Dental investment material

The use of silicone powder in dental investment materials addresses the challenge of metal casting shrinkage at low mold temperatures by providing stable, irreversible expansion, ensuring consistent mold compensation and preventing surface issues.

JP2024141194AActive Publication Date: 2024-10-10SHOFU INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023052703
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing dental investment materials struggle to effectively compensate for metal casting shrinkage when mold temperatures are low, leading to issues such as reaction layers, rough surfaces, and inconsistent mold expansion due to factors like oxidation and temperature variability.

Method used

Incorporation of silicone powder, which irreversibly expands upon heating, into the dental investment material to stabilize mold expansion and compensate for metal casting shrinkage even at lower mold temperatures.

Benefits of technology

Stable mold expansion is maintained, ensuring consistent compensation for metal casting shrinkage without oxidation or decomposition, even at temperatures below 700°C, thereby preventing surface roughness and reaction layers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an irreversible expansion agent-containing dental investment material applicable for metal casting, where the dental investment material incorporates a component that exhibits irreversible expansion upon heating, making it possible to compensate for metal casting shrinkage even at low mold temperatures.SOLUTION: A dental investment material powder comprises silicone powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dental investment material containing an irreversible expander for use in the dental field. [Background technology]

[0002] When indirectly producing metal prosthetic devices for dental prosthetic restoration, the method known as the lost wax method is generally used. This method is explained as follows.

[0003] A model that reproduces the patient's dental defect shape outside the mouth is made by taking a mold shape of the dental defect shape using a mold material called an impression material, and injecting a model material such as gypsum into it. Next, the shape of the shape to be restored is reproduced on this model using wax to obtain a prototype. This prototype is called a wax pattern. A mold is made to replace the obtained wax pattern with metal. The mold is made by pouring a slurry made of a powder material called an investment material and a liquid material such as water or / and a colloidal silica aqueous solution into the mold material to embed the wax pattern. After the investment material hardens, it is heated to incinerate the wax pattern in the mold, and the molten metal is poured into the space of the mold that has been formed. After further cooling, the mold is broken and the cast is removed to obtain the desired metal prosthetic device. The lost wax method is generally used to make these prosthetic devices.

[0004] Commonly known investment materials include gypsum-based investment materials used for alloys with relatively low melting points (low melting alloys) such as gold alloys, silver alloys, and gold-silver-palladium alloys; phosphate-based investment materials used for alloys with relatively high melting points (high melting alloys) such as gold alloys for porcelain fusing, semi-precious alloys for porcelain fusing, Ni-Cr alloys, and Co-Cr alloys; and non-phosphate-based investment materials including alumina cement and magnesia cement used for metals with higher melting points and higher activity such as titanium and titanium alloys. These investment materials are composed of powder and liquid materials. The powder materials include a binder that maintains the shape of the mold and a refractory material that gives the mold heat resistance. The liquid material is an aqueous solution containing water and / or colloidal silica. The powder and liquid materials are mixed in appropriate amounts, and the mixture reacts and hardens to produce the mold.

[0005] In general, in dental casting, casting shrinkage occurs when a molten alloy is poured into a mold cavity, and in order to ensure compatibility, an expanded mold is required to compensate for this casting shrinkage. Here, the casting shrinkage of metal refers to the solidification shrinkage when the molten alloy solidifies and the thermal shrinkage when the solidification is completed to room temperature. In order to obtain a mold that compensates for casting shrinkage, both the hardening expansion that occurs when the investment material hardens and the thermal expansion that occurs when the hardened mold is heated are used.

[0006] For example, the composition of phosphate-based investment materials is composed of powder materials containing magnesium oxide and primary ammonium phosphate as binders, refractory materials such as silica, alumina, and zirconium silicate, and liquid materials containing water and / or colloidal silica. A mold can be made by mixing and hardening these materials. By adjusting the concentration of the liquid material containing colloidal silica, it is possible to obtain a total expansion (the sum of hardening expansion and heating expansion) that matches the casting shrinkage of various metals.

[0007] The hardening expansion can be changed by the particle size and concentration of colloidal silica. Furthermore, when the hardened mold is heated to 700-1000°C to burn the wax pattern, thermal expansion also occurs. The sum of this hardening expansion and thermal expansion compensates for the metal casting shrinkage and adjusts the fit of the prosthetic device.

