Plastic optical fiber, optical cord, and active optical cable
The POF design with a specific refractive index distribution and trench configuration enhances bandwidth and reduces bending loss over short distances, addressing the limitations of existing POFs with trenches.
Patent Information
- Application Number
- JP2023052389
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Plastic optical fibers (POFs) with trenches to reduce bending loss experience a reduction in bandwidth due to light reflection, especially at short distances, with existing technologies failing to improve bandwidth over short distances effectively.
A POF design with a core having a first region with decreasing refractive index and a second region with a constant index, surrounded by a trench with a lower refractive index, where the second region thickness is between 2 μm and 5 μm, effectively confining light within the core to minimize reflection and maintain high bandwidth.
The POF achieves a high bandwidth of 40 MHz·km or more over short distances of 5 m or less while maintaining low bending loss, suitable for short-distance applications.
Smart Images

Figure 2024140985000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to plastic optical fibers, optical cords, and active optical cables. [Background technology]
[0002] An optical fiber includes a central core that transmits light, and a region called a cladding or trench that is provided around the core and serves to confine light within the core.
[0003] There are two types of optical fibers: plastic optical fiber (hereinafter referred to as "POF"), whose core is made of a resin material, and glass optical fiber (hereinafter referred to as "GOF"), whose core is made of a glass material. POF is more flexible than GOF, and has better bending resistance (i.e., flexibility) and workability than GOF. Therefore, POF is generally used for short-distance applications at the end of optical fiber transmission networks (e.g., household wiring, etc.).
[0004] There are two types of POF: SI (step index) type POF and GI (graded index) type POF. SI type POF is a POF with a uniform refractive index of the core. GI type POF is a POF with a refractive index distribution in which the refractive index of the core decreases from the center of the core to the outer edge of the core. With SI type, the propagation time differs depending on the optical path (mode), so the signal pulse spreads and the bandwidth is low. In contrast, GI type POF has a high bandwidth and enables high-speed communication because the propagation time difference is significantly reduced due to the refractive index distribution.
[0005] In addition, in GI POF, in order to reduce bending loss and enable a wider range of light to be received (i.e., to achieve a larger numerical aperture (NA)), a trench is provided around the core that is optically designed to have a lower refractive index than the refractive index of the outer edge of the core.
[0006] For example, Patent Document 1 discloses a multimode optical fiber that is strong against bending and suppresses the influence of leaky modes, which is realized by optical design of a trench. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-527547 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, trenches provided for the purpose of reducing bending loss, etc., reduce the bandwidth due to the reflection of light incident on the trench. The reduction in bandwidth due to light reflection on the trench is significant when the POF distance is short, and the effect becomes smaller as the POF distance becomes longer. This is because when light is guided through the POF, components of the light that cause the bandwidth reduction, such as light that enters the POF at an angle larger than the numerical aperture (NA) of the POF and scattered light, are lost. In other words, the longer the POF distance, the fewer the components of the light that reduce the bandwidth.
[0009] As mentioned above, POF is generally used for short distances (for example, 1m to 100m), and is susceptible to optical components that reduce the bandwidth over shorter distances. However, no technology has been proposed to date that focuses on improving the bandwidth over short distances for POF, particularly for POF with a trench to reduce bending loss.
[0010] The present disclosure has an object to provide a POF having an improved bandwidth over a short distance with respect to a POF having a trench for improving bending loss, and further has an object to provide an optical cord and an active optical cable including such a POF having an improved bandwidth over a short distance. [Means for solving the problem]
[0011] The POF according to the first aspect of the present disclosure is A core, A trench disposed on the outer periphery of the core; Equipped with The core is a first region having a refractive index n1 that decreases in a direction from the center to the outer edge; a second region located on the outer periphery of the first region, including the outer edge of the core, and having a constant refractive index n2; having the refractive index n2 of the second region is equal to or less than the refractive index n1 of the first region, The thickness of the second region is equal to or greater than 2 μm and less than 5 μm, The refractive index n3 of the trench is lower than the refractive index n2 of the second region.
[0012] An optical cord according to the second aspect of the present disclosure includes the POF according to the first aspect of the present disclosure.
[0013] An active optical cable according to a third aspect of the present disclosure includes the optical cord according to the second aspect of the present disclosure and an optical / electrical hybrid module. Effect of the Invention
[0014] According to the present disclosure, it is possible to provide a POF having an improved bandwidth over a short distance. Furthermore, the present disclosure can provide an optical cord and an active optical cable including a POF having such an improved bandwidth over a short distance. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram showing an example of a cross-sectional structure of a POF according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a graph illustrating a refractive index profile of a POF according to an embodiment of the present disclosure. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a cross-sectional structure of a modified example of a POF according to an embodiment of the present disclosure. [Figure 4] FIG. 4 is a schematic cross-sectional view showing an example of a manufacturing apparatus that can be used to manufacture the POF according to the embodiment of the present disclosure. [Diagram 5] FIG. 5 is a schematic diagram illustrating an example of an optical code according to an embodiment of the present disclosure. [Figure 6] FIG. 6 is a schematic diagram illustrating an example of an active optical cable according to an embodiment of the present disclosure. [Figure 7] FIG. 7 is a schematic diagram showing a measurement system for measuring bending loss of a POF in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] (definition) In this specification, the refractive index refers to a value measured by the prism coupler method.
[0017] In this specification, the term "optical loss when a plastic optical fiber (POF) is bent into a U shape with a bending radius R mm" refers to the optical loss determined by the following procedure. (a) Connect a light source to the input side of the POF (length: 5 m) and connect an optical power meter to the receiving side of the POF. (b) A 1m section on the input side of the POF is wrapped 10 times around a φ12.5mm cylinder to eliminate cladding modes. (c) The center part (2.5 m part) of the POF is set on a plate with a U-shaped groove of bending radius R and the POF is bent. (d) Check the change in insertion loss caused by changing from a straight state to a bent state, and calculate the optical loss.
[0018] (Embodiments of the present disclosure) A POF according to an embodiment of the present disclosure will be described.
[0019] Fig. 1 is a schematic diagram showing an example of a cross-sectional structure of a POF according to an embodiment of the present disclosure, and Fig. 2 is a graph showing a refractive index profile of the POF according to an embodiment of the present disclosure.
[0020] The POF 10 according to this embodiment includes a core 11 and a trench 12 disposed on the outer periphery of the core 11. The core 11 includes a first region 111 and a second region 112. The first region 111 has a refractive index n1 that decreases in a direction from the center 11a toward the outer edge 11b of the core 11. The second region 112 is located on the outer periphery of the first region 111, includes the outer edge 11b of the core 11, and has a constant refractive index n2. The refractive index n2 of the second region 112 is equal to or lower than the refractive index n1 of the first region 111. The thickness of the second region 112 is equal to or greater than 2 μm and less than 5 μm. The refractive index n3 of the trench 12 is lower than the refractive index n2 of the second region 112 of the core 11. The refractive indexes of the core 11 (the first region 111 and the second region 112) and the trench 12 are the refractive indexes for light having a wavelength (e.g., 850 nm) that propagates through the core 11.
[0021] In the POF 10 according to this embodiment, the refractive index n1 of the first region 111 of the core 11 has a refractive index distribution. Therefore, the POF 11 according to this embodiment is a GI type. Specifically, as shown in FIG. 2, the center of the first region 111 of the core 11 has the maximum refractive index, and the refractive index of the first region 111 gradually decreases toward the second region 112. The refractive index of the second region 112 is constant. Here, "the refractive index of the second region 112 is constant" means that the difference between the maximum refractive index and the minimum refractive index of the second region 112 is 0.005 or less. Furthermore, the refractive index of the trench 12 may also be constant, for example. "The refractive index of the trench 12 is constant" means that the difference between the maximum refractive index and the minimum refractive index of the trench 12 is 0.005 or less. As shown in FIG. 2, the POF diameter means the diameter of the POF having the core 11 and the trench 12. Also, the vertical axis in FIG. 2 means the relative height of the refractive index.
