Adhesive composition, and prepreg, adhesive sheet, laminate and printed wiring board containing the same

A cyclic polyolefin resin with unsaturated bonds and a filler provides enhanced heat resistance and dielectric properties, addressing issues in existing resins by enabling low-temperature curing and maintaining performance in high-frequency applications.

JP2024141650APending Publication Date: 2024-10-10TOYOBO MC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023053420
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing cyclic olefin resins used in prepregs for printed wiring boards face issues with heat resistance and dielectric properties due to the generation of hydroxyl groups during epoxy resin curing or insufficient crosslinking at low temperatures.

Method used

A composition comprising a cyclic polyolefin resin with specific unsaturated bonds and a filler, allowing for radical curing at lower temperatures, maintaining excellent dielectric properties and adhesive strength.

Benefits of technology

The adhesive composition exhibits improved heat resistance, adhesive strength, and dielectric properties, suitable for high-frequency applications in printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141650000001
    Figure 2024141650000001
Patent Text Reader

Abstract

To provide an adhesive composition having excellent heat resistance, adhesive strength and dielectric properties and capable of being cured at a lower temperature and to provide a prepreg, a metal-clad laminate and a printed wiring board containing the same.SOLUTION: There is provided an adhesive composition comprising a cyclic polyolefin resin (A), a polyolefin resin having an unsaturated bond (B) and a filler (C), which satisfies the following requirements (1) to (3). (1) A copolymer having a cyclic olefin (α) unit having no functional group in the side chain and a cyclic olefin (β) unit having an unsaturated bond in the side chain as constitutional units. (2) When the total of the (α) units and (β) units in the cyclic polyolefin resin (A) is defined as 100 mass%, the content of (α) units is 90 to 99.9 mass% and the content of (β) units is 0.1 to 10 mass%. (3) Having a 5-membered ring in the main chain.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive composition. More specifically, the present invention relates to an adhesive resin composition for use in prepregs, metal copper-clad laminates, and printed wiring boards, and to prepregs, metal copper-clad laminates, and printed wiring boards containing the same. [Background technology]

[0002] Many prepregs for printed wiring boards (electronic circuit boards) are manufactured by impregnating a fiber base material with a resin varnish and then drying it. In recent years, electronic devices have become smaller, lighter, denser, and more powerful, and the requirements for the performance of printed wiring boards have become increasingly sophisticated. In particular, the fifth generation communication system "5G", whose development is currently accelerating, is expected to further increase capacity and speed of communication. In 5G, the frequency used will become higher, and in order to realize high-speed communication using high frequencies, further improvement in the performance of the board material will be required. For example, it is important to have low dielectric properties to reduce transmission loss. Insulating material resins used in prepregs, metal-clad laminates, and printed wiring boards are also required to exhibit low dielectric properties and high heat resistance while ensuring adhesion to low-roughness copper foil. Against this background, cyclic olefin resin compositions (Patent Document 1, Patent Document 2) have been proposed as resin compositions with high heat resistance and low dielectric properties. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] : JP 8-20692 [Patent Document 2] : JP2023-7603 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the cyclic olefin resin described in Patent Document 1 needs to be cured with an epoxy resin. After curing, epoxy resin generates hydroxyl groups, which deteriorates the dielectric properties. The cyclic olefin described in Patent Document 2 has vinyl groups and is cured by a radical reaction, so no hydroxyl groups are generated and the dielectric properties are maintained. However, the cyclic olefin resin has vinyl groups in the side chains, and when cured at low temperatures, the heat resistance is poor due to insufficient crosslinking.

[0005] An object of the present invention is to provide an adhesive composition which has excellent heat resistance, adhesive strength and dielectric properties and can be cured at a lower temperature, and to provide a prepreg, a metal-clad laminate and a printed wiring board which contain the same. [Means for solving the problem]

[0006] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the means described below, and have arrived at the present invention. That is, the present invention has the following configuration. [1] An adhesive composition comprising a cyclic polyolefin resin (A), a polyolefin resin having an unsaturated bond (B), and a filler (C), which satisfy the following requirements (1) to (3): (1) A copolymer having, as structural units, cyclic olefin (α) units having no functional groups in the side chains and cyclic olefin (β) units having unsaturated bonds in the side chains. (2) When the total of the (α) units and the (β) units in the cyclic polyolefin resin (A) is taken as 100% by mass, the content of the (α) units is 90 to 99.9% by mass and the content of the (β) units is 0.1 to 10% by mass. (3) Has a five-membered ring in the main chain [2] The adhesive composition according to [1], wherein the weight average molecular weight of the cyclic polyolefin resin (A) is 5,000 or more and 100,000 or less. [3] The adhesive composition according to [1] or [2], wherein the unsaturated bond in the side chain of the cyclic olefin (β) unit having an unsaturated bond in the side chain is an unsaturated bond in a methacryloyl group. [4] The adhesive composition according to any one of [1] to [3], wherein the polyolefin resin (B) is a polybutadiene having an unsaturated bond in a side chain. [5] The adhesive composition according to any one of [1] to [4], wherein the filler (C) is silica. [6] A prepreg impregnated with the adhesive composition according to any one of [1] to [5]. [7] An adhesive sheet having an adhesive layer made of the adhesive composition according to any one of [1] to [6]. [8] A laminate using the prepreg described in [6] or the adhesive sheet described in [7]. [9] A printed wiring board comprising the laminate according to [8] as a component. Effect of the Invention

[0007] The adhesive composition of the present invention has excellent heat resistance, adhesive strength, and dielectric properties, and can be cured at a lower temperature. For these reasons, the adhesive composition is suitable for use in adhesive compositions, prepregs containing the same, metal-clad laminates, and printed wiring boards. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] An embodiment of the present invention will be described in detail below. However, the present invention is not limited to this embodiment, and can be practiced in various modified forms within the scope of the above description.

[0009] The adhesive composition of the present invention contains a cyclic polyolefin resin (A), a polyolefin resin having an unsaturated bond (B), and a filler (C), which will be described later.

