is generated by partial crosslinking at a content of 10 to 30% by mass. Even more preferably, the partially crosslinked product in which a gel is generated by partial crosslinking at a content of 10 to 30% by mass, and the generated gel is uniformly dispersed.

[0037] By using the partially crosslinked product as the component (a), the components (a) and (b) can be easily dispersed well. Moreover, the components (a) and (b) are melt-kneaded in advance to disperse well, and then the components (c) and (d) are added and melt-kneaded, so that dynamic crosslinking between the components (a) and (b) can be efficiently performed.

[0038] The content of the gel in the component (a) (gel fraction) is preferably 35% by mass or less, more preferably 30% by mass or less, from the viewpoint of flexibility. There is no particular lower limit for the gel content, but it is usually 10% by mass or more, preferably 15% by mass or more.

[0039] In this specification, the content of the gel in the component (a) is calculated from the mass of the insoluble matter trapped on a 200-mesh wire screen after removing the solvent when 0.2 g of a sample is added to 200 ml of methyl ethyl ketone at 23° C. and stirred for 24 hours.

[0040] The partially crosslinked product may be crosslinked when melt-kneaded with the components (b), (c), and (d), but is preferably obtained by crosslinking before melt-kneading with the components (b), (c), and (d). Note that "partial crosslinking" means that the thermoplasticity is maintained even after the crosslinking reaction.

[0041] The form of the powder of the component (a) is not particularly limited and may be any. It may have a core-shell structure. The particle size of the powder is not particularly limited, but the average particle size at which the cumulative amount from the smallest particles is 50 mass % in a particle size distribution curve measured using a laser diffraction / scattering particle size analyzer is usually about 0.2 to 20 mm.

[0042] The Mooney viscosity (ML) of the above component (a) was measured according to JIS K6300-1-2013 using an L-shaped rotor with a preheating time of 1 minute, a rotor rotation time of 4 minutes, and a test temperature of 150°C. 1+4 150° C.) is preferably 15 to 40, more preferably 20 to 35, from the viewpoints of heat resistance, oil resistance, compression set resistance, and mechanical properties.

[0043] (b) Polypropylene-based polymer The polypropylene polymer of component (b) is a polymer mainly containing structural units derived from propylene. The component (b) contributes to heat resistance and moldability. Here, "mainly containing structural units derived from propylene" means that the content of structural units derived from propylene is usually 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and typically 75 to 100% by mass.

[0044] Examples of the component (b) include propylene homopolymers, random copolymers of propylene and small amounts of other α-olefin comonomers, and block copolymers of propylene and α-olefin comonomers.

[0045] Examples of the α-olefin comonomer include ethylene, 1-butene, 2-methyl-1-propene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-ethyl-1-butene, 2,3-dimethyl-1-butene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3,3-dimethyl-1-butene, 1-heptene, methyl-1-hexene, dimethyl Examples of the α-olefin comonomer include 1-pentene, ethyl-1-pentene, trimethyl-1-butene, methylethyl-1-butene, 1-octene, methyl-1-pentene, ethyl-1-hexene, dimethyl-1-hexene, propyl-1-heptene, methylethyl-1-heptene, trimethyl-1-pentene, propyl-1-pentene, diethyl-1-butene, 1-nonene, 1-decene, 1-undecene, and 1-dodecene. The α-olefin comonomer may be one of these or a mixture of two or more of them.

[0046] Specific examples of the random copolymer of propylene with a small amount of another α-olefin comonomer include propylene-ethylene random copolymer, propylene-1-butene random copolymer, propylene-1-hexene random copolymer, propylene-1-octene random copolymer, propylene-ethylene-1-butene random copolymer, propylene-ethylene-1-hexene random copolymer, and propylene-ethylene-1-octene random copolymer.

[0047] The block copolymer of propylene and an α-olefin comonomer is a copolymer composed of a crystalline polypropylene component and a copolymer rubber component of propylene and an α-olefin comonomer. The crystalline polypropylene component is composed of a propylene homopolymer or a random copolymer of propylene and a small amount of another α-olefin comonomer.