[0022] The POF 10 according to the present embodiment has a configuration in which a second region 112 having a constant refractive index n2 that satisfies the relationship of n1≧n2>n3 is provided between a first region 111 (refractive index n1) of the core 11 having a refractive index distribution and a trench 12 (refractive index n3) provided to confine light in the core 11. Furthermore, the thickness of the second region 112 is 2 μm or more and less than 5 μm. This configuration can prevent light propagating through the core 11 from reaching the trench 12, that is, prevent light from entering the trench 12. Therefore, the POF 10 according to the present embodiment can suppress a decrease in the bandwidth due to reflection of light entering the trench 12. As a result, the POF 10 according to the present embodiment can achieve a low bandwidth over a short distance while having a low bending loss.
[0023] Here, a short-distance POF is, for example, a POF of 30 m or less, preferably a POF of 10 m or less, and more preferably a POF of 5 m or less. A short-distance POF is, for example, 1 m or more.
[0024] The POF 10 according to this embodiment can achieve a -1.5 dB bandwidth value of 40 MHz·km or more when overfill light is incident at 5 m, for example. Thus, the POF 10 according to this embodiment can achieve a high bandwidth of 40 MHz·km or more even at a very short distance of 5 m. The bandwidth of the POF 10 according to this embodiment is a value measured by a pulse method among the methods compliant with IEC60793-1-41, and is performed under excitation conditions of all-mode excitation using overfill light. Overfill light is light whose numerical aperture (NA) of incident light is larger than the numerical aperture (NA) of the POF to be measured, and whose beam diameter is larger than the core diameter of the POF to be measured.
[0025] Here, in this specification, the core diameter of the POF refers to the outer diameter of the core. The outer diameter of the core is the diameter at 5% light intensity measured by the near-field pattern method (hereinafter referred to as the "NFP method") using light with a wavelength of 850 nm among the methods conforming to IEC60793-1-20 and IEC60793-2-40 subcategory A4h. The diameter at 5% light intensity refers to the diameter of an approximate circle specified by a point having 5% light intensity of the peak light intensity. Also, the point with 100% brightness means the point with the highest brightness in the core. The outer edge 11b of the core 11 can be specified by the same method as the core diameter, that is, the NFP method.
[0026] In the POF 10 according to this embodiment, the first region 111 and the second region 112 of the core 11 can be specified by using the NFP method, similarly to the above-mentioned method for measuring the core diameter of the POF. The refractive index in the core 11 can be confirmed by the surface distribution of the light intensity of the emitted light obtained by measurement by the NFP method. Therefore, by using the surface distribution of the intensity of the emitted light to differentiate the surface distribution and obtain an inflection point, it is possible to distinguish the first region 111 having a refractive index distribution from the second region 112 having a constant refractive index. The outer edge of the second region 112 is the outer edge 11b of the core 11, that is, corresponds to the interface (core / trench interface) between the core 11 and the trench 12. Therefore, the second region 112 is a region between the inflection point and the core / trench interface. The outer diameter of the first region 111 can be specified by the inflection point, and the outer diameter of the second region 112 can be specified by the core / trench interface. By specifying the outer diameters of each region, the thickness of the second region 112 can be obtained.
[0027] The outer diameter of the trench 12 can also be determined using the NFP method, similar to the core diameter.
[0028] The refractive index n1 of the first region 111 of the core 11, the refractive index n2 of the second region 112, and the refractive index n3 of the trench 12 can be obtained by the following method. Using the core material and the trench material, a sheet-shaped test piece is prepared by hot pressing. Using the test piece, the refractive index of the core material and the trench material is obtained by the prism coupler method. Next, the aperture angle is measured by the far-field pattern method to obtain the refractive index difference between the core and the trench. Then, referring to 2.4 of the paper (Tachibana Mitsuhiro, "Method of Measuring the Refractive Index Distribution of Optical Fibers," Applied Physics, Vol. 48, No. 8), the refractive index n1 of the first region 111 of the core 11, the refractive index n2 of the second region 112, and the refractive index n3 of the trench 12 are calculated.
[0029] In the POF 10 according to this embodiment, the first optical loss when bent into a U-shape with a bending radius of 1.5 mm is preferably 3.0 dB or less, more preferably 1.0 dB or less. The POF 10 according to this embodiment is a POF in which the core 10 is made of a resin material, so that the bending loss is lower than that of a GOF, and furthermore, since the POF 10 according to this embodiment is provided with a trench 12, the bending loss can be suppressed to within the above range. With this configuration, the POF 10 according to this embodiment can realize a high bandwidth in a short distance while suppressing the bending loss to within the above range. The first optical loss is, for example, 0.5 dB or more, 0.7 dB or more, or 0.75 dB or more. The method for measuring the first optical loss, which is the bending loss, will be described in the examples below.
[0030] In the POF 10 according to this embodiment, the second optical loss when bent into a U-shape with a bending radius of 2.0 mm is preferably, for example, 0.5 dB or less. With this configuration, the POF 10 according to this embodiment can achieve a high bandwidth over a short distance while suppressing the bending loss to within the above range. The second optical loss is, for example, 0.1 dB or more, 0.3 dB or more, or 0.4 dB or more. A method for measuring the second optical loss, which is the bending loss, will be described in the examples below.
[0031] In order to further improve the bandwidth, the thickness of the second region 112 in the core 11 of the POF 10 according to this embodiment is preferably, for example, 2.9 μm or more and 4.8 μm or less. In order to further improve the bandwidth, the thickness of the second region 112 is more preferably 2.9 μm or more and 4.5 μm or less. In order to further improve the bandwidth, the thickness of the second region 112 is more preferably 3.5 μm or more and 4.4 μm or less.
[0032] The POF 10 according to the present embodiment can achieve a large numerical aperture (NA) by providing the trench 12. Therefore, the POF 10 according to the present embodiment can receive light in a wider range. The POF 10 according to the present embodiment has a numerical aperture (NA) of, for example, 0.190 or more and 0.235 or less.
[0033] Each component of the POF 10 of this embodiment will be described in more detail below.
[0034] (Core 11) The core 11 is a region that transmits light. As described above, the core 11 has the first region 111 having a refractive index distribution (refractive index n1) and the second region 112 having a constant refractive index n2. The refractive indices of the first region 111 and the second region 112 (i.e., the refractive indexes n1 and n2) are higher than the refractive index n3 of the trench 12. With this configuration, the light that enters the core 11 is confined inside the core 11 by the trench 12 and propagates through the POF 10.
[0035] Core 11 includes a first resin. Core 11 may include the first resin as a main component. Here, "core 11 includes the first resin as a main component" means that the component contained in core 11 in the largest amount by mass ratio is the first resin. Core 11 may include 75% by mass or more of the first resin, 80% by mass or more, or 85% by mass or more.
[0036] The core 11 may further contain an additive in addition to the first resin. The additive is, for example, a refractive index adjuster. That is, the core 11 may be formed of a resin composition containing the first resin and an additive such as a refractive index adjuster. As the refractive index adjuster, for example, a known refractive index adjuster used in the material of the core 11 of the POF 10 may be used. The material of the core 11 may contain an additive other than the refractive index adjuster.
[0037] The first region 111 of the core 11 has a refractive index distribution in which the refractive index decreases in the direction from the center 11a to the outer edge 11b of the core 11. Such a refractive index distribution can be formed, for example, by adding a refractive index adjuster to the first resin and diffusing (for example, thermally diffusing) the refractive index adjuster in the first resin. The second region 111 of the core 11 having a constant refractive index n2 can be formed, for example, by adjusting the conditions (for example, diffusion temperature and diffusion time) when diffusing (for example, thermally diffusing) the refractive index adjuster in the first resin, or the discharge amount of the core material when the POF 10 according to this embodiment is manufactured by a melt spinning method.
[0038] The first resin contained in the core 11 is not particularly limited as long as it is a resin having high transparency. Examples of the first resin include fluorine-containing resins, acrylic resins such as methyl methacrylate, styrene resins, and carbonate resins.