[0010] <Cyclic polyolefin resin (A)> The cyclic polyolefin resin (A) in the present invention has, as structural units, a cyclic olefin (α) having no functional group in the side chain and a cyclic olefin (β) having an unsaturated bond in the side chain. Here, the cyclic polyolefin resin refers to a resin mainly composed of cyclic olefin monomer units, which does not contain any olefin other than the cyclic olefin monomer as a copolymerization component, or if it does contain any olefin, the amount is very small, at most about 1 mol %,

[0011] Examples of the cyclic olefin (α) that does not have a functional group in the side chain include bicyclic compounds such as 2-norbornene and norbornadiene, tricyclic compounds such as dicyclopentadiene and dihydrodicyclopentadiene, tetracyclic compounds such as tetracyclododecene, pentacyclic compounds such as cyclopentadiene trimer, or alkyl (methyl, ethyl, propyl, butyl, etc.) substituted compounds of these polycyclic compounds, alkenyl (vinyl, etc.) substituted compounds, alkylidene (ethylidene, etc.) substituted compounds, aryl (phenyl, tolyl, naphthyl, etc.) substituted compounds, etc., and these can be used alone or in combination of two or more kinds. Among these, norbornene-based monomers selected from the group consisting of norbornene, dicyclopentadiene, or alkyl substituted compounds thereof are particularly preferred from the viewpoint of solvent solubility.

[0012] Examples of the unsaturated bond in the side chain of the cyclic olefin (β) having an unsaturated bond in the side chain include unsaturated bonds in maleimide groups, vinyl groups, allyl groups, acrylic groups, and methacryloyl groups, and the unsaturated bond in the methacryloyl group is particularly preferred. By having a methacryloyl group with particularly high reactivity, it is possible to cure at a lower temperature than before, and when forming a laminate, the influence of thermal degradation on other layers is small. In addition, it is possible to proceed with a radical curing reaction without a radical generator, and therefore good dielectric properties can be maintained.

[0013] The cyclic olefin (β) having an unsaturated bond in the side chain can be obtained by modifying a cyclic olefin monomer having a functional group such as a carboxyl group or a hydroxyl group in the side chain that can react with an isocyanate compound with an isocyanate compound having an unsaturated bond. The cyclic olefin monomer having a functional group in the side chain that can react with an isocyanate compound is not particularly limited, but examples thereof include 5-norbornene-2-carboxylic acid, 5-norbornene-2,3-dicarboxylic acid, 5-norbornene-2,3-dicarboxylic anhydride, and 5-norbornene-2-methanol, and these can be used alone or in combination. Particularly preferred is 5-norbornene-2-carboxylic acid. The structure of the main chain can be the same as that exemplified for the cyclic olefin (α) having no functional group in the side chain, and particularly preferred is a norbornene-based monomer selected from the group consisting of norbornene, dicyclopentadiene, or alkyl-substituted products thereof.

[0014] The isocyanate compound having an unsaturated bond is not particularly limited, but specific examples include 2-isocyanate ethyl methacrylate, 2-(2-methacryloyloxyethyloxy)ethyl isocyanate, and the like.

[0015] The cyclic polyolefin resin (A) in the present invention is a copolymer having a cyclic olefin (α) having no functional group in the side chain and a cyclic olefin (β) having an unsaturated bond in the side chain as a constituent unit, and the content of the (α) unit is 90 to 99.9 mass% and the content of the (β) unit is 0.1 to 10 mass% in the total of (α) and (β) in the copolymer, which is 100 mass%. The content of the (β) unit is preferably 0.5 to 5 mass%, more preferably 1 to 4 mass%. By making the (β) component in the copolymer below the upper limit, the influence of the acrylic skeleton or amide skeleton, which has inferior dielectric properties compared to the cyclic olefin (α) having no functional group in the side chain, on the dielectric loss tangent becomes minor, and by making it above the lower limit, crosslinking during curing is ensured, so that the adhesive strength and heat resistance can be maintained.

[0016] The cyclic polyolefin resin (A) in the present invention has a five-membered ring in the main chain. Since the five-membered ring and the ethylene skeleton are linked in the monomer unit, the cyclic polyolefin resin (A) has a better solvent solubility than the main chain skeleton in which ring structures are linked obtained by conventional addition polymerization, and is particularly preferable for use as an adhesive.

[0017] The polymerization method and polymerization conditions for polymerizing the monomer components are not particularly limited, and may be appropriately set according to conventional methods.

[0018] The weight average molecular weight (Mw) of the cyclic polyolefin resin (A) of the present invention is preferably 5,000 to 100,000. More preferably, it is 6,000 or more, and even more preferably, it is 7,500 or more. Also, it is more preferably 90,000 or less, and even more preferably 85,000 or less. By setting the weight average molecular weight within the above range, it becomes easy to impregnate the resin into the fiber substrate when forming a prepreg, and a certain strength as a resin is ensured. The weight average molecular weight is measured by the method described in the Examples.

[0019] The cyclic polyolefin resin (A) of the present invention is preferably one in which the carbon-carbon double bonds in the main chain are hydrogenated. By hydrogenating the double bonds, particularly excellent dielectric properties are exhibited. The proportion of hydrogenated double bonds among the carbon-carbon double bonds in the main chain is preferably 80% or more, more preferably 90% or more, and even more preferably 95% or more.

[0020] <Production method of cyclic polyolefin resin (A)> The method for producing the cyclic polyolefin resin (A) of the present invention is not particularly limited, but various conventionally known polymerization methods such as solution polymerization and bulk polymerization can be adopted as the polymerization method, and it is particularly preferable to adopt the solution polymerization method. For example, it can be produced by the following method. That is, it is obtained by polymerizing a cyclic olefin monomer having no functional group on the side chain and a cyclic olefin monomer having a carboxyl group on the side chain in a suitable polymerization solvent under a metal catalyst by ring-opening metathesis (ROMP) polymerization, and then modifying the resulting product with an isocyanate compound having an unsaturated bond.

[0021] The solvent usable in the polymerization reaction according to the present invention is not particularly limited, but examples thereof include aromatic hydrocarbons, cyclohexane, toluene, ethylbenzene, xylene, propylbenzene, isopropylbenzene, t-butylbenzene, mesitylene, and the like, and capped glycol ethers such as propylene glycol monomethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and the like, and mixtures thereof, with cyclohexane and toluene being preferred.

