Flexible ion adsorption electrode, production method, polluted soil purification device and method
The innovative production method for flexible ion adsorption electrodes, using carbon charcoal, zeolite, and natural binders, enhances performance and reproducibility, addressing the limitations of conventional electrodes in electrokinetic soil purification and water treatment.
Patent Information
- Application Number
- JP2023052496
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional flexible ion adsorption electrodes lack sufficient performance and reproducibility, and existing electrokinetic methods face challenges in treating large areas and secondary contamination from wastewater.
A method for producing a flexible ion adsorption electrode involving a mixing step with specific materials, solidification, drying, softening, and compression processes, using carbon charcoal as the conductive material, zeolite as the adsorbent, and abaca and starch powder as the binder, with a mat-like shape and improved manufacturing steps to enhance adsorption, conductivity, and flexibility.
The resulting electrode exhibits superior adsorption properties, conductivity, and flexibility, enabling effective purification of contaminated soil and water by adsorbing pollutants, including heavy metals and radioactive cesium, with improved reproducibility and ease of handling.
Smart Images

Figure 2024141057000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode used in a horizontal electrode type electrokinetic method and a method for producing the same. [Background technology]
[0002] Electrokinetic techniques that utilize electrokinetic phenomena (interfacial electrokinetic phenomena) are known as a method for in-situ purification of contaminated soil. In electrokinetic techniques, heavy metals in soil are collected near electrodes by applying a DC voltage to moist soil. In conventional electrokinetic techniques, electrodes are inserted into the soil at regular intervals and a DC voltage is applied between the electrodes to induce an interfacial electrokinetic phenomenon, which moves contaminants in the direction of the electric field and removes them from the soil.
[0003] Conventional electrokinetic methods have difficulty in treating large areas in situ, and there is concern about secondary pollution from wastewater, so a horizontal electrode electrokinetic method (FEM-EK method) has been developed as an improvement over conventional electrokinetic methods. A typical example of the horizontal electrode electrokinetic method is one in which a mat-shaped electrode and a rod-shaped electrode are used, the mat-shaped electrode is placed in close contact with the soil surface as the cathode, and the rod-shaped electrode is inserted into the soil as the anode to perform electrokinetic treatment in the vertical direction (see, for example, Patent Document 1 and Non-Patent Document 1).
[0004] The mat-like electrode used in the horizontal electrode electrokinetic method must have the ability to adsorb pollutants, electrical conductivity, and flexibility, and a method for fabricating the electrode and the evaluation results of the electrode are described in Non-Patent Document 1. Hereinafter, this electrode will be referred to as a flexible ion-adsorbing electrode. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-136515 A [Non-patent literature]
[0006] [Non-Patent Document 1] Yoshitaka Hatakeyama et al., "Preparation of flexible ion adsorption electrodes using natural zeolite and charcoal," Journal of the Electrostatic Society of Japan, 41, 2 (2017) 111-116 Summary of the Invention [Problem to be solved by the invention]
[0007] As mentioned above, flexible ion-adsorbing electrodes are required to have excellent adsorptive properties, electrical conductivity, and flexibility, and efforts have been made to improve each of these properties. For example, it has been reported that flexibility can be improved by incorporating a compression process into the manufacturing process of flexible ion-adsorbing electrodes. However, the performance of conventional flexible ion-adsorbing electrodes is not sufficient, and the low reproducibility of the performance of flexible ion-adsorbing electrodes is also an issue that needs to be resolved.
[0008] An object of the present invention is to provide a flexible ion-adsorbing electrode and a method for producing the same which are superior in performance and reproducibility to conventional flexible ion-adsorbing electrodes, and further to provide a contaminated soil remediation device, a contaminated soil remediation method, and a contaminated water remediation method which use the flexible ion-adsorbing electrode. [Means for solving the problem]
[0009] The present invention provides a method for producing a flexible ion-adsorbing electrode, which includes a mixing step of mixing water, a conductive material, an adsorbent, and a binder, a solidification step of dehydrating and solidifying the mixture obtained through the mixing step, a compression step of compressing the solidified material, and a finishing step of drying the compressed solidified material, and is characterized in that the method further includes, between the solidification step and the compression step, a drying step of drying the solidified material, and a softening step of immersing the dried solidified material obtained through the drying step in water to soften it.
[0010] In the method for producing a flexible ion-adsorbing electrode according to the present invention, the flexible ion-adsorbing electrode is a mat-shaped electrode used in a horizontal electrode type electrokinetic method, and is characterized in that the conductive material is charcoal, the adsorbent is zeolite, and the binder is abaca and starch powder.
[0011] In the method for producing a flexible ion-adsorbing electrode of the present invention, the mixing process includes a first mixing process in which hot water, the starch powder, the zeolite, and the abaca are stirred and mixed, and a second mixing process in which the mixture obtained in the first mixing process is stirred and mixed with the charcoal, and is characterized in that the stirring speed in the second mixing process is slower than the stirring speed in the first mixing process.
[0012] The method for producing a flexible ion-adsorbing electrode according to the present invention is characterized in that it includes a pretreatment step of drying the conductive material before the mixing step.
[0013] The present invention is a flexible ion-adsorbing electrode formed into a mat-like shape by mixing charcoal, zeolite, abaca, and starch powder, characterized in that the amount of adsorption per unit weight of the flexible ion-adsorbing electrode is 50 to 65 mg / kg when immersed in a non-radioactive cesium solution with a concentration of 500 ppb and measured, the conductivity of the flexible ion-adsorbing electrode is 5000 to 7000 μS / m when measured by applying a direct current voltage of 10 V in a wet state, and the flexible ion-adsorbing electrode has dimensions of long sides 97 mm, short sides 68 mm, and a thickness of 6 mm, and when the flexible ion-adsorbing electrode is fixed at a width of 10 mm from one end of the long side to the other end and the other end of the long side is pulled up with a load of 70 g, the lifted height is 70 to 80 mm.