[0039] The first resin contained in the core 11 may be at least one selected from the group consisting of a fully fluorinated resin, a partially fluorinated resin, a partially chlorinated resin, and a partially deuterated resin. The partially fluorinated resin, the partially chlorinated resin, and the partially deuterated resin refer to resins known in the art as a core material for POF, in which some of the hydrogen atoms in the C-H bonds are substituted with fluorine, chlorine, and deuterium, respectively. The fully fluorinated resin refers to resins known in the art as a core material for POF, in which all of the hydrogen atoms in the C-H bonds are substituted with fluorine. Examples of resins known in the art as a core material include acrylic resins such as methyl methacrylate, styrene resins, and carbonate resins, as described above. A polymer having an aliphatic ring structure, such as a polymer having a dioxolane structure, may be used.
[0040] The first resin is preferably at least one selected from the group consisting of fully fluorinated resins and partially fluorinated resins, that is, the first resin is preferably a fluorine-containing resin.
[0041] The first resin of core 11 is preferably a fluororesin containing a fluoropolymer. Hereinafter, the fluororesin contained in core 11 will be referred to as a first fluororesin, and the fluoropolymer contained in the first fluororesin will be referred to as a first fluoropolymer.
[0042] The first fluorine-containing polymer contained in the first fluorine-containing resin preferably does not substantially contain hydrogen atoms from the viewpoint of suppressing light absorption due to the stretching energy of C-H bonds, and it is particularly preferable that all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms. That is, it is preferable that the first fluorine-containing polymer does not substantially contain hydrogen atoms and is fully fluorinated. In this specification, the term "the fluorine-containing polymer does not substantially contain hydrogen atoms" means that the content of hydrogen atoms in the fluorine-containing polymer is 1 mol% or less.
[0043] The first fluorine-containing polymer preferably has a fluorine-containing alicyclic structure. The fluorine-containing alicyclic structure may be contained in the main chain of the fluorine-containing polymer, or may be contained in a side chain of the first fluorine-containing polymer. The first fluorine-containing polymer has, for example, a constitutional unit (A) represented by the following structural formula (1). [ka]
[0044] In formula (1), R ff 1 ~R ff 4 R each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms. ff 1 and R ff 2 may be linked to form a ring. "Perfluoro" means that all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms. In formula (1), the number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1. The perfluoroalkyl group may be linear or branched. Examples of the perfluoroalkyl group include a trifluoromethyl group, a pentafluoroethyl group, and a heptafluoropropyl group.
[0045] In the formula (1), the number of carbon atoms in the perfluoroalkyl ether group is preferably 1 to 5, and more preferably 1 to 3. The perfluoroalkyl ether group may be linear or branched. Examples of the perfluoroalkyl ether group include a perfluoromethoxymethyl group.
[0046] R ff 1 and R ff 2When they are linked to form a ring, the ring may be a 5-membered ring or a 6-membered ring. Examples of the ring include a perfluorotetrahydrofuran ring, a perfluorocyclopentane ring, and a perfluorocyclohexane ring.
[0047] Specific examples of the structural unit (A) include structural units represented by the following formulas (A1) to (A8). [ka]
[0048] Of the structural units represented by the above formulas (A1) to (A8), the structural unit (A) is preferably the structural unit (A2), that is, the structural unit represented by the following formula (2). [ka]
[0049] The first fluorine-containing polymer may contain one or more kinds of structural units (A). In the first fluorine-containing polymer, the content of the structural units (A) is preferably 20 mol% or more, more preferably 40 mol% or more, based on the total of all structural units. When the structural units (A) are contained in an amount of 20 mol% or more, the first fluorine-containing polymer tends to have higher heat resistance. When the structural units (A) are contained in an amount of 40 mol% or more, the first fluorine-containing polymer tends to have higher transparency and high mechanical strength in addition to high heat resistance. In the first fluorine-containing polymer, the content of the structural units (A) is preferably 95 mol% or less, more preferably 70 mol% or less, based on the total of all structural units.
[0050] The structural unit (A) is derived from a compound represented by the following formula (3), for example. ff 1 ~R ff 4is the same as formula (1). The compound represented by formula (3) can be obtained by a known production method, for example, the production method disclosed in JP-A-2007-504125. [ka]
[0051] Specific examples of the compound represented by the above formula (3) include compounds represented by the following formulae (M1) to (M8). [ka]
[0052] The fluorine-containing polymer may further contain other structural units in addition to the structural unit (A). Examples of the other structural units include the following structural units (B) to (D).
[0053] The structural unit (B) is represented by the following formula (4). [ka]
[0054] In formula (4), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. 4 represents a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms.
[0055] The fluorine-containing polymer may contain one or more types of structural unit (B). In the fluorine-containing polymer, the content of the structural unit (B) is preferably 5 to 10 mol% based on the total of all structural units. The content of the structural unit (B) may be 9 mol% or less, or may be 8 mol% or less.
[0056] The structural unit (B) is derived from a compound represented by the following formula (5), for example. 1 ~R 4 is the same as formula (4). The compound represented by formula (5) is a fluorine-containing vinyl ether such as perfluorovinyl ether. [ka]
[0057] The structural unit (C) is represented by the following formula (6). [ka]
[0058] In formula (6), R 5 ~R 8 each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms.
[0059] The fluorine-containing polymer may contain one or more types of structural unit (C). In the fluorine-containing polymer, the content of the structural unit (C) is preferably 5 to 10 mol% based on the total of all structural units. The content of the structural unit (C) may be 9 mol% or less, or may be 8 mol% or less.
[0060] The structural unit (C) is derived from a compound represented by the following formula (7), for example: 5 ~R 8 is the same as formula (6). The compound represented by formula (7) is a fluorine-containing olefin such as tetrafluoroethylene or chlorotrifluoroethylene. [ka]
[0061] The structural unit (D) is represented by the following formula (8). [ka]
[0062] In formula (8), Z is an oxygen atom, a single bond, or -OC(R 19 R 20 )O-, R 9 ~R 20 each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkoxy group may be substituted with halogen atoms other than fluorine atoms. s and t each independently represent an integer of 0 to 5, and s+t is an integer of 1 to 6 (with the proviso that Z is -OC(R 19 R 20 )O-, s+t may be 0.
[0063] The structural unit (D) is preferably represented by the following formula (9): The structural unit represented by the following formula (9) is the case where Z is an oxygen atom, s is 0, and t is 2 in the above formula (8). [ka]
[0064] In formula (9), R 141 , R 142 , R 151 , and R 152each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkoxy group may be substituted with halogen atoms other than fluorine atoms.
[0065] The fluorine-containing polymer may contain one or more types of structural unit (D). In the fluorine-containing polymer, the content of the structural unit (D) is preferably 30 to 67 mol% based on the total of all structural units. The content of the structural unit (D) is, for example, 35 mol% or more, and may be 60 mol% or less, or may be 55 mol% or less.
[0066] The structural unit (D) is derived from a compound represented by the following formula (10): 9 ~R 18 , s and t are the same as in formula (4). The compound represented by formula (10) is a fluorine-containing compound which has two or more polymerizable double bonds and is capable of cyclopolymerization. [ka]
[0067] The structural unit (D) is preferably derived from a compound represented by the following formula (11): 141 , R 142 , R 151 , and R 152 is the same as equation (9). [ka]
[0068] Specific examples of the compound represented by formula (10) or formula (11) include the following compounds. CF2=CF2CF=CF2 CF2=CFOCF(CF3)CF=CF2 CF2=CF2CF2CF=CF2 CF2=CF0CF2CF(CF3)CF=CF2 CF2=CFFOCF(CF3)CF2CF=CF2 CF2=CFOCFClCF2CF=CF2 CF2=CFOCCl2CF2CF=CF2 CF2=CFOCF2OCF=CF2 CF2=CFOC(CF3)2OCF=CF2 CF2=CF2CF(OCF3)CF=CF2 CF2=CFCF2CF=CF2 CF2=CFCF2CF2CF=CF2 CF2=CFCF2OCF2CF=CF2 CF2=CFOCF2CFClCF=CF2 CF2=CFOCF2CF2CCl=CF2 CF2=CFOCF2CF2CF=CFCl CF2=CFOCF2CF(CF3)CCl=CF2 CF2=CFOCF2OCF=CF2 CF2=CFOCCl2OCF=CF2 CF2=CClOCF2OCCl=CF2
[0069] The first fluorine-containing polymer may further contain other structural units than the structural units (A) to (D), but preferably does not substantially contain other structural units than the structural units (A) to (D). The phrase "the fluorine-containing polymer does not substantially contain other structural units than the structural units (A) to (D)" means that the total of the structural units (A) to (D) is 95 mol % or more, preferably 98 mol % or more, of the total of all structural units in the fluorine-containing polymer.
