Retroreflective sheet, adhesive composition, and overlaminate film

A retroreflective sheet with a printed layer and adjacent layer of (meth)acrylic acid and ethoxylated alkyl alcohol, and inorganic nanoparticles, addresses the lower retroreflectivity of inkjet-printed sheets, enhancing retroreflectivity and durability while maintaining weather resistance.

JP2024141666AInactive Publication Date: 2024-10-103M INNOVATIVE PROPERTIES CO
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053449
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Retroreflective sheets formed by inkjet printing exhibit lower retroreflectivity compared to those formed by silk printing, and there is a need for improved durability and weather resistance.

Method used

A retroreflective sheet with multiple layers, including a printed layer and an adjacent layer comprising (meth)acrylic acid and ethoxylated alkyl alcohol, and inorganic nanoparticles, with a refractive index of 1.50 to 1.55, to enhance retroreflectivity and durability.

Benefits of technology

The retroreflective sheet achieves excellent retroreflectivity, durability, and weather resistance even when printed by inkjet, with adjustable refractive index and reduced light scattering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide: a retroreflective sheet that has improved retroreflectivity; and an adhesive composition and an overlaminate film that are usable for the retroreflective sheet.SOLUTION: A retroreflective sheet with multiple layers includes at least a printed layer and an adjacent layer in contact with the printed layer. The adjacent layer contains inorganic nanoparticles, and an acrylic resin that has a constituent unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol. The adjacent layer has a refractive index from 1.50 to 1.55.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a retroreflective sheet, a pressure-sensitive adhesive composition, and an overlaminate film. [Background technology]

[0002] 2. Description of the Related Art Retroreflective sheets that reflect incident light directly back toward the light source, i.e., have retroreflective properties, are widely used in road signs, guide signs, and the like, because they provide high visibility even at night.

[0003] This retroreflective sheeting usually comprises a retroreflective layer for imparting retroreflectivity, a printed layer for displaying necessary information, and a protective layer (adjacent layer) for protecting the printed layer. Of these, the printed layer is generally formed by silk printing.

[0004] In this silk screen printing, printing plates are made for each color, so although it is suitable for producing a large number of identical printed items, it is not suitable for producing a small number of different printed items. In response to this, for example, Patent Document 1 proposes a method of forming the printing layer of the retroreflective sheet by inkjet printing, which allows on-demand printing. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2013 / 145946 Summary of the Invention [Problem to be solved by the invention]

[0006] However, as a result of the inventors' research, it became clear that there is room for improvement in the retroreflectivity of a retroreflective sheet having a printed layer formed by inkjet printing, compared to a retroreflective sheet having a printed layer formed by silk printing.

[0007] Therefore, an object of the present disclosure is to provide a retroreflective sheeting with improved retroreflectivity, as well as a pressure-sensitive adhesive composition and an overlaminate film that can be used therefor. [Means for solving the problem]

[0008] One aspect of the present disclosure relates to a retroreflective sheet having multiple layers, comprising at least a printed layer and an adjacent layer in contact with the printed layer, the adjacent layer containing an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol and inorganic nanoparticles, and the refractive index of the adjacent layer is 1.50 to 1.55.

[0009] Such a retroreflective sheeting has excellent retroreflectivity even though the printed layer is formed by inkjet printing. Furthermore, such a retroreflective sheeting has excellent durability, weather resistance, and the like.

[0010] The retroreflective sheet may have a retroreflective layer, a printed layer, a pressure-sensitive adhesive layer, and a protective film layer in this order, with the adjacent layer being a pressure-sensitive adhesive layer.

[0011] The ester of (meth)acrylic acid and ethoxylated alkyl alcohol may be 2-(2-ethoxyethoxy)ethyl acrylate or poly(ethylene glycol) methyl ether acrylate, which further improves the dispersibility of inorganic nanoparticles in adjacent layers and makes it easier to adjust the refractive index.

[0012] The inorganic nanoparticles may be zirconia particles, which further improves the dispersibility of the inorganic nanoparticles in the adjacent layer and makes it easier to adjust the refractive index.