[0048] From the viewpoint of heat resistance, the above component (b) is preferably a propylene homopolymer or a block copolymer of propylene and an α-olefin comonomer in which the crystalline polypropylene component is a propylene homopolymer, and more preferably a propylene homopolymer.

[0049] Commercially available examples of the above component (b) include propylene homopolymer "VS200A (trade name)" manufactured by SunAllomer Co., Ltd. and propylene homopolymer "PM900A (trade name)" manufactured by SunAllomer Co., Ltd.

[0050] As the component (b), one or a mixture of two or more of these can be used.

[0051] From the viewpoint of molding processability, the component (b) preferably has a melt mass flow rate (MFR) of 0.1 to 100 g / 10 min, measured in accordance with JIS K 7210-1999 under conditions of 230° C. and 21.18 N.

[0052] From the viewpoint of heat oil resistance, the above component (b) has a peak top melting point of preferably 150° C. or higher, more preferably 160° C. or higher, of a peak appearing on the highest temperature side in a second melting curve (a melting curve measured during the final heating process) measured using a Diamond DSC type differential scanning calorimeter manufactured by PerkinElmer Japan Co., Ltd., with a program of holding at 230° C. for 5 minutes, cooling to −10° C. at 10° C. / min, holding at −10° C. for 5 minutes, and heating to 230° C. at 10° C. / min. The upper limit of the peak top melting point is not particularly limited, but for polypropylene polymers, it is at most 167° C.

[0053] The amount of the component (b) is 10 parts by mass or more, preferably 20 parts by mass or more, based on 100 parts by mass of the component (a), from the viewpoint of improving the fluidity and the appearance of the molded product. Also, from the viewpoint of suppressing the oil resistance, compression set resistance, and hardness, it is 50 parts by mass or less, preferably 40 parts by mass or less. When the amount of the component (b) is within the above range, a thermoplastic elastomer composition having an excellent balance between the fluidity, the oil resistance, and the compression set resistance can be obtained. However, the component (b) does not include the component (c) described later.

[0054] (c) Epoxy-modified polypropylene Component (c) is a polypropylene-based polymer containing an epoxy group. Component (c) improves the compatibility of components (a) and (b). Furthermore, component (c) contains an epoxy group, which reacts with the carboxyl group of component (a), improving the molded appearance and enhancing the mechanical properties.

[0055] The above component (c) can be obtained by copolymerizing a propylene monomer with a monomer having a glycidyl group or an epoxy group. The above component (c) can be obtained by modifying (graft polymerizing) a polypropylene homopolymer or copolymer with a monomer having a glycidyl group or an epoxy group by reacting it with an organic peroxide.

[0056] Examples of the polypropylene homopolymer or copolymer include the polypropylene-based polymers shown as component (b) above.

[0057] Examples of the monomer having a glycidyl group or an epoxy group include glycidyl (meth)acrylate, 4-hydroxybutyl acrylate glycidyl ether, and allyl glycidyl ether.

[0058] Organic peroxides can be used as polymerization initiators. Examples of the organic peroxides include peroxides such as di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, dicumyl peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide, and lauroyl peroxide; and azonitriles such as azobisisobutyronitrile and azobisisopropionitrile.

[0059] Specific examples of the component (c) include glycidyl (meth)acrylate-modified polypropylene, glycidyl (meth)acrylate-modified ethylene-propylene copolymer, glycidyl (meth)acrylate-modified ethylene-propylene-diene copolymer, etc. Among these, the component (c) is preferably at least one selected from the group consisting of glycidyl methacrylate-modified ethylene-propylene copolymer and glycidyl methacrylate-modified polypropylene, and more preferably glycidyl methacrylate-modified polypropylene (hereinafter sometimes abbreviated as GMA-modified polypropylene) from the viewpoint of fluidity and oil resistance.

[0060] The method for producing the above component (c) is not particularly limited, and examples thereof include a radical graft reaction (i.e., a reaction in which radical species are generated in the polymer that is to become the main chain, and a monomer is graft polymerized using the radical species as a polymerization initiation point).

[0061] The epoxy modification rate of the component (c) is preferably 1 to 20% by mass, and more preferably 2 to 10% by mass, from the viewpoints of molding processability and appearance of the molded product.

