Manufacturing method for all-solid secondary battery

A multi-step compression process with intermediate layers and protective sheets addresses the homogeneity and stability issues in all-solid-state secondary batteries, enhancing alignment and bonding to improve battery uniformity and reduce damage.

JP2024141227APending Publication Date: 2024-10-10HONDA MOTOR CO LTD

Patent Information

Application Number
JP2023052751
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing all-solid-state secondary batteries face challenges in achieving homogeneity and stability, particularly in the bonding and alignment of electrode layers, leading to potential warpage and damage during compression.

Method used

A multi-step compression process involving specific pressures and the use of intermediate layers and protective sheets to align and bond electrode layers, ensuring uniformity and minimizing damage, including forming positive and negative electrode layers on both sides of a current collector.

Benefits of technology

The method enhances the homogeneity and flatness of the all-solid-state secondary battery by improving the alignment and bonding of electrode layers, reducing warpage and damage, while maintaining dimensional accuracy and ion conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for an all-solid secondary battery with excellent homogeneity.SOLUTION: A manufacturing method for an all-solid secondary battery includes a positive electrode layer forming step, a first compressing step, an electrolyte layer stacking step, a second compressing step, an intermediate layer stacking step, a third compressing step, a combining step, and a fourth compressing step. A second pressure in the second compressing step is higher than each of a first pressure in the first compressing step, a third pressure in the third compressing step, and a fourth pressure in the fourth compressing step.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an all-solid-state secondary battery. [Background technology]

[0002] In recent years, research and development has been conducted on secondary batteries that contribute to energy efficiency in order to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. Among secondary batteries, all-solid-state secondary batteries have attracted attention because of their excellent properties in terms of safety, life, output, etc. As a method for manufacturing all-solid-state secondary batteries, a method of pressing a laminate consisting of a positive electrode layer, a solid electrolyte, and a negative electrode layer is known (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6251974 Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, in the technology relating to secondary batteries, a challenge is to obtain uniformity in all-solid-state batteries.

[0005] The present invention has been made in view of the above circumstances, and aims to achieve a method for producing an all-solid-state secondary battery having excellent homogeneity, which will in turn contribute to improving energy efficiency. [Means for solving the problem]

[0006] In order to solve the above problems, the following means are provided.

[0007] A method for producing an all-solid-state secondary battery according to one embodiment of the present invention includes a cathode layer forming step of forming a cathode layer containing a cathode active material, a first compression step of compressing the cathode layer at a first pressure to obtain a first compressed body, an electrolyte layer lamination step of laminating an electrolyte layer containing a solid electrolyte on a surface of the first compressed body where the cathode layer is exposed, a second compression step of compressing the cathode layer and the electrolyte layer at a second pressure to obtain a second compressed body, an intermediate layer lamination step of preparing an anode layer and an intermediate layer and laminating the intermediate layer on the anode layer, a third compression step of compressing the anode layer and the intermediate layer at a third pressure to obtain a third compressed body, an integration step of integrating the second compressed body with the third compressed body so that the electrolyte layer of the second compressed body faces the intermediate layer of the third compressed body to obtain an integrated member, and a fourth compression step of compressing the integrated member at a fourth pressure. The second pressure is higher than each of the first pressure, the third pressure, and the fourth pressure.

[0008] According to this method, the positive electrode layer can be preliminarily compressed by carrying out the first compression step. This can promote the alignment of the particles constituting the positive electrode layer. Therefore, the positive electrode density in the positive electrode layer can be easily stabilized. By carrying out the second compression step, the density of the positive electrode layer can be increased while improving the bond between the positive electrode layer and the electrolyte layer. By carrying out the third compression step, damage to the negative electrode layer can be suppressed and the intermediate layer can be densified. By carrying out the fourth compression step, the second compressed body and the third compressed body which constitute an integral member can be joined to each other. Furthermore, since the smoothness of the interface between the electrolyte layer and the intermediate layer is improved, an all-solid-state secondary battery with excellent homogeneity can be realized.

[0009] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, in the positive electrode layer forming step, a positive electrode current collector having a first surface and a second surface opposite to the first surface may be prepared, and the positive electrode layer may be formed on each of the first surface and the second surface.

[0010] According to this method, a positive electrode layer is formed on the first surface of the positive electrode current collector. Similarly, a positive electrode layer is formed on the second surface of the positive electrode current collector. That is, a structure in which a positive electrode layer is formed on both surfaces of the positive electrode current collector is obtained. In such a structure, even after the first compression step, the second compression step, the third compression step, and the fourth compression step, the restoring force of the positive electrode layer generated on the first surface and the restoring force of the positive electrode layer generated on the second surface cancel each other out. Therefore, the occurrence of warping is suppressed in the entire all-solid-state secondary battery. Therefore, the flatness of the all-solid-state secondary battery can be improved. In particular, when the roll press method is used in the first compression step, the second compression step, the third compression step, and the fourth compression step, the difference in the friction coefficient between the surface of the roll and the surface of the laminate laminated on both surfaces of the positive electrode current collector can be reduced. This can improve the flatness of the all-solid-state secondary battery.

[0011] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, the intermediate layer may include a solid electrolyte, a carbide, and a binder.

[0012] Generally, the electrolyte layer is made of powder. Therefore, in a structure in which the electrolyte layer is directly bonded to the anode layer, the adhesion of the anode layer to the electrolyte layer is low. In contrast, in the method for producing an all-solid-state secondary battery according to one aspect of the present invention, an intermediate layer is interposed between the anode layer and the electrolyte layer, and the intermediate layer includes a solid electrolyte, a carbide, and a binder. Therefore, compared to a structure in which the electrolyte layer is directly bonded to the negative electrode layer, a structure including an intermediate layer can improve the bonding strength of the negative electrode layer to the electrolyte layer. Furthermore, the intermediate layer is compressed at a third pressure lower than the second pressure, and at a fourth pressure lower than the second pressure, thereby making it possible to suppress segregation of particles constituting the solid electrolyte, carbide, and binder contained in the intermediate layer.