[0008] If the temperature of the mold when burning the wax pattern becomes higher than necessary, the molten metal and the mold material will react and burn, forming a reaction layer, or the surface of the casting may become rough overall or partially, causing roughness of the casting surface, and the compatibility may be deteriorated due to surface removal of the casting. For example, in the case of casting titanium, if the mold temperature is high, a thick reaction layer will be formed between the titanium and the mold, so casting in a mold with a high temperature of 700°C to 1000°C will cause a significant reaction, so it is necessary to avoid this, and preferably, casting in a mold with a temperature of 400°C or less, more preferably at room temperature, can suppress the reaction between the titanium and the mold.

[0009] However, when casting is performed at a mold temperature of 400°C or less, for example, silica used in refractory materials that expands when heated tends to shrink, and the casting shrinkage of metal may not be compensated for. Therefore, by adding a component that expands irreversibly when heated to the investment material, it is expected that the casting shrinkage of metal can be compensated for even when the mold temperature is low.

[0010] Patent Document 1 discloses a technique for compensating for metal casting shrinkage by adding metallic zirconium powder. Specifically, the technique involves heating metallic zirconium powder at high temperatures to oxidize it, and utilizing the volume expansion that occurs during this process to compensate for casting shrinkage. However, with this technique, metallic zirconium powder easily reacts with oxygen, hydrogen, nitrogen, and the like in the air, such as by oxidation, making it difficult to stably store the investment material for a long period of time.

[0011] Patent Document 2 discloses a technique for compensating for metal casting shrinkage by adding alumina and magnesia. Specifically, this technique involves heating alumina and magnesia at high temperatures, which causes them to react to generate spinel, which then expands irreversibly in volume, thereby compensating for casting shrinkage. However, in this technique, the spinel reaction occurs rapidly at a firing temperature of 1200°C or less, so the amount of expansion varies depending on the set temperature of the furnace for firing the mold. Therefore, in a furnace with poor temperature distribution, the amount of expansion differs in parts of the mold even within the same furnace, which may cause differences in the suitability of the mold.

[0012] Patent Document 3 discloses a technique for compensating for metal casting shrinkage by adding aluminum fine powder. Specifically, this technique involves mixing aluminum fine powder into an investment material, and expanding the mold by the pressure of the hydrogen gas generated. However, this technique has problems such as the generation of bubbles due to the reaction between the metal and water, the generation of cracks during heating, and roughness of the casting surface after casting. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] Japanese Patent Application Publication No. 61-9940 [Patent Document 2] Japanese Patent Application Publication No. 1-31549 [Patent Document 3] Japanese Patent Application Publication No. 59-218237 Summary of the Invention [Problem to be solved by the invention]

[0014] The present invention aims to provide a dental investment material that can be used for metal casting, which contains an irreversible expansion agent and is expected to compensate for the casting shrinkage of metal even when the mold temperature is low, by adding a component that expands irreversibly when heated. [Means for solving the problem]

[0015] As a result of extensive research into these problems, the present inventors have arrived at the present invention. That is, the present invention is a dental investment powder characterized by containing a silicone powder. Effect of the Invention

[0016] The effect of the present invention is that the mold expansion capable of compensating for the casting shrinkage of the metal can be maintained stably even when the mold temperature is low. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The dental investment material according to the present invention will be specifically described below. However, the present invention is not limited to the following examples. The dental investment material according to the present invention is composed of a powder material and a liquid material.

[0018] The silicone powder in the present invention includes silicone rubber powder, silicone resin powder, and composite silicone powder having a silicone rubber portion and a silicone resin portion.

[0019] The silicone rubber powder in the present invention is a crosslinked polysiloxane powder having a structure in which a linear silicone main chain is crosslinked, and contains as a functional group at least one of the following: alkyl groups, such as methyl groups, ethyl groups, propyl groups, butyl groups, pentyl groups, hexyl groups, heptyl groups, octyl groups, decyl groups, undecyl groups, dodecyl groups, tetradecyl groups, pentadecyl groups, hexadecyl groups, heptadecyl groups, octadecyl groups, nonadecyl groups, and icosyl groups; alkenyl groups, such as vinyl groups, allyl groups, propenyl groups, butenyl groups, pentenyl groups, hexenyl groups, heptenyl groups, octenyl groups, decenyl groups, undecenyl groups, and dodecenyl groups; allyl groups, such as phenyl groups, tolyl groups, and naphthyl groups; and aralkyl groups, such as benzyl groups and phenethyl groups. Specific examples of silicone resin powders include crosslinked powders of polydimethylpolysiloxane and polydiethylpolysiloxane. The silicone resin powder of the present invention is a polyorganosilsesquioxane powder having a silicone main chain crosslinked in a three-dimensional network shape, and contains at least one of the following functional groups: alkyl groups, such as methyl groups, ethyl groups, propyl groups, butyl groups, pentyl groups, hexyl groups, heptyl groups, octyl groups, decyl groups, undecyl groups, dodecyl groups, tetradecyl groups, pentadecyl groups, hexadecyl groups, heptadecyl groups, octadecyl groups, nonadecyl groups, and icosyl groups; alkenyl groups, such as vinyl groups, allyl groups, propenyl groups, butenyl groups, pentenyl groups, hexenyl groups, heptenyl groups, octenyl groups, decenyl groups, undecenyl groups, and dodecenyl groups; allyl groups, such as phenyl groups, tolyl groups, and naphthyl groups; and aralkyl groups, such as benzyl groups and phenethyl groups. Specific examples of silicone resin powder include polymethylsilsesquioxane and polyphenylsilsesquioxane powder. The silicone composite powder in the present invention is a powder having a structure in which the silicone rubber powder particles are coated with the resin of the silicone resin powder. The functional groups applied to the silicone rubber powder and the silicone resin powder are the same as those described above. Of the above silicone powders, it is most preferable to use silicone resin powder, since it contains a relatively small amount of carbon within its structure and causes the greatest expansion of the mold.