[0022] When the polymerization is carried out in a solvent, the total concentration of the monomer and polymer is preferably 1 to 80% by weight, more preferably 2 to 60% by weight. If the total concentration of the monomer and polymer is 1% by weight or less, the productivity is poor, and if it is 80% by weight or more, the solution viscosity after polymerization is too high, which may make the subsequent handling difficult.

[0023] The polymerization temperature is not particularly limited, but is generally −30 to 200° C., and preferably 0 to 180° C. The polymerization time is not particularly limited, and is from 1 minute to 100 hours.

[0024] The catalyst used in the ring-opening metathesis polymerization includes a metal carbene organic complex, the metal being, but not necessarily, a transition metal such as ruthenium, molybdenum, osmium or tungsten. The catalyst used can be sufficiently reacted at 50 to 1000 ppm based on the total weight of the monomers having polymerizable functional groups.

[0025] In such a polymerization reaction, a monomer capable of reacting with the above-mentioned cyclic olefin monomer can be used as a molecular weight regulator to adjust the molecular weight of the polymer. Examples of such molecular weight regulators include α-olefins such as 1-butene, 1-pentene, 1-hexene, and 1-octene; styrenes such as styrene and vinyl toluene; ethers such as ethyl vinyl ether, butyl vinyl ether, and allyl glycidyl ether; halogen-containing vinyl compounds such as allyl chloride; and nitrogen-containing vinyl compounds such as acrylonitrile and acrylamide. In particular, a molecular weight regulator that does not contain a heteroatom is suitable for improving the dielectric properties. In addition, a polymer having a desired molecular weight can be obtained by using 0.1 to 100 mol % of the molecular weight regulator relative to the monomer.

[0026] The method for producing a hydrogenated product involves hydrogenating the carbon-carbon double bonds in the polymer backbone in a solution in the presence of hydrogen and a hydrogenation catalyst. Examples of the hydrogenation catalyst used in the hydrogenation include homogeneous catalysts such as Ziegler catalysts consisting of a combination of a transition metal compound and an alkali metal compound, such as cobalt acetate and triethylaluminum, nickel acetylacetonate and triisobutylaluminum, titanocene dichloride and n-butyllithium, zirconocene dichloride and sec-butyllithium, and tetrabutoxytitanate and dimethylmagnesium, ruthenium-carbene catalysts, dichlorotris(triphenylphosphine)rhodium, and noble metal complex catalysts consisting of ruthenium compounds. In addition, heterogeneous catalysts, such as nickel / silica and palladium / carbon, in which metals such as nickel, palladium, platinum, rhodium, and ruthenium are supported on a support such as carbon, silica, diatomaceous earth, alumina, and titanium oxide can also be used. The hydrogenation reaction is usually carried out in an organic solvent. The organic solvent can be appropriately selected depending on the solubility of the hydrogenated product to be produced, and the same organic solvent as the polymerization solvent can be used. Therefore, after the polymerization reaction, the hydrogenation catalyst can be added directly without replacing the solvent, and the reaction can be continued.

[0027] The hydrogenation reaction conditions may be appropriately selected depending on the type of hydrogenation catalyst used. The reaction temperature is usually -20 to 250°C, preferably -10 to 220°C, and more preferably 0 to 200°C. If the reaction temperature is less than -20°C, the reaction rate slows down, and conversely, if the reaction temperature exceeds 250°C, side reactions tend to occur. The hydrogen pressure is usually 0.01 to 10.0 MPa, preferably 0.05 to 8.0 MPa, and more preferably 0.1 to 5.0 MPa. If the hydrogen pressure is less than 0.01 MPa, the hydrogenation rate slows down, and if the hydrogen pressure exceeds 10.0 MPa, a high-pressure reactor is required. The hydrogenation reaction time is appropriately selected to control the hydrogenation rate. The reaction time is usually in the range of 0.1 to 50 hours, and 80% or more, preferably 90% or more, and more preferably 95% or more of the carbon-carbon double bonds in the main chain of the polymer can be hydrogenated.

[0028] After the hydrogenation reaction, it is preferable to remove the catalyst, which can be removed by known methods such as adsorption and removal using an adsorbent such as silica, alumina, activated carbon, etc., removal using an ion exchange resin, insolubilization of the catalyst residue by adding a chelating agent and then filtration, and solidification and separation of the polymer solution with a large amount of a poor solvent such as methanol followed by drying.

[0029] <Polyolefin resin having unsaturated bonds (B)> The polyolefin resin (B) having an unsaturated bond is not particularly limited, but is preferably polybutadiene or a modified product thereof from the viewpoints of dielectric properties, adhesive strength, and low water absorption. In addition, it is preferable that the polyolefin resin (B) having an unsaturated bond is not a cyclic olefin resin.

[0030] The polyolefin resin (B) having an unsaturated bond preferably has a weight average molecular weight of 500 to 20,000, more preferably 1,000 to 10,000, and even more preferably 1,000 to 7,000. If the weight average molecular weight is within the range, the solvent solubility and compatibility are excellent, and the viscosity of the varnish is reduced, so that the impregnation of the fiber substrate in the prepreg is excellent. Specifically, for example, styrene-butadiene copolymer (SBR: RICON-100, RICON-181, RICON-184, all manufactured by Cray Valley, etc.) and polybutadiene (B-1000, B-2000, B-3000, all manufactured by Nippon Soda Co., Ltd.) can be mentioned.

[0031] The amount of the polyolefin resin (B) having an unsaturated bond in the adhesive composition of the present invention is preferably 0.1 to 30 parts by mass, more preferably 5 to 28 parts by mass, and even more preferably 10 to 25 parts by mass, per 100 parts by mass of the cyclic polyolefin resin (A) of the present invention. By making the amount equal to or greater than the lower limit, particularly good adhesive strength can be achieved. On the other hand, by making the amount equal to or less than the upper limit, the solvent solubility becomes particularly good, and a homogeneous composition can be produced.

