Wood laminate and manufacturing method thereof
A wood laminate with a wooden veneer and porous material combination addresses the lack of design, lightness, and flexibility in existing laminates by enhancing load distribution, ensuring comfort and durability.
Patent Information
- Application Number
- JP2023052864
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing wood laminates lack a combination of design aesthetics, lightness, and flexibility with effective load dispersion properties, leading to discomfort during prolonged use and loss of design and lightness.
A wood laminate comprising a wooden veneer layer with a specific gravity of 0.3 or more and a porous material layer with a specific gravity of 0.5 or less, both with thicknesses between 0.2 to 3 mm, laminated with an adhesive layer, achieving a volume ratio of 25/100 to 500/100, to create a flexible and lightweight structure with improved load distribution.
The laminate provides excellent design, lightness, and load distribution properties, allowing for stress absorption and shape retention while maintaining flexibility and reducing stress concentration.
Smart Images

Figure 2024141297000001 
Figure 2024141297000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a wood laminate, and more particularly to a wood laminate that is excellent in design as a wood product, lightweight, and has excellent flexibility in the lamination direction and pressure dispersion, and a method for producing the same. [Background technology]
[0002] Wood has a unique appearance such as wood grain, and is a material with excellent design properties that gives impressions such as "warm," "soft," and "luxurious. Among them, plywood, which is made by laminating veneers of wood, is widely used as a wooden component for small to large items such as accessories, furniture, and building materials.
[0003] Plywood is usually manufactured by laminating wooden veneers and gluing them together. Although plywood obtained by this manufacturing method has a "soft" impression, it is actually hard and does not deform. For this reason, there is a problem that, for example, sitting on a wooden chair for a long time causes pain in the body. To address this situation, a method such as installing a cushion on the seat is generally used, but this causes another problem in that the design and lightness of the wooden product itself are lost due to the cushion.
[0004] On the other hand, attempts have been made to make the plywood itself flexible in the planar direction by laminating layers of different materials on the wooden veneer. For example, Patent Document 1 describes that laminating an acrylic foam, which is an elastomer, on the wooden veneer allows the plywood to conform to deformation in the planar direction. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-68712 Summary of the Invention [Problem to be solved by the invention]
[0006] However, after extensive investigations, the inventors found that the method of Patent Document 1 had insufficient load distribution and resulted in a so-called "hard" material. Therefore, there remains a problem that there is no material that combines the design and light weight of a wood product with flexibility during use, i.e., load distribution.
[0007] SUMMARY OF THE PRESENT DISCLOSURE An object of the present invention is to provide a lightweight, flexible wood laminate that has excellent design properties as a wood product and excellent load distribution properties, and a method for producing the same. [Means for solving the problem]
[0008] As a result of intensive research conducted by the inventors in the above-mentioned background, the inventors found that the above-mentioned problems can be solved by combining specific layers, and thus completed the present invention. That is, the inventors found that by laminating a specific wooden veneer (A) layer and a porous body (B) layer with a pressure-sensitive adhesive (C) layer, it is possible to provide a flexible wood laminate that is excellent in design as a wood product, lightweight, and has excellent load distribution properties, and thus completed the present invention.
[0009] The present invention has the following aspects. [1] A wood laminate having a wooden veneer (A) layer, a porous body (B) layer, and an adhesive (C) layer, characterized in that the wooden veneer (A) is a wooden veneer having a specific gravity of 0.3 or more and a thickness of 0.2 to 3 mm, and the porous body (B) is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm. [2] The wood laminate according to [1], wherein at least one outermost surface is a wood veneer (A) layer. [3] The wood laminate according to [1] or [2], wherein the porous body (B) has a tensile modulus of elasticity of 1 to 30 MPa. [4] The wood laminate according to any one of [1] to [3], wherein the specific gravity of the wood laminate is 0.4 or less. [5] The total volume (A V ) relative to the total volume of the porous body (B) layer (B V ) volume ratio (B V / A V ) is 25 / 100 to 500 / 100. [6] A method for producing a wood laminate according to any one of [1] to [5], comprising a step of laminating a wooden veneer (A), a porous body (B), and an adhesive (C) and bonding them together under pressure, wherein the adhesive (C) is in sheet form. Effect of the Invention
[0010] The wood laminate of the present invention can provide a wood product that is excellent in design, lightweight, and flexible with excellent load distribution.