[0013] In the method for producing an all-solid-state secondary battery according to one embodiment of the present invention, a compression member is used to compress an object to be compressed in each of the first compression step, the second compression step, the third compression step, and the fourth compression step, and in at least one of the first compression step, the second compression step, the third compression step, and the fourth compression step, the compression member may compress the object to be compressed with a protective sheet interposed between the object to be compressed and the compression member.

[0014] According to this method, at least one of the first compression step, the second compression step, the third compression step, and the fourth compression step is performed using a protective sheet. Therefore, even if pressure is applied to the layers constituting the all-solid-state secondary battery, damage to the layers can be suppressed. Here, the layers constituting the all-solid-state secondary battery are, for example, a positive electrode collector, a negative electrode layer, and a negative electrode collector. In particular, when the layers constituting the all-solid-state secondary battery are made of a thin foil-like material, the effect of suppressing damage to the layers can be obtained.

[0015] In a manufacturing method for an all-solid-state secondary battery according to one embodiment of the present invention, a thin film electrolyte layer containing a solid electrolyte and thinner than the electrolyte layer may be prepared, and after the third compression step, the thin film electrolyte layer may be laminated on a surface of the third compression body where the intermediate layer is exposed, and in the integration step, the second compression body and the third compression body may be integrated to sandwich the thin film electrolyte layer, thereby obtaining the integrated member. In a manufacturing method for an all-solid-state secondary battery according to one embodiment of the present invention, a thin film electrolyte layer containing a solid electrolyte and thinner than the electrolyte layer may be prepared, and after the second compression step, the thin film electrolyte layer may be laminated on a surface of the second compression body where the electrolyte layer is exposed, and in the integration step, the second compression body and the third compression body may be integrated to sandwich the thin film electrolyte layer, thereby obtaining the integrated member.

[0016] According to this method, the uneven shape of the thin-film electrolyte layer can be maintained and the thin-film electrolyte can be maintained in a low-density state before the fourth compression step is performed. Furthermore, the thin-film electrolyte can function as an adhesive that bonds the second compressed body and the third compressed body in the fourth compression step.

[0017] In the method for producing an all-solid-state secondary battery according to one aspect of the present invention, the electrolyte layer may have a porous substrate.

[0018] According to this method, when the electrolyte layer is thin, the dimensional precision of the electrolyte layer can be maintained even if the electrolyte layer is compressed with the second pressure in the second compression step. Effect of the Invention

[0019] According to the method for producing an all-solid-state secondary battery according to one aspect of the present invention, it is possible to provide a method for producing an all-solid-state secondary battery having excellent homogeneity. [Brief description of the drawings]

[0020] [Figure 1] 1 is a cross-sectional view partially showing the structure of an all-solid-state secondary battery according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a part of a roll press device, illustrating a roll press method used in the production of the all-solid-state secondary battery according to the first embodiment of the present invention. [Diagram 3] FIG. 2 is a diagram for explaining the method for producing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a first compressed body obtained in the middle of the production. [Figure 4] FIG. 2 is a diagram for explaining the method for producing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a second compressed body obtained in the middle of the production. [Diagram 5] FIG. 2 is a diagram for explaining the method for producing the all-solid-state secondary battery according to the first embodiment of the present invention, and is a cross-sectional view partially showing the structure of a third compressed body obtained in the middle of the production. [Figure 6]FIG. 4 is a cross-sectional view partially showing the structure of an all-solid-state secondary battery according to a second embodiment of the present invention. [Figure 7] FIG. 11 is a diagram for explaining a method for producing an all-solid-state secondary battery according to a second embodiment of the present invention, and is a cross-sectional view partially showing the structure of a first compressed body obtained in the middle of the production. [Figure 8] FIG. 11 is a diagram for explaining the method for producing an all-solid-state secondary battery according to the second embodiment of the present invention, and is a cross-sectional view partially showing the structure of a second compressed body obtained in the middle of the production. [Figure 9] FIG. 11 is a diagram for explaining a method for producing an all-solid-state secondary battery according to a second embodiment of the present invention, and is a cross-sectional view partially showing the structure of a third compressed body obtained in the middle of the production. [Figure 10] FIG. 11 is a diagram for explaining a method for producing an all-solid-state secondary battery according to a third embodiment of the present invention, and is a cross-sectional view partially showing the structure of a second compressed body obtained in the middle of the production. [Figure 11] FIG. 11 is a diagram for explaining a method for producing an all-solid-state secondary battery according to a third embodiment of the present invention, and is a cross-sectional view partially showing the structure of a third compressed body obtained in the middle of the production. [Figure 12] FIG. 13 is a cross-sectional view illustrating a part of a roll press device, illustrating a roll press method used in the manufacture of an all-solid-state secondary battery according to a fifth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A method for producing an all-solid-state secondary battery according to an embodiment of the present invention will be described with reference to the drawings. In the drawings used in the following description, the scale of each component has been appropriately changed so that each component is of a recognizable size. The meaning of the term "laminating" is not limited to molding a layer onto a target member, but includes pre-molding a layer and transferring the layer onto the target member. The meaning of the term "facing" is not limited to two members facing each other so as to be in contact with each other, but also includes two members facing each other so that there is an intervening object between the two members.