[0032] <Filler (C)> The filler (C) is not particularly limited, and organic fillers and inorganic fillers can be used. Specifically, the organic fillers include powders of heat-resistant resins such as polyimide, polyamideimide, fluororesin, and liquid crystal polyester. In addition, the inorganic fillers include, for example, silica (SiO2), alumina (Al2O3), titania (TiO2), tantalum oxide (Ta2O5), zirconia (ZrO2), silicon nitride (Si3N4), boron nitride (BN), calcium carbonate (CaCO3), calcium sulfate (CaSO4), zinc oxide (ZnO), magnesium titanate (MgO·TiO2), barium sulfate (BaSO4), organic bentonite, clay, mica, aluminum hydroxide, and magnesium hydroxide. Among them, silica is particularly preferable because of its ease of dispersion and heat resistance improvement effect.

[0033] As the silica, hydrophobic silica and hydrophilic silica can be used, but in order to impart moisture absorption resistance, hydrophobic silica treated with dimethyldichlorosilane, hexamethyldisilazane, octylsilane, or the like is preferred.

[0034] The amount of the filler (C) in the adhesive composition of the present invention is preferably 0.05 to 100 parts by mass, more preferably 1 to 80 parts by mass, and even more preferably 5 to 70 parts by mass, based on 100 parts by mass of the cyclic polyolefin resin (A) of the present invention. By making the amount equal to or greater than the lower limit, further heat resistance can be exhibited. On the other hand, by making the amount equal to or less than the upper limit, poor dispersion of the filler (C) and excessively high solution viscosity can be suppressed, resulting in good workability.

[0035] The adhesive composition of the present invention may contain a compound having a terminal unsaturated hydrocarbon group as an additive for further improving heat resistance. Since the terminal unsaturated hydrocarbon group can react with the cyclic polyolefin resin (A) of the present invention, the crosslinking density between these compounds can be increased to achieve excellent solder heat resistance. Here, the terminal unsaturated hydrocarbon group refers to a group having a CH2=C structure, such as a vinyl group, a vinylidene group, an allyl group, an acrylic group, a methacrylic group, or a styrene group. In addition, other components such as a flame retardant, an acid generator, a heat resistance improver, a development assistant, a plasticizer, a polymerization inhibitor, an ultraviolet absorber, an antioxidant, a matting agent, an antifoaming agent, a leveling agent, an antistatic agent, a dispersant, a slip agent, a surface modifier, a thixotropic agent, a surfactant, a coupling agent such as a silane-based, aluminum-based, or titanium-based, a polyhydric phenol compound, or an organic solvent may be blended according to the purpose and required characteristics of each application.

[0036] <Crosslinking agent> The adhesive composition of the present invention may contain a crosslinking agent. Examples of the crosslinking agent include crosslinking agents having two or more reactive groups. Examples of the reactive groups include vinyl groups, allyl groups, (meth)acryloyl groups, vinylphenyl groups, and maleimide groups.

[0037] Examples of the crosslinking agent having two or more reactive groups include styrene-butadiene rubber, polybutadiene rubber, triallyl isocyanurate, divinylbenzene, etc., and at least one selected from these can be used. The crosslinking agent can be contained in an amount of 5 parts by mass or more and 200 parts by mass or less, preferably 10 parts by mass or more and 180 parts by mass or less, and more preferably 20 parts by mass or more and 150 parts by mass or less, relative to 100 parts by mass in total of the cyclic polyolefin resin (A) and the polyolefin resin (B) having an unsaturated bond.

[0038] The adhesive composition of the present invention preferably has a relative dielectric constant (εc) of 2.4 or less at a frequency of 10 GHz, more preferably 2.2 or less, and even more preferably 2.1 or less. There is no particular lower limit, but in practical use it is 2.0. Moreover, the relative dielectric constant (εc) over the entire frequency range of 1 GHz to 60 GHz is preferably 2.7 or less, more preferably 2.6 or less, and even more preferably 2.3 or less.

[0039] The adhesive composition of the present invention preferably has a dielectric loss tangent (tan δ) of less than 0.0020 at a frequency of 10 GHz. More preferably, it is less than 0.0018, and even more preferably, it is less than 0.0015. There is no particular lower limit, but in practical use, it is 0.0001 or more. Moreover, the dielectric loss tangent (tan δ) over the entire frequency range of 1 GHz to 60 GHz is preferably 0.0025 or less, more preferably less than 0.0020, and even more preferably less than 0.0015.

[0040] <Radical generator> The adhesive composition of the present invention may contain a radical generator. The adhesive composition of the present invention may react compounds having unsaturated bonds by heating, but the radicals generated by the radical generator efficiently react unsaturated hydrocarbon groups with each other, increasing the crosslinking density and improving the heat resistance. The radical generator is not particularly limited, but it is preferable to use an organic peroxide. The organic peroxide is not particularly limited, but examples thereof include peroxides such as di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, dicumyl peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide, lauroyl peroxide, and 2,5-dimethyl-2,5-di(tertiary butyl peroxy)hexane; and azonitriles such as azobisisobutyronitrile and azobisisopropionitrile. Among them, from the viewpoint of dielectric properties, a radical generator that does not contain heteroatoms other than oxygen is preferable.

[0041] The one-minute half-life temperature of the radical generator is preferably 140° C. or higher. By setting the temperature to 140° C. or higher, the solvent in the adhesive composition varnish is volatilized to prevent the initiation of a radical reaction when an adhesive sheet is produced, and excellent adhesiveness can be exhibited.

[0042] When the adhesive composition contains a radical generator, the amount of the radical generator is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, relative to 100 parts by mass of the total of the resin components. Also, the amount is preferably 50 parts by mass or less, more preferably 20 parts by mass or less. By keeping the amount within the above range, an optimal crosslink density can be achieved, and both adhesion and heat resistance can be achieved.

[0043] The adhesive composition of the present invention can be applied to a substrate or the like, and then dried and cured to form an adhesive layer. In this case, the curing temperature is preferably 160 to 190°C, more preferably 170 to 180°C. By setting the temperature within the above range, the influence of thermal deterioration on other layers can be reduced when a laminate is formed. When the cyclic polyolefin resin (A) contained in the adhesive composition of the present invention has a methacryloyl group in the side chain, it is particularly preferable for curing at low temperatures.

[0044] The form of use of the adhesive composition of the present invention is not particularly limited, but examples include a resin film made of the adhesive composition, a resin film with a carrier in which the resin film is provided on a carrier substrate, a prepreg obtained by impregnating a fiber substrate with the adhesive composition, a metal-clad laminate in which a metal layer is disposed on at least one surface of a cured product of the prepreg, a resin substrate provided with an insulating layer made of a cured product of the adhesive composition, and a printed wiring board in which a circuit layer is formed on the surface of the metal-clad laminate or the resin substrate.

