Resin composition, cured material, and organic el display device
The resin composition addresses the issues of low water absorption and flatness in organic EL display devices by using polyimide precursors with specific diamine residues and a photoacid generator, achieving high sensitivity and durability for improved display performance.
Patent Information
- Application Number
- JP2023053079
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing resin compositions for organic EL display devices lack sufficient performance in terms of low water absorption and high flatness, which are essential for reliable and high-quality display performance, especially with increasing pixel density and substrate size.
A resin composition comprising polyimide or polyimide precursors with specific diamine residues and a photoacid generator, optimized to achieve high sensitivity, low water absorption, and excellent surface flattening properties, using components with trifluoromethyl and phenolic hydroxyl groups, and a thermal crosslinking agent for improved durability.
The resin composition achieves high sensitivity, low water absorption, and excellent surface flattening, resulting in improved display quality by reducing moisture sensitivity and enhancing the reliability of organic EL devices.
Smart Images

Figure 2024141430000013 
Figure 2024141430000001 
Figure 2024141430000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a cured product using the same, and an organic EL display device including the cured product. [Background technology]
[0002] 2. Description of the Related Art Many products using organic electroluminescence (hereinafter, "organic EL") display devices have been developed as display devices having thin displays, such as smartphones, tablet PCs, and televisions.
[0003] In general, an organic EL display device has a driving circuit, a planarization layer, a first electrode, a pixel division layer, a light-emitting layer, and a second electrode on a substrate, and can emit light by applying a voltage between the opposing first and second electrodes or by passing a current between them. Among these, photosensitive resin compositions that can be patterned by ultraviolet irradiation are generally used as materials for the planarization layer and the pixel division layer. Among these, photosensitive resin compositions using polyimide-based or polybenzoxazole-based resins are preferably used because they have high heat resistance and generate less gas components from the cured product, and therefore can provide highly reliable organic EL display devices (see, for example, Patent Document 1 and Patent Document 2).
[0004] On the other hand, organic EL elements are considered to be vulnerable to moisture, and in order to obtain a highly reliable organic EL display device, it is necessary to reduce the moisture generated from the surrounding materials as much as possible, and low water absorption materials are required for the planarization layer and pixel division layer. Furthermore, organic EL display devices are becoming increasingly dense in pixels and wiring, and materials that can highly planarize the surfaces of objects with uneven surfaces are required. Also, for reasons such as larger substrates and improved productivity, resin compositions are required to have higher sensitivity in order to shorten exposure times.
[0005] In response to these problems, mixing a novolac resin or a polyhydroxystyrene resin with a polyimide resin or a polybenzoxazole resin has been investigated as a resin composition capable of increasing sensitivity (see, for example, Patent Documents 3 and 4). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-91343 A [Patent Document 2] JP 2002-116715 A [Patent Document 3] JP 2005-352004 A [Patent Document 4] JP 2014-59463 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, it is difficult to say that the materials proposed in the above-mentioned patent documents have sufficient performance in terms of low water absorption, high flatness, etc. In view of the above problems, the present invention aims to provide a resin composition that is highly sensitive and capable of highly flattening the surface of an object having an uneven surface, and further has low water absorption after curing. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention has the following configuration. [1] A resin composition containing one or more resins selected from the group consisting of polyimides, polyimide precursors, and copolymers thereof (hereinafter, sometimes referred to as component (A)), and a photoacid generator (hereinafter, sometimes referred to as component (B)), The component (A) has one or more acid dianhydride residues and two or more diamine residues, two of the two or more kinds of diamine residues are a diamine residue having a trifluoromethyl group and a phenolic hydroxyl group (hereinafter, may be referred to as a DA1 residue), and a diamine residue having a trifluoromethyl group and no phenolic hydroxyl group (hereinafter, may be referred to as a DA2 residue); At least one diamine residue among the DA2 residues has a melting point as a diamine compound of 110° C. or higher and 180° C. or lower; A resin composition in which the ratio of DA2 residues is 15 mol % or more and 40 mol % or less when the total amount of diamine residues in the component (A) is taken as 100 mol %. [2] The resin composition according to [1], wherein all or a part of the one or more types of acid dianhydride residues are acid dianhydride residues having a diphenyl ether structure. [3] The resin composition according to [1] or [2], wherein the DA1 residue is a diamine residue represented by formula (1).
[0009] [ka]
[0010] (In formula (1), R 1 represents -C(CF3)2- or -CH(CF3)-. * represents the point of attachment to the imide structure, amic acid structure, or amic acid ester structure. [4] The resin composition according to any one of [1] to [3], wherein at least one diamine residue among the DA2 residues is a diamine residue having a diphenyl ether structure. [5] The resin composition according to any one of [1] to [4], wherein the component (A) contains either or both of an acid anhydride residue having a reactive unsaturated bond and a monoamine residue having a reactive unsaturated bond. [6] The resin composition according to any one of [1] to [5], further comprising a thermal crosslinking agent (hereinafter, may be referred to as component (C)). [7] The photosensitive resin composition according to [6], wherein all or a part of the component (C) is one or more types of thermal crosslinking agents selected from the group consisting of an isocyanuric ring structure-containing epoxy thermal crosslinking agent, an alicyclic epoxy thermal crosslinking agent, and an aliphatic epoxy thermal crosslinking agent. [8] A cured product obtained by curing the resin composition according to any one of [1] to [7]. [9] An organic electroluminescence display device comprising the cured product according to [8]. Effect of the Invention
[0011] INDUSTRIAL APPLICABILITY The resin composition of the present invention is capable of giving a cured product that is highly sensitive, has excellent planarization ability for uneven surfaces, and has low water absorption, and is suitable for use in planarization layers and bank layers in organic electroluminescence display devices. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a cross-sectional view of a flatness evaluation sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will now be described in detail with reference to examples.
[0014] The resin composition of the present invention is a resin composition containing one or more resins (component (A)) selected from the group consisting of polyimides, polyimide precursors, and copolymers thereof, and a photoacid generator (component (B)), The component (A) has one or more acid dianhydride residues and two or more diamine residues, two of the two or more diamine residues have a diamine residue having a trifluoromethyl group and a phenolic hydroxyl group (DA1 residue) and a diamine residue having a trifluoromethyl group and no phenolic hydroxyl group (DA2 residue); At least one diamine residue among the DA2 residues has a melting point as a diamine compound of 110° C. or higher and 180° C. or lower; When the total amount of diamine residues in the component (A) is taken as 100 mol %, the ratio of DA2 residues is 15 mol % or more and 40 mol % or less in the resin composition.
[0015] The resin composition of the present invention is highly sensitive, has excellent flattening properties on uneven surfaces, and can give a cured product with low water absorption.
[0016] In the present invention, the acid dianhydride residue is a structure derived from an acid dianhydride or its derivative as a raw material for polyimide or polyimide precursor resin, and is a tetravalent structural portion obtained by removing two acid anhydride groups from an acid dianhydride.Similarly, the diamine residue is a structure derived from a diamine or its derivative as a raw material for polyimide or polyimide precursor resin, and is a divalent structural portion obtained by removing two amino groups from a diamine.