[0062] A commercially available example of the above component (c) is glycidyl methacrylate modified polypropylene "SCONA TPPP 8104 (product name)" manufactured by BYK Japan Co., Ltd.

[0063] The above component (c) can be used alone or in combination of two or more kinds.

[0064] A particularly preferred combination of the above component (b) and component (c) is a combination of a polypropylene homopolymer and a glycidyl methacrylate-modified polypropylene.

[0065] The amount of the component (c) is 5 parts by mass or more, preferably 10 parts by mass or more, based on 100 parts by mass of the component (a), from the viewpoints of improving fluidity, tensile strength, and the appearance of the molded product. Also, from the viewpoints of oil resistance, suppression of fluidity, suppression of hardness, and resistance to compression set, the amount is 50 parts by mass or less, preferably 30 parts by mass or less. When the amount of the component (c) is within the above range, a thermoplastic elastomer composition having an excellent balance between fluidity, oil resistance, and resistance to compression set can be obtained.

[0066] (d) Crosslinking Agent The component (d) is added to crosslink the component (a) carboxyl group-containing acrylic rubber, and has the function of crosslinking the acrylic rubber by covalently bonding with the carboxyl group of the acrylic rubber. As the component (d), an epoxy group-containing acrylic resin is preferred.

[0067] Examples of epoxy group-containing acrylic resins include epoxy group-containing acrylic copolymers obtained by copolymerizing an epoxy group-containing monomer having one epoxy group and one ethylenically unsaturated group such as a (meth)acryloyl group in one molecule, such as glycidyl (meth)acrylate or allyl glycidyl ether, with another polymerizable unsaturated monomer.

[0068] Examples of other polymerizable unsaturated monomers copolymerizable with the epoxy group-containing monomer include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, and lauryl (meth)acrylate; (meth)acrylic acid cycloalkyl esters such as cyclohexyl (meth)acrylate; (meth)acrylic acid hydrochlorides such as hydroxyethyl (meth)acrylate and hydroxybutyl (meth)acrylate; These include hydroxyl group-containing ethylenically unsaturated monomers such as hydroxyalkyl esters or adducts of these with ε-caprolactone; (meth)acrylic acid fluoroalkyl esters such as perfluorooctyl (meth)acrylate; vinyl aromatic compounds such as styrene and vinyl toluene; unsaturated nitrile compounds such as (meth)acrylonitrile; fluoroolefins such as tetrafluoroethylene, trifluorochloroethylene, vinylidene fluoride and vinyl fluoride; vinyl esters, olefin compounds, and the like, and these can be used alone or in combination of two or more.

[0069] The copolymerization of the epoxy group-containing monomer with the other polymerizable unsaturated monomer is not particularly limited, and can be carried out by any conventionally known method, such as solution polymerization, suspension polymerization, or emulsion polymerization.

[0070] The epoxy group-containing acrylic copolymer contains 5 to 60 mass %, preferably 15 to 55 mass %, and particularly preferably 20 to 50 mass %, of structural units derived from the epoxy group-containing monomer based on the mass of the copolymer.

[0071] An example of a commercially available example of the above component (d) is an epoxy group-containing acrylic-styrene resin "Marproof G0250SP (product name)" manufactured by NOF Corporation.

[0072] The above component (d) can be used alone or in combination of two or more kinds.

[0073] The epoxy index of the component (d) is measured using a potentiometric titrator according to JIS K7236:2001, and is preferably 0.2 meq. / g or more, more preferably 1.0 meq. / g or more, from the viewpoint of improving the tensile elongation and the appearance of the molded article, and is preferably 6.0 meq. / g or less, more preferably 4.0 meq. / g or less, from the viewpoint of improving the appearance of the molded article.

[0074] The amount of the component (d) is 0.5 parts by mass or more, preferably 1 part by mass or more, based on 100 parts by mass of the component (a) from the viewpoint of compression set resistance. Also, from the viewpoint of suppressing hardness and improving the appearance of the molded article, it is 10 parts by mass or less, preferably 3.6 parts by mass or less. When the amount of the component (d) is within the above range, a thermoplastic elastomer composition having an excellent balance between fluidity and compression set resistance can be obtained.