[0045] (Resin substrate) The resin substrate of the present embodiment can include an insulating layer made of a cured product of a thermosetting resin composition. Such a resin substrate can be made to be free of glass fibers and can be used for a printed wiring board.

[0046] (Prepreg) The prepreg of the present embodiment is obtained by impregnating a fiber substrate with the adhesive composition. For example, the prepreg can be used as a sheet-like material obtained by impregnating a fiber substrate with the adhesive composition and then semi-curing the same. The sheet-like material having such a structure is excellent in various properties such as dielectric properties and mechanical and electrical connection reliability under high temperature and humidity, and is suitable for manufacturing an insulating layer of a printed wiring board.

[0047] The method for impregnating the adhesive composition into a fiber substrate is not particularly limited, but examples include a method of dissolving the adhesive composition in a solvent to prepare a resin varnish and immersing the fiber substrate in the resin varnish, a method of applying the resin varnish to the fiber substrate using various coaters, a method of spraying the resin varnish onto the fiber substrate using a sprayer, and a method of laminating both sides of the fiber substrate with the resin film consisting of the adhesive composition.

[0048] In this embodiment, the prepreg can be used to form, for example, an insulating layer in a build-up layer or an insulating layer in a core layer of a printed wiring board. When the prepreg is used to form an insulating layer in a core layer of a printed wiring board, for example, two or more prepregs can be stacked and the resulting laminate can be heat-cured to form an insulating layer for the core layer.

[0049] The fiber substrate is not particularly limited, but includes glass fiber substrates such as glass woven fabric and glass nonwoven fabric; polyamide resin fibers such as polyamide resin fibers, aromatic polyamide resin fibers, and wholly aromatic polyamide resin fibers; polyester resin fibers such as polyester resin fibers, aromatic polyester resin fibers, and wholly aromatic polyester resin fibers; synthetic fiber substrates composed of woven or nonwoven fabrics mainly composed of either polyimide resin fibers or fluororesin fibers; paper substrates mainly composed of kraft paper, cotton linter paper, or mixed paper of linter and kraft pulp; and the like. Any of these can be used. Among these, glass fiber substrates are preferred. This allows for the production of a resin substrate with low water absorption, high strength, and low thermal expansion.

[0050] The thickness of the fiber base material is not particularly limited, but is preferably 5 μm to 150 μm, more preferably 10 μm to 100 μm, and even more preferably 12 μm to 90 μm. By using a fiber base material having such a thickness, the handleability during the production of the prepreg can be further improved.

[0051] When the thickness of the fiber substrate is equal to or less than the upper limit, the impregnation of the adhesive composition in the fiber substrate is improved, and the occurrence of strand voids and deterioration of insulation reliability can be suppressed. In addition, the formation of through holes by carbon dioxide, UV, excimer, or other lasers can be facilitated. In addition, when the thickness of the fiber substrate is equal to or more than the lower limit, the strength of the fiber substrate and prepreg can be improved. As a result, the handling property can be improved, the preparation of prepreg can be facilitated, and warping of the resin substrate can be suppressed.

[0052] As the above-mentioned glass fiber substrate, for example, a glass fiber substrate formed of one or more types of glass selected from E glass, S glass, D glass, T glass, NE glass, UT glass, L glass, HP glass and quartz glass is suitably used.

[0053] (Metal-clad laminate) In the present embodiment, the metal-clad laminate is a laminate in which a metal layer is disposed on at least one surface of the cured product of the prepreg. A method for producing the metal-clad laminate using the prepreg is, for example, as follows.

[0054] A metal foil is placed on both the upper and lower sides or one side of the outer side of a prepreg or a laminate of two or more prepregs, and these are bonded under high vacuum conditions using a laminator or Becquerel device, or a metal foil is placed on both the upper and lower sides or one side of the outer side of the prepreg as is. When two or more prepregs are laminated, a metal foil is placed on both the upper and lower sides or one side of the outermost side of the laminated prepregs. Next, a metal-clad laminate can be obtained by hot-press molding the laminate of the prepreg and the metal foil. Here, it is preferable to continue pressing until the end of cooling during hot-press molding.

[0055] Examples of the metal constituting the metal foil include copper, copper-based alloys, aluminum, aluminum-based alloys, silver, silver-based alloys, gold, gold-based alloys, zinc, zinc-based alloys, nickel, nickel-based alloys, tin, tin-based alloys, iron, iron-based alloys, Fe-Ni-based alloys such as Kovar (trade name), 42 alloy, Invar, and Super Invar, W, and Mo. Among these, the metal constituting the metal foil 105 is preferably copper or a copper alloy because it has excellent conductivity, is easy to form a circuit by etching, and is inexpensive. That is, copper foil is preferable as the metal foil 105. In addition, a metal foil with a carrier or the like can also be used as the metal foil. The thickness of the metal foil is preferably 0.5 μm or more and 20 μm or less, and more preferably 1.5 μm or more and 18 μm or less. According to this embodiment, by adopting such a resin film or a prepreg using the same, it is possible to form an insulating layer in a printed wiring board with a reduced linear expansion coefficient in the planar direction.

[0056] (Printed wiring board) The printed wiring board of the present embodiment is provided with an insulating layer made of a cured product of the above-mentioned adhesive composition. EXAMPLES

[0057] The present invention will be described in detail below with reference to examples. In the examples and comparative examples, "parts" simply refers to "parts by mass."