[0013] Another aspect of the present disclosure relates to a pressure-sensitive adhesive composition containing an acrylic resin having structural units derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles.

[0014] The pressure-sensitive adhesive composition can be suitably used for the retroreflective sheeting. Furthermore, the pressure-sensitive adhesive composition allows the refractive index to be adjusted according to the application.

[0015] Yet another aspect of the present disclosure relates to an overlaminate film having a transparent substrate layer and an adhesive layer, the adhesive layer containing an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles.

[0016] Such an overlaminate film can be suitably used for the retroreflective sheeting. Furthermore, the refractive index of the overlaminate film can be adjusted according to the application. Effect of the Invention

[0017] The retroreflective sheeting of the present disclosure has excellent retroreflectivity even when the printed layer is formed by inkjet printing. In addition, the retroreflective sheeting of the present disclosure has excellent durability, weather resistance, and the like.

[0018] The pressure-sensitive adhesive composition and overlaminate film of the present disclosure can be used for the retroreflective sheet. In addition, the pressure-sensitive adhesive composition and overlaminate film of the present disclosure can adjust the refractive index depending on the application. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a retroreflective sheet according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present disclosure will be described in detail. Note that the drawings may be partially simplified or exaggerated for ease of understanding, and the dimensional ratios and the like are not limited to those shown in the drawings.

[0021] <Retroreflective sheeting> The retroreflective sheet of this embodiment has a plurality of layers including at least a printed layer and an adjacent layer in contact with the printed layer. The retroreflective sheet of this embodiment may have a retroreflective layer, a printed layer, an adhesive layer, and a protective film in this order. The adjacent layer may be an adhesive layer. Each layer will be described below.

[0022] (Retroreflective layer) The retroreflective layer may be a sheet, film, or the like having a property of reflecting an obliquely incident light ray in a direction antiparallel or nearly antiparallel to the incident direction, thereby returning the incident light ray to the light source or its vicinity, i.e., having retroreflective properties. The retroreflective layer may be a bead-like or prism-like layer as is conventionally known.

[0023] As the retroreflective layer, many films that are commonly used for signage applications can be used. TM Diamond Grade TM DG 3 Examples include a printed prism sheet sold under the product name "Ultra-brightness reflective sheet wide-angle prism type (full cube)."

[0024] (Printing layer) The printed layer can be formed on the retroreflective layer by applying a colorant such as ink or toner to the retroreflective layer using a printing technique such as gravure printing, silk printing, offset printing, electrostatic printing, inkjet printing, thermal transfer printing, etc. Among these, inkjet printing is preferred because it allows on-demand printing, and inkjet printing using a UV inkjet printer is more preferred.

[0025] The print layer is preferably formed from an ultraviolet-curable ink. The ultraviolet-curable ink usually has a refractive index of 1.50 to 1.55 (particularly, 1.51 to 1.54). For example, an ultraviolet-curable ink is available from 3M Company under the name "3M TMIt is possible to use inks of various colors (Blue, Black, Red, Yellow, Magenta, Cyan) sold under the product name "Piezo Inkjet Series 8900UV Ink".

[0026] (Adjacent layer (adhesive layer)) The adjacent layer is formed so as to be in contact with the printed layer. The adjacent layer may be an adhesive layer having adhesive properties.

[0027] The refractive index of the adjacent layer is 1.50 to 1.55. This makes it possible to improve the retroreflectivity of the retroreflective sheeting even when the printed layer is formed by inkjet printing. The reason for this is not necessarily clear, but the present inventors speculate as follows.

[0028] In inkjet printing, printing is performed by directly spraying droplets of ink. Therefore, the printed layer formed by inkjet printing has unevenness on the surface due to the droplets. Here, if the difference in refractive index between the printed layer and the adjacent layer is relatively large, light scattering due to the unevenness occurs at the interface between these layers, and retroreflectivity decreases. On the other hand, by setting the refractive index of the adjacent layer to 1.50 to 1.55 and matching it with the refractive index of the ultraviolet-curable ink that constitutes the printed layer, it is possible to suppress light scattering due to the unevenness, and it is considered that retroreflectivity can be improved.