[0017] Each component will be described in detail below, but the present invention is not limited thereto.
[0018] <Component (A)> The component (A), which is one of the components of the resin composition of the present invention, can be synthesized by a known method. Examples of polyimide precursors include polyamic acid, polyamic acid ester, polyamic acid amide, polyisoimide, etc. A copolymer of two types of resins selected from polyimide and polyimide precursors can be synthesized by a known method.
[0019] The component (A) has one or more types of acid dianhydride residues and two or more types of diamine residues, two of which are a diamine residue having a trifluoromethyl group and a phenolic hydroxyl group (DA1 residue), and a diamine residue having a trifluoromethyl group and no phenolic hydroxyl group (DA2 residue).
[0020] The acid dianhydride residue contained in the component (A) is not particularly limited, but it is preferable that at least one of the one or more acid dianhydride residues has a diphenyl ether structure. Examples of acid dianhydrides that give acid dianhydride residues having a diphenyl ether structure include bis(3,4-dicarboxyphenyl)ether dianhydride (ODPA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BSAA), and 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride (HQDA). In terms of flattening property and folding resistance, bis(3,4-dicarboxyphenyl)ether dianhydride and 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride are particularly preferable.
[0021] The ratio of the diphenyl ether structure-containing acid dianhydride residues to the total amount of the dianhydride residues is preferably 51 mol% or more. The dianhydride that provides the other dianhydride residues that can be used as the dianhydride residues contained in the component (A) is not particularly limited as long as it is a dianhydride, but examples thereof include aromatic tetracarboxylic dianhydrides such as pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, and 2,2',3,3'-benzophenonetetracarboxylic dianhydride, and aliphatic tetracarboxylic dianhydrides such as butanetetracarboxylic dianhydride and 1,2,3,4-cyclopentanetetracarboxylic dianhydride.
[0022] From the viewpoint of sensitivity when the photosensitive resin composition is prepared, the diamine residues (DA1 residues) having a trifluoromethyl group and a phenolic hydroxyl group contained in the component (A) are preferably 60 mol% to 85 mol% based on 100 mol% of all diamine residues. The diamine residues (DA2 residues) having a trifluoromethyl group and no phenolic hydroxyl group contained in the component (A) are 15 mol% to 40 mol% based on 100 mol% of all diamine residues. The component (A) may contain diamine residues other than the DA1 residues and the DA2 residues.
[0023] In the resin composition of the present invention, it is important to use a diamine compound corresponding to at least one diamine residue among the DA2 residues contained in the component (A) that has a melting point of 110°C or more and 180°C or less. The diamine compound corresponding to the diamine residue is a diamine compound having a structure in which an amino group is bonded to the bonding point of the diamine residue. By using a diamine compound corresponding to the DA2 residue that has a melting point of 110°C or more and 180°C or less, excellent flattening properties are achieved for the surface of an object having an uneven surface.
[0024] In the resin composition of the present invention, when the total amount of diamine residues contained in the (A) component is taken as 100 mol%, the ratio of DA2 residues is 15 mol% or more and 40 mol% or less, and by being in this range, it is possible to achieve both the sensitivity of the photosensitive resin composition and the low water absorption and planarization properties of the cured product. From the viewpoint of low water absorption and planarization properties, when the total amount of diamine residues is taken as 100 mol%, the ratio of DA2 residues is particularly preferably 30 mol% or more and 40 mol% or less.
[0025] Examples of diamines from which the diamine residue (DA1) having a trifluoromethyl group and a phenolic hydroxyl group is derived include, but are not limited to, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 1,1,1-trifluoro-2,2-bis(3-amino-4-hydroxyphenyl)ethane (Bis-AP-EF), and diamine compounds represented by the following formula (2). Two or more of these may be used in combination.
[0026] [ka]
[0027] In the diamine compound represented by formula (2), a part or all of the phenolic hydroxyl group undergoes dehydration condensation with the adjacent amide group during thermal curing to form a benzoxazole ring, and the number of phenolic hydroxyl groups in the cured resin composition can be reduced. For this reason, it is particularly preferable to use the diamine compound represented by formula (2) from the viewpoint of low water absorption. As the diamine that provides the DA1 residue, only the diamine compound represented by formula (2) may be used, or other diamines having a trifluoromethyl group and a phenolic hydroxyl group may be used in combination. Among the diamine residues (DA2 residues) having a trifluoromethyl group and no phenolic hydroxyl group, examples of diamines having a melting point of 110° C. or more and 180° C. or less as a diamine compound include, but are not limited to, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (6FODA) (melting point: 126° C.), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP) (melting point: 160° C.), 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene (p-6FAPB) (melting point: 134° C.), 1,1,1-trifluoro-2,2-bis(4-aminophenyl)ethane ( Bis-A-EF) (melting point: 138°C), 1,1,1-trifluoro-2,2-bis(3-methyl-4-aminophenyl)ethane (Bis-3-AT-EF) (melting point: 142°C), 1,1,1-trifluoro-2,2-bis(3,5-dimethyl-4-aminophenyl)ethane (Bis-3,5-AX-EF) (melting point: 146°C), 4,4'-{[bis(trifluoromethyl)methylene]bis(4,1-phenyleneoxy)}bis[3-(trifluoromethyl)aniline](HFHAPP) (melting point: 155°C), 1,1,1-trifluoro-2,2-bis(2,5-dimethyl-4-aminophenyl)ethane (Bis-2,5-AX-EF) (melting point: 164°C). These diamine compounds may be used alone or in combination of two or more.By using a diamine compound corresponding to the DA2 residue having a melting point of 110°C or more and 180°C or less, when a resin film obtained by applying the resin composition onto an uneven surface of an object is heat cured, the resin composition has a fluidity sufficient to flow into the recesses of the uneven surface of the object, and does not fill holes such as contact holes patterned by light irradiation, making it possible to achieve both planarization and resolution. In terms of folding resistance, diamine residues having a diphenyl ether structure are particularly preferred, and examples of diamines from which diamine residues having a diphenyl ether structure are 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether and 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.
[0028] Among the diamine residues (DA2 residues) having a trifluoromethyl group and no phenolic hydroxyl group, examples of diamines having a melting point as a diamine compound of less than 110°C or more than 180°C include 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane (Bis-AT-AF) (melting point: 105°C), 3-(trifluoromethyl)-4-(4-aminophenoxy)aniline (TFDPE) (melting point: 109°C), 2,2'-bis(trifluoromethyl)benzidine (TFMB) (melting point: 183°C), 2,2-bis(4-aminophenyl)hexafluoropropane (Bis-A-AF) (melting point: 195°C), and 5-trifluoromethyl-1,3-diaminobenzene (DATF) (melting point: 89°C). In order to adjust the fluidity of the polyimide or polyimide precursor, these diamines having a melting point of less than 110° C. or more than 180° C. as diamine compounds may be used in combination as appropriate.