[0020] When the wax pattern is burned, the mold is heated in the temperature range of 700 to 1000 ° C., so that the oxidation start temperature of the silicone powder is preferably 700 ° C. or less in order to realize the effect of the present invention. The silicone powder in the present invention expands in volume by oxidizing at about 400 ° C., and by pushing apart the particles of other refractory materials, the mold expands, and even if it is cooled to room temperature, the oxidized and decomposed silicone powder does not shrink, and the irreversible expansion of the mold is maintained. In the gypsum-based investment material, since the gypsum, which is the binding material, decomposes at 750 ° C. or more and shows significant shrinkage, it is desirable to bake the gypsum-based investment material at 750 ° C. or less. Therefore, if the oxidation start temperature of the silicone powder to be added is higher than 700 ° C., sufficient effect may not be obtained.

[0021] The amount of silicone powder added to the powder material of the present invention is preferably 0.1 to 10.0 wt%, more preferably 0.5 to 3.0 wt%. The silicone powder of the present invention, when added in an appropriate amount, efficiently propagates the expansion caused by the crystal growth of the binder when the investment material hardens, thereby increasing the hardening expansion. The investment material to which the silicone powder of the present invention is added increases the amount of expansion of the mold when hardening, and the mold expands irreversibly when heated, so that the expansion of the mold is maintained even when the mold is cooled, and the casting shrinkage of the metal can be compensated for. If the amount of silicone powder is less than 0.1 wt%, there is a possibility that the expansion that compensates for the casting shrinkage cannot be obtained, and if it exceeds 10.0 wt%, there is a possibility that the investment material may crack or crack when incinerated.

[0022] The average particle size of the silicone powder in the present invention is preferably 0.1 to 30 μm, and particularly preferably 0.5 to 5 μm. If it is 30 μm or more, the investment material may break or crack when incinerated, and if it is 0.1 μm or less, there is a problem that expansion sufficient to compensate for casting shrinkage cannot be obtained. In the present invention, the term "average particle size" refers to the particle size at an integrated value of 50% in the particle size distribution determined by a precision particle size measuring device using the Coulter principle.

[0023] The dental investment material of the present invention is not particularly limited in the type of binder in order to achieve the effects of the present invention, and the same effects can be obtained with a phosphate-based investment material using ammonium phosphate and magnesium oxide as binders, a gypsum-based investment material using gypsum dihydrate and gypsum hemihydrate as binders, and a non-phosphate-based investment material using alumina cement or magnesia cement as binder.

[0024] The following describes a phosphate-based investment material as an example. The phosphate-based investment material contains magnesium oxide and primary ammonium phosphate in powder form, which reacts with the liquid material to cause a hardening reaction and form a mold.

[0025] The type of magnesium oxide contained in the powder constituting the dental investment material of the present invention is not particularly limited, but the higher the purity, the more preferable it is, and the more preferable it is finely divided. Hereinafter, the "average particle size" in the present invention means the particle size at the cumulative value of 50% in the particle size distribution obtained by the laser diffraction / scattering method. The average particle size of magnesium oxide is not particularly limited, but the average particle size is preferably 15 to 40 μm, and more preferably 20 to 30 μm. In addition, in the particle size distribution of magnesium oxide, particles of 100 μm or more are preferably within 1.0 wt%, and more preferably no particles of 100 μm or more are included. Furthermore, particles having a plurality of average particle sizes may be combined. When particles having a plurality of average particle sizes are combined, the average particle size after combination is preferably 15 to 40 μm. In order to obtain the effects of the present invention in the dental investment material of the present invention, the blending amount of magnesium oxide is preferably in the range of 1 to 30 wt% with respect to the powder material of the investment material. If it is less than 1 wt%, sufficient mold strength cannot be obtained, and it may become insufficient as a mold material, and if it exceeds 30 wt%, the breathability of the mold decreases, and cracks or fissures may occur when incinerated.