[0011] The inventors of the present invention speculate as follows on the principle of the excellent effects of the wood laminate of the present invention. That is, by laminating a wooden veneer (A) layer and a porous body (B) layer having specific physical properties, the porous body (B) layer deforms appropriately when a load is applied in the surface direction, absorbing stress. On the other hand, by using the wooden veneer (A) layer in combination, the wood is given a designability as wood, and the hardness of the wooden veneer (A) layer contributes to the shape retention of the entire wood laminate. In addition, the specific gravity of the porous body (B) is small, so the light weight of the wood laminate is maintained. As described above, it is speculated that the combination of these specific heterogeneous material layers contributes specifically to load distribution in the surface direction, resulting in a lightweight and flexible wood product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below, but these are examples of preferred embodiments. In this specification, "~" indicates a range of numbers including the numbers before and after it.
[0013] A wood laminate according to one embodiment of the present invention (hereinafter sometimes referred to as "this wood laminate") is a wood laminate having a wooden veneer (A) layer, a porous body (B) layer, and an adhesive (C) layer, characterized in that the wooden veneer (A) is a wooden veneer having a specific gravity of 0.3 or more and a thickness of 0.2 to 3 mm, and the porous body (B) is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm.
[0014] <Wood veneer (A) layer> The wooden veneer (A) layer is a layer composed of a wooden veneer (A). The wooden veneer (A) must have a specific gravity of 0.3 or more and a thickness of 0.2 to 3 mm.
[0015] The specific gravity of the wooden veneer (A) is preferably 0.2 or more, more preferably 0.3 or more, from the viewpoint of ensuring the strength of the wood laminate and improving the shape retention. On the other hand, the specific gravity of the wooden veneer (A) is preferably 0.9 or less, more preferably 0.8 or less, from the viewpoint of improving flexibility, i.e., load distribution, and reducing the weight. The specific gravity of the wooden veneer (A) can be determined by the method described in the Examples below.
[0016] The thickness of the wooden veneer (A) is preferably 0.2 to 2.8 mm, more preferably 0.4 to 2.4 mm, even more preferably 0.5 to 2.0 mm, and particularly preferably 0.6 to 1.5 mm, from the viewpoint of improving flexibility, ie, load distribution.
[0017] Examples of wood materials constituting the wooden veneer (A) include, but are not limited to, cedar, western hemlock, radiata pine, amplexicaule, silver fir, tahi, beihi, magnolia japonica, spruce, whitewood, spruce, Japanese walnut, sequoia, poplar, white pine, dwarf pine, Japanese cedar, Japanese cedar, hinoki cypress, yellow pine, willow, obeche, black pine, red pine, falcata, red cedar, juniper, sawara, hiba, and fir.
[0018] The wooden veneer (A) may be a wooden veneer produced by a known method using the above-mentioned materials. Examples of wooden veneers produced by a known method include wooden veneers produced by using a cutting device from a specific log or a flitch obtained by sawing the log to a specified size. More specifically, examples of such wooden veneers include rotary veneers obtained by peeling a specific log, and sliced veneers obtained by cutting a specific log into square lumber or the like and planing it with a slicer. The wooden veneer (A) may be a processed wooden veneer. The processing method of the wooden veneer is not limited to the following, but may be, for example, an impregnation process in which a resin component or the like is impregnated into the wooden veneer. When the wooden veneer is processed, the specific gravity of the processed wooden veneer is used.
[0019] <Porous material (B) layer> The porous body (B) layer is a layer constituted by a porous body (B). The porous body (B) is required to be an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm.
[0020] The specific gravity of the porous body (B) is preferably 0.4 or less, more preferably 0.35 or less, from the viewpoint of improving flexibility, i.e., load dispersion, and weight reduction. The specific gravity of the porous body (B) is preferably 0.05 or more, more preferably 0.1 or more, from the viewpoint of ensuring the strength of the wood laminate and improving shape retention. The specific gravity of the porous body (B) can be determined by the method described in the Examples below.
[0021] The thickness of the porous body (B) is preferably 0.3 to 2.8 mm, more preferably 0.4 to 2.4 mm, even more preferably 0.5 to 2.0 mm, and particularly preferably 0.6 to 1.5 mm, from the viewpoint of improving flexibility, ie, load distribution.
[0022] From the viewpoint of absorbing load stress and improving load dispersibility, the tensile modulus of the porous body (B) is preferably 1 to 30 MPa, more preferably 1.5 to 29 MPa, and even more preferably 2 to 28 MPa. The tensile modulus of the porous body (B) can be measured by the method described in the examples below.
[0023] The tensile modulus of the porous body (B) can be set arbitrarily within the above range and is not limited to the following, and may be, for example, 10 to 30 MPa, 15 to 30 MPa, 20 to 30 MPa, or 1 to 15 MPa, 1 to 10 MPa, or 1 to 8 MPa.