[0029] The ratio of DA2 residues provided by a diamine compound having a melting point of 110° C. or more and 180° C. or less to DA2 residues provided by a diamine compound having a melting point less than 110° C. or more or more than 180° C. is preferably such that, when the total amount of DA2 residues is 100 mol %, the DA2 residues provided by a diamine compound having a melting point of 110° C. or more and 180° C. or less are 80 mol % or more.
[0030] In addition, the component (A) may contain diamine residues other than the DA1 residue and the DA2 residue, so long as the gist of the present invention is not impaired. Examples of diamine compounds that provide such diamine residues include bis(3-amino-4-hydroxyphenyl)sulfone, bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methylene, bis(3-amino-4-hydroxyphenyl)ether, bis(3-amino-4-hydroxy)biphenyl, bis(3-amino-4-hydroxyphenyl)fluorene, 4,4'-diaminodiphenyl ether sulfonate, dimercaptophenylenediamine, and the like. benzene, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl methane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminophenoxy)benzene, benzine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine Talylenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene residue, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, Examples of the aryloxy group include 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether, 3,3'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether, and 2,2',5,5'-tetrakis(trifluoromethyl)-4,4'-diaminodiphenyl ether.
[0031] In order to improve the storage stability of the resin composition of the present invention, the main chain of component (A) may be terminated with a known terminal-capping agent such as a monoamine, an acid anhydride, a monocarboxylic acid, a monoacid chloride compound, a monoactive ester compound, etc. For the purpose of improving the folding resistance and chemical resistance of the cured resin film obtained by heat curing, it is particularly preferable to use a monoamine or an acid anhydride having at least one reactive unsaturated bond such as an alkenyl group or an alkynyl group as the terminal-capping agent.
[0032] The monoamine having at least one reactive unsaturated bond such as an alkenyl group or an alkynyl group is not particularly limited, and examples thereof include 4-ethynylaniline and 4-vinylaniline.
[0033] The acid anhydride having at least one reactive unsaturated bond such as an alkenyl group or an alkynyl group is not particularly limited, and examples thereof include 5-norbornene-2,3-dicarboxylic anhydride, maleic anhydride, and methacrylic anhydride.
[0034] The reactive unsaturated bond refers to a chemically active unsaturated bond that serves as a reaction point with other compounds, such as a reaction point with other reactive unsaturated bonds or with the thermal crosslinking agent (C) component described below.
[0035] In the component (A), the molar ratio of imide ring-closed structural units to all imide structural units and imide precursor structural units is called the imide ring-closure rate (R IM (%)), in the present invention, R IM The entire range of 0% to 100% can be used, but from the viewpoint of controlling alkali solubility, R IM is preferably 3% or more, more preferably 5% or more, and even more preferably 7% or more, and from the viewpoint of sensitivity, is preferably 50% or less, more preferably 40% or less, even more preferably 30% or less, and particularly preferably 20% or less. IM Polyimide precursors are those with 0% or more and less than 80% R IMIn this case, the term "polyimide" refers to a material having a molecular weight of 80% or more and 100% or less.
[0036] The imide ring closure rate (R IM (%)) can be obtained, for example, by the following method. First, the infrared absorption spectrum of the polymer is measured, and the absorption peak (1,780 cm) of the imide structure due to the polyimide is detected. -1 Near 1,377 cm -1 The presence of an absorption peak (around 1,470 cm) due to aromatic rings was confirmed. -1 When the peak intensity at 1,377 cm -1 The peak intensity (Y) around the aromatic ring is then measured. The polymer is then heat-treated at 350°C for 1 hour, and the infrared absorption spectrum is measured. -1 When the peak intensity at 1,377 cm -1 The peak intensity (Z) around the annealed polymer is calculated. The ratio of these peak intensities corresponds to the imide group content in the polymer before heat treatment, i.e., the imide ring closure rate (R IM = Y / Z × 100(%)).
[0037] In the (A) component, other structural units than the imide structural unit and the imide precursor structural unit may be included as long as the gist of the present invention is not impaired. Examples of such structural units include benzoxazole and benzoxazole precursor, amide, amideimide, and other structural units, and from the viewpoints of heat resistance and low water absorption, benzoxazole structural unit and benzoxazole precursor structural unit are preferred. The structural unit referred to here is also called a repeating unit.
[0038] The weight average molecular weight of component (A) can be determined in terms of polystyrene by gel permeation chromatography (GPC), and from the viewpoint of folding resistance of the cured film, it is preferably more than 20,000, more preferably more than 22,000, even more preferably more than 23,000, and particularly preferably more than 25,000. On the other hand, from the viewpoint of alkali solubility, the weight average molecular weight of component (A) is preferably 40,000 or less, more preferably 38,000 or less, even more preferably 35,000 or less, and particularly preferably 30,000 or less.
[0039] It is more preferable that component (A) is obtained by precipitating the polymer in a poor solvent such as methanol or water after the polymerization reaction is completed, followed by washing and drying. This makes it possible to remove low molecular weight components of the polymer, and thus greatly improves the folding resistance of the resin composition after heat curing.
[0040] The integrated molecular weight distribution curve of the component (A) can be analyzed using GPC analysis software. From the integrated molecular weight distribution curve, the content of molecular weights of 1,000 or less determined is preferably 1.0% or less, more preferably 0.9% or less, even more preferably 0.8% or less, and particularly preferably 0.7% or less from the viewpoint of folding resistance of the cured film, and is preferably 0.1% or more from the viewpoint of storage stability of the resin composition.
[0041] <Photoacid generator (Component B)> The resin composition of the present invention contains a photoacid generator.
[0042] By including a photoacid generator, acid is generated in the light-irradiated area, increasing the solubility of the light-irradiated area in an alkaline aqueous solution, and a positive relief pattern in which the light-irradiated area dissolves can be obtained. The positive photosensitive resin composition can easily obtain a forward tapered pattern by obtaining a fine pattern through an exposure / development process and then curing the composition by heating. This forward tapered pattern has excellent coverage of the upper electrode when used as an insulating film for an organic EL display device, and can prevent disconnection and increase the reliability of the device.
[0043] Furthermore, by containing a photoacid generator and an epoxy compound or a thermal crosslinking agent described below, the acid generated in the light-irradiated areas promotes the crosslinking reaction of the epoxy compound or the thermal crosslinking agent, thereby obtaining a negative relief pattern in which the light-irradiated areas are insolubilized.
[0044] As the photoacid generator, a quinone diazide compound or an onium salt compound is preferably used.