[0029] From the viewpoint of further improving retroreflectivity, the difference between the refractive index of the adjacent layer and the refractive index of the printed layer is preferably 3.5% or less, more preferably 3% or less, and even more preferably 2.5% or less. The difference between the refractive index of the adjacent layer and the refractive index of the printed layer is calculated by the following formula (1). |Refractive index of adjacent layer - refractive index of printed layer| / refractive index of adjacent layer x 100 (%) … (1)

[0030] Here, when the printed layer is formed of a single ink, it is preferable that the difference between the refractive index of the adjacent layer and the refractive index of the ink is within the above-mentioned predetermined range. On the other hand, when the printed layer is formed of multiple inks having different refractive indices, it is preferable that the difference between the refractive index of the adjacent layer and the refractive index of at least one ink is within the above-mentioned predetermined range, and it is more preferable that the difference between the refractive index of the adjacent layer and the refractive index of all inks is within the above-mentioned predetermined range.

[0031] The adjacent layer contains an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles. The acrylic resin is preferable in that inorganic nanoparticles can be dispersed in the resin and the refractive index can be adjusted. In addition, since the structural unit in the acrylic resin does not have a hydroxyl group, it is possible to suppress corrosion caused by the presence of a hydroxyl group and reaction with other materials. Furthermore, since the structural unit in the acrylic resin does not have an aromatic ring, the weather resistance of the retroreflective sheet is excellent.

[0032] An ethoxylated alkyl alcohol refers to an alcohol having a structure in which one or more ethylene oxides are added to an alkyl alcohol, i.e., an alcohol having one or more consecutive oxyethylene groups between the alkyl group and the hydroxyl group in the alkyl alcohol.

[0033] The alkyl group in the alkyl alcohol may be, for example, an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 5 carbon atoms, or a methyl group or an ethyl group.

[0034] Specific examples of the ester of (meth)acrylic acid and ethoxylated alkyl alcohol include methoxy(polyethylene glycol)(meth)acrylate, ethoxy(polyethylene glycol)(meth)acrylate, 2-(2-ethoxyethoxy)ethyl(meth)acrylate, ethylene glycol methyl ether(meth)acrylate, diethylene glycol methyl ether(meth)acrylate, triethylene glycol methyl ether(meth)acrylate, tetraethylene glycol methyl ether(meth)acrylate, ethylene glycol ethyl ether(meth)acrylate, diethylene glycol ethyl ether(meth)acrylate, triethylene glycol ethyl ether(meth)acrylate, tetraethylene glycol ethyl ether(meth)acrylate, and diethylene glycol-2-ethylhexyl ether(meth)acrylate. Among these, 2-(2-ethoxyethoxy)ethyl acrylate or poly(ethylene glycol) methyl ether acrylate is preferred. The molecular weight of the methoxy(polyethylene glycol)(meth)acrylate or ethoxy(polyethylene glycol)(meth)acrylate can be, for example, 300 to 1,000.

[0035] The acrylic resin may be composed only of a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, or may have other structural units as long as the effect of the invention is not impaired. Examples of monomers constituting other structural units include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, and n-decyl (meth)acrylate, as well as dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, tricyclo[5.2.1.0 2.6]Decanyl (meth)acrylate, glycidyl (meth)acrylate, and the like.

[0036] The acrylic resin can be obtained by polymerizing the ester of the (meth)acrylic acid and an ethoxylated alkyl alcohol using a normal radical polymerization method, for example, solution polymerization, suspension polymerization, emulsion polymerization, bulk polymerization, etc. As the polymerization initiator, an azo-based polymerization initiator such as benzoyl peroxide, lauroyl peroxide, bis(4-tert-butylcyclohexyl)peroxydicarbonate, or 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl-2,2-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), dimethyl 2,2'-azobis(2-methylpropionate), or 2,2'-azobis(2,4-dimethylvaleronitrile) (AVN) can be used.