[0070] The polymerization method for the first fluorine-containing polymer is not particularly limited, and for example, a general polymerization method such as radical polymerization can be used. The polymerization initiator for polymerizing the fluorine-containing polymer may be a perfluorinated compound.
[0071] The first fluoropolymer constitutes a first fluororesin used as the first resin. The first glass transition temperature Tg1 of the first resin is not particularly limited and is, for example, 100° C. to 140° C., and may be 105° C. or higher, or 120° C. or higher. In this specification, Tg refers to the midpoint glass transition temperature (T mg )
[0072] The refractive index n1 of the first region 111 of the core 11 preferably has a refractive index profile such that g satisfies 1.9≦g≦2.1 in the following formula (1). Note that Δ in formula (1) is expressed by the following formula (2).
[0073] n1(r)=n A [1-2Δ(r / a) g ] 1 / 2 Formula (1)
[0074] Δ=(n A 2 -n B 2 ) / 2n A 2 Formula (2)
[0075] In formulas (1) and (2), r, a, n A , and n B is as follows: r: radius a: radius of the first region 111 of the core 11 n A : Refractive index value at the center of the core 11, i.e., r=0 n B : Refractive index value of the outer edge of the first region 111 of the core 11
[0076] The refractive index n1 of the first region 111 can be set within a range of 1.329 or more and 1.341 or less for a wavelength of 850 nm, for example.
[0077] The refractive index n2 of the second region 112 may be equal to or less than the refractive index n1, and may be within the range of 1.327 to 1.331 for a wavelength of 850 nm, for example.
[0078] (Trench 12) In the POF 10 of this embodiment, the trench 12 contains, for example, a second resin. The trench 12 may contain the second resin as a main component. Here, the trench 12 containing the second resin as a main component means that the component contained most abundantly in the trench 12 in terms of mass ratio is the second resin. The trench 12 may contain 80 mass % or more of the second resin, 90 mass % or more, or 95 mass % or more of the second resin. The trench 12 may be made of only the second resin. The trench 12 may further contain an additive in addition to the second resin.
[0079] The second resin contained in the trench 12 is not particularly limited as long as it is a resin having high transparency. Examples of the second resin are the same as those exemplified as the resin that can be used as the first resin. As with the first resin, a fluorine-containing resin is preferably used as the second resin.
[0080] The second resin of the trench 12 is preferably a fluororesin containing a fluoropolymer. Hereinafter, the fluororesin contained in the trench 12 will be referred to as a second fluororesin, and the fluoropolymer contained in the second fluororesin will be referred to as a second fluoropolymer.
[0081] As the second fluorine-containing resin, those exemplified as the fluorine-containing resin that can be used as the first fluorine-containing resin can be used.
[0082] As the second fluorine-containing resin, a fluorine-containing polymer which further contains a constituent unit (E) represented by the following formula (12) and has an amorphous structure, and a fluorine-containing plasticizer may be used. [ka] (In formula (12), Z is an oxygen atom, a single bond, or -OC(R 31 R 32 )O-, R 21 ~R 32 each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. "Perfluoro" means that all hydrogen atoms bonded to carbon atoms are substituted with fluorine atoms. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkoxy group may be substituted with halogen atoms other than fluorine atoms. s and t each independently represent an integer of 0 to 5, and s+t represents an integer of 1 to 6 (provided that Z is not -OC(R 31 R 32 ) In the case of O-, s+t may be 0. Each of u and v is independently 0 or 1.
[0083] The fluorine-containing polymer containing the structural unit (E) may further contain a structural unit (F) represented by the following formula (13). [ka] (In formula (13), R 33 ~R 36 each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms.
[0084] When the second fluorine-containing polymer is the above copolymer, the ratio of the structural units (E) to the structural units (F) is arbitrary and is not particularly limited.
[0085] The second fluorine-containing polymer is preferably, for example, at least one selected from the group consisting of a fluorine-containing polymer A and a fluorine-containing polymer B shown below.
[0086] The fluoropolymer A contains a structural unit (G) represented by the following formula (14) and a structural unit (H) represented by the following formula (15). 23 , R 24 , R 31 , and R 32 is the same as the above formula (12).
[0087] [ka] [ka] (In formula (15), R 37 ~R 40 each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. Some of the fluorine atoms may be substituted with halogen atoms other than fluorine atoms. Some of the fluorine atoms in the perfluoroalkyl group may be substituted with halogen atoms other than fluorine atoms.
[0088] The fluoropolymer B contains a structural unit (I) represented by the following formula (16). 21 ~R 24 , R 27 ~R 30 , R 31 , and R 32 is the same as the above formula (12). [ka]
[0089] The above-mentioned fluorine-containing polymer A and fluorine-containing polymer B have very high transparency, and further can have a refractive index that is very low compared with the general refractive index of the first fluorine-containing resin used as the material of the core 11. Therefore, the second fluorine-containing resin containing at least one selected from the group consisting of the fluorine-containing polymer A and the fluorine-containing polymer B as the second fluorine-containing polymer can further reduce the refractive index while maintaining the high transparency of the trench 12. As a result, the difference between the refractive index of the core 11 and the refractive index of the trench 12 can be further increased, so that the effect of confining light in the core 11 by the trench 12 is further improved, and it becomes easier to realize low transmission loss of the POF 10.
[0090] The second fluorine-containing polymer preferably contains a structural unit (J) represented by the following formula (17). [ka] (In formula (17), m and n are any integers.)
[0091] The second fluorine-containing polymer constitutes a second fluorine-containing resin used as the second resin. The second glass transition temperature Tg2 of the second resin is not particularly limited and is, for example, 100°C to 150°C, and may be 105°C or higher, or may be 125°C or higher.
[0092] The refractive index n3 of the trench 12 is not particularly limited as long as it is designed according to the refractive index n2 of the second region 112 of the core 11. The refractive index n3 of the trench 12 may be, for example, 1.34 or less or 1.33 or less at a wavelength of 850 nm. The refractive index n3 of the trench 12 may be, for example, 1.32 or more at a wavelength of 850 nm.
[0093] The difference between the refractive index n3 of the trench 12 and the refractive index n2 of the second region 112 of the core 11 is preferably 0.005 or more and 0.010 or less.
[0094] (Modification of POF) Fig. 3 shows a modified example of the POF of this embodiment. The POF 20 shown in Fig. 3 has a configuration in which a reinforcing layer 21 arranged around the outer periphery of the trench 12 is further provided in the POF 10. The reinforcing layer 21 is provided to improve the mechanical strength of the POF 10. For example, the material and configuration used as a reinforcing layer in a known POF can be applied to the reinforcing layer 21. Examples of materials for the reinforcing layer 21 include various engineering plastics such as polycarbonate, polyester, cycloolefin polymer, cycloolefin copolymer, polytetrafluoroethylene (PTFE), modified PTFE, and tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), or copolymers or mixtures thereof.
[0095] (POF manufacturing method) The POF of this embodiment is manufactured by, for example, a melt spinning method. That is, an example of a manufacturing method of the POF of this embodiment is as follows: Melting a core material and extruding it into a fiber shape to prepare a fiber-shaped molded body made of the core material; Melting a trench material and extruding it to cover the surface of the molded body, thereby producing a laminate in which the core material and the trench material are concentrically laminated; The core material includes, for example, a first resin, and the trench material includes, for example, a second resin.