[0014] The present invention is a contaminated soil remediation device that is characterized in that it is equipped with a flexible ion adsorption electrode obtained by the flexible ion adsorption electrode manufacturing method described above, or the flexible ion adsorption electrode, which is placed on the surface of the contaminated soil to be treated, and that it adsorbs contaminants in the contaminated soil to the flexible ion adsorption electrode by electrokinetic phenomena, thereby purifying the contaminated soil.
[0015] The contaminated soil purification apparatus of the present invention comprises the flexible ion-adsorbing electrode, an electrode different from the flexible ion-adsorbing electrode, and a DC voltage application means for applying a DC voltage between the flexible ion-adsorbing electrode and the electrode, and is characterized in that the electrokinetic phenomenon occurs when a DC voltage is applied between the flexible ion-adsorbing electrode and the electrode.
[0016] In the contaminated soil purification apparatus according to the present invention, the electrodes are electrode piles, and the electrode piles are inserted into the contaminated soil.
[0017] The contaminated soil remediation apparatus according to the present invention is characterized by further comprising a water supply means for wetting the contaminated soil and / or the flexible ion-adsorbing electrode.
[0018] In the contaminated soil purification apparatus according to the present invention, the contaminants are one or more of heavy metals and radioactive cesium.
[0019] The present invention relates to a method for remediating contaminated soil, which uses the contaminated soil remediation device, causes the flexible ion-adsorbing electrode to adsorb contaminants in the contaminated soil, and purifies the contaminated soil.
[0020] The present invention is a method for purifying contaminated soil, which uses a flexible ion-adsorbing electrode obtained by the method for producing a flexible ion-adsorbing electrode or the flexible ion-adsorbing electrode as an adsorbent for contaminants, and is characterized in that the flexible ion-adsorbing electrode is brought into contact with the contaminated soil to be treated, so as to adsorb the contaminants in the contaminated soil, and the contaminated soil is purified.
[0021] In the method for remediating contaminated soil according to the present invention, the contaminated soil and / or the flexible ion-adsorbing electrode are in a wet state.
[0022] The method for remediating contaminated soil according to the present invention is characterized in that the contaminants are one or more of heavy metals and radioactive cesium.
[0023] The present invention is a method for purifying contaminated water, which uses a flexible ion-adsorbing electrode obtained by the method for manufacturing a flexible ion-adsorbing electrode or the flexible ion-adsorbing electrode as an adsorbent for pollutants, and is characterized in that the flexible ion-adsorbing electrode is brought into contact with the contaminated water to be treated, so as to adsorb the pollutants in the contaminated water, and the contaminated water is purified.
[0024] In the method for purifying contaminated water according to the present invention, the contaminated water is wastewater or effluent containing the contaminants.
[0025] The method for purifying contaminated water according to the present invention is characterized in that the contaminants are one or more of heavy metals and radioactive cesium. Effect of the Invention
[0026] According to the present invention, it is possible to provide a flexible ion-adsorbing electrode and a method for producing the same which are superior in performance and reproducibility to conventional flexible ion-adsorbing electrodes, as well as a contaminated soil remediation device, a contaminated soil remediation method, and a contaminated water remediation method which use the flexible ion-adsorbing electrode. [Brief description of the drawings]
[0027] [Figure 1] 1 is a flowchart showing a procedure for producing a flexible ion-adsorbing electrode according to the present invention. [Diagram 2] FIG. 1 is a configuration diagram of a contaminated soil remediation apparatus 1 according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a diagram for explaining a method for remediating contaminated soil and a method for remediating contaminated water according to an embodiment of the present invention. [Figure 4] 4 shows the measurement results of the adsorption amount of the flexible ion-adsorbing electrode according to the present invention. [Diagram 5]4 shows the measurement results of the adsorption amount of the flexible ion-adsorbing electrode according to the present invention. [Figure 6] 4 shows the measurement results of the electrical conductivity of the flexible ion-adsorbing electrode according to the present invention. [Figure 7] 4 shows the measurement results of the flexibility of the flexible ion-adsorbing electrode according to the present invention. [Figure 8] 4 shows the measurement results of the flexibility of the flexible ion-adsorbing electrode according to the present invention. [Figure 9] FIG. 2 is a diagram for explaining the outline of a contaminated soil remediation experiment using the contaminated soil remediation method according to the present invention. [Figure 10] 1 shows the results of a contaminated soil remediation experiment using the contaminated soil remediation method according to the present invention. [Figure 11] 1 shows the results of a contaminated soil remediation experiment using the contaminated soil remediation method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] 1 is a flow chart showing the steps of producing a flexible ion-adsorbing electrode according to the present invention. The flexible ion-adsorbing electrode according to the present invention is a mat-shaped electrode used in a horizontal electrode type electrokinetic method, and the production steps include a pretreatment step (step S1) of drying a conductive material, a mixing step (step S2) of mixing water, a conductive material, an adsorbent, and a binder, a solidification step (step S3) of dehydrating and solidifying the mixture obtained through the mixing step, a drying step (step S4) of drying the solidified material, a softening step (step S5) of immersing the dried solidified material in water to soften it, a compression step (step S6) of compressing the softened solidified material, and a finishing step (step S7) of drying the compressed solidified material.
[0029] In the flexible ion-adsorbing electrode according to the present invention, the raw materials of the electrode are a conductive material, an adsorbent, and a binder. The conductive material is preferably smoked charcoal, the adsorbent is preferably zeolite, and the binder is preferably abaca and starch powder.
[0030] Smoked charcoal is made by carbonizing rice husks. Smoked charcoal does not need to be crushed or classified. In addition to charcoal, other conductive materials such as carbonized wood and bamboo, activated carbon, etc. can be used.
[0031] The zeolite is not particularly limited, but is preferably one that has excellent adsorption performance for the pollutants to be adsorbed and removed. The zeolite may be either natural zeolite or synthetic zeolite, but is preferably one that is inexpensively available. Zeolite classified using a sieve and having a particle size of 53 μm or less can be suitably used.