[0037] Inorganic nanoparticles are defined as particles having an average particle size of at least about 1, 2, 3, 4, 5, 6, 7, 8, 9, or even 10 nm, or at most about 15, 20, 25, 30, 35, 40, 45, or even 50 nm, where the average particle size can be measured, for example, by dynamic light scattering. Inorganic nanoparticles can be discrete (i.e., non-aggregated) particles, aggregates of particles, or both.

[0038] Inorganic nanoparticles can include oxide nanoparticles, such as, for example, silicon dioxide (silica), zirconia, titania, ceria, alumina, iron oxide, zinc oxide, vanadia, antimony oxide, tin oxide, and alumina / silica.

[0039] Inorganic nanoparticles can be in the form of colloidal dispersion. Examples of useful commercially available inorganic nanoparticles include zirconia sol available under the trade name "Nanouse OZ" (Nissan Chemical Co., Ltd.), titania sol available under the trade name "Nanouse OT" (Nissan Chemical Co., Ltd.), colloidal silica available under the trade name "NALCO COLLOIDAL SILICAS" (Nalco Chemical Co.), etc.

[0040] The adjacent layer can be formed, for example, by the following method. An acrylic resin solution is prepared by polymerizing an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol by solution polymerization. Inorganic nanoparticles are added to the acrylic resin solution to prepare a coating solution. The coating solution is applied onto a substrate, and then heated and dried to form an adjacent layer. A protective film, which will be described later, can be used as the substrate.

[0041] The content of inorganic nanoparticles in the adjacent layer can be appropriately adjusted so that the refractive index of the adjacent layer is 1.50 to 1.55, but it is preferably, for example, 25 to 55 mass %, and more preferably 20 to 50 mass %, based on the entire adjacent layer.

[0042] (protective film layer) The protective film layer may be a film generally used for protecting optical materials. Examples of the material that may be used include acrylic resin, urethane resin, epoxy resin, polyvinyl chloride resin, polyester resin, fluororesin, and mixtures thereof. Among these, acrylic resin or a mixture of fluororesin and acrylic resin is preferred, and polymethylmethacrylate (PMMA) or a mixture of polyvinylidene fluoride (PVDF) and polymethylmethacrylate (PMMA) is more preferred.

[0043] Fig. 1 is a schematic cross-sectional view showing an example of a retroreflective sheet according to this embodiment. The retroreflective sheet 10 in Fig. 1 has a structure in which a retroreflective layer 1, a printed layer 3, an adhesive layer (adjacent layer) 5, and a protective film layer 7 are laminated in this order. The adhesive layer (adjacent layer) 5 is composed of an acrylic resin 5a and inorganic nanoparticles 5b. The laminate composed of the protective film layer (transparent substrate layer) 7 and the adhesive layer 5 corresponds to an overlaminate film 20 described later.

[0044] <How to make retroreflective sheeting> The method for producing the retroreflective sheet is not particularly limited, but can be produced, for example, by the following method. First, a print layer is formed on the retroreflective layer by inkjet printing. Separately, a pressure-sensitive adhesive layer containing the above-mentioned acrylic resin and inorganic nanoparticles is formed on a protective film. The retroreflective layer on which the print layer is formed and the protective film on which the pressure-sensitive adhesive layer is formed are bonded together so that the print layer and the pressure-sensitive adhesive layer are in contact with each other, thereby producing a retroreflective sheet.

[0045] <Adhesive composition> The adhesive composition of the present embodiment contains an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles. The refractive index of the acrylic resin used in adhesives is usually about 1.47, but according to the adhesive composition of the present embodiment, the refractive index of the entire adhesive composition can be adjusted by dispersing inorganic nanoparticles having a relatively high refractive index. In addition, since the structural unit in the acrylic resin does not have a hydroxyl group, it is possible to suppress corrosion caused by the presence of a hydroxyl group and reaction with other materials. Furthermore, since the structural unit in the acrylic resin does not have an aromatic ring, it has excellent weather resistance.

[0046] The content of inorganic nanoparticles in the pressure-sensitive adhesive composition can be adjusted appropriately depending on the required refractive index of the pressure-sensitive adhesive composition, and can be adjusted, for example, between 10 to 90 mass % or 20 to 80 mass % based on the entire pressure-sensitive adhesive composition.