[0024] Preferred embodiments of the porous body (B) include fibrous bodies, resin foams, and porous bodies composed of metals, ceramics, glass, etc., of which fibrous bodies and resin foams are preferred because they are elastic and lightweight.
[0025] The fibrous body is not particularly limited as long as it is an aggregate of fibers having voids on the surface and inside thereof, and may be either a woven fabric or a nonwoven fabric such as felt. For example, the fibrous body may be an organic fiber such as animal or plant fiber, a resin fiber, or an inorganic fiber such as glass fiber, or a mixture thereof. More specifically, examples of such fibers include fibers mainly composed of animal and vegetable fibers such as cotton, wool, and wood wool; fibers mainly composed of organic fibers such as polyolefin fibers such as polyethylene, polypropylene, and copolymerized polypropylene; polyamide fibers such as nylon 6, nylon 66, and copolymerized polyamide; and polyester fibers such as polyethylene terephthalate, polybutylene terephthalate, copolymerized polyester, polylactic acid, polybutylene succinate, and polyethylene succinate; fibers mainly composed of inorganic fibers such as glass fibers and glass wool; and fibers composed of mixtures thereof. The fibers may contain a binder (bonding agent) as appropriate depending on the type and manufacturing method. The term "main component" refers to a component that occupies 70% by mass or more of the total amount of the fibers, preferably 80% by mass or more, and more preferably 90% by mass or more.
[0026] Among the above-mentioned fibrous bodies, from the viewpoint of improving flexibility, i.e., load distribution, a fibrous body containing organic fibers as a main component is preferred, a fibrous body containing polyester-based fibers as a main component is more preferred, and a fibrous body containing polyethylene terephthalate as a main component is particularly preferred.
[0027] The fibrous body is manufactured by a known method. For example, nonwoven fabrics such as felt can be appropriately manufactured using various methods such as a needle punch method, a chemical bond method, a thermal bond method, and a hydroentanglement method.
[0028] Examples of the resin foams that can be used include polyolefin foams such as polyurethane foam, polyethylene foam, and polypropylene foam; polystyrene foam; polyamide foam; polyester foams such as polyethylene terephthalate (PET) foam and polybutylene terephthalate (PBT); (meth)acrylic foam; phenol foam; polyvinyl chloride foam; polyimide foam; silicone resin foam; urea resin foam; melamine resin foam; ethylene propylene diene rubber (EPDM) foam; styrene butadiene rubber (SBR) foam; nitrile butadiene rubber (NBR) foam; ethylene-vinyl acetate copolymer (EVA) foam; ethylene-acrylic acid copolymer foam; and ethylene-ethyl acrylate copolymer (EEA) foam. As described above, when the term "polyurethane foam" is used, it means "a polyurethane foam containing polyurethane as a main component", and the "main component" means a component that occupies 70% by mass or more of the total amount of the resin foam, preferably 80% by mass or more, and more preferably 90% by mass or more. The same applies to foams other than polyurethane foam.
[0029] Among the above-mentioned resin foams, from the viewpoint of improving flexibility, that is, load dispersion, polyolefin foams are preferred, and polyethylene foams are more preferred.
[0030] The resin foam is produced by mixing various foaming agents in accordance with a conventional method, and can be appropriately produced using various methods such as a normal pressure foaming method, an extrusion foaming method, and a press foaming method.
[0031] The porous body (B) such as the fibrous body or the resin foam may be impregnated with various components such as a resin component. When such a process is performed, the specific gravity and tensile modulus of elasticity of the porous body (B) are the values of the specific gravity and tensile modulus of elasticity after the process.
[0032] <Adhesive (C) layer> The adhesive (C) layer is a layer composed of an adhesive (C). The adhesive (C) is not particularly limited as long as it has good adhesive properties with respect to the wooden veneer (A), and adhesives (C1), adhesives (C2), and mixtures thereof can be used.
[0033] Examples of the adhesive (C1) include acrylic adhesives, polyurethane adhesives, polyester adhesives, rubber adhesives, and silicone adhesives. Examples of the adhesive (C2) include thermoplastic adhesives (hot melt adhesives) such as polyolefin adhesives, ethylene vinyl acetate adhesives, polyamide adhesives, polyurethane adhesives, and polyester adhesives, and thermosetting adhesives such as acrylic urethane adhesives, modified silicone adhesives, cyanoacrylate adhesives, urea adhesives, phenol adhesives, and epoxy adhesives. Among these, the adhesive (C1) is preferred from the viewpoint of imparting flexibility to the wood laminate itself. Among the adhesives (C1), acrylic adhesives, polyurethane adhesives, and polyester adhesives are preferred from the viewpoint of further improving adhesion to the wooden veneer (A), and acrylic adhesives are more preferred.