[0032] Abaca is a durable, lightweight, and strong fibrous material obtained from the Manila hemp plant. The starch powder is not particularly limited, but it mainly acts as a binder for the zeolite.
[0033] A typical mixing ratio of the raw materials of the flexible ion-adsorbing electrode according to the present invention, that is, smoked charcoal, zeolite, abaca and starch powder, is 9.0-9.1 g of smoked charcoal, 1.0 g of abaca, 2.0 g of starch powder and 0.5-4.0 g of zeolite.
[0034] In the flexible ion-adsorbing electrode according to the present invention, the content of zeolite particularly affects the adsorption performance, and the higher the content of zeolite, the higher the adsorption performance. On the other hand, if the content of zeolite is extremely high, the electrical conductivity decreases and the shape retention decreases. From these points of view, the amount of zeolite added is 2.5 to 40%, preferably 5 to 20%, and more preferably 10 to 15%, in mass ratio to the charcoal + abaca, and may be appropriately selected depending on the type and concentration of contaminants at the place of use.
[0035] Hereinafter, the manufacturing process of the flexible ion-adsorbing electrode according to the present invention will be described in detail in comparison with conventional method 1 and conventional method 2, assuming that 9.1 g of charcoal, 1.0 g of zeolite, 1.0 g of abaca, and 2.0 g of starch powder are used as the conductive material, adsorbent, and binder, and that the water used in the mixing process (step S2) is 150 mL of boiling water.
[0036] In the pretreatment step (step S1), 9.1 g of charcoal, which is a conductive material, is dried. This drying operation is aimed at improving the dispersibility of the charcoal and improving the dehydration in the dehydration operation performed in the solidification step of step S3. Typically, drying is performed for 12 hours at 75°C using a thermostatic dryer.
[0037] The mixing step (step S2) is a step of mixing water, a conductive material, an adsorbent, and a binder, but in the present invention, the mixing step is carried out in two steps for the purpose of uniform mixing.
[0038] In the first mixing step (step S2-1), 2.0 g of starch powder, 1.0 g of zeolite, and 1.0 g of abaca are added to 150 mL of hot water, and the mixture is stirred and mixed using a stirrer. Dissolving starch powder in hot water increases the viscosity of the hot water (solution). By increasing the viscosity of the hot water, the zeolite and abaca, which have low specific gravity, can be submerged in the hot water once and prevented from floating up. This enables uniform mixing. In the first mixing step, the ratio of starch powder to hot water is higher than in conventional methods 1 and 2 in order to increase the viscosity of the hot water (solution). In conventional methods 1 and 2, 2.0 g of starch powder is added to 200 mL of hot water.
[0039] In the second mixing step (step S2-2), 9.1 g of charcoal is added to the mixture obtained in the first mixing step and mixed by stirring. The stirring speed in the second mixing step is preferably slower than that in the first mixing step. In the second mixing step, the slow stirring speed prevents the charcoal from being crushed or disintegrated.
[0040] The solidification step (step S3) is a step in which the mixture obtained in the second mixing step (step S2-2) is solidified by dehydrating it. To give a specific example, a mold for forming an electrode is prepared, the mixture is poured into it, and then suction filtration is performed using a vacuum pump to remove the moisture. A mesh is built into the mold to prevent unevenness in the electrode.
[0041] In the drying step (step S4), the solidified material obtained in the solidification step (step S3) is dried. This drying step is positioned as a pretreatment for the softening step of step S5, and the drying step (step S4) and the softening step (step S5) are set together. The drying step (step S4) is typically performed using a thermostatic dryer at 75°C for 12 hours.
[0042] In the softening step (step S5), the dried solidified material obtained in the drying step (step S4) is immersed in water to soften it. Typically, the dried solidified material is immersed in about 10 mL of water to soften it. The dried solidified material is softened by adding water again. When the dried solidified material is compressed, it is no longer possible to maintain the organic fiber state and the shape as an electrode. However, by softening the solidified material, it is possible to maintain the organic fiber state and the shape as an electrode even when compressed. This reduces the variation in the performance and characteristics of the final flexible ion-adsorbing electrode, and improves reproducibility.
[0043] In the compression step (step S6), the softened solidified material obtained in the softening step (step S5) is placed in a mold, and a press is used to compress the solidified material to these limited thicknesses. For example, when 9.1 g of smoked charcoal, 1.0 g of abaca, 2.0 g of starch powder, and 1.0 g of zeolite are used as raw materials, the thickness of the solidified material after the softening step (step S5) is about 10 mm, and it is compressed to the limit thickness of about 6 mm in the compression step (step S6). The compression operation is typically performed at a press pressure of 2.5 to 10 MPa for a press time of 1 minute.
[0044] The finishing step (step S7) is a step of drying the solidified material after the compression step (step S6), typically performed at 75° C. for 12 hours using a thermostatic dryer.
[0045] Through the above steps S1 to S7, a flexible ion-adsorbing electrode according to the present invention can be obtained.
[0046] Next, a method for evaluating the flexible ion-adsorbing electrode according to the present invention will be described. The evaluation items for the flexible ion-adsorbing electrode are (1) adsorptive property, (2) electrical conductivity, and (3) flexibility.
[0047] The method for evaluating the adsorptivity is as follows. A cesium solution was used to evaluate the adsorption. A cesium solution (hereinafter, solution) with a concentration of 500 ppb was prepared by mixing distilled water with a non-radioactive cesium standard solution (133Cs, 1000 mg / L) from Wako Pure Chemical Industries, Ltd. The flexible ion adsorption electrode (hereinafter, measurement electrode) was cut to 20 mm x 20 mm x 6 mm, and copper wire was wrapped around it. The copper wire was wrapped around it to prevent the measurement electrode from floating up and down in the solution.