[0022] First Embodiment <Structure of all-solid-state secondary battery> As shown in FIG. 1, the all-solid-state secondary battery 1 includes a positive electrode current collector 2, positive electrode layers 3U, 3L, electrolyte layers 4U, 4L, intermediate layers 5U, 5L, negative electrode layers 6U, 6L, and negative electrode current collectors 7U, 7L. The positive electrode current collector 2 has a first surface 2U and a second surface 2L opposite to the first surface 2U. A positive electrode layer 3U, an electrolyte layer 4U, an intermediate layer 5U, a negative electrode layer 6U, and a negative electrode current collector 7U are laminated in this order on the first surface 2U in the direction from the positive electrode current collector 2 toward the negative electrode current collector 7U. The positive electrode layer 3U, the electrolyte layer 4U, the intermediate layer 5U, the negative electrode layer 6U, and the negative electrode current collector 7U are compressed relative to the positive electrode current collector 2 to form a laminated compressed structure 1U. A positive electrode layer 3L, an electrolyte layer 4L, an intermediate layer 5L, a negative electrode layer 6L, and a negative electrode current collector 7L are laminated in this order on the second surface 2L in the direction from the positive electrode current collector 2 toward the negative electrode current collector 7L. The positive electrode layer 3L, the electrolyte layer 4L, the intermediate layer 5L, the negative electrode layer 6L, and the negative electrode current collector 7L are compressed against the positive electrode current collector 2 to form a laminated compressed structure 1L.

[0023] <Positive electrode current collector> The positive electrode current collector 2 is a layer in contact with the positive electrode layers 3U and 3L. There are no particular limitations on the material constituting the positive electrode current collector 2, and any known material that can be used as a positive electrode current collector for a solid secondary battery can be used for the positive electrode current collector 2. Examples of the positive electrode current collector 2 include metal foils such as stainless steel (SUS) foil and aluminum (Al) foil.

[0024] <Positive electrode layer> Each of the positive electrode layers 3U and 3L is a layer in contact with the electrolyte layers 4U and 4L. Each of the positive electrode layers 3U and 3L is a layer including a positive electrode active material. The positive electrode active material is not particularly limited, and a material known as a positive electrode active material for a solid secondary battery can be used. Examples of the positive electrode active material include LiCoO2, LiNiO2, NCM(Li(Ni x Co y Mn z)Ternary cathode materials such as O2, (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1)), layered cathode active material particles such as LiVO2, LiCrO2, spinel-type cathode active materials such as LiMn2O4, Li(Ni 0.25 Mn 0.75 )2O4, LiCoMnO4, Li2NiMn3O8, olivine-type cathode active materials such as LiCoPO4, LiMnPO4, LiFePO4, etc. can be used.

[0025] Each of the cathode layers 3U and 3L may further contain a solid electrolyte, a conductive aid, a binder, etc. in addition to the cathode active material. The solid electrolyte, the conductive aid, the binder, etc. are not particularly limited, and known substances as electrode materials for solid secondary batteries can be applied. An adhesive layer may be laminated on the outer surfaces of the cathode layers 3U and 3L.

[0026] <Electrolyte layer> Each of the electrolyte layers 4U and 4L is a layer that contacts the intermediate layers 5U and 5L. Each of the electrolyte layers 4U and 4L is a layer containing a solid electrolyte. In addition to the above, the electrolyte layers 4U and 4L may contain a binder, etc. The type of the solid electrolyte is not particularly limited, and examples of the solid electrolyte include sulfide-based solid electrolytes, oxide-based solid electrolytes, nitride-based solid electrolytes, halide-based solid electrolytes, etc. The material of the binder is not particularly limited, and examples of the binder material include polyvinylidene fluoride (PVdF), polymethyl methacrylate (PMMA), polyisobutene (PIB), styrene-butadiene rubber (SBR), polyethylene-vinyl acetate copolymer (PEVA), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), etc. These may be used alone or in combination of two or more.

[0027] <Intermediate layer> Each of the intermediate layers 5U and 5L is a layer that contacts the anode layers 6U and 6L. Examples of the material of the intermediate layers 5U and 5L include a solid electrolyte, a carbide, and a binder. As the carbide, for example, SnC can be used. The intermediate layer 5U has at least one of a function of increasing ion conductivity between the corresponding electrolyte layer 4U and the negative electrode layer 6U, and a function of protecting the surface of the negative electrode layer 6U. Similarly, the intermediate layer 5L has at least one of a function of increasing ion conductivity between the corresponding electrolyte layer 4L and the negative electrode layer 6L, and a function of protecting the surface of the negative electrode layer 6L.

[0028] <Negative electrode layer> Each of the negative electrode layers 6U and 6L is a layer in contact with the negative electrode current collectors 7U and 7L. Each of the negative electrode layers 6U and 6L is a layer including a negative electrode active material. The negative electrode active material is not particularly limited, and a material known as a negative electrode active material for solid secondary batteries can be used. As the negative electrode active material, for example, lithium titanate (Li4Ti5O 12 ), transition metal oxides such as TiO2, Nb2O3, and WO3, metal sulfides, metal nitrides, carbon materials such as graphite, soft carbon, and hard carbon, silicon-based materials such as silicon elemental, silicon alloys, and silicon compounds, as well as lithium metal, lithium alloys, and metallic indium. Each of the negative electrode layers 6U and 6L may further contain, in addition to the negative electrode active material, a solid electrolyte, a conductive additive, a binder, etc. The solid electrolyte, the conductive additive, the binder, etc. are not particularly limited, and any substance known as an electrode material for a solid secondary battery can be used.

[0029] <Negative electrode current collector> Each of the negative electrode current collectors 7U and 7L corresponds to the outermost layer of the all-solid-state secondary battery 1. In other words, the negative electrode current collector 7U corresponds to the outermost layer of the laminated compression structure 1U. The negative electrode current collector 7L corresponds to the outermost layer of the laminated compression structure 1L. The material of the negative electrode current collectors 7U and 7L is not particularly limited, and any known material can be used as a negative electrode current collector for a solid secondary battery. Examples of the negative electrode current collector include metal foils such as copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil.