[0096] When preparing a fiber-shaped molded body made of a core material, first, a first core material containing a refractive index adjuster is extruded to form a core inner layer portion, and then a second core material may be extruded to cover the outer periphery of the core inner layer portion 2 formed of the first core material 1a. In this case, the first region 111 and the second region 112 of the core 11 can be formed by diffusing the refractive index adjuster contained in the first core material toward the core outer periphery formed of the second core material. In order to form the second region 111 of the core 11 having a constant refractive index n2, for example, the conditions (e.g., diffusion temperature and diffusion time) for diffusing (e.g., thermal diffusion) the refractive index adjuster, the discharge amounts of the first core material and the second core material, etc. are adjusted.
[0097] FIG. 4 is a schematic cross-sectional view showing an example of a manufacturing apparatus that can be used to manufacture the POF 20 shown in FIG.
[0098] The apparatus 1000 shown in FIG. 4 includes a first extrusion device 101a for extruding a first core material, a second extrusion device 101b for extruding a second core material, a third extrusion device 101c for extruding a trench material, and a fourth extrusion device 101d for forming a coating layer.
[0099] The first extrusion device 101a has a first storage section 102a that stores the first core material 1a, and a first extrusion section 103a that extrudes the first core material 1a stored in the first storage section 102a from the first storage section 102a. The first extrusion device 101a is further provided with a heating section (not shown) so that the first core material 1a can be melted in the first storage section 102a and the melted first core material 1a can be kept in a molten state until it is molded. The rod-shaped first core material (preform) 1a is inserted into the first storage section 102a through an upper opening of the first storage section 102a and melted by being heated in the first storage section 102a.
[0100] In the first extrusion device 101a, the first core material 1a is extruded by gas extrusion from the first storage section 102a through the first extrusion section 103a to form the core inner layer section 2. The first core material 1a extruded through the first extrusion section 103a to form the core inner layer section 2 then moves vertically downward and is supplied to the first chamber 110.
[0101] The second extrusion device 101b has a second storage section 102b that stores the second core material 1b, and a second extrusion section 103b that extrudes the second core material 1b stored in the second storage section 102b from the second storage section 102b. The second extrusion device 101b extrudes the molten second core material so as to cover the outer periphery of the core inner layer section 2 formed of the first core material 1a extruded from the first extrusion device 101a. Specifically, the second core material extruded from the second extrusion device 101b is supplied to the first chamber 110. In the first chamber 110, the core inner layer section 2 formed of the first core material 1a is covered with the second core material, thereby forming the core outer periphery section 3 that covers the outer periphery of the core inner layer section 2. The laminate 4 formed of the core inner layer portion 2 and the outer core peripheral portion 3 covering the outer periphery of the core inner layer portion 2 moves from the first chamber 110 to the diffusion tube 120 arranged vertically below the first chamber 110. A heater (not shown) for heating the laminate is arranged in the diffusion tube 120. The diffusion tube 120 diffuses dopants such as a refractive index adjuster contained in the core inner layer portion 2 of the laminate 4 passing through the inside of the diffusion tube 120 toward the outer core peripheral portion 3. That is, the core inner layer portion 2 and the outer core peripheral portion 3 finally form a core.
[0102] The third extrusion device 101c has a third storage section 102c that stores the trench material 1c, and a third extrusion section 103c that extrudes the trench material 1c stored in the third storage section 102c from the third storage section 102c. The third extrusion device 101c extrudes the molten trench material 1c so as to cover the outer periphery of the laminate 4 that has passed through the diffusion tube 120. Specifically, the trench material 1c extruded from the third extrusion device 101c is supplied to the second chamber 130. In the second chamber 130, the laminate 4 (i.e., the core) is covered with the trench material 1c to form a trench 5 that covers the outer periphery of the core. Hereinafter, the laminate 4 is referred to as the core 4. The laminate formed of the core 4 and the trench 5 moves from the second chamber 130 to the third chamber 140 arranged vertically below the second chamber 130.
[0103] The fourth extrusion device 101d includes a fourth storage section 102d that stores the coating layer material 1d, a screw 104 disposed in the fourth storage section 102d, and a hopper 105 connected to the fourth storage section 102d. In the fourth extrusion device 101d, the coating layer material 1d, for example, in the form of pellets, is supplied to the fourth storage section 102d through the hopper 105. The coating layer material 1d supplied to the fourth storage section 102d is softened and made fluid by being heated and kneaded by the screw 104. The softened coating layer material 1d is extruded from the fourth storage section 102d by the screw 104.
[0104] The coating layer material 1d extruded from the fourth extrusion device 101d is supplied to the third chamber 140. In the third chamber 140, the surface of the laminate formed of the core 4 and the trench 5 is coated with the coating layer material 1d, thereby forming a coating layer 6 that covers the outer periphery of the trench 5.
[0105] The laminate 7, in which the core 4, the trench 5, and the coating layer 6 are laminated concentrically, flows from the third chamber 140 into the internal flow path through the inlet of the nozzle 150. The laminate 7 is reduced in diameter as it passes through the internal flow path, and is discharged from the outlet of the nozzle 150 in the form of a fiber.
[0106] The laminate 7 discharged in a fiber shape from the discharge port of the nozzle 150 flows into the internal space 161 of the cooling tube 160, is cooled while passing through the internal space 161, and is discharged from the opening to the outside of the cooling tube 160. The laminate 7 discharged from the cooling tube 160 passes between two rolls 171 and 172 of the nip roll 170, and further passes through guide rolls 173 to 175, and is taken up on a take-up roll 176 as POF 10. A displacement meter 180 for measuring the outer diameter of the POF 10 may be further provided in the vicinity of the take-up roll 176, for example, between the guide roll 175 and the take-up roll 176.
[0107] The POF according to this embodiment is also suitable for optical cords and active optical cables.
[0108] Fig. 5 is a schematic diagram showing an example of an optical cord including the POF 10 (or POF 20) of this embodiment. The optical cord 50 shown in Fig. 5 includes a cable 51 containing the POF 10 (or POF 20) of this embodiment, and a connector 52 attached to at least one end of the cable 51.
[0109] Fig. 6 is a schematic diagram showing an example of an active optical cable including the POF 10 (or POF 20) of this embodiment. The active optical cable 60 shown in Fig. 6 includes a cable 61 containing the POF 10 (or POF 20) of this embodiment, a first connector 62 attached to a first end 61a of the cable 61 and including a first conversion unit (not shown) that converts an electrical signal into an optical signal, and a second connector 63 attached to a second end 61b of the cable 61 and including a second conversion unit (not shown) that converts an optical signal into an electrical signal. EXAMPLES
[0110] Example 1 [Preparation of first fluorine-containing resin] As the first fluorine-containing resin, a polymer of perfluoro-4-methyl-2-methylene-1,3-dioxolane (PFMMD) was prepared. Perfluoro-4-methyl-2-methylene-1,3-dioxolane was synthesized by first synthesizing 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, fluorinating it, and separating the resulting carboxylate by decarboxylation. Perfluorobenzoyl peroxide was used as a polymerization initiator for the polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane.
[0111] The synthesis of 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, the fluorination of 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, the synthesis of perfluoro-4-methyl-2-methylene-1,3-dioxolane, and the polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane are described in detail below.
[0112] <Synthesis of 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane> A 3L three-neck flask equipped with a water-cooled condenser, a thermometer, a magnetic stirrer, and a pressure-equalizing dropping funnel were prepared, and 139.4 g (total 1.4 moles) of a mixture of 2-chloro-1-propanol and 1-chloro-2-propanol was added to the flask. The flask was cooled to 0°C, and methyl trifluoropyruvate was slowly added thereto and stirred for another 2 hours. 100 mL of dimethyl sulfoxide (DMSO) and 194 g of potassium carbonate were added thereto over 1 hour, and then the mixture was stirred for another 8 hours to obtain a reaction mixture. The reaction mixture thus formed was mixed with 1 L of water, and the aqueous phase was separated and further extracted with dichloromethylene. The dichloromethylene solution was mixed with the organic reaction mixture phase, and the solution was dried over magnesium sulfate. After removing the solvent, 245.5 g of crude product was obtained. This crude product was fractionally distilled under reduced pressure (12 Torr) to obtain 230.9 g of a purified product of 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane. The boiling point of the purified product was 77-78°C, and the yield was 77%. The purified product was found to be 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane by HNMR and 19 This was confirmed by FNMR.