[0075] (e) Plasticizers The component (e) is a plasticizer. By using the component (e), the thermoplastic elastomer composition of the present invention has good tensile properties, compression set resistance, oil resistance, and molded appearance. Examples of the component (e) include ester-based plasticizers and epoxy-based plasticizers.

[0076] Examples of the ester plasticizer include phthalate plasticizers, adipate plasticizers, trimellitate plasticizers, sebacate plasticizers, polyester plasticizers, and polyether ester plasticizers.

[0077] Examples of phthalate plasticizers include dibutyl phthalate, butylhexyl phthalate, diheptyl phthalate, di(2-ethylhexyl) phthalate, diisononyl phthalate, diisodecyl phthalate, diundecyl phthalate, ditridecyl phthalate, dilauryl phthalate, dicyclohexyl phthalate, and dioctyl terephthalate.

[0078] Examples of the adipate plasticizer include bis(2-ethylhexyl) adipate, dioctyl adipate, diisononyl adipate, and diisodecyl adipate.

[0079] Examples of trimellitic acid ester plasticizers include tri(2-ethylhexyl) trimellitate, tri(n-octyl) trimellitate, and tri(isononyl) trimellitate.

[0080] Examples of the sebacic acid ester plasticizer include dibutyl sebacate and dioctyl sebacate.

[0081] Examples of polyester plasticizers include polyesters in which ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,5-hexanediol, 1,6-hexanediol, neopentyl glycol, or the like is used as a polyhydric alcohol, and oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, trimellitic acid, pimelic acid, suberic acid, maleic acid, azelaic acid, sebacic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, or the like is used as a polycarboxylic acid, and where necessary, a monohydric alcohol or a monocarboxylic acid is used as a stopper.

[0082] Examples of the polyether ester plasticizer include polyesters of polyethers such as polyethylene glycol and polypropylene glycol and the above polyvalent carboxylic acids.

[0083] Epoxy plasticizers include epoxidized soybean oil, epoxidized linseed oil, epoxidized fatty acid octyl esters, and epoxidized fatty acid alkyl esters.

[0084] Of these, the component (e) is preferably a phthalate ester plasticizer, an adipate ester plasticizer, a polyether ester plasticizer, or an epoxy plasticizer, with a polyether ester plasticizer being more preferred.

[0085] Commercially available examples of the above component (e) include a polyether ester plasticizer "RS735 (trade name)" from Adeka Corporation, a phthalate ester plasticizer "Sansocizer DOP (trade name); di(2-ethylhexyl) phthalate" from New Japan Chemical Co., Ltd., an adipate ester plasticizer "W320 (trade name)" from Dainippon Ink Co., Ltd., and an epoxy plasticizer "O-130P (trade name); epoxidized soybean oil" from Adeka Corporation.

[0086] As the component (e), one or a mixture of two or more of these can be used.

[0087] The amount of the component (e) is usually 1 part by mass or more, preferably 10 parts by mass or more, based on 100 parts by mass of the component (a), from the viewpoints of oil resistance, compression set resistance, and suppression of hardness, while it is usually 150 parts by mass or less, preferably 100 parts by mass or less, from the viewpoints of tensile strength, suppression of flowability, and improving the appearance of the molded article.

[0088] (f) Antioxidants The thermoplastic elastomer composition of the present invention may further contain the above-mentioned component (f) as desired, to the extent that it does not contradict the object of the present invention. By using an antioxidant, it is possible to improve heat resistance and suppress discoloration and resin deterioration due to heat history.

[0089] Examples of the antioxidant include phenol-based antioxidants such as 2,6-di-tert-p-butyl-p-cresol, 2,6-di-tert-butylphenol, 2,4-dimethyl-6-tert-butylphenol, 4,4-dihydroxydiphenyl, tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, phosphite-based antioxidants, thioether-based antioxidants, etc. Among these, phenol-based antioxidants and phosphite-based antioxidants are preferred.

[0090] An example of a commercially available example of the above component (f) is the antioxidant "Irganox (registered trademark) B225" manufactured by BASF.

[0091] As the component (f), one or a mixture of two or more of these can be used.

[0092] The amount of the component (f) is preferably 0.1 part by mass or more, more preferably 0.2 part by mass or more, based on 100 parts by mass of the component (a) in terms of improving heat resistance, while it is preferably 2.0 parts by mass or less, more preferably 1.0 part by mass or less, in terms of bloom resistance.