[0030] <Method for manufacturing the all-solid-state secondary battery according to the first embodiment> Next, a method for manufacturing the all-solid-state secondary battery 1 according to the first embodiment will be described with reference to FIGS. The method for manufacturing the all-solid-state secondary battery 1 includes the following steps. Step 1: Positive electrode layer forming process Step 2: First compression process Step 3: Electrolyte layer deposition process Step 4: Second compression process Step 5: Interlayer Lamination Step 6: Third compression process Step 7: Integration process Step 8: Fourth compression process Furthermore, in the manufacturing method of the all-solid-state secondary battery 1, steps 1 to 8 are performed in this order. Furthermore, in the first compression step, the second compression step, the third compression step, and the fourth compression step, known compression steps are performed. As an example of the compression steps, in this embodiment, a roll press method is adopted.

[0031] <Roll press device> FIG. 2 is a cross-sectional view showing a part of a roll press apparatus for performing the roll press method. The roll press device has a first roll R1 and a second roll R2 facing each other, and a sending mechanism (not shown). The first roll R1 can rotate counterclockwise. The second roll R2 can rotate clockwise. The sending mechanism can send the compression object 20 to the gap between the first roll R1 and the second roll R2 in the direction from the insertion part 11 toward the discharge part 12. The distance between the first roll R1 and the second roll R2 can be adjusted as appropriate. In addition, the roll press device can appropriately adjust the compression force applied to the compression object 20. In the following description, when the first roll R1 and the second roll R2 are not distinguished from each other, the first roll R1 and the second roll R2 may be simply referred to as "roll R". Each of the first roll R1 and the second roll R2 is an example of a compression member that compresses the compression target.

[0032] <Roll press method> The compressed object 20 is a laminate having a first layer 10A and a second layer 10B. Before being compressed, the compressed object 20 has a thickness h0. First, the delivery mechanism sends the compressed object 20 to the gap between the first roll R1 and the second roll R2 through the insertion section 11. As the first roll R1 and the second roll R2 rotate, the compressed object 20 moves from the insertion section 11 toward the discharge section 12. The compressed object 20 is compressed by the first roll R1 and the second roll R2, and the thickness of the compressed object 20 gradually decreases. The thicknesses of the first layer 10A and the second layer 10B constituting the compressed object 20 also gradually decrease. After being compressed, the compressed object 20 has a thickness h that is thinner than the thickness h0.

[0033] Next, each of steps 1 to 8 will be described.

[0034] <Step 1: Positive electrode layer molding process> First, the positive electrode current collector 2 and the positive electrode layers 3U and 3L are prepared. Next, the positive electrode layer 3U is formed on the first surface 2U of the positive electrode collector 2. The positive electrode layer 3L is formed on the second surface 2L of the positive electrode collector 2. This results in a laminate in which the positive electrode collector 2 and the positive electrode layers 3U and 3L are laminated. In the positive electrode layer forming step, the positive electrode layers 3U and 3L are not limited to being directly laminated on the positive electrode current collector 2. The positive electrode layers 3U and 3L may be transferred to the positive electrode current collector 2 in advance.

[0035] <Step 2: First compression process> Next, the laminate obtained in the positive electrode layer molding step is compressed using a roll press device shown in FIG. 2. Specifically, the laminate obtained in the positive electrode layer molding step is inserted between a first roll R1 and a second roll R2 as a compression target 20. As the first roll R1 and the second roll R2 rotate, the laminate is gradually compressed. This results in a first compressed body 1MA shown in FIG. 3. In the first compression step, the pressure (first pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 500 MPa.

[0036] <Step 3: Electrolyte layer stacking process> Next, the electrolyte layers 4U and 4L are prepared. Next, an electrolyte layer 4U is laminated on the surface of the first compressed body 1MA where the positive electrode layer 3U is exposed. An electrolyte layer 4L is laminated on the surface of the first compressed body 1MA where the positive electrode layer 3L is exposed. This results in a laminate in which the positive electrode current collector 2, the positive electrode layers 3U and 3L, and the electrolyte layers 4U and 4L are laminated. In the electrolyte layer lamination step, the method of laminating the electrolyte layers 4U, 4L directly on the positive electrode layers 3U, 3L is not limited to this. The electrolyte layers 4U, 4L that have been separately formed in advance may be transferred to the positive electrode layers 3U, 3L.

[0037] <Step 4: Second compression process> Next, the laminate obtained in the electrolyte layer lamination step is compressed using a roll press device shown in FIG. 2. Specifically, the laminate obtained in the electrolyte layer lamination step is inserted between a first roll R1 and a second roll R2 as a compression target 20. As the first roll R1 and the second roll R2 rotate, the laminate is gradually compressed. This results in a second compressed body 1MB shown in FIG. 4. In the second compression step, the pressure (second pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 900 MPa to 1000 MPa. Therefore, in comparison between the first pressure and the second pressure, the second pressure is set higher than the first pressure.

[0038] <Step 5: Intermediate layer lamination process> Next, the intermediate layers 5U, 5L, the negative electrode layers 6U, 6L, and the negative electrode current collectors 7U, 7L are prepared. The negative electrode layer 6U has a first negative electrode surface 6UF and a second negative electrode surface 6US opposite to the first negative electrode surface 6UF. The negative electrode layer 6L has a first negative electrode surface 6LF and a second negative electrode surface 6LS opposite to the first negative electrode surface 6LF. The intermediate layer 5U is laminated on the first negative electrode surface 6UF. The negative electrode current collector 7U is laminated on the second negative electrode surface 6US. The intermediate layer 5L is laminated on the first negative electrode surface 6LF. The negative electrode current collector 7L is laminated on the second negative electrode surface 6LS. This results in a laminate in which the intermediate layer 5U, the negative electrode layer 6U, and the negative electrode current collector 7U are laminated in this order. Furthermore, a laminate in which the intermediate layer 5L, the negative electrode layer 6L, and the negative electrode current collector 7L are laminated in this order is obtained.