[0048] 150 mL of the prepared solution was transferred to a container, and the measurement electrode wrapped with copper wire was hung inside the container. The container was sealed to prevent the solution from evaporating during the experiment. 48 hours after addition, the measurement electrode was removed from the solution, the solution was filtered, and the amount of cesium remaining in the solution was measured using an ICP mass spectrometer (Agilent Technologies, Agilent 7500 series). The amount of cesium adsorbed by the measurement electrode was calculated by subtracting this value from the initial value of the solution, and the amount of adsorption per weight of the measurement electrode added was obtained.
[0049] The evaluation method for the electrical conductivity is as follows. The measurement electrode was sandwiched between a pair of upper and lower copper plate electrodes. The lower copper plate electrode was sufficiently large compared to the measurement electrode, and the upper copper plate electrode was circular and had a diameter of 20 mm. In order to further reduce leakage current, a guard electrode was installed on the upper surface of the measurement electrode around the copper plate electrode.
[0050] The positive pole of a digital multimeter (R8340 / 8340A, ADVANTEST) was connected to the upper copper plate electrode, and the negative pole of the digital multimeter was connected to the lower copper plate, and a DC voltage was applied and the current was measured. The resistance was calculated from the voltage-current characteristics, and the conductivity was calculated from this value. The conductivity of the measurement electrode was measured when the measurement electrode was in a dry and wet state, and a voltage of 100 V was applied to the measurement electrode in the dry state, and 10 V was applied to the measurement electrode in the wet state. When applying the voltage, a pressure of 100 Pa was applied to the measurement electrode to reduce contact resistance.
[0051] For the measurement of wet conductivity, 2 mL of tap water (6900 μS / cm) was dropped onto the center of the measurement electrode in a range of 2 to 10 mL, and 5 minutes after the drop, a voltage was applied and the current value was recorded. The voltage was applied for a short period of time to prevent the conductivity from changing due to electrolysis.
[0052] The conductivity was calculated from the applied voltage, the measured current, and the area of the copper plate using equation (1). σ = I / V × L / S (1) where σ is the conductivity (S / m), I is the measured current (A), and V is the applied voltage (V). L is the distance between the electrodes (m), S is the area of the electrode (m 2 )
[0053] The flexibility is evaluated as follows. The measurement electrode used was a rectangular prism with long sides of 97 mm, short sides of 68 mm, and a thickness of 6 mm. One end of the long side was fixed with a width of 10 mm parallel to the short side, and a string was tied to the other end of the long side, with a 70 g weight attached to the string. A round bar was placed above the measurement electrode, and the middle part of the string was hooked onto the round bar, and the weight was lowered to lift the measurement electrode. The height H of the other end of the measurement electrode at this time was measured, and the flexibility was calculated.
[0054] The measurement electrode is fixed at one end with a width of 10 mm, so the maximum lift height H 0 The maximum lifting height H 0 The ratio of H / H 0× 100. As with the electrical conductivity, the flexibility was measured when the measurement electrode was in a dry state and when it was wetted by increasing the amount of dripping by 2 mL increments in the range of 2 to 10 mL.
[0055] Next, the characteristics of the flexible ion-adsorbing electrode obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention will be described while comparing them with Conventional Method 1 and Conventional Method 2. Here, data from the Examples described later will be referred to as appropriate.
[0056] Conventional method 1 does not include the pretreatment step (step S1), drying step (step S4), softening step (step S5), and compression step (step S6) among the steps of producing a flexible ion-adsorbing electrode according to the present invention, as shown in Fig. 1. In addition, the mixing step (step S2) is performed in one step.
[0057] Conventional method 2 does not include the pretreatment step (step S1), drying step (step S4), and softening step (step S5) among the steps of producing a flexible ion-adsorbing electrode according to the present invention, as shown in Fig. 1. In addition, the mixing step (step S2) is performed in one step.
[0058] Representative values when the flexible ion-adsorbing electrode obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention is evaluated by the above evaluation method are: adsorption is 50 to 65 mg / kg, conductivity is 5000 to 7000 μS / m in a wet state with 10 mL of water added, height H of the other end of the measuring electrode in a wet state with 10 mL of water added is 70 to 80 mm, and flexibility is 80 to 90%.
[0059] As shown in Table 2 of the Examples and in Figure 4, the adsorptivity of the flexible ion-adsorbing electrode according to the present invention was comparable to that of the flexible ion-adsorbing electrode obtained by Conventional Method 1. Although the data does not include zeolite, as shown in Figure 5, the adsorption amount of the flexible ion-adsorbing electrode according to the present invention increased in proportion to the pressing pressure in the compression step (step S6).
[0060] In addition, the adsorptivity of the flexible ion-adsorbing electrode according to the present invention was improved by more than 100 times compared to conventional method 2, as shown in Fig. 5. This shows that the adsorptivity can be improved by drying the solidified material and then immersing it in water to soften it prior to the compression step (step S6).
[0061] The conductivity of the flexible ion-adsorbing electrode according to the present invention in a wet state was comparable to that of the flexible ion-adsorbing electrode obtained by Conventional Method 2, as shown in FIG. 6 of the Example. Meanwhile, the conductivity was improved by about 7 to 8 times compared with that of Conventional Method 1. This shows that the compression step (step S6) contributes to improving the conductivity of the flexible ion-adsorbing electrode.
[0062] The flexibility of the flexible ion-adsorbing electrode according to the present invention in a wet state was about 0.8 to 0.9 times that of the flexible ion-adsorbing electrode obtained by conventional method 2, as shown in Example FIG. 7. On the other hand, it was about 8 to 10 times improved compared with conventional method 1. This shows that the compression step (step S6) contributes to improving the flexibility of the flexible ion-adsorbing electrode.
[0063] Table 1 shows the comparison results of the characteristics of the flexible ion-adsorbing electrodes obtained through the manufacturing processes of the flexible ion-adsorbing electrodes according to the present invention, conventional method 1, and conventional method 2.