[0045] As the quinone diazide compound, a compound having a phenolic hydroxyl group and a sulfonic acid of naphthoquinone diazide sulfonic acid bonded by an ester is preferable. The compound having a phenolic hydroxyl group used here includes Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, methyl Lentris-FR-CR, BisRS-26X, DML-MBPC, DML-MBOC, DML-OCHP, DML-PCHP, DML-PC, DML-PTBP, DML-34X, DML-EP ,DML-POP, Dimethylol-BisOC-P, DML-PFP, DML-PSBP, DML-MTrisPC, TriML-P, TriML-35XL, TML-BP, TML-HQ, TML -pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TPHAP (all trade names, Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (all trade names, Asahi Organic Chemicals Co., Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, tetrahydroxybenzophenone, gallic acid methyl ester, bisphenol A, bisphenol E, methylene bisphenol, BisP-AP (all trade names, Honshu Chemical Industry Co., Ltd.). Suitable examples of the quinone diazide compound used in the present invention include compounds having these phenolic hydroxyl groups to which 4-naphthoquinone diazide sulfonic acid or 5-naphthoquinone diazide sulfonic acid has been introduced via an ester bond, but other compounds can also be used.
[0046] 4-naphthoquinone diazide sulfonyl ester compounds have absorption in the i-line region of a mercury lamp, making them suitable for i-line exposure. 5-naphthoquinone diazide sulfonyl ester compounds have absorption extending to the g-line region of a mercury lamp, making them suitable for g-line exposure. In the present invention, both 4-naphthoquinone diazide sulfonyl ester compounds and 5-naphthoquinone diazide sulfonyl ester compounds can be preferably used, but it is preferable to select 4-naphthoquinone diazide sulfonyl ester compounds or 5-naphthoquinone diazide sulfonyl ester compounds depending on the wavelength of exposure. In addition, naphthoquinone diazide sulfonyl ester compounds can be obtained in which 4-naphthoquinone diazide sulfonyl groups and 5-naphthoquinone diazide sulfonyl groups are used in combination in the same molecule, and 4-naphthoquinone diazide sulfonyl ester compounds and 5-naphthoquinone diazide sulfonyl ester compounds can also be used in combination.
[0047] The naphthoquinone diazide sulfonyl ester compound can be synthesized by an esterification reaction between a compound having a phenolic hydroxyl group and a naphthoquinone diazide sulfonic acid compound, and can be synthesized by a known method.
[0048] Examples of the onium salt compound include sulfonium salts, phosphonium salts, diazonium salts, and iodonium salts. Among them, sulfonium salts are preferred. These can be used alone or in combination. Furthermore, a sensitizer and the like can be included as necessary.
[0049] In the present invention, the content of the (B) component in the resin composition is preferably 0.01 to 50 parts by mass relative to 100 parts by mass of the (A) component. The content of the quinone diazide compound is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more relative to 100 parts by mass of the (A) component from the viewpoint of pattern formation, and is preferably 45 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less from the viewpoint of maintaining heat resistance. The content of the onium salt compound is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more relative to 100 parts by mass of the (A) component from the viewpoint of pattern formation, and is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less from the viewpoint of maintaining heat resistance.
[0050] <Thermal crosslinking agent (component C)> The resin composition of the present invention may contain a thermal crosslinking agent. The thermal crosslinking agent is a compound that reacts with other molecules by heat to form chemical bonds, and can improve the folding resistance of the cured resin composition.
[0051] As the thermal crosslinking agent, it is preferable to use one or more types of thermal crosslinking agents selected from the group consisting of an isocyanuric ring structure-containing epoxy thermal crosslinking agent, an alicyclic epoxy thermal crosslinking agent, and an aliphatic epoxy thermal crosslinking agent. These epoxy thermal crosslinking agents have a structure that does not have an aromatic ring in the molecule, which increases the solubility in an alkaline developer and allows pattern processing with high sensitivity. In addition, since the crosslinking part has a flexible structure, the flowability of the resin composition during thermal curing is increased, resulting in better planarization, and furthermore, decomposition due to heat or light irradiation including ultraviolet rays can be suppressed, so that it is also preferable in terms of expressing high bending resistance. The isocyanuric ring structure-containing epoxy thermal crosslinking agent is an epoxy thermal crosslinking agent that contains an isocyanuric ring structure in the compound structure. The alicyclic epoxy thermal crosslinking agent is an epoxy thermal crosslinking agent that has one or more alicyclic structures having 3 to 12 carbon atoms that may have a hetero element or a branched structure in a compound structure other than an ethylene oxide structure. The aliphatic epoxy thermal crosslinking agent is an epoxy thermal crosslinking agent that has a structure having 3 to 24 carbon atoms that is not an alicyclic structure that may have a hetero element or a branched structure in a compound structure other than an ethylene oxide structure. In addition, in the present application, an epoxy thermal crosslinking agent having an isocyanuric ring, an alicyclic structure, and further an aliphatic structure is classified as an isocyanuric ring structure-containing epoxy thermal crosslinking agent, and in the present application, an epoxy thermal crosslinking agent having an alicyclic structure and further an aliphatic structure is classified as an alicyclic epoxy thermal crosslinking agent.
[0052] From the viewpoint of enhancing the crosslinking ability of the resin, it is preferable that the isocyanuric ring structure-containing epoxy thermal crosslinking agent, the alicyclic epoxy thermal crosslinking agent, and the aliphatic epoxy thermal crosslinking agent have two or more epoxy groups in the molecule.
[0053] Examples of the isocyanuric ring structure-containing epoxy thermal crosslinking agent include "TEPIC" (registered trademark)-S, TEPIC-G, TEPIC-L, TEPIC-VL (all trade names, manufactured by Nissan Chemical Industries, Ltd.), MA-DGIC (trade name, manufactured by Shikoku Kasei Co., Ltd.), and the like. Examples of alicyclic epoxy thermal crosslinking agents include "CELLOXIDE" (registered trademark) 2021P, "CELLOXIDE" 2081, "CELLOXIDE" 8000, "CELLOXIDE" 8010 (trade names, manufactured by Daicel Corporation), "Denacol" (registered trademark) EX-252 (trade name, manufactured by Nagase ChemteX Corporation), "EPOCALIC" (registered trademark) THI-DE, "EPOCALIC" DE-102, "EPOCALIC" DE-103 (trade names, manufactured by ENEOS Corporation), and "SHOFREE" (registered trademark) CDMDG (trade name, manufactured by Showa Denko K.K.). Examples of aliphatic epoxy thermal crosslinking agents include "Denacol". Examples of such crosslinking agents include "DENACOL" (registered trademark) EX-614B, "DENACOL" EX-313, "DENACOL" EX-512, "DENACOL" EX-321L, "DENACOL" EX-810, "DENACOL" EX-861, and "DENACOL" EX-211 (all trade names, manufactured by Nagase ChemteX Corporation), EPOGOSE" (registered trademark) BD, "EPOGOSE" NPG, and "EPOGOSE" HD (trade names, manufactured by Yokkaichi Synthetic Co., Ltd.), and "SHOFREE" (registered trademark) PETG (trade name, manufactured by Showa Denko K.K.), each of which is available from the respective companies. Two or more types of thermal crosslinking agents may be used in combination.