[0039] <Step 6: Third compression process> Next, the two laminates obtained in the intermediate layer lamination step are compressed using a roll press device shown in FIG. 2. Specifically, the two laminates obtained in the intermediate layer lamination step are inserted between a first roll R1 and a second roll R2 as compression objects 20. As the first roll R1 and the second roll R2 rotate, the laminate is gradually compressed. As a result, two third compressed bodies 1MC shown in FIG. 5 are obtained. In the third compression step, the pressure (third pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 300 MPa to 400 MPa, or 400 MPa or more. Therefore, in comparison between the second pressure and the third pressure, the second pressure is set higher than the third pressure.

[0040] <Step 7: Integration process> An integrated member is obtained by integrating the second compressed body 1MB and two third compressed bodies 1MC so that the electrolyte layers 4U, 4L of the second compressed body 1MB face the intermediate layers 5U, 5L of the third compressed body 1MC. Specifically, the second compressed body 1MB and two third compressed bodies 1MC are integrated so that the second compressed body 1MB is sandwiched between the two third compressed bodies 1MC.

[0041] <Step 8: Fourth compression process> Next, the integrated member obtained in the integration step is compressed using a roll press device shown in FIG. 2. Specifically, the integrated member is inserted between the first roll R1 and the second roll R2 as the compression target 20. As the first roll R1 and the second roll R2 rotate, the integrated member is gradually compressed. This results in the all-solid-state secondary battery 1 shown in FIG. 1. In the fourth compression step, the pressure (fourth pressure) applied to the laminate by the first roll R1 and the second roll R2 is, for example, 200 MPa or less. Therefore, in comparison between the second pressure and the fourth pressure, the second pressure is set higher than the fourth pressure.

[0042] Regarding the first pressure in the first compression step, the second pressure in the second compression step, the third pressure in the third compression step, and the fourth pressure in the fourth compression step, the second pressure is higher than each of the first pressure, the third pressure, and the fourth pressure. More preferably, the first pressure to the fourth pressure are set so as to obtain a pressure relationship of "fourth pressure<third pressure<first pressure<second pressure".

[0043] <Action and effect> According to this method, the positive electrode layers 3U, 3L can be preliminarily compressed by performing the first compression step. The first pressure in the first compression step is about 500 MPa, which is lower than the second pressure. Therefore, the first compression step can be performed at a low pressure, and the positive electrode layers 3U, 3L are prevented from becoming too hard. Therefore, the bonding between the electrolyte layers 4U, 4L and the positive electrode layers 3U, 3L can be improved. Furthermore, by carrying out the first compression step, the alignment of the particles constituting the positive electrode layers 3U, 3L can be promoted, and therefore the positive electrode density in the positive electrode layers 3U, 3L can be easily stabilized.

[0044] By carrying out the second compression step, the density of the positive electrode layers 3U, 3L can be increased while improving the bond between the positive electrode layers 3U, 3L and the electrolyte layers 4U, 4L. By carrying out the third compression process, it is possible to densify the intermediate layers 5U, 5L while suppressing damage to the negative electrode layers 6U, 6L. The layers constituting each of the negative electrode layers 6U, 6L are thin films. The thin films constituting each of the negative electrode layers 6U, 6L are, for example, Li foils. According to the third compression process, it is possible to suppress damage to the thin films in the negative electrode layers 6U, 6L. By carrying out the fourth compression step, the second compressed body 1MB and the third compressed body 1MC which constitute an integral member can be joined to each other. The first pressure in the fourth compression step is about 200 MPa or less, which is lower than the second pressure, so that the fourth compression step can be performed at a low pressure and deformation of the positive electrode layers 3U and 3L can be suppressed. Furthermore, since the smoothness at the interfaces between the electrolyte layers 4U, 4L and the intermediate layers 5U, 5L is improved, an all-solid-state secondary battery 1 with excellent homogeneity can be realized.

[0045] Further, a positive electrode layer 3U is formed on the first surface 2U of the positive electrode current collector. Similarly, a positive electrode layer 3U is formed on the second surface 2L of the positive electrode current collector. That is, a structure in which the positive electrode layers 3U and 3L are formed on both surfaces of the positive electrode current collector is obtained. In such a structure, even after the first compression step, the second compression step, the third compression step, and the fourth compression step, the restoring forces of the positive electrode layers 3U and 3L generated on the first surface 2U and the restoring forces of the positive electrode layers 3U and 3L generated on the second surface 2L cancel each other out. Therefore, the occurrence of warping is suppressed in the entire all-solid-state secondary battery 1. Therefore, the flatness of the all-solid-state secondary battery 1 can be improved. In particular, when the roll press method is used in the first compression step, the second compression step, the third compression step, and the fourth compression step, the difference in the friction coefficient between the surface of the roll and the surface of the laminate laminated on both surfaces of the positive electrode current collector can be reduced. This can improve the flatness of the all-solid-state secondary battery 1.