[0034] Examples of acrylic adhesives include acrylic adhesives in which the base polymer (50% by mass or more of the entire acrylic adhesive) is an acrylic polymer (homopolymer or copolymer) using one or more types of (meth)acrylic acid alkyl esters as a monomer component. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and butyl (meth)acrylate. Examples of (meth)acrylic acid C1-20 alkyl esters include nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Note that "(meth)acrylic" means acrylic or methacrylic.
[0035] The adhesive (C1) preferably has a glass transition temperature (Tg) of 20° C. or lower, more preferably 10° C. or lower, and particularly preferably 0° C. or lower. The adhesive preferably has a glass transition temperature (Tg) of −100° C. or higher, more preferably −70° C. or higher, and particularly preferably −50° C. or higher. Within these ranges, the adhesion tends to be further improved.
[0036] The glass transition temperature is calculated, for example, by the Fox formula. For example, the glass transition temperature of an acrylic pressure-sensitive adhesive is calculated as follows.
number
[0037] That is, the glass transition temperature (Tg) is a value calculated by applying the glass transition temperature and weight fraction when each monomer constituting the pressure-sensitive adhesive is made into a homopolymer to the Fox formula. The glass transition temperature when the monomer constituting the pressure-sensitive adhesive (C1) is made into a homopolymer is usually measured by a differential scanning calorimeter (DSC), and can be measured by a method conforming to JISK7121-1987 or JISK6240.
[0038] The adhesive (C) layer may contain additives other than the adhesive (C) as long as the adhesive does not impair the adhesion to the wooden veneer (A) and the porous body (B). Examples of the additives include crosslinkers, tackifiers, plasticizers, pigments, dyes, fillers, antioxidants, conductive materials, antistatic agents, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, antioxidants, etc. These may be used alone or in combination of two or more.
[0039] The pressure-sensitive adhesive (C) may be in the form of pellets, powder, sheet, etc., but is preferably in the form of a sheet from the viewpoint of workability and from the viewpoint of achieving the effects of the present invention more prominently.
[0040] The sheet-like adhesive (C) may or may not have a substrate, but is preferably a substrate coated with the adhesive on both sides. Examples of the substrate include nonwoven fabric, synthetic resin film, and foam. Specific examples include polyester substrate, nonwoven fabric, polyethylene substrate, and paper substrate.
[0041] The thickness of the adhesive (C) layer is selected according to the type and shape of the wood laminate, but is usually 10 to 400 μm, preferably 20 to 300 μm, more preferably 30 to 250 μm, and particularly preferably 40 to 180 μm. If the thickness is below these ranges, the adhesion between the adhesive (C) layer and the wooden veneer (A) layer and the porous body (B) layer tends to decrease. On the other hand, if the thickness exceeds these ranges, the strength of the wood laminate tends to decrease.
[0042] <Other layers> The wood laminate may contain other layers in addition to the wooden veneer (A) layer, the porous body (B) layer, and the adhesive (C) layer, as long as the effect of the present invention is not impaired. Examples of the other layers include layers made of wood materials with a specific gravity of less than 0.3 and porous bodies with a specific gravity of more than 0.5. The other layers may be layers made of resins such as polyethylene, polypropylene, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polyvinyl chloride, nylon 610 (PA610), nylon 6T (PA6T), polyphenylene sulfide, elastomers, and polystyrene; metals such as iron, stainless steel, copper, and aluminum; and fiber-reinforced plastics such as CFRP, either alone or in combination of two or more of these.
[0043] The present wood laminate may include the other layers, but from the viewpoint of significantly achieving the effects of the present invention, it is preferable that the present wood laminate does not include the other layers. However, if the present wood laminate includes the other layers for any purpose, the total volume (W V ) to the total volume of the other layers (E V ) volume ratio (E V / W V ) is, for example, preferably less than 10 / 100, more preferably less than 5 / 100, and particularly preferably less than 2 / 100.
[0044] <Manufacturing method of this wood laminate> This wood laminate is produced by a manufacturing method including a step of laminating a wooden veneer (A), a porous body (B), and a pressure-sensitive adhesive (C) and bonding them together under pressure. Specifically, this wood laminate can be produced by, but is not limited to, applying a pressure-sensitive adhesive (C) to at least one of the wooden veneer (A) and the porous body (B), or by placing a sheet-like pressure-sensitive adhesive (C) between the two layers (between (A) and (B)) and then applying pressure to them.