[0113] HNMR(ppm):4.2-4.6,3.8-3.6(CHCH2,muliplet,3H),3.85-3.88(COOCH3,multiplet,3H),1.36-1.43(CCH3,multiplet,3H) 19 FNMR(ppm):-81.3(CF3,s,3F)
[0114] <Fluorination of 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane> 4 L of 1,1,2-trichlorotrifluoroethane was poured into a 10 L stirred reactor. Nitrogen was flowed at a flow rate of 1340 cc / min and fluorine was flowed at a flow rate of 580 cc / min in the stirred reactor to create a nitrogen / fluorine atmosphere. After 5 minutes, 290 g of the previously prepared 2-carbomethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane was dissolved in 750 mL of 1,1,2-trichlorotrifluoroethane solution, and this solution was added to the reactor at a rate of 0.5 ml / min. The reactor was cooled to 0°C. After all the dioxolane had been added in 24 hours, the fluorine gas flow was stopped. After purging the nitrogen gas, an aqueous potassium hydroxide solution was added until it became weakly alkaline.
[0115] After removing the volatiles under reduced pressure, the reaction vessel was cooled and then dried under reduced pressure at 70°C for 48 hours to obtain a solid reaction product. The solid reaction product was dissolved in 500mL of water and separated into an organic phase and an aqueous phase by adding excess hydrochloric acid. The organic phase was separated and distilled under reduced pressure to obtain perfluoro-2,4-dimethyl-1,3-dioxolane-2-carboxylic acid. The boiling point of the main distillate was 103°C-106°C / 100mmHg. The fluorination yield was 85%.
[0116] <Synthesis of perfluoro-4-methyl-2-methylene-1,3-dioxolane> The distillate was neutralized with an aqueous potassium hydroxide solution to obtain perfluoro-2,4-dimethyl-2-potassium carboxylate-1,3-dioxolane. The potassium salt was vacuum dried at 70°C for 1 day. The salt was decomposed at 250°C to 280°C under a nitrogen or argon atmosphere. Condensation was carried out in a cold trap cooled to -78°C to obtain perfluoro-4-methyl-2-methylene-1,3-dioxolane in 82% yield. The boiling point of the product was 45°C / 760mmHg. 19 The products were identified using FNMR and GC-MS.
[0117] 19 FNMR:-84ppm(3F,CF3),-129ppm(2F,=CF2) GC-MS:m / e244(Molecular ion)225,197,169,150,131,100,75,50.
[0118] <Polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane> 100 g of perfluoro-4-methyl-2-methylene-1,3-dioxolane obtained by the above method and 1 g of perfluorobenzoyl peroxide were sealed in a glass tube. The glass tube was refilled with argon after oxygen was removed from the system by freeze degassing, and heated at 50°C for several hours. The contents became solid, but when further heated at 70°C overnight, 100 g of a transparent rod-like product was obtained.
[0119] The obtained transparent rod-like matter was dissolved in Fluorinert FC-75 (manufactured by Sumitomo 3M Limited), and the obtained solution was poured onto a glass plate to obtain a thin film of the polymer. The obtained polymer had a glass transition temperature of 117°C and was completely amorphous. The transparent rod-like matter was dissolved in hexafluorobenzene, and chloroform was added thereto to cause precipitation, thereby purifying the product. The glass transition temperature of the purified polymer was about 131°C. This polymer was designated as the first fluorine-containing resin.
[0120] [Refractive index adjuster] As a refractive index adjuster, chlorotrifluoroethylene oligomer (molecular weight 585) was used. Specifically, Daikin Industries, Ltd.'s "Daifloil #10" was distilled, and only the component with a molecular weight of 585 was separated. The separated component with a molecular weight of 585 was filtered through a 40 nm pore size filter "DFA1ANDESW44" (PALL Corporation) to obtain a refractive index adjuster.
[0121] [First core material] The first fluorine-containing resin prepared by the above method was dissolved in a solvent, Vertrel XF-UP (manufactured by Mitsui-Chemours Fluoroproducts). The solution was filtered twice with a filter "LPJ-CTA-001-N3" (manufactured by Roki Techno) with a pore size of 100 nm, and the filtrate was dropped into a Hastelloy container heated to 260°C to evaporate the solvent and dry it. The fluorine-containing resin obtained by drying and filtration and the refractive index adjuster were melt-mixed at 260°C to prepare a resin composition. The concentration of the refractive index adjuster in the obtained resin composition was 12% by mass. This resin composition was used as the first core material.
[0122] [Second core material] The first fluororesin prepared by the above method was filtered in the same manner as in the filtration of the fluororesin in the preparation of the first core material to obtain a filtered fluororesin, which was used as the second core material.
[0123] [Trench material] A second fluorine-containing resin was prepared as a trench material. "Teflon AF1600" (manufactured by Mitsui-Chemours Fluoroproducts) as a second fluorine-containing resin and "Fomblin YR" (manufactured by Solvay) as a viscosity modifier were dissolved in a solvent, Vertrel XF-UP (manufactured by Mitsui-Chemours Fluoroproducts). The mixing ratio of "Teflon AF1600" to "Fomblin YR" was "Teflon AF1600": "Fomblin YR" = 7: 3 by mass ratio. The obtained solution was filtered through a filter "LPA-SLF-003-N2" (manufactured by Roki Techno Co., Ltd.) with a pore size of 300 nm, and the filtrate was dropped into a Hastelloy container heated to 260 ° C. to evaporate the solvent and dry it. The resin composition obtained by drying it was used as a trench material.
[0124] [Coating layer material] Xylex (manufactured by SABIC, glass transition temperature: 113° C.) was used as the covering layer material.
[0125] [Fabrication of POF] Using the first core material, the second core material, the trench material, and the coating layer material prepared by the above-mentioned methods, a POF having a structure similar to that of the POF 20 shown in Fig. 3 was produced by a melt spinning method. In this example, the manufacturing apparatus shown in Fig. 4 was used to manufacture the POF.
[0126] In this embodiment, the inner diameter of the diffusion tube 120 was 6.3 mm. The length of the diffusion tube 120 was set so that the diffusion time was 120 minutes.
[0127] In this embodiment, the melting temperature of the first core material was 250°C, the melting temperature of the second core material was 255°C, the melting temperature of the trench material was 260°C, and the melting temperature of the covering layer material was 240°C. The temperature of the diffusion tube 120 was set to 275°C. The first core material and the second core material formed a core. The temperature of the drawdown of the laminate 7 consisting of the core, trench, and covering layer was 240°C.
[0128] The melt extrusion was performed with the volume ratio of each material being 1:1.04 for the second core material, 0.705 for the trench material, and 40.438 for the covering layer material relative to the first core material.
[0129] In the first chamber 110 shown in Fig. 4, the temperature of the confluence die used when coating the core inner layer portion formed of the first core material with the second core material was set to 260°C. In the second chamber 130 shown in Fig. 4, the temperature of the confluence die used when coating the core with the trench material was set to 205°C. In the third chamber 140 shown in Fig. 4, the temperature of the confluence die used when coating the surface of the laminate formed of the core and trench with the coating layer material was set to 250°C.
[0130] For the POF produced in Example 1, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 2.85 μm, the outer diameter of the trench was 58 μm (i.e., the thickness of the trench was 4 μm), and the outer diameter of the coating layer was 230 μm.
[0131] Example 2 The POF of Example 2 was produced in the same manner as Example 1, except that the volume ratio of each material discharged was changed to 1:1.441 for the second core material, 1.559 for the trench material, and 47.660 for the coating layer material relative to the first core material.
[0132] For the POF produced in Example 2, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 4.01 μm, the outer diameter of the trench was 64 μm (i.e., the thickness of the trench was 7 μm), and the outer diameter of the coating layer was 230 μm.
[0133] Example 3 The POF of Example 3 was produced in the same manner as Example 1, except that the volume ratio of each material discharged was changed to 1:1.602 for the second core material, 1.661 for the trench material, and 50.785 for the coating layer material relative to the first core material.