[0054] The content of the (C) component in the resin composition is preferably 1 part by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, based on 100 parts by mass of the (A) component, from the viewpoint of the folding resistance of the cured film, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 35 parts by mass or less, from the viewpoint of maintaining heat resistance.
[0055] The resin composition of the present invention may contain a solvent. Preferred examples of the solvent include polar aprotic solvents such as N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethylsulfoxide, ethers such as tetrahydrofuran, 1,4-dioxane, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, ketones such as acetone, methyl ethyl ketone, and diisobutyl ketone, esters such as ethyl acetate, butyl acetate, isobutyl acetate, propyl acetate, propylene glycol monomethyl ether acetate, and 3-methyl-3-methoxybutyl acetate, alcohols such as ethyl lactate, methyl lactate, diacetone alcohol, and 3-methyl-3-methoxybutanol, and aromatic hydrocarbons such as toluene and xylene. Two or more of these may be contained.
[0056] When the resin composition of the present invention contains a solvent, the content of the solvent is preferably 70 parts by mass or more, more preferably 100 parts by mass or more, per 100 parts by mass of component (A), from the viewpoint of resin solubility, and is preferably 2,500 parts by mass or less, more preferably 2,000 parts by mass or less, from the viewpoint of obtaining an appropriate film thickness.
[0057] The resin composition of the present invention may contain, as necessary, other components, such as an adhesion improver, a surfactant, a compound having a phenolic hydroxyl group, inorganic particles, and a thermal acid generator, in addition to the components (A), (B), and (C) and a solvent.
[0058] Next, the method for producing the resin composition of the present invention will be described. For example, the resin composition can be obtained by dissolving or dispersing the above-mentioned (A) component and (B) component, and optionally the (C) component, an adhesion improver, a surfactant, a compound having a phenolic hydroxyl group, inorganic particles, a thermal acid generator, etc., in an organic solvent.
[0059] Methods for dissolving or dispersing in a solvent include stirring and heating. When heating, the heating temperature is preferably set within a range that does not impair the performance of the resin composition, and is usually room temperature to 80° C. The order of dissolving each component is not particularly limited, and examples include a method of dissolving the components in order starting from the least soluble compound.
[0060] The obtained resin composition is preferably filtered using a filter to remove dust and particles. The filter pore size is, for example, 0.5 μm, 0.2 μm, 0.1 μm, 0.07 μm, 0.05 μm, 0.02 μm, etc., but is not limited thereto. The material of the filter includes polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., and polyethylene and nylon are preferred.
[0061] Next, a method for producing a cured product from the resin composition of the present invention will be described. More specifically, the resin composition is applied onto a substrate to form a resin film, the resin film is dried, and the resin film is heat-treated to produce a cured product. At this time, the portion having the structure of an imide precursor in component (A) can be ring-closed into an imide ring. Furthermore, when the polyimide precursor or polyimide resin of component (A) has a reactive unsaturated bond at the end, they can be crosslinked with each other to extend the molecular chain. Furthermore, when component (C) is contained, components (C) can be thermally crosslinked with each other or between component (C) and component (A).
[0062] First, a resin composition is applied onto a substrate to form a resin film. Examples of application methods include spin coating, slit coating, dip coating, spray coating, and printing. Among these, the slit coating method is preferred because it can be applied with a small amount of coating liquid and is advantageous in reducing costs. The amount of coating liquid required for the slit coating method is about 1 / 5 to 1 / 10 compared to the spin coating method. As the slit coater used for application, for example, "Linear Coater" (registered trademark) manufactured by SCREEN Finetech Solutions Co., Ltd., "Spinless" (registered trademark) manufactured by Tokyo Ohka Kogyo Co., Ltd., "TS Coater" manufactured by Toray Engineering Co., Ltd., "Table Coater" (registered trademark) manufactured by Chugai Ro Kogyo Co., Ltd., "CS Series" and "CL Series" manufactured by Tokyo Electron Limited, "In-line Slit Coater" manufactured by Cermatronics Trading Co., Ltd., and "Head Coater HC Series" manufactured by Hirata Machinery & Engineering Co., Ltd. can be selected. When using a slit coater, the coating speed is preferably in the range of 10 mm / sec to 400 mm / sec. The coating thickness varies depending on the solid content and viscosity of the resin composition, but is usually applied so that the coating thickness after drying is 0.1 to 10 μm, preferably 0.3 to 5 μm.
[0063] The substrate may be, but is not limited to, glass, silicon, ceramics, gallium arsenide, or the like wafer, or a substrate having metal formed thereon as an electrode or wiring.
[0064] Next, particularly when a solvent is used, the resin film provided on the substrate is dried, that is, the volatile matter that volatilizes at a temperature up to the drying temperature is removed. The drying method can be a known method such as a method using a hot plate, an oven, or infrared rays. In addition, the substrate on which the coating film is formed may be dried under reduced pressure. The heating temperature and heating time vary depending on the type and purpose of the coating film, but the heating temperature is preferably 50°C to 180°C, and the heating time is preferably 1 minute to several hours.
[0065] A cured film can be obtained by heat-curing the resin film. Heat-curing can remove components with low heat resistance, so that heat resistance and chemical resistance can be further improved. The heat-curing temperature is preferably 150°C or higher, more preferably 200°C or higher, and even more preferably 230°C or higher from the viewpoint of improving the heat resistance of the cured film, and is preferably 400°C or lower, more preferably 350°C or lower, even more preferably 300°C or lower, and particularly preferably 280°C or lower from the viewpoint of improving the film toughness of the cured film. In this temperature range, the temperature may be raised stepwise or continuously. The heat-curing time is preferably 30 minutes or more from the viewpoint of improving the heat resistance of the cured film. In addition, it is preferably 3 hours or less from the viewpoint of improving the film toughness of the cured film. For example, a method of heat-treating at 150°C and 260°C for 60 minutes each, or a method of heat-treating while linearly increasing the temperature from room temperature to 270°C over 2 hours can be mentioned.
[0066] Next, a method for producing a patterned cured product from the resin composition of the present invention will be described. More specifically, the resin composition is applied onto a substrate to form a resin film, the resin film is dried, the resin film is exposed to light, the exposed resin film is developed, and the developed resin film is heat-treated to produce a cured product. The coating process, drying process, and heat treatment process are as described above, and the exposure process and development process of the resin film will be described below.
[0067] As described above, the resin composition is applied onto a substrate to form a resin film, the resin film is dried, and then the resin film is exposed to light. The desired pattern can be formed by irradiating the film with actinic radiation through a mask having the desired pattern and developing the film.
[0068] Examples of actinic rays used for exposure include ultraviolet rays, visible rays, electron beams, and X-rays. In the present invention, it is preferable to use i-rays (365 nm), h-rays (405 nm), and g-rays (436 nm) from a mercury lamp. When the film has positive photosensitivity, the exposed area dissolves in the developer. When the film has negative photosensitivity, the exposed area hardens and becomes insoluble in the developer.