[0064] [Table 1]
[0065] As described above, the flexible ion-adsorbing electrode obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention is superior in adsorptivity, conductivity, and flexibility compared to conventional methods. Furthermore, the flexible ion-adsorbing electrode obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention is superior in reproducibility of adsorptivity, conductivity, and flexibility. Although the flexible ion-adsorbing electrode in the mat shape has been described in the above embodiment, the flexible ion-adsorbing electrode may be in the form of a sheet.
[0066] 2 is a configuration diagram of a contaminated soil remediation apparatus 1 according to an embodiment of the present invention. The contaminated soil remediation apparatus 1 includes a flexible ion-adsorbing electrode 10 placed on a contaminated soil surface 101, an electrode 20 inserted into the contaminated soil 100, and a DC voltage application device 30.
[0067] The flexible ion-adsorbing electrode 10 is a mat- or sheet-shaped flexible ion-adsorbing electrode obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention. The flexible ion-adsorbing electrode 10 may have adsorptivity, electrical conductivity, and flexibility appropriate for the state of the contaminated soil 100 to be treated.
[0068] The state of the contaminated soil 100 includes the unevenness of the contaminated soil surface 101, the contaminants contained in the contaminated soil 100 and their concentrations, and the moisture content of the contaminated soil 100. Here, the contaminants include heavy metals such as lead, mercury, arsenic, cadmium, nickel, and hexavalent chromium, and radioactive cesium.
[0069] When the surface 101 of the contaminated soil is highly uneven, a flexible ion-adsorbing electrode 10 having excellent flexibility may be used. The adsorption properties of the flexible ion-adsorbing electrode 10 may be selected according to the type and concentration of the contaminant. When the moisture content of the contaminated soil 100 is low, a flexible ion-adsorbing electrode 10 having excellent conductivity may be used. However, the moisture content of the contaminated soil 100 can be addressed by providing separate water supply means and water sprinkling means (not shown) and using these to moisten the contaminated soil 100 and the flexible ion-adsorbing electrode 10.
[0070] The electrode 20 is an electrode pile 20 that can be inserted into the contaminated soil 100. The electrode pile 20 includes a conductive pile body 21, which is covered with an electrical insulating material 24 except for a tip end 22 and a base end 23 to which a DC voltage application device 30 is connected.
[0071] The DC voltage application device 30 is connected to the flexible ion-adsorbing electrode 10 and the base end 23 of the electrode pile 20 , and applies a DC voltage between the flexible ion-adsorbing electrode 10 and the electrode (electrode pile) 20 .
[0072] A method for purifying contaminated soil 100 using the contaminated soil purification device 1 will be described. As shown in FIG. 2, the flexible ion-adsorbing electrode 10 is placed on the surface 101 of the contaminated soil 100 to be treated. Meanwhile, the electrode 20 is inserted into the contaminated soil 100. The DC voltage application device 30 connects the flexible ion-adsorbing electrode 10 as the cathode and the electrode 20 as the anode, and applies a DC voltage between the flexible ion-adsorbing electrode 10 and the electrode (electrode pile) 20. This method is called the horizontal electrode electrokinetic method (FEM-EK method). When the flexible ion-adsorbing electrode 10 and / or the contaminated soil 100 are dry, water is supplied or sprayed as appropriate to moisten the flexible ion-adsorbing electrode 10 and / or the contaminated soil 100.
[0073] When a DC voltage is applied between the flexible ion-adsorbing electrode 10 and the electrode (electrode pile) 20, interfacial electrokinetic phenomena (electrokinetic phenomena) such as electrolysis, electrophoresis, and electroosmosis are induced. As a result, cationic contaminants contained in the contaminated soil 100 move to the side of the flexible ion-adsorbing electrode 10, which is the cathode, and are adsorbed by the flexible ion-adsorbing electrode 10. This enables the contaminated soil 100 to be purified.
[0074] As described above, the contaminated soil remediation device 1 has a simple device configuration and is easy to handle, and can be suitably used for in-situ remediation. As shown in the examples described later, the flexible ion-adsorbing electrode 10 according to the present invention, which uses zeolite as an adsorbent, has excellent cesium adsorption performance, and the contaminated soil remediation method according to the present invention can be suitably used for remediating soil contaminated with radioactive cesium.
[0075] FIG. 3(A) is a diagram for explaining a method for remediating contaminated soil as one embodiment of the present invention, and FIG. 3(B) is a diagram for explaining a method for remediating contaminated water as one embodiment of the present invention.
[0076] In this embodiment, the flexible ion-adsorbing electrode 10 obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention is used as an adsorbent to purify contaminated soil or contaminated water. As shown in the examples described later, the flexible ion-adsorbing electrode 10 of the present invention has excellent adsorption performance for pollutants and can be suitably used as an adsorbent.
[0077] Contaminated soil and contaminated water are not particularly limited, and examples of contaminated water include wastewater and effluent containing contaminants, such as heavy metals such as lead, mercury, arsenic, cadmium, nickel, and hexavalent chromium, and radioactive cesium.
[0078] To purify contaminated soil 100 using the flexible ion-adsorbing electrode 10 obtained through the manufacturing process of the flexible ion-adsorbing electrode according to the present invention as an adsorbent, the mat- or sheet-shaped flexible ion-adsorbing electrode 10 may be placed on the surface 101 of the contaminated soil 100 as shown in Fig. 3(A). When the flexible ion-adsorbing electrode 10 and / or the contaminated soil 100 are dry, water is supplied or sprayed as appropriate to moisten the flexible ion-adsorbing electrode 10 and / or the contaminated soil 100.
[0079] As a result, contaminants on the surface 101 of the contaminated soil 100 are adsorbed by the flexible ion-adsorbing electrode 10, and the contaminated soil 100 is purified. As another method, the flexible ion-adsorbing electrode 10 may be buried in the contaminated soil 100. If necessary, the contaminated soil 100 and the flexible ion-adsorbing electrode 10 may be brought into contact with each other.
[0080] To purify contaminated water 200 using the flexible ion-adsorbing electrode 10 obtained through the manufacturing process of the flexible ion-adsorbing electrode of the present invention as an adsorbent, the flexible ion-adsorbing electrode 10 is simply immersed in the contaminated water 200 as shown in Figure 3 (B).