[0045] The pressure in the pressurizing step is usually 0.01 to 10 MPa, preferably 0.1 to 5 MPa, and particularly preferably 0.2 to 2 MPa. If the pressure is above or below these ranges, the intended shape of the wood laminate tends not to be sufficiently secured.
[0046] The method for producing the present wood laminate may also include a step of applying pressure and heating depending on the type of adhesive (C) and the desired shape of the wood laminate. The heating temperature in this step is preferably 60 to 150° C., more preferably 80 to 140° C., and particularly preferably 90 to 130° C. As the heating method, for example, a method of heating by heat transfer from a press facility, a method of heating with hot air, a method of heating with electromagnetic waves, or any other known method generally used for heating in the production of plywood can be used.
[0047] In the method for producing the present wood laminate, examples of the method for disposing a layer of adhesive (C) between the wooden veneer (A) layer and the porous body (B) layer include a method in which a sheet-like adhesive (C) is disposed between the wooden veneer (A) and the porous body (B), a method in which the adhesive (C) is made into a solution and applied to the wooden veneer (A) and / or the porous body (B) and then laminated, a method in which a particulate adhesive (C) is disposed between the wooden veneer (A) and the porous body (B) and melted by heating, etc. Among these, the method in which a sheet-like adhesive (C) is disposed between the wooden veneer (A) and the porous body (B) is preferred from the viewpoint of more easily producing the present wood laminate.
[0048] <Wood laminate> The present wood laminate may have a multi-layer structure having at least one layer each of a wooden veneer (A), a porous body (B), and an adhesive (C), and any layer structure may be adopted depending on the intended use, etc.
[0049] The shape and thickness of the wood laminate are selected according to the intended use. The thickness of the wood laminate is preferably 0.5 to 6.0 cm, more preferably 0.7 to 5.0 cm, and particularly preferably 0.8 to 4.0 cm. Within this range, it tends to be easier to achieve both light weight and flexibility, i.e., load dispersion.
[0050] The number of wooden veneer (A) layers in the present wood laminate is selected according to the thickness and shape of the wood laminate, and examples include 1 to 20 layers, 3 to 18 layers, and 5 to 15 layers. By keeping the number within this range, it tends to be easier to achieve both light weight and flexibility, i.e., load distribution. The types and shapes (including thickness) of the multiple wooden veneer (A) layers included in the wood laminate may be the same or different.
[0051] The number of porous body (B) layers in the wood laminate is selected according to the thickness and shape of the wood laminate, and examples include 1 to 20 layers, 3 to 18 layers, and 5 to 15 layers. By keeping the number within this range, it tends to be easier to achieve both light weight and flexibility, i.e., load distribution. The types and shapes (including thickness) of the multiple porous body (B) layers included in the wood laminate may be the same or different.
[0052] The number of layers of the adhesive (C) in the wood laminate is set according to the number of layers of the wooden veneer (A), the porous body (B), etc. The types and shapes (including thickness) of the multiple adhesive (C) layers included in the wood laminate may be the same or different.
[0053] In order to increase the flexibility of the wood laminate, which is lightweight and has excellent load distribution properties, the total volume (A V ) relative to the total volume of the porous body (B) layer (B V ) volume ratio (B V / A V From the viewpoint of significantly exhibiting the effects of the present invention, the volume ratio (B V / A V) is preferably 50 / 100 or more, more preferably 70 / 100 or more. V / A V ) is preferably 300 / 100 or less, more preferably 200 / 100 or less.
[0054] The wood laminate is lightweight and has excellent load distribution properties, and in order to increase flexibility, the total volume (W V The total volume (A) of the wood veneer (A) layer and the porous body (B) layer V +B V ) volume ratio ((A V +B V ) / W V It is preferable that the volume ratio ((A V +B V ) / W V ) may be 90 / 100 or more, 95 / 100 or more, or 98 / 100 or more.
[0055] As for the layer structure of the present wood laminate, for example, in a wood laminate having two or more layers of wooden veneer (A), it is preferable that the wooden veneers (A) are laminated with their fiber directions parallel to each other (parallel lamination).
[0056] From the viewpoint of improving the lightness, the specific gravity of the present wood laminate is preferably 0.4 or less, more preferably 0.38 or less, and even more preferably 0.35 or less. From the viewpoint of maintaining shape retention, the specific gravity of the present wood laminate is preferably 0.25 or more, and particularly preferably 0.30 or more. The specific gravity of the present wood laminate can be measured by the method described in the examples below.