[0134] For the POF produced in Example 3, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 4.53 μm, the outer diameter of the trench was 64 μm (i.e., the thickness of the trench was 7 μm), and the outer diameter of the coating layer was 230 μm.
[0135] Example 4 The POF of Example 4 was produced in the same manner as Example 1, except that the volume ratio of each material discharged was changed to 1:1.74 for the second core material, 1.47 for the trench material, and 53.787 for the coating layer material relative to the first core material.
[0136] For the POF produced in Example 4, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 4.96 μm, the outer diameter of the trench was 62 μm (i.e., the thickness of the trench was 6 μm), and the outer diameter of the coating layer was 230 μm.
[0137] Example 5 The POF of Example 5 was produced in the same manner as Example 1, except that the volume ratio of each material discharged was changed to 1:1.100 for the second core material, 0.726 for the trench material, and 41.618 for the coating layer material in relation to the first core material.
[0138] For the POF produced in Example 5, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 2.89 μm, the outer diameter of the trench was 58 μm (i.e., the thickness of the trench was 4 μm), and the outer diameter of the coating layer was 230 μm.
[0139] Comparative Example 1 FONTEX (manufactured by AGC) was prepared as the POF of Comparative Example 1. For the POF of Comparative Example 1, the core diameter (outer diameter of the core) measured by the method described below was 55 μm, the thickness of the second region of the core was 0 μm, the outer diameter of the trench was 65 μm (i.e., the thickness of the trench was 5 μm), and the outer diameter of the coating layer was 490 μm.
[0140] Comparative Example 2 The POF of Comparative Example 2 was produced in the same manner as in Example 1, except that the volume ratio of each material discharged was changed to 1:1.815 for the second core material, 1.513 for the trench material, and 55.241 for the coating layer material relative to the first core material.
[0141] For the POF produced in Comparative Example 2, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 5.00 μm, the outer diameter of the trench was 62 μm (i.e., the thickness of the trench was 6 μm), and the outer diameter of the coating layer was 230 μm.
[0142] Comparative Example 3 The POF of Comparative Example 3 was produced in the same manner as in Example 1, except that the volume ratio of each material discharged was changed to 1:1.873 for the second core material, 1.544 for the trench material, and 56.370 for the coating layer material relative to the first core material.
[0143] For the POF produced in Comparative Example 3, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 5.12 μm, the outer diameter of the trench was 62 μm (i.e., the thickness of the trench was 6 μm), and the outer diameter of the coating layer was 230 μm.
[0144] Comparative Example 4 The POF of Comparative Example 4 was produced in the same manner as in Example 1, except that the volume ratio of each material discharged was changed to 1:1.973 for the second core material, 1.898 for the trench material, and 58.031 for the coating layer material relative to the first core material.
[0145] For the POF produced in Comparative Example 4, the core diameter (outer diameter of the core) measured by the method described below was 50 μm, the thickness of the second region of the core was 5.22 μm, the outer diameter of the trench was 64 μm (i.e., the thickness of the trench was 7 μm), and the outer diameter of the coating layer was 230 μm.
[0146] Comparative Example 5 Giga-POF-50SR (manufactured by Chromis) was prepared as the POF of Comparative Example 5. The POF of Comparative Example 5 had a core diameter (outer diameter of the core) of 50 μm, a thickness of the second region of the core of 0 μm, and an outer diameter of the coating layer of 490 μm, all of which were measured by a method described below. The POF of Comparative Example 5 had no trench.
[0147] (POF evaluation) [Measurement of the core diameter, thickness of the second region of the core, and outer diameter of the trench] The core diameter, the thickness of the second region of the core, and the outer diameter of the trench were determined by the NFP method using light with a wavelength of 850 nm, which is one of the methods conforming to IEC60793-1-20 and IEC60793-2-40 subcategory A4h. Specifically, the outer edge 11b of the core 11 and the outer edge of the trench were identified using the surface distribution of the POF output light intensity, and the core diameter and the outer diameter of the trench were determined. The outer edge 11b of the core 11 corresponds to the interface (core / trench interface) between the core 11 and the trench 12. Furthermore, the surface distribution of the output light intensity of the POF was differentiated to determine the inflection point, thereby distinguishing the first region 111 having a refractive index distribution from the second region 112 having a constant refractive index, and the outer diameter of the first region 111 was determined. Since the outer edge of the second region 112 is the outer edge 11b of the core 11 (i.e., the core / trench interface), the core / trench interface identified by the NFP method was identified as the outer edge of the second region 112. The thickness of the second region 112 was calculated from the outer diameters of the identified regions.
[0148] [Measurement of the outer diameter of the coating layer] The POF was cut to a length of 2 cm, and the POF was placed so that its axis was perpendicular to the sample stage of a digital microscope (Keyence VHX-950F). The light source attached to the microscope was irradiated onto one end of the POF, and the transmitted light emitted from the other end was observed to measure the coating layer of the POF.
[0149] [Refractive index measurement] The refractive index n1 of the first region of the core, the refractive index n2 of the second region of the core, and the refractive index n3 of the trench were measured under a room temperature (about 23°C) environment using a prism coupler (model 2010 / M) manufactured by Metricon. Specifically, the materials of the core and the trench were each hot-press molded at about 210°C to obtain a sheet with a thickness of about 100 μm. The obtained sheet was then introduced into a prism coupler (model 2010 / M) manufactured by Metricon to obtain the refractive index. Furthermore, the aperture angle was measured by the far-field pattern method to obtain the refractive index difference between the core and the trench. Finally, the refractive index n1 of the first region of the core, the refractive index n2 of the second region of the core, and the refractive index n3 of the trench 12 were calculated with reference to 2.4 of the paper (Mitsuhiro Tachibana, "Method of Measuring the Refractive Index Distribution of Optical Fibers," Applied Physics, Vol. 48, No. 8). It was confirmed by this method that the POFs of Examples 1 to 5 satisfy the refractive index relationship of n1≧n2>n3. It was confirmed by the same method that the POFs of Comparative Examples 2 to 4 also satisfied the refractive index relationship of n1≧n2>n3.
[0150] [Band Rating] The 5m bandwidth of the POFs of Examples 1 to 5 and Comparative Examples 1 to 5 was measured by the pulse method, which is a method conforming to IEC60793-1-41. However, in order to measure the bandwidth of the POFs of a very short distance of 5m, a device capable of oscillating ultra-high speed pulses was used as the optical pulse generator, and a device capable of image recognition in a short time was used as the optical receiver. Specifically, the bandwidth was measured by the following method.
[0151] The optical pulse generator used was InSightX3+ manufactured by SpectraPhisics. A laser with a wavelength of 850 nm was oscillated by this optical pulse generator. The oscillated laser was coupled to an OM1 fiber ("M31L01-OM1, 0.275 NA, Graded-Index Patch Cable" manufactured by THORLABS) through a lens, and mode scrambled by FM-1 manufactured by Newport Corporation. The output side was connected to a 2m OM1 fiber with a mode filter (Test Reference Code MRC-625-EFC-SCFC manufactured by FLUKE Networks, Inc.), and the POF to be measured was connected to the output side of the OM1 fiber.
[0152] It was confirmed that the core diameter of the light incident on the POF to be measured was 57.3 μm and the numerical aperture (NA) was 0.26, which were larger than the core diameter and numerical aperture (NA) of the POF to be measured, respectively. In other words, the bandwidth of the POF was measured by incident overfill light.
[0153] The receiver used was a universal streak camera C10910 series manufactured by Hamamatsu Photonics K.K. The pulse waveform was obtained using this receiver.
[0154] Measurements at a distance of 5 m were performed in the following manner. First, a 7 m long POF was prepared, an optical pulse was input from one end, and the optical pulse of the output light at 7 m was measured. After that, the POF was cut to a length of 2 m, and an optical pulse was input and the output pulse was measured in the same manner. The two output pulses were subjected to Fourier transform specified in IEC60793-1-41 to obtain the transfer function, and the frequency at -1.5 dB in optical power was obtained. The results are shown in Table 1. Table 1 shows both the bandwidth measurement results (unit: GHz) obtained when measuring at a distance of 5 m, and the measurement results converted into the unit "MHz km". The "5 m bandwidth value" shown in Table 1 is the bandwidth value obtained by bandwidth evaluation.