[0069] Next, the exposed resin film is developed. In the case of a positive type, the exposed portion is removed with a developer to form a desired pattern. The developer is preferably an aqueous solution of an alkaline compound such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, or hexamethylenediamine. To these alkaline aqueous solutions, one or more of polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, γ-butyrolactone, or dimethylacrylamide, alcohols such as methanol, ethanol, or isopropanol, esters such as ethyl lactate or propylene glycol monomethyl ether acetate, or ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, or methyl isobutyl ketone may be added. The developing method may be spray, paddle, immersion, ultrasonic, or the like.
[0070] Next, the pattern formed by development is preferably rinsed with pure water. Alcohols such as ethanol and isopropyl alcohol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. may be added to the pure water for rinsing. Then, the above-mentioned heat treatment is performed to produce a patterned cured product.
[0071] The resin composition of the present invention is suitably used for bank layers in organic EL display devices, planarizing layers in TFT substrates for driving organic EL display devices, wiring protection and insulating layers in circuit boards, surface protection layers and interlayer insulating layers in semiconductor elements, on-chip microlenses in solid-state imaging devices, and planarizing layers for various displays and solid-state imaging devices.
[0072] The organic EL display device of the present invention comprises a cured product obtained by curing the resin composition of the present invention. The structure of the organic EL display device has at least a planarization layer, a first electrode, a bank layer, a light-emitting layer, and a second electrode on a substrate, and it is preferable that either or both of the planarization layer and the bank layer are made of the cured product of the present invention. The organic EL light-emitting material is easily deteriorated by moisture, and may have adverse effects such as a decrease in the area ratio of the light-emitting portion to the area of the light-emitting pixel. However, the cured product obtained by curing the resin composition of the present invention has low water absorption, so stable driving and light-emitting characteristics can be obtained. Furthermore, if there is a step in the pixel, color unevenness, color mixing, etc. may occur, and the display quality may decrease, but by providing a planarization layer, the step under the light-emitting layer can be highly planarized, and the display quality can be improved. EXAMPLES
[0073] The present invention will be described below with reference to examples, but the present invention should not be construed as being limited to these examples. First, the evaluation method will be described.
[0074] [Evaluation method] (1) Film thickness The thickness of the resin coating on the supporting substrate was measured using an optical interference type film thickness measuring device (Lambda Ace VM-1030, manufactured by SCREEN Holdings Co., Ltd.) The refractive index was measured at 1.629.
[0075] (2) Sensitivity The resin composition was applied onto an 8-inch silicon wafer by spin coating using a coating and developing apparatus (ACT-8 manufactured by Tokyo Electron Limited) and baked at 120°C for 2 minutes to produce a pre-baked film with a thickness of 3.0 μm. Thereafter, using an exposure device i-line stepper (NSR-2005i9C manufactured by Nikon Corporation), the wafer was exposed to light at a dose of 50 to 300 mJ / cm through a mask having a pattern of 5 μm contact holes. 2 in the range of 10 mJ / cm 2Thereafter, using the ACT-8, the film was treated with a 2.38% by mass aqueous solution of tetramethylammonium hydroxide (hereinafter, TMAH) as a developer until the film thickness of the unexposed area became 2.5 μm, and then rinsed with pure water and spun off to dry, to obtain a pattern.
[0076] The obtained pattern was observed at a magnification of 50 times using a microscope MX61 (Olympus Corporation) to measure the opening diameter of the contact hole. The minimum exposure dose at which the opening diameter of the contact hole reached 5 μm was determined. The smaller the minimum exposure dose, the higher the sensitivity.
[0077] (3) Change in aperture diameter before and after heat treatment The substrate with the resin film after development obtained in (2) was heated in a clean oven (KOYO THERMO SYSTEMS CO., LTD. CLH-21CD-S) at 250°C for 60 minutes under a nitrogen gas flow. The aperture diameter at the minimum exposure dose obtained in (2) was determined as (CD DEV ), and the opening diameter at the same location after heat treatment (CD CURE ), then (CD DEV -CD CURE ) was observed and measured at a magnification of 50 times using the microscope MX61.
[0078] (4) Water absorption rate The resin composition was applied to an 8-inch silicon wafer by spin coating using the ACT-8, and baked at 120°C for 2 minutes to prepare a pre-baked film with a thickness of 6.5 μm. Then, using the ACT-8, a 2.38% by mass TMAH aqueous solution was used to treat the film until the film thickness became 6.0 μm, and then the film was rinsed with pure water, water droplets on the film were shaken off, and the film was dried. The substrate with the resin film after the treatment was heated at 250°C for 60 minutes under a nitrogen stream using a clean oven CLH-21CD-S to form a cured film. The substrate with the cured film was immersed in 45% by mass hydrofluoric acid for 5 minutes to peel off the cured film from the substrate. The obtained film was thoroughly washed with pure water, and the cured film was dried in a ventilated oven at 80°C for 5 hours, and the dry weight of the cured film was measured with a precision balance immediately after removing it from the oven. The cured film was then immersed in pure water at 23°C for 24 hours, and immediately wiped off after removal from the water. After 5 minutes, the water absorption weight of the cured film was measured using a precision balance. The water absorption rate (wt%) of the cured film was calculated from the dry weight of the cured film and the water absorption weight.
[0079] (5) Flatness FIG. 1 shows a cross-sectional view of a flatness evaluation sample. The resin composition was applied by spin coating onto a stepped substrate of a silicon wafer having a diameter of 8 inches, in which five copper line patterns, each having a thickness of 1.0 μm and a width of 5 μm, were patterned in parallel at intervals of 5 μm in the center of the substrate, using the ACT-8. A pre-baked film was prepared so that the film thickness of the flat portion where the line patterns were not present was 2.8 μm after baking at 120° C. for 2 minutes. Thereafter, the film was treated using a 2.38 mass % TMAH aqueous solution using the ACT-8 until the film thickness of the portion not affected by the steps was 2.3 μm, and then rinsed with pure water, water droplets on the film were shaken off, and the film was dried to obtain a resin film. The resin film-attached substrate after the treatment was heated at 250° C. for 60 minutes under a nitrogen stream using a clean oven CLH-21CD-S to prepare a cured film. The surface step heights on the three line patterns, excluding the two outermost lines, of the obtained cured film were measured using a surface profiler (P·15; KLA-Tencor Corporation), and the average value of the step heights (heights of the cured film represented by h1 to h3 in Fig. 1) was taken as the surface step height (μm). The baseline of each step height was defined as a line connecting the points where the film thickness of the concave portions on the left and right sides of each mountain-like resin film portion where h1 to h3 are measured is the smallest, as seen from Fig. 1. A specific example is described below. In Fig. 1, the straight line connecting the bottoms a1 and a2 of the step height shape was taken as the baseline, and the length h1 was defined as the intersection point between the line drawn perpendicularly from the top b1 of the step height shape to the substrate surface and the baseline. h2 is defined as the length from the top b2 of the step shape to the intersection of a line drawn perpendicular to the substrate surface and the baseline, with the line connecting a2 and a3 as the baseline, and h3 is defined as the length from the top b3 of the step shape to the intersection of a line drawn perpendicular to the substrate surface and the baseline, with the line connecting a3 and a4 as the baseline.