[0057] The stress (15 mm) of this wood laminate when bent as measured by the method described in the Examples below is, for example, less than 5.0 N, preferably 4.5 N or less, and more preferably 4.0 N or less. When the stress when bent is equal to or less than the upper limit, flexibility tends to be increased.
[0058] The wood laminate has a load distribution ratio of, for example, 40% or more, preferably 45% or more, and more preferably 50% or more, as measured by the method described in the Examples below. A load distribution ratio of at least the lower limit tends to increase flexibility.
[0059] The wood laminate has a resilience of, for example, 25% or more, preferably 35% or more, and more preferably 40% or more, as measured by the method described in the Examples below. Having a resilience of at least the lower limit tends to increase elastic strength.
[0060] Specific examples of the layer structure of the present wood laminate include, but are not limited to, "A1 / C1 / B1", ... Any layer structure may be used, such as "A1 / C1 / B1 / C2 / A2", "A1 / C1 / B1 / C2 / A2 / C3 / B2 / C4 / A3 / C5 / B3", "A1 / C1 / B1 / C2 / A2 / C3 / B2 / C4 / A3 / C5 / B3 / C6 / A4", or "D1 / C1 / A1 / C2 / B1 / C3 / A2 / C4 / A3 / C5 / B2 / C6 / A4 / C7 / D2". Among these, it is preferable that at least one or both of the outermost surfaces of the wood laminate is a wood veneer (A) layer.
[0061] In addition, in the present wood laminate, for example, a porous body (B+C) having a pressure-sensitive adhesive (C) layer can be used as the porous body (B) layer and the pressure-sensitive adhesive (C) layer of the present wood laminate. Specifically, for example, a three-layer sheet-like porous body (B+C) having pressure-sensitive adhesive (C) layers on both sides of the porous body (B) can be used. As a method for producing the present wood laminate using such a sheet-like porous body (B+C), the present wood laminate can be obtained by placing the sheet-like porous body (B+C) between the wooden veneers (A).
[0062] In addition, among the porous bodies (B+C) having a pressure-sensitive adhesive (C) layer, the pressure-sensitive adhesive (C1) layer of the porous body (B+C) has a pressure-sensitive adhesive (C1) layer, and the pressure-sensitive adhesive (C1) layer is sufficiently thin and sufficiently flexible, so that the "thickness", "specific gravity" and "tensile modulus" measured for the porous body (B+C) having a pressure-sensitive adhesive (C1) layer can be regarded as the "thickness", "specific gravity" and "tensile modulus" of the porous body (B). In other words, "the porous body (B) is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm" in the present invention implies "the porous body (B+C) having a pressure-sensitive adhesive (C1) layer is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm". In addition, "the tensile modulus of the porous body (B) is 1 to 30 MPa" in the present invention implies "the tensile modulus of the porous body (B+C) having a pressure-sensitive adhesive (C1) layer is 1 to 30 MPa".
[0063] In other words, this wood laminate is a wood laminate having a wooden veneer (A) layer and a porous body (B+C) layer having an adhesive (C1) layer, in which the wooden veneer (A) is a wooden veneer having a specific gravity of 0.3 or more and a thickness of 0.2 to 3 mm, and the porous body (B+C) having an adhesive (C1) layer is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm. The present wood laminate also refers to a wood laminate having a wooden veneer (A) layer and a porous body (B+C) layer having an adhesive (C1) layer, in which the wooden veneer (A) is a wooden veneer having a specific gravity of 0.3 or more and a thickness of 0.2 to 3 mm, and the porous body (B+C) having an adhesive (C1) layer is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm and a tensile modulus of elasticity of 1 to 30 MPa.
[0064] <Application> The wood laminate is suitable for use in wood components or wood products such as stationery, small items, toys, furniture, building materials, automotive parts, etc. In addition, the wood laminate has spring deformation properties, making it useful in that it can be reused repeatedly. EXAMPLES
[0065] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0066] First, the following materials were prepared. ·Wood veneer (A): Cedar veneer (specific gravity 0.38, thickness 1mm) Porous material (B): Polyester felt manufactured by Sunfelt (specific gravity 0.15, tensile modulus 26.4 MPa, thickness 1 mm) Porous body with adhesive layers on both sides (B+C): Teraoka Seisakusho double-sided tape, No. 7811 (double-sided tape with acrylic adhesive layers on both sides of a polyethylene foam: specific gravity 0.25, tensile modulus 3.23 MPa, thickness 1.2 mm) Porous body with adhesive layers on both sides (B+C'): 3M double-sided tape, VHB, Y-4950 (double-sided tape with acrylic adhesive layers on both sides of acrylic foam: specific gravity 0.71, tensile modulus 0.91MPa, thickness 1.14mm) Adhesive (C1): Nittо double-sided tape, No. 5000NS (acrylic adhesive, thickness 0.16 mm) Adhesive (C2): Modified polyvinyl acetate resin emulsion adhesive manufactured by Franklin Co.