[0047] <Overlaminate film> The overlaminate film of the present embodiment is an overlaminate film having a transparent substrate layer and an adhesive layer, and the adhesive layer contains an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles. Such an overlaminate film can be suitably applied to the surface protection of optical materials, and further, since the above-mentioned adhesive composition is used, it is excellent in that the refractive index can be adjusted.

[0048] In addition, for the pressure-sensitive adhesive composition and the overlaminate film, the acrylic resin and inorganic nanoparticles can be the same as those described in the adjacent layer. In addition, for the transparent substrate layer, the same as the protective film can be used. In addition, "transparent" means that the average transmittance of visible light, i.e., the wavelength range of 380 nm to 780 nm, is about 60% or more, preferably about 80% or more, more preferably about 90% or more.

[0049] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments.

[0050] The present invention may, for example, relate to the following aspects. [A1] A retroreflective sheet having multiple layers, The printing layer has at least a printing layer and an adjacent layer in contact with the printing layer, the adjacent layer contains an acrylic resin having structural units derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol and inorganic nanoparticles; A retroreflective sheeting in which the refractive index of adjacent layers is 1.50 to 1.55. [A2] The retroreflective sheet according to [A1], in which the adjacent layer is a pressure-sensitive adhesive layer, and which has a retroreflective layer, a printed layer, a pressure-sensitive adhesive layer, and a protective film layer in this order. [A3] The retroreflective sheeting according to [A1] or [A2], wherein the ester of (meth)acrylic acid and an ethoxylated alkyl alcohol is 2-(2-ethoxyethoxy)ethyl acrylate or poly(ethylene glycol) methyl ether acrylate. [A4] The retroreflective sheeting according to any one of [A1] to [A3], wherein the inorganic nanoparticles are zirconia particles. [A5] The retroreflective sheet according to any one of [A1] to [A4], wherein the printed layer is a printed layer formed by inkjet printing. [A6] The retroreflective sheet according to [A5], wherein the inkjet printing is performed using a UV inkjet printer. [A7] The retroreflective sheet according to any one of [A1] to [A6], wherein the printed layer is formed from an ultraviolet-curable ink. [B1] A pressure-sensitive adhesive composition comprising an acrylic resin having structural units derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles. [B2] The pressure-sensitive adhesive composition according to [B1], wherein the ester of (meth)acrylic acid and an ethoxylated alkyl alcohol is 2-(2-ethoxyethoxy)ethyl acrylate or poly(ethylene glycol) methyl ether acrylate. [B3] The pressure-sensitive adhesive composition according to [B1] or [B2], wherein the inorganic nanoparticles are zirconia particles. [C1] An overlaminate film having a transparent substrate layer and a pressure-sensitive adhesive layer, An overlaminate film, the adhesive layer of which contains an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles. [C2] The overlaminate film according to [C1], wherein the ester of (meth)acrylic acid and an ethoxylated alkyl alcohol is 2-(2-ethoxyethoxy)ethyl acrylate or poly(ethylene glycol) methyl ether acrylate. [C3] The overlaminate film according to [C1] or [C2], wherein the inorganic nanoparticles are zirconia particles. EXAMPLES

[0051] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples. The abbreviations, compound names, product names, and sources of materials used in the examples and comparative examples are as follows. EEEA: 2-(2-ethoxyethoxy)ethyl acrylate (ethyl carbitol acrylate) (product name: Viscoat #190, manufactured by Osaka Organic Chemical Industry Co., Ltd.) PEGME: Poly(ethylene glycol) methyl ether acrylate (methoxypolyethylene glycol acrylate) (molecular weight: 620 g / mol, product name: MPE550A, manufactured by Osaka Organic Chemical Industry Co., Ltd.) AVN: 2,2'-azobis(2,4-dimethylvaleronitrile) (product name: V-65, Fujifilm Wako Pure Chemical Industries, Ltd.) Nanoparticle dispersion: Zirconia nanoparticle dispersion (particle refractive index: 1.85 to 1.90, dispersion medium: methyl ethyl ketone, particle size: 10 to 30 nm (dispersed particle size by dynamic light scattering method), product name: Nanouse OZ-S40K-AC, manufactured by Nissan Chemical) MEK: Methyl ethyl ketone (manufactured by Yamaichi Chemical Industry Co., Ltd.) Ethyl acetate: Ethyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd.)