[0080] (6) Folding resistance First, a 25 μm thick “Kapton” (registered trademark) film cut to 10 cm x 10 cm was fixed with Kapton tape so as to cover one side of a 10 cm x 10 cm x 0.5 mm thick glass substrate. A resin composition was applied to the Kapton film of the glass substrate with the Kapton film by spin coating using a spin coater (MS-A100 manufactured by Mikasa Co., Ltd.), and baked at 120°C for 2 minutes to prepare a pre-baked film with a thickness of 5 μm. Then, a 2.38 mass% TMAH aqueous solution was used for treatment until the film thickness reached 4.5 μm, and the substrate was rinsed with pure water. The treated substrate was heated at 250°C for 60 minutes under a nitrogen stream using a clean oven CLH-21CD-S. After the heat treatment, the "Kapton" (registered trademark) film with the cured film was removed from the glass substrate, and the "Kapton" (registered trademark) film with the cured film was cut into pieces of 1 cm wide and 5 cm long to prepare test pieces. As the folding resistance evaluation jig, one piece (lower jig) was prepared, which was a stainless steel plate measuring 10 cm long x 10 cm wide x 1 cm thick, with a rectangular recess (hereinafter simply referred to as a groove) measuring 5 cm long x 10 cm wide in the center of one side, and with depths of 0.1 mm, 0.2 mm, 0.3 mm, and 0.4 mm, respectively (lower jig), and a stainless steel plate (upper jig) measuring 10 cm long x 10 cm wide x 1 cm thick without a groove was also prepared. The test piece was bent slightly with the Kapton film surface facing inward and the cured film surface facing outward, with the short sides of the test piece overlapping each other, and the overlapping short sides were fixed at a point about 1 cm away from the center of the groove of the lower jig toward the wall of the groove so that the short sides of the overlapping test piece were parallel to the wall of the groove. Next, the upper jig was placed on the lower jig so that the loop of the sample appearing on the lower jig was placed in the groove, and the test piece was left to stand for 1 minute. After leaving the test piece to stand, the test piece taken out of the jig was observed with a microscope MX61 to observe the presence or absence of cracks at the bending position (i.e., near the midpoint of the test piece in the longitudinal direction). This measurement was performed using each lower jig prepared, and the minimum groove depth at which no cracks were generated was recorded.
[0081] [Synthesis example] Synthesis Example 1: Synthesis of diamine compound (HA) 164.8g (0.45mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane was dissolved in 900mL of acetone and 156.8g (2.7mol) of propylene oxide, and cooled to -15℃. A solution of 183.7g (0.99mol) of 3-nitrobenzoyl chloride dissolved in 900mL of acetone was added dropwise to the solution. After the addition, the mixture was reacted at -15℃ for 4 hours, and then the mixture was returned to room temperature. The precipitated white solid was filtered and dried in vacuum at 50℃.
[0082] 270g of the solid was placed in a 3L stainless steel autoclave and dispersed in 2400mL of methyl cellosolve, and 5g of 5% palladium-carbon was added. Hydrogen was introduced into the mixture using a balloon, and the reduction reaction was carried out at room temperature. After 2 hours, the reaction was terminated when it was confirmed that the balloon was no longer deflating. After the reaction was completed, the mixture was filtered to remove the palladium compound catalyst, and the mixture was concentrated using a rotary evaporator to obtain a diamine compound represented by the following formula (hereinafter referred to as HA).
[0083] [ka]
[0084] Synthesis Example 2 Synthesis of polyamic acid ester resin (A-1) Under a dry nitrogen stream, 42.3 g (0.07 mol) of the diamine compound HA obtained in Synthesis Example 1 and 10.1 g (0.03 mol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (hereinafter, 6FODA) were dissolved in 300 g of N-methylpyrrolidone (hereinafter, NMP). 21.7 g (0.07 mol) of bis(3,4-dicarboxyphenyl)ether dianhydride (hereinafter, ODPA) was added together with 20 g of NMP, and the mixture was reacted at 20°C for 1 hour, and then at 50°C for 2 hours. Next, 9.8 g (0.06 mol) of 5-norbornene-2,3-dicarboxylic anhydride (hereinafter, NA) was added together with 10 g of NMP as a terminal blocking agent, and the mixture was reacted at 50°C for 2 hours. Then, 19.1 g (0.16 mol) of N,N-dimethylformamide dimethyl acetal was added, and the mixture was stirred at 50°C for 3 hours. After stirring, the solution was cooled to room temperature and then poured into 5 L of water to obtain a precipitate. This precipitate was collected by filtration, and 5 L of water was added and filtered to collect the precipitate. This washing procedure was repeated three times, and the precipitate was then dried in a vacuum dryer at 80°C for 24 hours to obtain a powder of polyamic acid ester resin (A-1).
[0085] Synthesis Example 3: Synthesis of polyimide resin (A-20) Under a dry nitrogen stream, 42.3g (0.07 mol) of the diamine compound HA obtained in Synthesis Example 1, 10.1g (0.03 mol) of 6FODA, and 9.8g (0.06 mol) of NA as a terminal blocking agent were dissolved in 300g of NMP. 21.7g (0.07 mol) of ODPA was added together with 100g of NMP, and the mixture was stirred at 20°C for 1 hour, and then stirred at 50°C for 4 hours. Then, 15g of xylene was added, and the mixture was stirred at 150°C for 5 hours while azeotroping water with xylene. After the stirring was completed, the solution was cooled to room temperature, and then the solution was poured into 5L of water to obtain a precipitate. The precipitate was collected by filtration, and 5L of water was added, and the precipitate was collected by filtration. This was washed three times, and then dried in a vacuum dryer at 80°C for 24 hours to obtain a powder of polyamide resin (A-20).
[0086] Synthesis Examples 4 to 21 Synthesis of polyamic acid ester resins (A-2 to A-19) Powders of polyamic acid ester resins (A-2 to A-19) were obtained in the same manner as in Synthesis Example 2, except that the acid dianhydrides, diamines, and end-capping agents used were replaced as shown in Table 1.
[0087] Synthesis Examples 22 to 23 Synthesis of polyimide resins (A-21, A-22) Powders of polyimide resins (A-21, A-22) were obtained in the same manner as in Synthesis Example 3, except that the acid dianhydride, diamine, and end-capping agent used were replaced as shown in Table 1.