[0046] Generally, the electrolyte layer is made of powder. Therefore, in a structure in which the electrolyte layer is directly bonded to the anode layers 6U and 6L, the bondability of the anode layer to the electrolyte layer is low. In contrast, in a method for manufacturing an all-solid-state secondary battery 1 according to one embodiment of the present invention, intermediate layers 5U and 5L are interposed between the anode layers 6U and 6L and the electrolyte layers 4U and 4L, and the intermediate layers 5U and 5L have a solid electrolyte, a carbide, and a binder. Therefore, compared to a structure in which the electrolyte layers 4U, 4L are directly bonded to the negative electrode layers 6U, 6L, the structure including the intermediate layers 5U, 5L can improve the bonding strength between the negative electrode layers 6U, 6L and the electrolyte layers 4U, 4L. Furthermore, the intermediate layers 5U and 5L are compressed at a third pressure lower than the second pressure, and at a fourth pressure lower than the second pressure, so that segregation of the particles constituting the solid electrolyte, carbide, and binder contained in the intermediate layers 5U and 5L can be suppressed.

[0047] Furthermore, the third compression step and the fourth compression step are each performed in a state where the second negative electrode surface 6US of the negative electrode layer 6U is covered with the negative electrode current collector 7U. Similarly, the third compression step and the fourth compression step are each performed in a state where the second negative electrode surface 6LS of the negative electrode layer 6L is covered with the negative electrode current collector 7L. In this case, the roll R does not come into contact with each of the negative electrode layers 6U and 6L. Therefore, damage to the negative electrode layers 6U and 6L can be suppressed.

[0048] <Modification 1 of the First Embodiment> The above-mentioned electrolyte layers 4U, 4L may have a porous substrate. The porous substrate may have a uniform surface with respect to each surface of the positive electrode layers 3U, 3L, or with respect to each surface of the intermediate layers 5U, 5L. Examples of materials constituting the porous substrate include polymers, ceramics, metals, nonwoven fabrics, etc. The material of the porous substrate is not limited as long as it has a three-dimensional skeleton.

[0049] As a comparative example, a case where the electrolyte layer is compressed at the second pressure in the second compression step is considered. Since the second pressure is a high pressure of 900 MPa to 1000 MPa, the electrolyte layer is deformed, and it is difficult to maintain the dimensional accuracy of the electrolyte layer. In contrast, in a configuration in which the electrolyte layers 4U and 4L have a porous substrate, the dimensional accuracy of the electrolyte layers 4U and 4L can be maintained even if the electrolyte layers are compressed at the second pressure in the second compression step. In particular, even if the thickness of each of the electrolyte layers 4U and 4L is thin, the dimensional accuracy of the electrolyte layers 4U and 4L can be maintained.

[0050] <Modification 2 of the First Embodiment> The timings of performing the positive electrode layer forming step, the first compression step, the electrolyte layer lamination step, and the second compression step, and the timings of performing the intermediate layer lamination step and the third compression step are not limited to those of the above-mentioned first embodiment. This is because the processing steps of the positive electrode current collector 2, the positive electrode layers 3U, 3L, and the electrolyte layers 4U, 4L in the positive electrode layer forming step, the first compression step, the electrolyte layer lamination step, and the second compression step, and the processing steps of the intermediate layers 5U, 5L, the negative electrode layers 6U, 6L, and the negative electrode current collectors 7U, 7L in the intermediate layer lamination step and the third compression step are independent of each other. Therefore, the intermediate layer lamination step and the third compression step may be performed while performing the positive electrode layer molding step, the first compression step, the electrolyte layer lamination step, and the second compression step, or the positive electrode layer molding step, the first compression step, the electrolyte layer lamination step, and the second compression step may be performed after performing the intermediate layer lamination step and the third compression step.

[0051] <Second embodiment> Next, the all-solid-state secondary battery 21 according to the second embodiment will be described. The second embodiment differs from the first embodiment in the configuration of the electrolyte layer. In the second embodiment, the same members as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0052] <Structure of all-solid-state secondary battery> As shown in FIG. 6, the all-solid-state secondary battery 21 includes a positive electrode current collector 2, positive electrode layers 3U, 3L, first electrolyte layers 4UF, 4LF, second electrolyte layers 4US, 4LS, intermediate layers 5U, 5L, negative electrode layers 6U, 6L, and negative electrode current collectors 7U, 7L.

[0053] <First electrolyte layer> The first electrolyte layer 4UF has the same configuration as the electrolyte layer 4U described above. Similarly, the first electrolyte layer 4LF has the same configuration as the electrolyte layer LU described above. For this reason, the reference characters 4U and 4L are shown together in FIG.

[0054] <Second electrolyte layer> The second electrolyte layers 4US and 4LS are an example of a thin-film electrolyte layer. The material constituting the second electrolyte layers 4US, 4LS may be the same as that of the electrolyte layers 4U, 4L. As a modification, the binder content in the second electrolyte layers 4US, 4LS may be less than the binder content in the first electrolyte layers 4UF, 4LF.

[0055] The thickness of the second electrolyte layer 4US is thinner than that of the first electrolyte layer 4UF. The thickness of the second electrolyte layer 4LS is thinner than that of the first electrolyte layer 4LF. Since the second electrolyte layers 4US and 4LS are made of the same material as the electrolyte layers 4U and 4L, the reference characters 4U and 4L are shown together in FIG.

[0056] <Method for manufacturing all-solid-state secondary battery according to the second embodiment> Next, a method for manufacturing the all-solid-state secondary battery 21 according to the second embodiment will be described. First, a positive electrode layer molding step and a first compression step are performed. As a result, a first compression body 21MA shown in Fig. 7 is obtained. Then, an electrolyte layer lamination step and a second compression step are performed. As a result, a second compression body 21MB shown in Fig. 8 is obtained. The second compression body 21MB has first electrolyte layers 4UF and 4LF.