[0058] <Weight average molecular weight and molecular weight distribution> Measurements were performed using gel permeation chromatography (GPC) under the following conditions, and the weight average molecular weight and molecular weight distribution (weight average molecular weight / number average molecular weight) values ​​converted to standard polystyrene were calculated for the cyclic olefin resins produced in the Synthesis Examples and Comparative Synthesis Examples using analysis software (LabSolutions™, manufactured by Shimadzu Corporation). Measuring device: Tosoh HLC-8220 Column: 2 TSK gel super HM-H and 1 Super H2500 connected in series Detector: Refractive index (RI) detector Solution preparation: Use tetrahydrofuran as the solvent and a 0.05 wt% solution of the sample. Column temperature: 40℃ Injection volume: 20μL Flow rate: 0.6ml / min

[0059] <Side chain unsaturated bond quantitative measurement> Using a 600 MHz nuclear magnetic resonance spectrometer (hereinafter sometimes abbreviated as NMR), 1H-NMR measurement was carried out under the following conditions to confirm whether an unsaturated bond was introduced into the side chain of the cyclic olefin resin. (1H-NMR measurement conditions) Equipment: BRUKER AVANCE NEO 600 spectrometer Measurement solvent: deuterated chloroform Sample concentration: approx. 20 mg / approx. 0.60 mL Resonance frequency: 600MHz Flip angle: 30 degrees Data acquisition time: 4 seconds Pulse repetition time: 1 second Accumulation count: 64 Measurement temperature: 50℃

[0060] <Synthesis Example 1> (Preparation of cyclic polyolefin resin (a-1)) In a four-neck flask, 100 parts by weight of 2-norbornene (Tokyo Chemical Industry Co., Ltd.), 4.58 parts by weight of 5-norbornene-2-carboxylic acid (Tokyo Chemical Industry Co., Ltd.), 4.06 parts by weight of 1-hexene (Tokyo Chemical Industry Co., Ltd.), 0.03 g of dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinylidene](benzylidene)(tricyclohexylphosphine)ruthenium(II) (Sigma-Aldrich Co., Ltd.), and 165 parts by weight of tetrahydrofuran (Fujifilm Wako Pure Chemical Industries Co., Ltd.) as a solvent were added at room temperature under a nitrogen atmosphere, and the mixture was stirred and polymerized for 2 hours at room temperature. Next, as a hydrogenation step, 100 parts by weight of the solution was transferred to a SUS autoclave with an internal volume of 1 L that had been thoroughly substituted with nitrogen. After adding 0.89 parts by weight of Pd-C (Pd10%) (about 55% water-wet product, manufactured by Tokyo Chemical Industry Co., Ltd.), hydrogen gas (H2) was introduced at a pressure of 0.20 MPaG, the temperature was raised to 60 ° C, and the mixture was stirred for 4 hours to complete the hydrogenation reaction. Insoluble matter was removed by filtration, and the mixture was purified with a large excess of methanol to obtain a cyclic polyolefin resin. 52.3 parts by weight of the obtained cyclic polyolefin resin was dissolved in 43 parts by weight of toluene (manufactured by Nacalai Tesque Co., Ltd.) in a four-neck flask at room temperature under a nitrogen atmosphere, and 3.97 parts by weight of 2-isocyanatoethyl methacrylate (manufactured by Resonac Co., Ltd.) and 0.01 parts by weight of 1,8-diazabicyclo[5,4,0]-7-undecene (manufactured by Tokyo Chemical Industry Co., Ltd.) were added, and the mixture was stirred at 80 ° C for 4 hours. The above reaction solution was purified with a large excess of methanol to obtain a cyclic polyolefin resin (a-1). The weight average molecular weight (Mw) of the obtained resin measured under the above conditions was 7,900, and the molecular weight distribution (Mw / Mn) was 2.0. The unsaturated terminal group content of the obtained cyclic olefin resin was 3.0 mol% based on the total monomer units of the polymer.

[0061] <Synthesis Example 2> (Preparation of cyclic polyolefin resin (a-2)) In a four-neck flask, 100 parts by weight of dicyclopentadiene (manufactured by Tokyo Chemical Industry Co., Ltd.), 2.08 parts by weight of 5-norbornene-2-carboxylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.45 parts by weight of 1-hexene (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.5 parts by weight of dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinylidene](benzylidene)(tricyclohexylphosphine)ruthenium(II) (manufactured by Sigma-Aldrich Co., Ltd.) were added at room temperature under a nitrogen atmosphere. 03 parts by weight, and 165 parts by weight of tetrahydrofuran (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) as a solvent, were stirred at room temperature for 2 hours and polymerized. Next, as a hydrogenation process, 100 parts by weight of the solution was transferred to a SUS autoclave with an internal volume of 1 L that had been fully replaced with nitrogen, and 0.89 parts by weight of Pd-C (Pd10%) (about 55% water-wet product, manufactured by Tokyo Chemical Industry Co., Ltd.) was added, and hydrogen gas (H2) was introduced at a pressure of 0.20 MPaG, the temperature was raised to 60°C, and the mixture was stirred for 4 hours to complete the hydrogenation reaction. Insoluble matter was removed by filtration, and the mixture was purified with a large excess of methanol to obtain a cyclic olefin resin. 51.1 parts by weight of the obtained cyclic olefin resin was dissolved in 44 parts by weight of toluene (manufactured by Nacalai Tesque, Inc.) in a four-neck flask at room temperature under a nitrogen atmosphere, and 2.65 parts by weight of 2-isocyanatoethyl methacrylate (manufactured by Resonac, Inc.) and 0.01 parts by weight of 1,8-diazabicyclo[5,4,0]-7-undecene (manufactured by Tokyo Chemical Industry Co., Ltd.) were added, followed by stirring at 80°C for 4 hours. The weight average molecular weight (Mw) of the obtained resin measured under the above conditions was 81,000, and the molecular weight distribution (Mw / Mn) was 2.3. The unsaturated terminal group content of the obtained cyclic olefin resin was 1.4 mol% based on the total monomer units of the polymer.