[0081] As a result, contaminants contained in the contaminated water 200 are adsorbed by the flexible ion-adsorbing electrode 10, and the contaminated water 200 is purified. As another method, the contaminated water may be poured over the flexible ion-adsorbing electrode 10. If necessary, the contaminated water 200 and the flexible ion-adsorbing electrode 10 may be brought into contact with each other.
[0082] The flexible ion-adsorbing electrode 10 used in the contaminated soil purification method and the contaminated water purification method of this embodiment is flexible, and further, if a mat- or sheet-shaped flexible ion-adsorbing electrode 10 is used, it is easy to recover the flexible ion-adsorbing electrode 10 with adsorbed pollutants. EXAMPLES
[0083] Example 1 This is a flexible ion-adsorbing electrode produced by the method for producing a flexible ion-adsorbing electrode according to the present invention. 2.0 g of starch powder, 0.5 g of natural zeolite (Tohoku Zeolite Industrial Co., Ltd.) of 53 μm or less that was crushed with a mixer (SKS-H TIGER) and classified with a sieve (SKH-01 AS ONE), and 1.0 g of abaca were added to 150 mL of hot water, and the mixture was stirred and mixed at 1000 rpm with a stirrer (SMT-102 AS ONE). Then, 9.1 g of smoked charcoal that had been dried at 75°C for 12 hours in a thermostatic dryer (STAC P-50K AS ONE) was added, and the mixture was stirred and mixed at 500 rpm.
[0084] The mixture was poured into a mold for forming an electrode, and the mixture was filtered by suction using a vacuum pump to remove water and obtain a solidified product. A mesh was incorporated into the mold to prevent the electrode from becoming non-uniform. The solidified product was then dried at 75°C for 12 hours using a thermostatic dryer.
[0085] The dried solid was immersed in about 10 mL of water to soften the solid. The softened solid was then placed in a compression molding mold and compression molded for 1 minute at a pressure of 2.5 MPa using a heat press (H300-01K AS ONE). The compression molded solid was then dried at 75°C for 12 hours using a thermostatic dryer to obtain a flexible ion-adsorbing electrode.
[0086] Examples 2 to 5, Reference Examples 1 to 3 The zeolite content and the pressing pressure of a heat press machine (H300-01K AS ONE) were changed, and flexible ion-adsorbing electrodes were produced in the same manner as in Example 1. Reference Examples 1 to 3 are flexible ion-adsorbing electrodes that do not contain zeolite.
[0087] Comparative Example 2 This is a flexible ion adsorption electrode made by conventional method 1. 2.0 g of starch powder was dissolved in 200 mL of hot water, and 0.5 g of natural zeolite (Tohoku Zeolite Industry Co., Ltd.) of 53 μm or less that had been crushed in a mixer (SKS-H TIGER) and classified using a sieve (SKH-01 AS ONE) was added to the solution, along with 1.0 g of abaca and 9.0 g of smoked charcoal, and the mixture was thoroughly stirred until homogenous.
[0088] The mixture was poured into a mold for forming an electrode, and the water was removed by suction filtration using a vacuum pump to obtain a solidified material. A mesh was incorporated into the mold to prevent unevenness of the electrode. The solidified material was then dried at 75°C for 12 hours using a thermostatic dryer to obtain a flexible ion-adsorbing electrode.
[0089] Comparative Examples 1, 3 to 5 Flexible ion-adsorbing electrodes were prepared in the same manner as in Comparative Example 2, except that the zeolite content was changed.
[0090] Comparative Example 7 This is a flexible ion adsorption electrode made by conventional method 2. 2.0 g of starch powder was dissolved in 200 mL of hot water, to which 0.5 g of natural zeolite (Tohoku Zeolite Industry Co., Ltd.) of 53 μm or less that had been crushed in a mixer (SKS-H TIGER) and classified using a sieve (SKH-01 AS ONE) was added, along with 1.0 g of abaca and 9.0 g of smoked charcoal, and the mixture was thoroughly stirred until homogenous.
[0091] The mixture was poured into a mold for forming an electrode, and the mixture was filtered by suction using a vacuum pump to remove the moisture and obtain a solidified material. A mesh was incorporated into the mold to prevent unevenness in the electrode. The solidified material was then placed into a mold for compression molding, and compression molded for 1 minute at a pressure of 2.5 MPa using a heat press (H300-01K AS ONE). The compressed solidified material was then dried at 75°C for 12 hours using a thermostatic dryer to obtain a flexible ion-adsorbing electrode.
[0092] Comparative Examples 6, 8 to 13 Flexible ion-adsorbing electrodes were produced in the same manner as in Comparative Example 7, except that the zeolite content and the pressing pressure of a heat press machine (H300-01K AS ONE) were changed.
[0093] The flexible ion-adsorbing electrodes of Examples 1 to 5, Reference Examples 1 to 3, Comparative Examples 1 to 5, and Comparative Examples 6 to 13 were measured for adsorptivity, conductivity, and flexibility by the methods described in paragraphs
[0046] to
[0054] . The results are shown in Table 2 and Figures 4 to 8. In the results shown in Table 2 and Figures 4 to 8, the conductivity and flexibility are values in a wet state with 10 mL of water added. The adsorptivity of Comparative Examples 1 and 2 was evaluated using a 50 ppb cesium solution.
[0094] [Table 2]
[0095] The flexible ion-adsorbing electrode obtained by the manufacturing method according to the present invention had an adsorption amount of 51.6 to 58.4 mg / kg, a conductivity of 5340 to 6100 μS / m, and a flexibility of 79 to 86% in a zeolite content range of 5 to 20 wt %.
[0096] The flexible ion-adsorbing electrode obtained by the manufacturing method according to Conventional Method 1 had an adsorption amount of 55.9 mg / kg, a conductivity of 800 to 850 μS / m, and a flexibility of 7.5 to 11% in a zeolite content range of 5 to 20 wt%.