[0093] The thermoplastic elastomer composition of the present invention may further contain, as desired, inorganic fillers, various weather resistance agents such as antioxidants, hydrolysis inhibitors, light stabilizers, and ultraviolet absorbers, various lubricants such as modified silicone oils, silicone oils, waxes, acid amides, fatty acids, and fatty acid metal salts, various nucleating agents such as aromatic phosphate metal salts and gelols, various antistatic agents such as glycerin fatty acid esters, and various organic and inorganic flame retardants, to the extent that the purpose of the present invention is not adversely affected. Note that these additives are preferably highly compatible with the thermoplastic elastomer composition of the present invention in order to prevent problems such as bleeding out and blooming on the surface of the molded article.

[0094] In the thermoplastic elastomer composition of the present invention, the blending ratio of the above-mentioned components (c) and (d) to the above-mentioned component (a) (in other words, the blending ratio of the carboxyl group of the component (a) to the epoxy group of the components (c) + (d)) is usually 5% or more, preferably 10% or more, from the viewpoint of improving compatibility, while it is usually 60% or less, preferably 50% or less, from the viewpoint of hardness and moldability.

[0095] In the thermoplastic elastomer composition of the present invention, the blending amounts of the above components (b) and (c) are preferably 25 parts by mass or more, more preferably 30 parts by mass or more, based on 100 parts by mass of the above component (a), from the viewpoints of flowability and molded appearance, while being preferably 100 parts by mass or less, more preferably 50 parts by mass or less, from the viewpoints of hardness, oil resistance and compression set resistance.

[0096] (Method of producing thermoplastic elastomer composition) The thermoplastic elastomer composition of the present invention can be obtained by adding the above components (a) to (e), the optional component (f) used as desired, and other optional components simultaneously or in any order, and melt-kneading them using any kneader.

[0097] From the viewpoint of ensuring that components (c) and (d) function properly, the melt-kneading is preferably carried out at a temperature of 180° C. or higher for 1 minute or longer, and more preferably at a temperature of 190° C. or higher for 1 minute or longer. The melt-kneading temperature may be usually 240° C. or lower, preferably 220° C. or lower, from the viewpoints of mechanical properties, manufacturability of the composition, and moldability.

[0098] Examples of the melt kneader include batch kneaders such as pressure kneaders and mixers; extrusion kneaders such as single screw extruders, co-rotating twin screw extruders, and counter-rotating twin screw extruders; and calendar roll kneaders. These may be used in any combination. The obtained composition can be pelletized by any method and then molded into an article by any method.

[0099] The pelletization can be carried out by a method such as hot cutting, strand cutting, and underwater cutting.

[0100] <Goods> The article of the present invention contains the above-mentioned thermoplastic elastomer composition. The thermoplastic elastomer composition of the present invention has excellent oil resistance, compression set resistance, and mechanical properties, and can provide an excellent appearance (molded appearance) when molded into an article, and therefore can be suitably used as a material for sheet or film molded products, in-vehicle parts, oil-resistant and chemical-resistant tubes and hoses, etc.

[0101] That is, examples of the articles of the present invention include sheet or film molded products, vehicle mounted parts, oil-resistant and chemical-resistant tubes and hoses, etc.

[0102] The article of the present invention can be obtained by molding the thermoplastic elastomer composition of the present invention into a desired shape by any molding method, such as blow molding, extrusion molding, injection molding, press molding, compression molding, or a combination of two or more of these.