[0062] <Comparative Synthesis Example 1> (Preparation of Cyclic Olefin Resin (a-3)) In a four-neck flask, 100 parts by weight of 2-norbornene (manufactured by Tokyo Chemical Industry Co., Ltd.), 2.41 parts by weight of 1-hexene (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.03 parts by weight of dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinylidene](benzylidene)(tricyclohexylphosphine)ruthenium(II) (manufactured by Sigma-Aldrich Co., Ltd.), and 154 parts by weight of tetrahydrofuran (manufactured by Fuji Film Wako Pure Chemical Industries Co., Ltd.) as a solvent were added at room temperature under a nitrogen atmosphere, and the mixture was polymerized under stirring at room temperature for 2 hours. Next, as a hydrogenation step, 100 parts by weight of the solution was transferred to a SUS autoclave with an internal volume of 1 L that had been thoroughly substituted with nitrogen, and 0.89 parts by weight of Pd-C (Pd10%) (approximately 55% water-wet product, manufactured by Tokyo Chemical Industry Co., Ltd.) was added, and the mixture was subjected to a hydrogenation process under a pressure of 0.20 MPaG. Hydrogen gas (H2) was introduced under pressure, the temperature was raised to 60°C, and the mixture was stirred for 4 hours to complete the hydrogenation reaction. Insoluble matter was removed by filtration, and the mixture was purified with a large excess of methanol to obtain a cyclic olefin resin. 50 parts by weight of the obtained cyclic olefin resin, 2.5 parts by weight of maleic anhydride, and 2 parts by weight of 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne were mixed, and melt-kneaded at 260°C using a twin-screw extruder with a diameter of 30 mm and a vent device to obtain a maleic anhydride-modified cyclic olefin resin (a-3). The weight average molecular weight (Mw) of the obtained resin measured under the above conditions was 16,900, and the molecular weight distribution (Mw / Mn) was 2.2. The acid anhydride group content of the obtained modified polymer was 2.9 mol% based on the total monomer units of the polymer.

[0063] <Comparative Synthesis Example 2> (Preparation of cyclic polyolefin resin (a-4)) In a four-neck flask, 100 parts by weight of 2-norbornene (manufactured by Tokyo Chemical Industry Co., Ltd.), 18.0 parts by weight of 5-norbornene-2-carboxylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), 4.01 parts by weight of 1-hexene (manufactured by Tokyo Chemical Industry Co., Ltd.), and dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinylidene](benzylidene)(tricyclohexylphosphine)ruthenium(II) (Sigma-Aldrich) were added at room temperature under a nitrogen atmosphere. The mixture was stirred and polymerized at room temperature for 2 hours with 0.04 parts by weight of tetrahydrofuran (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a solvent. Next, as the hydrogenation step, 100 parts by weight of the solution was transferred to a SUS autoclave with an internal volume of 1 L that had been thoroughly substituted with nitrogen, and 0.89 parts by weight of Pd-C (Pd10%) (about 55% water-wet product, manufactured by Tokyo Chemical Industry Co., Ltd.) was added, followed by introducing hydrogen gas (H2) at a pressure of 0.20 MPaG and heating to 60°C. The mixture was stirred for 4 hours to complete the hydrogenation reaction. Insoluble matters were removed by filtration, and the mixture was purified with a large excess of methanol to obtain a cyclic olefin resin. 59.0 parts by weight of the obtained cyclic polyolefin resin was dissolved in 121 parts by weight of toluene (manufactured by Nacalai Tesque, Inc.) in a four-neck flask at room temperature under a nitrogen atmosphere, and 19.0 parts by weight of 2-isocyanatoethyl methacrylate (manufactured by Resonac, Inc.) and 0.06 parts by weight of 1,8-diazabicyclo[5,4,0]-7-undecene (manufactured by Tokyo Chemical Industry Co., Ltd.) were added, and the mixture was stirred at 80°C for 4 hours. The above reaction solution was purified with a large excess of methanol to obtain a cyclic polyolefin resin (a-4). The weight average molecular weight (Mw) of the obtained resin measured under the above conditions was 9,600, and the molecular weight distribution (Mw / Mn) was 2.0. The unsaturated terminal group content of the obtained cyclic olefin resin was 13.0 mol% based on the total monomer units of the polymer.

[0064] <Comparative Synthesis Example 3> (Preparation of cyclic polyolefin resin (a-5)) In a three-neck flask, 8.6 parts by weight of toluene, 100.0 parts by weight of norbornene, 3.4 parts by weight of 5-vinyl-2-norbornene, 4.1 parts by weight of triethylsilane, 42.4 parts by weight of 1-butanol, and 182.8 parts by weight of anisole were added at room temperature under a nitrogen atmosphere to obtain a reaction solution. The reaction solution was bubbled with nitrogen and then heated to 75°C. A catalyst (palladium (II) (acetonitrile) bis (triisopropylphosphine) acetate tetrakis (2,3,4,5,6-pentafluorophenyl) borate, Pd-1206) and a co-catalyst (N,N-dimethylanilinium tetrakis (pentafluorophenyl) borate, DANFABA) were dissolved in a toluene: ethyl acetate = 6: 4 solution, and added to the reaction solution so that the total amount of norbornene monomer: catalyst: co-catalyst = 20000: 1: 1 (molar ratio). The mixture was stirred at 80°C for 2 hours. After the polymerization was completed, the reaction was stopped by cooling. After the reaction was completed, 37.9 parts by weight of the reaction solution was dropped into a mixed solution of 500 parts by weight of methanol and 150 parts by weight of THF to cause reprecipitation. After collecting the polymer by filtration, the residue was washed with a mixed solution of 100 parts by weight of methanol and 100 parts by weight of THF and then filtered. Finally, the polymer was purified by vacuum drying at 80°C to obtain a cyclic polyolefin resin (a-4). The weight average molecular weight (Mw) of the obtained resin measured under the above conditions was 8,800, and the molecular weight distribution (Mw / Mn) was 2.2. The unsaturated terminal group content of the obtained cyclic polyolefin resin was 3.3 mol% based on the total monomer units of the polymer.