[0088] [Table 1]
[0089] ODPA: Bis(3,4-dicarboxyphenyl)ether dianhydride BSAA: 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride 6FDA: 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride 6FAP: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane 6FODA: 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether (melting point: 126°C) HFBAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (melting point: 160°C) Bis-A-EF: 1,1,1-trifluoro-2,2-bis(4-aminophenyl)ethane (melting point: 138°C) Bis-AT-AF: 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane (melting point: 105°C) TFMB: 2,2'-bis(trifluoromethyl)benzidine (melting point: 183°C) BAP: 2,2-bis(3-amino-4-hydroxyphenyl)propane 4,4'-DDS: 4,4'-diaminodiphenyl sulfone NA: 5-norbornene-2,3-dicarboxylic anhydride MA: Maleic anhydride PA: Phthalic anhydride EA: 4-ethynylaniline MAP: 3-aminophenol Synthesis Example 24: Synthesis of quinone diazide compound (B-1) Under a dry nitrogen stream, 42.4g (0.1 mol) of 4,4'-[1-[4-[1-(4-hydroxyphenyl)-1-methylethyl]phenyl]ethylidene]bisphenol and 53.6g (0.20 mol) of 5-naphthoquinone diazide sulfonic acid chloride were dissolved in 450g of 1,4-dioxane and brought to room temperature. 25.0g of triethylamine mixed with 100g of 1,4-dioxane was added dropwise so that the temperature in the system did not exceed 35°C. After the dropwise addition, the mixture was stirred at 40°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The precipitate was then collected by filtration and washed with 1L of 1% hydrochloric acid. Then, it was washed twice with 2L of water. The precipitate was dried in a vacuum dryer to obtain a quinone diazide compound (B-1), which is a photoacid generator represented by the following formula.
[0090] [ka]
[0091] [Other ingredients] Thermal crosslinker: "Showfree" (registered trademark) PETG (C-1) (Aliphatic epoxy thermal crosslinking agent, compound shown in the chemical formula below, manufactured by Showa Denko K.K.)
[0092] [ka]
[0093] "TEPIC" (registered trademark)-VL (C-2) (Isocyanuric ring structure-containing epoxy thermal crosslinking agent, compound shown in the chemical formula below, manufactured by Nissan Chemical Industries, Ltd.)
[0094] [ka]
[0095] "Techmore" (registered trademark) VG3101L (C-3) (Thermal crosslinking agent having an aromatic ring and an epoxy group, a compound shown in the chemical formula below, manufactured by Printec Co., Ltd.)
[0096] [ka]
[0097] "Nikalac" (registered trademark) MX-270 (C-4) (Compound shown in the chemical formula below, manufactured by Nippon Carbide Industries Co., Ltd.)
[0098] [ka]
[0099] [Preparation of resin composition] Each component was placed in a 100 mL vial according to the composition in Table 2, and mixed using a stirring and degassing device (ARE-310 manufactured by Thinky Corporation) under conditions of 10 minutes of stirring and 1 minute of degassing. After dissolving, the mixture was filtered through a 0.2 μm polytetrafluoroethylene filter (manufactured by Sumitomo Electric Industries, Ltd.) to prepare resin compositions (V-1 to 26). In Table 2, "PGME" stands for propylene glycol monomethyl ether, and "EL" stands for ethyl lactate.
[0100] [Table 2]
[0101] [Examples 1 to 17, Comparative Examples 1 to 9] The resin compositions thus prepared were used to evaluate the water absorption and sensitivity according to the above-mentioned methods. The results are shown in Table 3.
[0102] [Table 3]
[0103] The ones shown in Examples 1 to 17 have a sensitivity of 140 mJ / cm 2 The change in opening diameter was less than 0.1 mm, the water absorption rate was less than 1.2%, the flatness was less than 0.22 μm, and the folding resistance was less than 0.3 mm, and all of the characteristics showed good results.
[0104] On the other hand, the comparative examples 1 to 9 were inferior in at least one of these properties. [Industrial Applicability]
[0105] The resin composition of the present invention is suitably used for bank layers in organic EL display devices, planarizing layers in TFT substrates for driving organic EL display devices, wiring protection and insulating layers in circuit boards, surface protection layers and interlayer insulating layers in semiconductor elements, on-chip microlenses in solid-state imaging devices, and planarizing layers for various displays and solid-state imaging devices.
[0106] The cured product of the present invention exhibits low water absorption, high flatness, and high folding endurance, and is therefore suitable for use as a bank layer in an organic EL display device, a planarizing layer in a TFT substrate for driving an organic EL display device, a wiring protection insulating layer in a circuit board, a surface protection layer or an interlayer insulating layer in a semiconductor element, an on-chip microlens in a solid-state imaging element, and a planarizing layer for various displays and solid-state imaging elements. [Explanation of symbols]
[0107] 1. Stepped board 2 Cured film 3. Baseline
Claims
1. A resin composition comprising one or more resins selected from the group consisting of polyimides, polyimide precursors, and copolymers thereof (hereinafter, referred to as component (A)), and a photoacid generator, The component (A) has one or more acid dianhydride residues and two or more diamine residues, two of the two or more diamine residues are a diamine residue having a trifluoromethyl group and a phenolic hydroxyl group (hereinafter, DA1 residue), and a diamine residue having a trifluoromethyl group and no phenolic hydroxyl group (hereinafter, DA2 residue), At least one diamine residue among the DA2 residues has a melting point as a diamine compound of 110° C. or higher and 180° C. or lower; A resin composition in which the ratio of DA2 residues is 15 mol % or more and 40 mol % or less when the total amount of diamine residues in the component (A) is 100 mol %.
2. The resin composition according to claim 1 , wherein all or a part of the one or more types of acid dianhydride residues are acid dianhydride residues having a diphenyl ether structure.
3. The resin composition according to claim 1 or 2, wherein the DA1 residue is a diamine residue represented by formula (1). 【Chemistry 1】 (In formula (1), R 1 is -C(CF 3 ) 2 - or -CH(CF 3 )-. * indicates a bond point to the imide structure, amic acid structure, or amic ester structure.
4. The resin composition according to claim 1 or 2, wherein at least one diamine residue among the DA2 residues is a diamine residue having a diphenyl ether structure.
5. 3. The resin composition according to claim 1, wherein the component (A) contains either or both of an acid anhydride residue having a reactive unsaturated bond and a monoamine residue having a reactive unsaturated bond.
6. The resin composition according to claim 1 or 2, further comprising a thermal crosslinking agent (hereinafter, component (C)).
7. 7. The resin composition according to claim 6, wherein all or a part of the component (C) is one or more types of thermal crosslinking agents selected from the group consisting of an isocyanuric ring structure-containing epoxy thermal crosslinking agent, an alicyclic epoxy thermal crosslinking agent, and an aliphatic epoxy thermal crosslinking agent.
8. A cured product obtained by curing the resin composition according to claim 1 or 2.
9. An organic electroluminescence display device comprising the cured product according to claim 8 .
Citation Information
Patent Citations
Display device
JP2002091343A
Display device
JP2002116715A
Positive photosensitive resin precursor composition
JP2005352004A
Photosensitive resin composition
JP2014059463A