[0103] As described above, the thermoplastic elastomer composition of the present invention uses epoxy-modified polypropylene as a compatibilizer between the carboxyl group-containing acrylic rubber and the polypropylene-based polymer, and dynamically crosslinks the carboxyl group-containing acrylic rubber and the polypropylene-based polymer. In addition, the crosslinking density is further increased by the reaction between the crosslinking agent and the carboxyl group-containing acrylic rubber. As a result, the carboxyl group of the acrylic rubber reacts with the epoxy-modified polypropylene or the epoxy group of the crosslinking agent, and the crosslinked rubber of the polypropylene (fluid phase) is finely dispersed, improving the compatibility between the carboxyl group-containing acrylic rubber and the polypropylene-based polymer. Therefore, the thermoplastic elastomer composition of the present invention is superior in oil resistance, compression set resistance, and mechanical properties compared to a composition to which epoxy-modified polypropylene is not added as a compatibilizer, and an excellent appearance (molded appearance) can be obtained when the article is molded. EXAMPLES

[0104] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0105] <Ingredients used> (a) Carboxyl group-containing acrylic rubber: (a-1) OMNOVA's "SaniGum P95 (product name)". Acid value 0.8 KOHmg / g, Mooney viscosity (ML 1+4 150℃)30, molecular weight 140000, gel content 28% by mass.

[0106] (b) Polypropylene-based polymer: (b-1) Polypropylene homopolymer "VS200A (product name)" from SunAllomer Co., Ltd. Melt mass flow rate: 0.45 (g / 10 min), melting point: 164°C.

[0107] (c) Epoxy-modified polypropylene (c-1) SCONA TPPP 8104 (product name) is a glycidyl methacrylate (GMA) modified polypropylene (PP) from BYK Japan Co., Ltd. Epoxy index (FA) 0.2 meq. / g, epoxy modification rate (GMA content): 2.5 mass%.

[0108] (c) Comparative components: (c'-1) Ethylene-glycidyl methacrylate (E-GMA) copolymer "Bondfast (registered trademark), BF-E (product name)" manufactured by Sumitomo Chemical Co., Ltd. (c'-2) DOW maleic acid modified polypropylene "FUSABOND (registered trademark), P353 (product name)".

[0109] (d) Crosslinking Agent (d-1) NOF Corporation's epoxy group-containing acrylic-styrene resin "Marploop G0250SP (product name)". Weight average molecular weight (Mw): 20,000, epoxy index: 3.2 (meq. / g), glass transition temperature (Tg): 74 (℃).

[0110] (d-2) Epoxy group-containing monomer (diethylene glycol diglycidyl ether) "SR-2EG (product name)" from Sakamoto Pharmaceutical Co., Ltd. Epoxy index (=1000 / epoxy equivalent) 6.7 meq / g (d-3) Epoxy group-containing monomer (diethylene glycol diglycidyl ether) "SR-3EG (product name)" from Sakamoto Pharmaceutical Co., Ltd. Epoxy index (=1000 / epoxy equivalent) 0.1 meq / g

[0111] (e) Plasticizers: (e-1) ADEKA Corporation’s polyether polyester plasticizer “ADEKA Cizer RS-735 (product name).” (e-2) New Japan Chemical Co., Ltd.'s phthalate ester plasticizer (di(2-ethylhexyl) phthalate: DOP) "Sansocizer DOP (product name)". (e-3) Adipate ester plasticizer “W320 (product name)” by Dainippon Ink Co., Ltd. (e-4) ADEKA Corporation’s epoxidized soybean oil “O-130P (product name).”

[0112] (e) Comparison component: (e'-1) Paraffinic mineral oil "Diana Process Oil PW-100 (product name)" from Idemitsu Kosan Co., Ltd.

[0113] (f) Antioxidants (f-1) Phenolic antioxidant “Irganox (registered trademark) B225 (product name)” from BASF Japan Ltd.

[0114] <Measurement method> (1)Melt Mass Flow Rate (MFR): Using the composition obtained below, measurements were carried out under conditions of 230°C and 10 kg in accordance with JIS K 7112. (Judgment criteria) An MFR in the range of 3 to 200 (g / 10 min) was deemed acceptable, with a more preferable range being 5 to 80 (g / 10 min).

[0115] (2)Hardness: Using the composition obtained below, an injection molding machine with a clamping pressure of 120 tons was used to produce an injection sheet with a length of 13 cm, width of 13 cm, and thickness of 2 mm at a molding temperature of 250°C. A press sheet with a thickness of 6 mm was produced using the obtained injection sheet. The obtained press sheet was used as a sample and the durometer hardness (type A) was measured after 15 seconds according to ASTM D2240. (Judgment criteria) A hardness in the range of 50 to 95 was considered acceptable. A more preferable range is 50 to 92.