[0155] [Bending loss evaluation] A POF with a length of 5 m was prepared. FIG. 7 is a schematic diagram showing a measurement system for measuring the bending loss of a POF in the examples and comparative examples. In the measurement system 70, a FOLS-01 (850 nm wavelength LED) manufactured by Sawaki Kobo Co., Ltd. was connected as a light source 72 to the incident side 71a of the POF 71. An optical power meter 8230E manufactured by ADC Co., Ltd. was connected as an optical power meter 73 to the light receiving side 71b of the POF 70. A 1 m portion on the incident side was wrapped around a cylinder with a diameter of 12.5 mm 10 times to remove the cladding mode, and the central part (2.5 m part) of the POF was set on a plate 74 with a U-shaped groove with a bending radius R as shown in FIG. 7 to bend the POF. In this way, the change in insertion loss from a straight state to a bent state was confirmed, and the optical loss was obtained. In this embodiment and the comparative example, the optical loss (first optical loss) was measured when the fiber was bent into a U shape with a bending radius R of 1.5 mm, and the optical loss (second optical loss) was measured when the fiber was bent into a U shape with a bending radius R of 2.0 mm. The results are shown in Table 1.
[0156] [Evaluation of numerical aperture (NA)] The numerical aperture (NA) was measured using the FFP (Far Field Pattern) method using light with a wavelength of 850 nm, which is one of the methods compliant with IEC60793-1-43 and IEC60793-2-40 sub-category A4h. A 6m long POF was prepared, and 850nm LED light was incident on one end. The light intensity distribution for the angular position of the emitted light 6m ahead was measured, and the numerical aperture (NA) was calculated.
[0157] [Table 1]
[0158] As shown in Table 1, the POFs of Examples 1 to 5, which have a trench and a second region with a thickness of 2 μm or more and less than 5 μm, were able to achieve a high bandwidth of 40 MHz km or more over a short distance of 5 m while suppressing bending loss to a small extent. In contrast, Comparative Example 1, which has a trench but does not have a second region, had a low bandwidth value because the bandwidth was reduced by the light reflected by the trench. On the other hand, Comparative Examples 2 to 4, which have a trench but have a second region with a thickness of 5 μm or more, had a higher bandwidth value than Comparative Example 1 but a lower bandwidth value than the Examples because the second region was thick and the bandwidth was reduced by the reflection of light incident on the second region. The POF of Comparative Example 5, which did not have a trench, had a high bandwidth value, but a large bending loss and a small numerical aperture (NA).
[0159] [Note] To summarize the above, one aspect of the present disclosure is as follows.
[0160] (1) A plastic optical fiber, The plastic optical fiber is A core, A trench disposed on the outer periphery of the core; Equipped with The core is a first region having a refractive index n1 that decreases in a direction from the center to the outer edge; a second region located on the outer periphery of the first region, including the outer edge of the core, and having a constant refractive index n2; having the refractive index n2 of the second region is equal to or less than the refractive index n1 of the first region, The thickness of the second region is equal to or greater than 2 μm and less than 5 μm, The refractive index n3 of the trench is lower than the refractive index n2 of the second region. Plastic optical fiber.
[0161] (2) The -1.5 dB bandwidth when overfill light is input at 5 m is 40 MHz km or more. The plastic optical fiber according to (1) above.
[0162] (3) When the plastic optical fiber is bent into a U-shape with a bending radius of 1.5 mm, the first optical loss is 3.0 dB or less. The plastic optical fiber according to (1) or (2) above.
[0163] (4) The first optical loss is 1.0 dB or less. The plastic optical fiber according to (3) above.
[0164] (5) When the plastic optical fiber is bent into a U-shape with a bending radius of 2.0 mm, the second optical loss is 0.5 dB or less. A plastic optical fiber according to any one of (1) to (4) above.
[0165] (6) The thickness of the second region is 2.9 μm or more and 4.8 μm or less. A plastic optical fiber according to any one of (1) to (5) above.
[0166] (7) The thickness of the second region is 2.9 μm or more and 4.5 μm or less. The plastic optical fiber according to (6) above.
[0167] (8) The thickness of the second region is 3.5 μm or more and 4.4 μm or less. The plastic optical fiber according to (7) above.
[0168] (9) The numerical aperture (NA) of the plastic optical fiber is 0.190 or more and 0.235 or less. A plastic optical fiber according to any one of (1) to (8) above.
[0169] (10) Equipped with a plastic optical fiber according to any one of (1) to (9) above, Optical code.
[0170] (11) The optical code according to (10) above; An optoelectronic hybrid module; An active optical cable. [Industrial Applicability]
[0171] The POF of the present disclosure can realize a high bandwidth over a short distance while suppressing bending loss to a small extent, and is therefore suitable for use in short-distance signal transmission within the home, for example. [Explanation of symbols]
[0172] 1a First core material 1b Second core material 1c Trench Material 1d Covering layer material 2. Inner core 3 Core Outer Part 4 Laminated body (core) 5. Trench 6 Covering layer 7 Laminate 10, 20 POF 11 cores 11a center 11b Outer edge 111 First area 112 Second area 12. Trench 21 Covering layer 50 Optical Code 51 Cable 52 Connector 60 Active Optical Cable 61 Cable 61a First end 61b Second end 62 1st Connector 63 Second Connector 70 Measurement Systems 71 POF 71a Incidence side 72 Light source 73 Optical Power Meter 74 Plate 101a First extrusion device 101b Second extrusion device 101c Third extrusion device 101d Fourth extrusion device 102a First storage section 102b Second storage section 102c Third Storage Unit 102d 4th Storage Unit 103a First extrusion section 103b Second extrusion section 103c Third extrusion section 104 Screw 105 Hopper 110 Room 1 120 Diffusion tube 130 Room 2 140 Room 3 150 nozzles 160 Cooling pipe 161 Interior Space 170 Nip Roll 171,172 rolls 173,174,175 Guide roll 176 Winding Roll 180 Displacement Gauge 1000 manufacturing equipment
Claims
1. A plastic optical fiber, The plastic optical fiber is A core, A trench disposed on the outer periphery of the core; Equipped with The core is A first region having a refractive index n1 that decreases in a direction from the center to the outer edge; a second region located on the outer periphery of the first region, including the outer edge of the core, and having a constant refractive index n2; having The refractive index n2 of the second region is equal to or less than the refractive index n1 of the first region, The thickness of the second region is equal to or greater than 2 μm and less than 5 μm, The refractive index n3 of the trench is lower than the refractive index n2 of the second region; Plastic optical fiber.
2. The -1.5 dB bandwidth value when overfill light is input at 5 m is 40 MHz km or more.
2. The plastic optical fiber according to claim 1.
3. The first optical loss when the plastic optical fiber is bent into a U shape with a bending radius of 1.5 mm is 3.0 dB or less.
2. The plastic optical fiber according to claim 1.
4. The first optical loss is 1.0 dB or less. The plastic optical fiber according to claim 3.
5. The second optical loss when the plastic optical fiber is bent into a U-shape with a bending radius of 2.0 mm is 0.5 dB or less.
2. The plastic optical fiber according to claim 1.
6. The thickness of the second region is 2.9 μm or more and 4.8 μm or less.
2. The plastic optical fiber according to claim 1.
7. The thickness of the second region is 2.9 μm or more and 4.5 μm or less. The plastic optical fiber according to claim 6.
8. The thickness of the second region is 3.5 μm or more and 4.4 μm or less. The plastic optical fiber according to claim 7.
9. The numerical aperture (N.A.) of the plastic optical fiber is 0.190 or more and 0.235 or less.
2. The plastic optical fiber according to claim 1.
10. Equipped with a plastic optical fiber according to any one of claims 1 to 9, Optical code.
11. An optical code according to claim 10; An optoelectronic hybrid module; An active optical cable.
Citation Information
Patent Citations
Multi-mode optical fiber with high bending resistance and reduced influence of leakage mode
JP2016527547A