[0065] <Evaluation of Adhesive Composition> (Dielectric constant (εc) and dielectric tangent (tanδ)) The adhesive composition was applied to a 100 μm thick Teflon (registered trademark) sheet so that the thickness after drying was 25 μm, and dried at 140° C. for 3 minutes. Then, after hardening by heat treatment at 180° C. for 3 hours, the Teflon (registered trademark) sheet was peeled off to obtain an adhesive resin sheet for testing. The obtained adhesive resin sheet for testing was then cut into strips of 8 cm×3 mm to obtain test samples. The relative dielectric constant (εc) and dielectric tangent (tanδ) were measured using a network analyzer (manufactured by Anritsu Corporation) by a cavity resonator perturbation method at a temperature of 23° C. and a frequency of 10 GHz. <Evaluation criteria for dielectric constant> ○: 2.4 or less ×:Over 2.4 <Evaluation criteria for dielectric tangent> ◎: Less than 0.0015 ○: 0.0015 or more, less than 0.0020 ×:0.0020 or more

[0066] (Peel strength (adhesive strength)) The adhesive composition was applied to a 12.5 μm thick polyimide film (Apical (registered trademark) manufactured by Kaneka Corporation) so that the thickness after drying was 25 μm, and dried at 130 ° C for 3 minutes. The adhesive film (B stage product) thus obtained was laminated to a rolled copper foil (ESPANEX series manufactured by Nippon Steel Chemical & Material Co., Ltd.) having a thickness of 18 μm. The laminate was pressed for 280 seconds at 170 ° C under a pressure of 2 MPa so that the shiny surface of the rolled copper foil was in contact with the adhesive layer. The laminate was then heat-treated at 180 ° C for 3 hours to harden the film, and a sample for peel strength evaluation was obtained. The peel strength was measured under the conditions of 25 ° C, film pulling, tensile speed 50 mm / min, and 90 ° peeling. This test shows the adhesive strength at room temperature. <Evaluation criteria> ○:1.0N / mm or more ×: Less than 1.0N / mm

[0067] (solder heat resistance) An evaluation sample was prepared in the same manner as for measuring the peel strength described above, and a 2.0 cm x 2.0 cm sample piece was immersed in a bath of molten solder at 288°C to check for any changes in appearance such as blistering. <Evaluation criteria> ◎: No swelling for 60 seconds or more ○: Swelling occurs within 30 to 60 seconds ×: Swelling occurs within 10 seconds

[0068] (Gel fraction) The adhesive composition was applied to a 100 μm thick Teflon (registered trademark) sheet so that the thickness after drying was 25 μm, and dried at 140 ° C for 3 minutes. Then, after hardening by heat treatment at 180 ° C for 3 hours, the Teflon (registered trademark) sheet was peeled off to obtain a test adhesive resin sheet. Then, the obtained test adhesive resin sheet was cut into a sample of 8 cm × 3 mm strips to obtain a test sample. After measuring the weight of the test sample, it was immersed in a toluene solution for 1 hour. Then, the solution was filtered to recover the filtrate, dried at 100 ° C for 1 hour, and the weight was measured. The gel fraction was calculated by the following formula. It was evaluated whether it could be hardened at a low temperature based on the gel fraction. (Weight after drying) ÷ (Weight before drying) × 100 = Gel fraction (%) ○: 75% or more ×: Less than 75%

[0069] The following describes production examples of adhesive compositions according to the present invention and comparative adhesive compositions. The adhesive composition used was as follows: Polyolefin resin having unsaturated bonds (B): B-1000 (manufactured by Nippon Soda Co., Ltd.) Filler (C): Silica (GT grade, manufactured by Denka) Epoxy compound: JER-152 (Mitsubishi Chemical) Radical generator: Luperox 12 (Arkema Yoshitomi Co., Ltd.)

[0070] Example 1 80 parts by mass of the cyclic polyolefin resin (a-1) obtained in Synthesis Example 1 was dissolved in 150 parts by mass of toluene, and 20 parts by mass of polybutadiene (B-1000, manufactured by Nippon Soda Co., Ltd.) and 50 parts by mass of silica (GT grade, manufactured by Denka Co., Ltd.) were further blended as compound (B) to obtain adhesive composition 1. The resulting adhesive composition 1 was evaluated for dielectric properties, peel strength (adhesiveness), solder heat resistance, and gel fraction (low temperature curing). The results are shown in Table 1.

[0071] (Example 2, Comparative Examples 1 to 3) Adhesive compositions 2 to 5 were prepared in the same manner as in Example 1, except that the blending amounts were changed as shown in Table 1, and each evaluation was carried out. The evaluation results are shown in Table 1.

[0072] [Table 1]

[0073] As is clear from Table 1, in Examples 1 and 2, the dielectric properties, peel strength, solder heat resistance, and gel fraction are excellent. On the other hand, in Comparative Example 1, the dielectric properties were poor because the cyclic olefin resin did not have an unsaturated bond in the side chain, and curing was performed by the epoxy resin and a site derived from maleic anhydride, instead of radical curing. In Comparative Example 2, the (β) component ratio in the cyclic olefin was high, and the influence of the acrylic skeleton was large, resulting in poor dielectric properties. In Comparative Example 3, the gel fraction was low, and the solder heat resistance was insufficient. [Industrial Applicability]

[0074] The adhesive composition of the present invention has excellent heat resistance, adhesive strength, and dielectric properties, and can be cured at a lower temperature. Therefore, it is useful as an adhesive for printed wiring boards, adhesive sheets, and prepregs applied to printed circuit boards (flexible boards, rigid boards, and package boards) in the high frequency range.

Claims

1. An adhesive composition comprising a cyclic polyolefin resin (A), a polyolefin resin having an unsaturated bond (B), and a filler (C), which satisfy the following requirements (1) to (3): (1) A copolymer having, as structural units, a cyclic olefin (α) unit having no functional group in the side chain and a cyclic olefin (β) unit having an unsaturated bond in the side chain. (2) When the total of the (α) units and the (β) units in the cyclic polyolefin resin (A) is taken as 100 mass%, the content of the (α) units is 90 to 99.9 mass%, and the content of the (β) units is 0.1 to 10 mass%. (3) Having a five-membered ring in the main chain

2. 2. The adhesive composition according to claim 1, wherein the cyclic polyolefin resin (A) has a weight average molecular weight of 5,000 or more and 100,000 or less.

3. 3. The adhesive composition according to claim 1, wherein the unsaturated bond in the side chain of the cyclic olefin (β) unit is an unsaturated bond in a methacryloyl group.

4. 3. The adhesive composition according to claim 1, wherein the polyolefin resin (B) is a polybutadiene having an unsaturated bond in a side chain.

5. 3. The adhesive composition according to claim 1, wherein the filler (C) is silica.

6. A prepreg impregnated with the adhesive composition according to claim 1.

7. An adhesive sheet having an adhesive layer comprising the adhesive composition according to claim 1.

8. A laminate using the prepreg according to claim 6 or the adhesive sheet according to claim 7.

9. A printed wiring board comprising the laminate according to claim 8 as a component.