[0116] (3) Tensile test: In accordance with JIS K 6251-2010, a No. 3 dumbbell punched out from the 2 mm thick injection sheet obtained above was used as a test piece, and measurements were performed at a tensile speed of 500 mm / min. (Judgment criteria) A tensile strength of 4 MPa or more was considered acceptable, with a more preferable range being 5 MPa or more. A tensile elongation of 85% or more was considered acceptable, with a more preferable range being 120%.

[0117] (4) Compression set (resistance to compression set under high temperature conditions): In accordance with JIS K 6262-2003, the specimen was subjected to a compressive deformation of 25%, and the measurement was carried out at a temperature of 70°C for 22 hours. (Judgment criteria) A compression set of less than 80% was considered acceptable, with a more preferable range being less than 75%.

[0118] (5) Oil resistance (oil resistance in high temperature environments): In accordance with JIS K 6258-2003, test pieces were punched out from the 2 mm thick injection sheet obtained above, and the volume swelling ratio was measured after immersion in IRM#903 oil at a temperature of 120° C. for 22 hours. (Judgment criteria) For oil resistance, a volume expansion rate of less than 30% by volume was deemed acceptable, with a more preferable range being less than 21% by volume.

[0119] (6) Evaluation of molded appearance: The surface of the strand during the production of the composition was visually observed and touched with the hand, and was judged according to the following criteria. (Judgment criteria) ○: The surface of the strand is smooth. △: The surface of the strand is slightly rough (rough). ×: Significantly poor appearance such as scales was observed on the surface of the strand.

[0120] <Examples 1 to 21 and Comparative Examples 1 to 11> The components in the amounts (parts by mass) shown in any one of Tables 1 to 5 were melt-kneaded using an apparatus equipped with a twin-screw extruder with a diameter of 28 mm and an L / D of 42 manufactured by Japan Steel Works, Ltd., and a water-cooled strand-cut type granulator, at a screw speed of 600 rpm and an extruder outlet temperature of 200°C, to obtain pellets of the composition. The above tests (1) to (6) were carried out. The results are shown in any one of Tables 1 to 5.

[0121] [Table 1]

[0122] [Table 2]

[0123] [Table 3]

[0124] [Table 4]

[0125] [Table 5]

[0126] The thermoplastic elastomer composition of the present invention is excellent in mechanical properties, resistance to compression set in a high-temperature environment, oil resistance, and molded appearance, whereas the comparative examples are insufficient in at least one of the mechanical properties, resistance to compression set in a high-temperature environment, oil resistance, and molded appearance.

Claims

1. (a) 100 parts by mass of a carboxyl group-containing acrylic rubber; (b) polypropylene-based polymer: 10 to 50 parts by mass; (c) epoxy-modified polypropylene: 5 to 50 parts by mass; (d) 0.5 to 10 parts by mass of a crosslinking agent; and (e) Ester-based plasticizer and / or epoxy-based plasticizer: 1 to 150 parts by mass A thermoplastic elastomer composition comprising at least one of the following: However, the component (b) does not include the component (c).

2. The thermoplastic elastomer composition according to claim 1, wherein the acid value of the component (a) is 0.1 to 5 KOHmg / g.

3. The thermoplastic elastomer composition according to claim 1 , wherein the component (d) is an epoxy group-containing acrylic resin.

4. The thermoplastic elastomer composition according to claim 3, wherein the epoxy group-containing acrylic resin has an epoxy index of 0.2 to 6 meq. / g.

5. The thermoplastic elastomer composition according to claim 1 , wherein the component (e) is a polyetherester plasticizer.

6. 10. The thermoplastic elastomer composition of claim 1, further comprising: (f) an antioxidant.

7. A crosslinked product of the thermoplastic elastomer composition according to any one of claims 1 to 6.

8. An article comprising the crosslinked product according to claim 7.

Citation Information

Patent Citations

  • Thermoplastic resin composition

    JP1991014855A

  • Thermoplastic elastomer composition and its production

    JP1995003090A

  • Thermoplastic resin composition

    JP2001187830A

  • Thermoplastic elastomer composition

    JP2016145265A

  • Olefinic thermoplastic elastomer and its molded product

    JP2003277571A