[0097] The flexible ion-adsorbing electrode obtained by the manufacturing method according to Conventional Method 2 had a conductivity of 6000 to 6700 μS / m and a flexibility of 91 to 103% when the zeolite content was in the range of 5 to 20 wt %.
[0098] Contaminated soil purification experiment 1 A contaminated soil purification experiment was carried out using the contaminated soil purification device 1 according to the present invention in the following manner. For the flexible ion-adsorbing electrode 10, activated carbon was used instead of charcoal as the conductive material, and the flexible ion-adsorbing electrode 10 was prepared in the same manner as in Example 2. The zeolite content was 10 wt %. For the electrode 20, a stainless steel mesh 20 was used.
[0099] Fig. 9 shows a contaminated soil purification experimental apparatus 1. Uncontaminated soil 110 was filled into a container 150 to a thickness of 20 mm. A stainless steel mesh 20 was placed on the uncontaminated soil 110, and artificially contaminated soil 100 with a cesium concentration of 50 ppm was filled on top of the stainless steel mesh 20 to a thickness of 50 mm. The filled uncontaminated soil 110 weighed 150 g, and the filled contaminated soil 100 weighed 350 g, and tap water was added to both to adjust the water content to 60%. After filling the container 150 with soil, a lid 160 was placed on top.
[0100] The cathode of the DC voltage application device 30 was connected to the flexible ion-adsorbing electrode 10, and the anode was connected to the stainless steel mesh 20. Furthermore, a 1 Ω resistor 40 was attached midway through the cable connecting the DC voltage application device 30 and the flexible ion-adsorbing electrode 10, and a data logger 50 was installed in parallel with the resistor 40. The distance between the flexible ion-adsorbing electrode 10 and the stainless steel mesh 20 was 50 mm.
[0101] A voltage of 10 V (200 V / m) was applied between both electrodes for 7 consecutive days via the DC voltage application device 30. After that, the contaminated soil 100 was divided into upper, middle, and lower layers, soil was collected from each layer, and the cesium concentration in the flexible ion adsorption electrode 10 and in the soil of each layer was measured. Data without voltage application was also obtained.
[0102] The results of the experiment are shown in Figures 10 and 11. Figure 10 shows the cesium concentration in the contaminated soil 100, and Figure 11 shows the measurement results of the cesium concentration adsorbed to the flexible ion-adsorbing electrode 10. When a voltage was applied for seven consecutive days, the cesium concentrations in each layer and the flexible ion-adsorbing electrode 10 were 47 ppm in the lower layer, 49 ppm in the middle layer, and 54 ppm in the upper layer, and the cesium concentration in the flexible ion-adsorbing electrode 10 was 21 ppm. The cesium concentration in the uncontaminated soil 110 was 6.4 ppm, and the closer to the flexible ion-adsorbing electrode 10 the higher the cesium concentration, indicating that cesium is migrating toward the flexible ion-adsorbing electrode 10.
[0103] When no voltage was applied, the cesium concentrations in each layer and the flexible ion-adsorbing electrode 10 were 52 ppm in the lower layer and 53 ppm in the upper layer, and the cesium concentration in the flexible ion-adsorbing electrode 10 was 4.4 ppm. The cesium concentration in the uncontaminated soil 110 was 10 ppm. There was almost no difference in cesium concentration between the upper and lower layers of the contaminated soil 100, and it can be seen that when no voltage was applied, cesium did not move toward the flexible ion-adsorbing electrode 10.
[0104] The cesium concentration measured before (initial stage) use of the flexible ion-adsorbing electrode 10 was 0.66 ppm, which shows that even without applying a voltage, the flexible ion-adsorbing electrode 10 adsorbs cesium simply by bringing the flexible ion-adsorbing electrode 10 into contact with the contaminated soil 100. This shows that the flexible ion-adsorbing electrode 10 functions as an adsorbent for cesium.
[0105] Contaminated soil purification experiment 2 Contaminated soil remediation experiment 2 was carried out in the same manner as contaminated soil remediation experiment 1, but using a different soil. Leaf mold with a cesium concentration of 100 ppm was used as contaminated soil 100. The filled uncontaminated soil 110 weighed 100g, and the contaminated soil 100 weighed 280g, and ion-exchanged water was added to both to bring the water content to 200%. The filling heights of the uncontaminated soil 110 and the contaminated soil 100 were the same as in contaminated soil remediation experiment 1.
[0106] When a voltage was applied for seven consecutive days, the cesium concentrations in the lower and upper halves of the contaminated soil 100 were 41 ppm and 150 ppm, respectively. The cesium concentration in the uncontaminated soil 110 was 1.7 ppm, and the closer to the flexible ion-adsorbing electrode 10 the higher the cesium concentration, suggesting that cesium is migrating toward the flexible ion-adsorbing electrode 10.
[0107] When no voltage was applied, the cesium concentrations in the lower and upper halves of the contaminated soil 100 were 87 ppm and 100 ppm, respectively, and the cesium concentration in the uncontaminated soil 110 was 7.8 ppm. It can be seen that the difference in cesium concentration between the lower and upper halves of the contaminated soil 100 is small, and that when no voltage is applied, cesium hardly moves toward the flexible ion adsorption electrode 10.
[0108] Contaminated soil purification experiment 3 Contaminated soil remediation experiment 3 was carried out in the same manner as contaminated soil remediation experiment 2, except that the water added to the contaminated soil 100 was changed from ion-exchanged water to distilled water.
[0109] When a voltage was applied for seven consecutive days, the cesium concentrations in the lower and upper halves of the contaminated soil 100 were 64 ppm and 120 ppm, respectively. The cesium concentration in the uncontaminated soil 110 was 2.4 ppm, and the closer to the flexible ion-adsorbing electrode 10 the higher the cesium concentration, suggesting that cesium is migrating toward the flexible ion-adsorbing electrode 10.