[0057] Next, an intermediate layer lamination step and a third compression step are performed. As a result, two third compressed bodies 21MC shown in FIG. 9 are obtained. After the third compression step is performed, a second electrolyte layer 4US is laminated on the surface of the third compressed body 21MC where the intermediate layer 5U is exposed. Similarly, a second electrolyte layer 4LS is laminated on the surface of the third compressed body 21MC where the intermediate layer 5L is exposed. Next, an integration step is performed, whereby the second compressed body 21MB and the two third compressed bodies 21MC are integrated together so as to sandwich the second electrolyte layers 4US, 4LS. Next, in a fourth compression step, the integrated member obtained in the integration step is compressed, thereby obtaining the all-solid-state secondary battery 21 shown in FIG.

[0058] <Action and effect> According to this method, the same or similar effects as those obtained by the first embodiment described above can be obtained. Furthermore, the second electrolyte layers 4US, 4LS can maintain their uneven shape and low density before the fourth compression step is performed. Furthermore, the second electrolyte layers 4US, 4LS can function as an adhesive that bonds the second compressed body 21MB and the two third compressed bodies 21MC in the fourth compression step.

[0059] <Third embodiment> Next, an all-solid-state secondary battery 31 according to a third embodiment will be described. The structure of the all-solid-state secondary battery 31 is the same as the structure of the all-solid-state secondary battery 21 according to the second embodiment. In the third embodiment, the same members as those in the first and second embodiments are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0060] <Method for manufacturing all-solid-state secondary battery according to the third embodiment> Next, a method for manufacturing the all-solid-state secondary battery 31 according to the third embodiment will be described. First, a positive electrode layer forming step, a first compression step, an electrolyte layer lamination step, and a second compression step are performed. As a result, a second compressed body 31MB shown in Fig. 10 is obtained. The second compressed body 31MB has first electrolyte layers 4UF and 4LF.

[0061] Next, after carrying out the second compression step, the second electrolyte layer 4US is laminated on the surface of the second compression body 31MB where the first electrolyte layer 4UF is exposed, and the second electrolyte layer 4LS is laminated on the surface where the first electrolyte layer 4LF is exposed.

[0062] Next, an intermediate layer laminating step and a third compression step are performed, thereby obtaining two third compressed bodies 31MC shown in FIG. Next, an integration step is performed, whereby the second compressed body 31MB and the two third compressed bodies 31MC are integrated together so as to sandwich the second electrolyte layers 4US, 4LS.

[0063] Next, in a fourth compression step, the integrated member obtained in the integration step is compressed, thereby obtaining the all-solid-state secondary battery 31 shown in FIG.

[0064] <Action and effect> According to this method, the same or similar effects as those obtained by the first embodiment described above can be obtained. Furthermore, the second electrolyte layers 4US and 4LS can maintain their uneven shape and low density before the fourth compression step is performed. Furthermore, the second electrolyte layers 4US and 4LS can function as an adhesive that bonds the second compressed body 31MB and the two third compressed bodies 31MC in the fourth compression step.

[0065] <Fourth embodiment> Next, an all-solid-state secondary battery according to a fourth embodiment will be described. The fourth embodiment differs from the first embodiment in the configurations of the negative electrode layers 6U, 6L and the negative electrode current collectors 7U, 7L. In the fourth embodiment, the same members as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0066] <Negative electrode layer> In the fourth embodiment, each of the negative electrode layers 6U and 6L has both a function of a negative electrode layer and a function of a negative electrode current collector. Each of the negative electrode layers 6U and 6L corresponds to the outermost layer of the all-solid-state secondary battery 21. In other words, the negative electrode layer 6U corresponds to the outermost layer of the laminated compression structure 1U. The negative electrode layer 6L corresponds to the outermost layer of the laminated compression structure 1L. Each of the negative electrode layers 6U and 6L has a structure in which a negative electrode active material layer and a negative electrode current collector layer are laminated. The negative electrode active material layer contains the negative electrode active material described in the first embodiment. The negative electrode current collector layer is a metal foil such as copper (Cu) foil, stainless steel (SUS) foil, or aluminum (Al) foil.

[0067] <Action and effect> According to this method, each of the negative electrode layers 6U and 6L is a laminate of a negative electrode active material layer and a negative electrode current collector layer. Therefore, it is not necessary to prepare the negative electrode current collectors 7U and 7L described in the intermediate layer lamination process. Therefore, the number of steps required to manufacture an all-solid-state secondary battery can be reduced.

[0068] <Fifth embodiment> Next, a method for manufacturing the all-solid-state secondary battery according to the fifth embodiment will be described. The fifth embodiment differs from each of the first to fourth embodiments described above in that a protective sheet is interposed between the compression object 20 and the roll R. In the fifth embodiment, the same members as those in the first to fourth embodiments are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0069] <Protective sheet> In at least one of the above-mentioned first compression step, second compression step, third compression step, and fourth compression step, a protective sheet 30 is interposed between the compression target 20 and the first roll R1, as shown in Fig. 12. In other words, the protective sheet 30 is interposed between the first compression surface RF1 of the first roll R1 and the first compression target surface 20F of the compression target 20. Similarly, the protective sheet 30 is interposed between the compression object 20 and the second roll R2. In other words, the protective sheet 30 is interposed between the second compression surface RF2 of the second roll R2 and the second compression surface 20S of the compression object 20. In this state, the first roll R1 and the second roll R2 compress the compression target 20 while rotating.

[0070] In the method for producing the all-solid-state secondary battery according to the embodiment described above, the protective sheet 30 can be interposed between the positive electrode current collector 2 and the roll R. The protective sheet 30 can be interposed between each of the negative electrode layers 6U, 6L and the roll R. In addition, the protective sheet 30 can be interposed between each of the negative electrode current collectors 7U, 7L and the roll R.