[0067] The specific gravity and tensile modulus were measured by the following methods.
[0068] <Specific gravity measurement test> Using test specimens (15 mm long x 50 mm wide) made from wood veneer (A), porous body (B), and porous body with adhesive layers on both sides (B+C, B+C'), the air-dry weight (g) at a constant weight was measured in a constant temperature and humidity environment of 20°C and 65% RH, and the volume (cm) was calculated from the geometric shape. 3 ) (g / cm 3 ).
[0069] <Tensile elasticity measurement test> The tensile modulus of elasticity of the porous body (B) and the porous bodies having pressure-sensitive adhesive layers on both sides (B+C, B+C') was measured as follows. The porous body was cut to prepare rectangular specimens measuring 15 mm in width and 50 mm in length. Tensile tests were carried out using a Shimadzu Corporation universal testing machine AGS-X under conditions of a temperature of 23°C ± 2°C, relative humidity of 50% ± 10%, with a chuck distance of 50 mm and a speed of 5 mm / min, to measure the tensile modulus of elasticity (MPa).
[0070] <Example 1> Using wooden veneer (A), porous body (B), and adhesive (C1), the following layer structure was created with wooden veneer (A) as the outermost layer on both sides, and cold pressed (at room temperature) at a pressing pressure of 0.5 MPa for 30 seconds to obtain a wood laminate with a thickness of 8.5 mm. Note that wooden veneer (A) is a parallel layer. [Layer configuration] A / C1 / B / C1 / A / C1 / B / C1 / A / C1 / B / C1 / A
[0071] <Example 2> Using wooden veneer (A) and porous bodies (B+C) with adhesive layers on both sides, the wooden veneer (A) and the porous bodies (B+C) were arranged alternately, with the wooden veneer (A) being the outermost layer on both sides, as shown below, and cold pressed (at room temperature) at a pressing pressure of 0.5 MPa for 30 seconds to obtain a wood laminate with a thickness of 7.2 mm. The wooden veneer (A) was a parallel laminate. [Layer configuration] A / B+C / A / B+C / A / B+C / A
[0072] <Comparative Example 1> Using the wooden veneer (A) and adhesive (C2), the following layer structure was formed, with the wooden veneer (A) being the outermost layer on both the front and back sides, and cold pressing (at room temperature) was performed at a pressing pressure of 0.5 MPa for a pressing time of 6 hours to obtain a wood laminate with a thickness of 7.2 mm. The application amount of adhesive (C2) was 150 g / m 2 and the wood veneer (A) is parallel laminated. [Layer configuration] A / C2 / A / C2 / A / C2 / A / C2 / A / C2 / A / C2 / A
[0073] <Comparative Example 2> Using wooden veneer (A) and porous body (B+C') with adhesive layers on both sides, wooden veneer (A) and porous body (B+C') were arranged alternately, with wooden veneer (A) being the outermost layer on both sides, as shown below, and cold pressed (at room temperature) with a pressing pressure of 0.5 MPa and a pressing time of 30 seconds to obtain a wood laminate with a thickness of 7.3 mm. The wooden veneer (A) is a parallel laminate. [Layer composition] A / B+C' / A / B+C' / A / B+C' / A
[0074] The following tests were carried out on the obtained laminate, and the results are shown in Table 1.