[0026] The primary ammonium phosphate contained in the powder material constituting the dental investment material of the present invention is not particularly limited as long as it is soluble, and any average particle size or shape can be used without any problem. However, the maximum particle size of primary ammonium phosphate is preferably small in order to function as a binder in the investment material. In order to maintain the smoothness of the surface of the cast metal, it is preferable that there are no particles with a particle size of 60 μm or more, and more preferably, among the particles with a particle size of 60 μm or less, the particles with a particle size of 25 μm or less are 10 to 45 wt%, and even more preferably, 20 to 35 wt%. In order to express the effect of the present invention in the dental investment material of the present invention, the blending amount of primary ammonium phosphate must be in the range of 1 to 30 wt% with respect to the powder material of the investment material. If the blending amount is less than 1 wt%, sufficient mold strength cannot be obtained, and the mold material becomes insufficient, and if it exceeds 30 wt%, the breathability of the mold decreases, and cracks or fissures may occur during incineration.

[0027] Next, the compounding ratio of magnesium oxide and ammonium phosphate contained in the powder constituting the dental investment material of the present invention is preferably magnesium oxide / ammonium phosphate=0.3 to 1.0 by weight, and more preferably magnesium oxide / ammonium phosphate=0.4 to 0.6.

[0028] Taking a gypsum-based investment material as an example, the type and manufacturing method of the hemihydrate gypsum contained in the powder material constituting the dental investment material of the present invention are not particularly limited, and for example, conventionally known α-type hemihydrate gypsum or β-type hemihydrate gypsum can be used alone or in combination. In order to achieve the effects of the present invention in the dental investment material of the present invention, the amount of hemihydrate gypsum is preferably in the range of 10 to 80 wt%, more preferably 20 to 50 wt%, based on the powder material of the investment material. If the amount is less than 10 wt%, sufficient mold strength cannot be obtained, making the material insufficient as a mold material, and if it exceeds 80 wt%, problems may occur such as the surface properties of the cast being rough or sufficient thermal expansion not being obtained.

[0029] Taking a non-phosphate-based investment material as an example, the type and manufacturing method of the alumina cement contained in the powder material constituting the dental investment material of the present invention are not particularly limited, and for example, commercially available grade products can be used. In order to achieve the effects of the present invention in the dental investment material of the present invention, the amount of alumina cement mixed is preferably in the range of 2 to 50 wt% relative to the powder material of the investment material, and more preferably 10 to 35 wt%. If the amount is less than 2 wt%, sufficient mold strength cannot be obtained, making it insufficient as a mold material, and if it exceeds 50 wt%, a problem of insufficient thermal expansion may occur.

[0030] Next, the powder material constituting the dental investment material of the present invention contains a refractory material, and any refractory material used in dental investment materials can be used without any restrictions. Specific examples of such materials include quartz, cristobalite, zirconium silicate, zirconia, spinel, alumina, amorphous silica, calcia, mullite, and yttria. In order to adjust the fluidity of the investment material, refractory materials with an average particle size of 5 to 300 μm can be used in combination.

[0031] Although there is no particular restriction on the amount of these refractory materials to be blended in the dental investment material of the present invention in order to achieve the effects of the present invention, the amount of the refractory materials having low thermal expansion coefficients, such as zirconium silicate, zirconia, spinel, alumina, and amorphous silica, blended in total is preferably 10 to 90 wt%. If the amount is less than 5 wt% or exceeds 90 wt%, cracks may occur in the investment material.

[0032] The liquid material to be used in combination with the dental investment powder of the present invention is not limited, but may be an aqueous colloidal silica solution, an aqueous alumina sol solution, an aqueous zirconia sol solution, water, or the like, and is particularly preferably an aqueous colloidal silica solution. EXAMPLES

[0033] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The particle size of the silicone resin powder was measured using a precision particle size measuring device using the Coulter principle. The particle size of magnesium oxide was measured using a laser diffraction / scattering type particle size distribution measuring device.