[0071] The protective sheet 30 is separate from each of the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L. In other words, the protective sheet 30 is a member that does not constitute an all-solid-state secondary battery. For this reason, the protective sheet 30 is removed from the compression target 20 after each of the above-mentioned multiple compression steps is completed. Note that the protective sheet 30 may remain covering the compression target 20 from the end of one compression step until the next compression step is performed. In the example shown in FIG. 12, the protective sheets 30 are placed on both sides of the compression target 20, but it is sufficient that the protective sheet 30 is placed on at least one side of the compression target 20.

[0072] Examples of the material for the protective sheet 30 include metal foil and resin film. Examples of the metal foil include copper (Cu) foil, stainless steel (SUS) foil, and aluminum (Al) foil. Examples of the resin film include polyimide, polyetherimide, and fluororesin. The thickness of the protective sheet 30 is within a range of 5 to 150 μm, for example.

[0073] <Action and effect> This method provides the same or similar effects as those provided by the above-described first embodiment. Even if pressure is applied to the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L in at least one of the first compression step, the second compression step, the third compression step, and the fourth compression step, damage to the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L can be suppressed because the protective sheet 30 is used. In particular, when the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L are made of thin foil-like materials, the effect of suppressing damage to the positive electrode collector 2, the negative electrode layers 6U, 6L, and the negative electrode collectors 7U, 7L can be obtained.

[0074] <Modification> In the above-described embodiment, the laminated compressed structures 1U and 1L are formed on the first surface 2U and the second surface 2L of the positive electrode current collector 2, respectively. The laminated compressed structure may be formed on only one surface of the positive electrode current collector 2. In the above-described embodiment, the roll press method is used as an example of the compression step. However, a compression method other than the roll press method may be used as long as the compression target 20 can be compressed using a compression member.

[0075] Although the embodiments of the present invention have been described above, it should be understood that these are illustrative of the present invention and should not be considered as limiting. Additions, omissions, substitutions, and other modifications can be made without departing from the scope of the present invention. Therefore, the present invention should not be considered as being limited by the above description, but is limited by the scope of the claims. [Explanation of symbols]

[0076] 1, 21, 31 All-solid-state secondary battery 1U, 1L stacked compression structure 1MA First Compression Body 1MB 2nd compressed body 1MC 3rd compression body 2 Positive electrode current collector 2U 1st side 2L 2nd side 3U, 3L positive electrode layer 4U, 4L electrolyte layer 4UF, 4LF 1st electrolyte layer (electrolyte layer) 4US, 4LS 2nd electrolyte layer (thin film electrolyte layer) 5U, 5L middle tier 6U, 6L negative electrode layer 6UF, 6LF 1st negative electrode 6US, 6LS 2nd negative electrode surface 7U, 7L negative electrode current collector 10A 1st layer 10B 2nd layer 11 Insertion section 12 Discharge section 20 Compression target 30 Protective Sheet 3U positive electrode layer R1 First roll R2 Second Roll R Roll

Claims

1. a positive electrode layer forming step of forming a positive electrode layer including a positive electrode active material; a first compression step of compressing the positive electrode layer at a first pressure to obtain a first compressed body; an electrolyte layer lamination step of laminating an electrolyte layer including a solid electrolyte on a surface of the first compressed body on which the positive electrode layer is exposed; a second compression step of compressing the positive electrode layer and the electrolyte layer at a second pressure to obtain a second compressed body; an intermediate layer lamination step of preparing a negative electrode layer and an intermediate layer, and laminating the intermediate layer on the negative electrode layer; a third compression step of compressing the negative electrode layer and the intermediate layer at a third pressure to obtain a third compressed body; an integration step of integrating the second compressed body with the third compressed body so that the electrolyte layer of the second compressed body faces the intermediate layer of the third compressed body to obtain an integrated member; a fourth compression step of compressing the integrated member at a fourth pressure; having the second pressure is higher than each of the first pressure, the third pressure, and the fourth pressure; A method for manufacturing an all-solid-state secondary battery.

2. In the positive electrode layer forming step, providing a positive electrode current collector having a first surface and a second surface opposite the first surface; forming the positive electrode layer on each of the first surface and the second surface; The method for producing the all-solid-state secondary battery according to claim 1 .

3. The intermediate layer includes a solid electrolyte, a carbide, and a binder. The method for producing the all-solid-state secondary battery according to claim 1 .

4. In each of the first compression step, the second compression step, the third compression step, and the fourth compression step, a compression member that compresses a compression target is used, In at least one of the first compression step, the second compression step, the third compression step, and the fourth compression step, the compression member compresses the compression object with a protective sheet interposed between the compression object and the compression member. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.

5. preparing a thin-film electrolyte layer including a solid electrolyte and thinner than the electrolyte layer; After the third compression step, the thin-film electrolyte layer is laminated on a surface of the third compressed body where the intermediate layer is exposed, In the integration step, the second compressed body and the third compressed body are integrated together so as to sandwich the thin-film electrolyte layer, thereby obtaining the integrated member. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.

6. preparing a thin-film electrolyte layer including a solid electrolyte and thinner than the electrolyte layer; After the second compression step, the thin-film electrolyte layer is laminated on a surface of the second compressed body where the electrolyte layer is exposed, In the integration step, the second compressed body and the third compressed body are integrated together so as to sandwich the thin-film electrolyte layer, thereby obtaining the integrated member. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.

7. The electrolyte layer has a porous substrate. The method for producing the all-solid-state secondary battery according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Method of manufacturing electrode body

    JP2015026530A

  • Laminated electrode body having dense electrolyte layer on negative electrode layer side before lamination press

    JP2015032535A

  • Method of manufacturing all-solid battery

    JP2017010816A

  • Solid-state secondary battery and manufacturing method of all-solid secondary battery

    JP2018206469A

  • All solid state battery and manufacturing method thereof

    JP2020126800A

Cited By

  • Method for manufacturing solid-state secondary battery

    JP2024146636A