[0075] <Load deflection test> The load deflection test of the wood laminate was carried out as follows. A test specimen measuring 8 mm thick x 12 mm wide x 195 mm long was prepared from the wood laminate, and a three-point bending test was carried out with a support distance of 180 mm and a loading speed of 3 mm / min to determine the stress (N) at a bending deflection of 15 mm. The long side of the test specimen was parallel to the grain direction. The temperature and humidity environment for the test was 20°C and 65% RH. (Evaluation Criteria) ○: Less than 5.0N ×: 5.0N or more
[0076] <Load distribution test (load distribution rate)> The load distribution of the wood laminate was tested as follows. A test specimen measuring 100 mm wide x 100 mm long x 28 mm thick was prepared from the wood laminate, and the upper surface of the test specimen was covered with a load measuring sensor SR Soft Vision manufactured by Sumitomo Riko Co., Ltd., having a grid with a resolution of 22 mm square, and pressure was applied with a spherical surface made of Styrofoam (registered trademark) with a curvature radius of R300. When the grid directly under the lowest point of the sphere was pressurized to approximately 180 mmHg, the total load around the grid was measured, and the ratio of the load of the grid directly under the lowest point to the total load was obtained as the load dispersion rate (%). The calculation formula is as follows. The temperature and humidity environment of the test was 20°C and 65% RH. Load distribution rate (%) = Load of grid directly below lowest point / Total load x 100 (Evaluation Criteria) 〇: 40% or more ×: Less than 40%
[0077] <Rebound resilience test> The rebound resilience of the wood laminate was tested as follows. A test specimen measuring 100 mm wide x 100 mm long x 8 mm thick was prepared from the wood laminate. A steel ball (Grade G40, mass 16.8 g) with a diameter of 16 mm as specified by JIS B1501 was held at a specified height inside a vertical transparent tube with an inner diameter of 30 mm, and the steel ball was dropped without rotating into the center of the test specimen. The initial drop height of the steel ball was 500 mm from the surface of the test specimen to the bottom of the steel ball. The steel ball was allowed to fall freely, and the rebound height was recorded using a high-speed camera VW-6000 manufactured by Keyence Corporation. The rebound resilience (%) was calculated from the ratio of the maximum rebound height to the initial drop height. The presence or absence of a drop mark after the test was also confirmed. The temperature and humidity environment for the test was 20°C and 65% RH. (Evaluation Criteria) 〇: 25% or more ×: Less than 25%
[0078] <Specific gravity measurement test of laminate> A test specimen measuring 100 mm in width and 100 mm in length was prepared from the wood laminate. The air-dry weight (g) of the specimen when it reached a constant weight in a constant temperature and humidity environment of 20°C and 65% RH was calculated based on the volume (cm) calculated from the geometric shape. 3 ) (g / cm 3 ).
[0079] [Table 1]
[0080] From the above results, compared to Comparative Examples 1 and 2, the stress at the time of bending deflection of 15 mm was smaller in Examples 1 and 2, and the load distribution rate was clearly increased. Therefore, it can be said that when a load is applied locally in the planar direction, the material is soft and can bear the load over a wide area by dispersing deformation even with a smaller load. This is because the wooden veneer (A) layer and the porous body (B) layer are appropriately combined, and the wooden laminate is more easily deformed by indentation and shear deformation, resulting in deformation over a wide area. In particular, when comparing Comparative Example 2 with Examples 1 and 2, there is a large difference in resilience despite the porous bodies being laminated in the same way, which clearly shows that the physical properties of the porous body (B) layer of the present invention have a large effect on the flexibility in the planar direction.
[0081] In addition, in Examples 1 and 2, the wooden veneer (A) is assisted in bending and restoring its shape when a steel ball is dropped, and the surface of the wooden veneer (A) is not marked with a striking ball drop, and the wooden veneer (A) is spring-deformed, making it possible to use the wooden veneer repeatedly. On the other hand, in Comparative Examples 1 and 2, the striking ball drop is noticeable, and it is clear that the impact energy is consumed in the plastic deformation of the wooden veneer (A) and the viscoplastic behavior of the adhesive layer, which causes durability problems in the applications shown below. [Industrial Applicability]
[0082] The wood laminate of the present invention can be used for a wide range of applications, such as small items, furniture, and building materials such as plywood, control panels, and structural plywood. In addition, because it is spring-deformed, it can be reused repeatedly.
Claims
1. The wood laminate has a wooden veneer (A) layer, a porous body (B) layer, and a pressure-sensitive adhesive (C) layer, characterized in that the wooden veneer (A) is a wooden veneer having a specific gravity of 0.3 or more and a thickness of 0.2 to 3 mm, and the porous body (B) is an elastic body having a specific gravity of 0.5 or less and a thickness of 0.2 to 3 mm.
2. 2. The wood laminate according to claim 1, wherein at least one outermost surface is a wood veneer (A) layer.
3. 3. The wood laminate according to claim 1, wherein the porous body (B) has a tensile modulus of elasticity of 1 to 30 MPa.
4. 3. The wood laminate according to claim 1, wherein the specific gravity of the wood laminate is 0.4 or less.
5. The total volume (A V The total volume of the porous body (B) layer relative to the total volume of the porous body (B) layer (B V ) volume ratio (B V / A V 3. The wood laminate according to claim 1, wherein the ratio of the laminated wood to the laminated wood is 25 / 100 to 500 / 100.
6. 3. A method for producing a wood laminate according to claim 1 or 2, comprising the steps of stacking a wooden veneer (A), a porous body (B) and an adhesive (C) and bonding them together under pressure, wherein the adhesive (C) is in sheet form.