[0110] When no voltage was applied, the cesium concentrations in the lower and upper halves of the contaminated soil 100 were 110 ppm and 97 ppm, respectively, and the cesium concentration in the uncontaminated soil 110 was 7.7 ppm. This result shows that when no voltage is applied, cesium does not move toward the flexible ion adsorption electrode 10. [Explanation of symbols]
[0111] 1. Contaminated soil purification equipment 10 Flexible ion adsorption electrode 20 Electrode, electrode pile, stainless steel mesh 21 Pile body 22 Tip 23 Proximal end 24 Electrical insulation materials 30 DC voltage application device 40 Resistance 50 Data Logger 100 Contaminated soil 101 Contaminated soil surface 110 Uncontaminated soil 150 containers 160 Lid 200 Contaminated Water
Claims
1. A method for producing a flexible ion-adsorbing electrode, comprising: a mixing step of mixing water, a conductive material, an adsorbent, and a binder; a solidification step of dehydrating and solidifying the mixture obtained through the mixing step; a compression step of compressing the solidified product; and a finishing step of drying the compressed solidified product, Between the solidifying step and the compressing step, a drying step of drying the solidified material; a softening step of immersing the dried solid obtained through the drying step in water to soften it; A method for producing a flexible ion-adsorbing electrode, comprising:
2. The flexible ion-adsorbing electrode is a mat-shaped electrode used in a horizontal electrode type electrokinetic method, 2. The method for producing a flexible ion-adsorbing electrode according to claim 1, wherein the conductive material is charcoal, the adsorbent is zeolite, and the binder is abaca and starch powder.
3. The mixing step comprises: a first mixing step of stirring and mixing hot water, the starch powder, the zeolite, and the abaca; A second mixing step of stirring and mixing the mixture obtained in the first mixing step with the charcoal; Including, 3. The method for producing a flexible ion-adsorbing electrode according to claim 2, wherein the stirring speed in the second mixing step is slower than the stirring speed in the first mixing step.
4. 4. The method for producing a flexible ion-adsorbing electrode according to claim 1, further comprising a pretreatment step of drying the conductive material before the mixing step.
5. A flexible ion-adsorbing electrode in which charcoal, zeolite, abaca and starch powder are mixed and formed into a mat shape, The amount of adsorption per unit weight of the flexible ion-adsorbing electrode measured by immersing it in a non-radioactive cesium solution with a concentration of 500 ppb is 50 to 65 mg / kg, the electrical conductivity of the flexible ion-adsorbing electrode measured by applying a DC voltage of 10 V in a wet state is 5000 to 7000 μS / m; The flexible ion-adsorbing electrode has dimensions of a long side of 97 mm, a short side of 68 mm, and a thickness of 6 mm, and is fixed with a width of 10 mm from one end of the long side to the other end, and is characterized in that when the other end of the long side is pulled up with a load of 70 g, the lifted height is 70 to 80 mm.
6. A flexible ion-adsorbing electrode obtained by the method for producing a flexible ion-adsorbing electrode according to any one of claims 1 to 4 or the flexible ion-adsorbing electrode according to claim 5, which is placed on a surface of contaminated soil to be treated, A contaminated soil purification device, characterized in that contaminants in the contaminated soil are adsorbed to the flexible ion adsorption electrode by electrokinetic phenomena, thereby purifying the contaminated soil.
7. The flexible ion-adsorbing electrode; an electrode different from the flexible ion-adsorbing electrode; a DC voltage application means for applying a DC voltage between the flexible ion-adsorbing electrode and the electrode; Equipped with 7. The contaminated soil purification apparatus according to claim 6, wherein a DC voltage is applied between the flexible ion-adsorbing electrode and the electrode, causing the electrokinetic phenomenon.
8. The electrode is an electrode pile; 8. The contaminated soil remediation apparatus according to claim 7, wherein the electrode pile is inserted into the contaminated soil.
9. 9. The contaminated soil remediation apparatus according to claim 6, further comprising a water supply means for wetting the contaminated soil and / or the flexible ion-adsorbing electrode.
10. 9. The contaminated soil purification apparatus according to claim 6, wherein the contaminant is one or more of heavy metals and radioactive cesium.
11. A method for purifying contaminated soil, comprising the steps of: using the contaminated soil purification apparatus according to any one of claims 6 to 10; and adsorbing contaminants in the contaminated soil to the flexible ion-adsorbing electrode to purify the contaminated soil.
12. A method for purifying contaminated soil, comprising using a flexible ion-adsorbing electrode obtained by the method for producing a flexible ion-adsorbing electrode according to any one of claims 1 to 4 or the flexible ion-adsorbing electrode according to claim 5 as an adsorbent for contaminants, A method for remediating contaminated soil, comprising contacting the flexible ion-adsorbing electrode with the contaminated soil to be treated, thereby adsorbing contaminants in the contaminated soil and purifying the contaminated soil.
13. 13. The method for remediating contaminated soil according to claim 12, wherein the contaminated soil and / or the flexible ion-adsorbing electrode are in a wet state.
14. 14. The method for remediating contaminated soil according to claim 12 or 13, wherein the contaminant is one or more of heavy metals and radioactive cesium.
15. A method for purifying polluted water, comprising using a flexible ion-adsorbing electrode obtained by the method for producing a flexible ion-adsorbing electrode according to any one of claims 1 to 4 or the flexible ion-adsorbing electrode according to claim 5 as an adsorbent for pollutants, A method for purifying polluted water, comprising contacting the flexible ion-adsorbing electrode with polluted water to be treated, thereby adsorbing pollutants in the polluted water, and purifying the polluted water.
16. 16. The method for purifying contaminated water according to claim 15, wherein the contaminated water is wastewater or waste liquid containing the contaminants.
17. 17. The method for purifying contaminated water according to claim 15 or 16, wherein the contaminant is one or more of heavy metals and radioactive cesium.
Citation Information
Patent Citations
Apparatus and method for decontaminating contaminated earth
JP2017136515A