[0034] (Silicone resin powder used) Silicone resin powder with an average particle size of 2 μm was used as the irreversible expanding agent. (Preparation of Magnesium Oxide) The magnesium oxide raw material was crushed and classified to prepare a powder with an average particle size of 25 μm and a ratio of particles of 100 μm or more within 1 wt %. (Preparation of Ammonium Monophosphate) Ammonium monophosphate was pulverized and then passed through a 250 mesh (60 μm) sieve, and the particles that passed through a 500 mesh (25 μm) sieve were adjusted to account for 30 wt % of the particles. (Preparation of Hemihydrate Gypsum) Hemihydrate gypsum was crushed and classified to prepare a powder with an average particle size of 25 μm and a ratio of particles of 100 μm or more within 1 wt %. (Preparation of alumina cement) The alumina cement raw material was crushed and classified to prepare a mixture with an average particle size of 3 μm and a ratio of particles of 50 μm or more within 1 wt%. (Preparation of fireproof material) The refractory materials used were alumina (77 μm, all-through), zirconium silicate (200 mesh (77 μm), all-through), cristobalite (200 mesh (77 μm), all-through), quartz (200 mesh (77 μm), all-through), and zirconia (200 mesh (77 μm), all-through).

[0035] (Powder Mixing) The powder materials shown in the example compositions in Tables 1 to 5 were mixed together, and the powder was stirred for 1 minute in a vinyl bag with a small amount of air added.The powder was then sieved through a 1000 μm sieve to obtain the powder materials.

[0036] (Adjustment of liquid material (aqueous colloidal silica solution)) As the aqueous solution containing colloidal silica, SN-ZL (manufactured by Nissan Chemical Industries, Ltd.) was used. (Adjustment of liquid material (water)) Tap water was used as the water for mixing.

[0037] (Measurement of linear thermal expansion coefficient) In the following Examples 1 to 14 and 16 to 19, the powder and liquid materials shown in the composition table were mixed and hardened, and then heated to 900°C and cooled to 25°C according to the standard of JIS T 6612:2020 (dental high-temperature casting investment material, pressed ceramics investment material, and ceramics refractory model material), and the linear thermal expansion coefficient at room temperature was measured. In Example 15, the maximum heating temperature was set to 700°C, and the linear thermal expansion coefficient at room temperature was measured by the above method. (Measurement of hardening expansion rate) In the following Examples 1 to 19, the powder and liquid materials listed in the composition table were used, and a stainless steel ring measuring 40 mm in diameter and 40 mm in height was lined with a ring liner, the inside of which was filled with the mixed slurry, and the hardening expansion rate was measured by placing a dial gauge on the upper surface of the mold. (Evaluation of overall expansion rate) The overall expansion coefficient in the following examples was calculated as the sum of the linear thermal expansion coefficient and the curing expansion coefficient at room temperature obtained using the powder materials and liquid materials shown in the composition table.

[0038] Overall expansion rate (comparison sample) For comparison, a reference sample was prepared which did not contain silicone powder, in contrast to the compositions of the examples, and the overall expansion rate was evaluated.

[0039] [Table 1]

[0040] [Table 2]

[0041] [Table 3]

[0042] [Table 4]

[0043] In Examples 1 to 19, the total expansion coefficient was 0.1% or more compared to the total expansion coefficient (comparison sample), so it was found that it was possible to compensate for the casting shrinkage of metal even when the mold temperature was low. It was confirmed from Examples 13 and 14 that it can be used regardless of the type of binder. (effect) From the above results, it is apparent that the present invention provides a dental investment material that can compensate for metal casting shrinkage by using silicone powder even when the mold temperature is low.

Claims

1. A dental investment powder comprising a silicone powder.

2. 2. The dental investment powder according to claim 1, characterized in that the silicone powder is contained in an amount of 0.1 to 10.0 wt %.

3. 3. The dental investment material powder according to claim 1, wherein the silicone powder is a silicone resin powder.

4. 4. The dental investment material according to claim 1, comprising 1 to 30 wt % magnesium oxide and 1 to 30 wt % ammonium phosphate.

5. 4. The dental investment material according to claim 1, further comprising 10 to 80 wt % of hemihydrate gypsum as a binder.

6. 4. The dental investment material according to claim 1, further comprising 2 to 50 wt % of alumina cement as a binder.

Citation Information

Patent Citations

  • Embedding material for dental molding

    JP1988141906A

  • Molding material

    JP1991035839A

  • Dental kit and method of retracting grooves

    JP2006521830A

  • Investment material for investing resin pattern and manufacturing cast material

    JP2021146355A

  • Magnesia-Phosphate bonded Investment

    KR1020050023550A