[0052] <Preparation of (meth)acrylic polymer solution A1> 100 parts by mass of 2-(2-ethoxyethoxy)ethyl acrylate (EEEA) was dissolved in 45 parts by mass of methyl ethyl ketone (MEK) and 103 parts by mass of ethyl acetate, and 0.4 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) (AVN) was added as a polymerization initiator. The mixture was allowed to react at 50°C for 24 hours under a nitrogen atmosphere to prepare a (meth)acrylic polymer solution A1.

[0053] <Preparation of (meth)acrylic polymer solution A2> A (meth)acrylic polymer solution was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A1. A nanoparticle dispersion (Nissan Chemical's Nanouse OZ-S40K-AC, solid content 40% by mass) was added to the obtained (meth)acrylic polymer solution, and the mixture was mixed and stirred so that the inorganic component content was 10% by mass, to prepare a (meth)acrylic polymer solution A2.

[0054] <Preparation of (meth)acrylic polymer solution A3> A (meth)acrylic polymer solution A3 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A2, except that the inorganic component content was adjusted to 30 mass %.

[0055] <Preparation of (meth)acrylic polymer solution A4> A (meth)acrylic polymer solution A4 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A2, except that the inorganic component content was adjusted to 50 mass %.

[0056] <Preparation of (meth)acrylic polymer solution A5> A (meth)acrylic polymer solution A5 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A2, except that the inorganic component content was adjusted to 70 mass %.

[0057] <Preparation of (meth)acrylic polymer solution B1> 100 parts by mass of poly(ethylene glycol) methyl ether acrylate (PEGME) was dissolved in 45 parts by mass of methyl ethyl ketone (MEK) and 103 parts by mass of ethyl acetate, and 0.4 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) (AVN) was added as a polymerization initiator. The mixture was then reacted at 50°C for 24 hours under a nitrogen atmosphere to prepare (meth)acrylic polymer solution B1.

[0058] <Preparation of (meth)acrylic polymer solution B2> A (meth)acrylic polymer solution was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution B1. A nanoparticle dispersion (Nissan Chemical's Nanouse OZ-S40K-AC, solid content 40% by mass) was added to the obtained (meth)acrylic polymer solution, and the mixture was mixed and stirred so that the inorganic component content was 30% by mass, to prepare a (meth)acrylic polymer solution B2.

[0059] <Preparation of (meth)acrylic polymer solution B3> A (meth)acrylic polymer solution B3 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution B2, except that the inorganic component content was adjusted to 50 mass %.

[0060] <Preparation of (meth)acrylic polymer solution C1> 50 parts by mass of 2-ethylhexyl acrylate (2EHA) manufactured by Osaka Organic Chemical Industry Co., Ltd. and 50 parts by mass of butyl acrylate (BA) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. were dissolved in 45 parts by mass of methyl ethyl ketone (MEK) and 103 parts by mass of ethyl acetate, and 0.4 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) (AVN) was added as a polymerization initiator, and the mixture was reacted at 50°C for 24 hours under a nitrogen atmosphere to prepare a (meth)acrylic polymer solution. A nanoparticle dispersion (Nissan Chemical, Nanouse OZ-S40K-AC, solid content 40% by mass) was added to the obtained (meth)acrylic polymer solution, and the mixture was mixed and stirred so that the inorganic component content was 10% by mass, to prepare a (meth)acrylic polymer solution C1. The obtained (meth)acrylic polymer solution C1 became cloudy and precipitates were generated, so further investigation was not performed.

[0061] <Preparation of (meth)acrylic polymer solution C2> 90 parts by mass of 2-ethylhexyl acrylate (2EHA) manufactured by Osaka Organic Chemical Industry Co., Ltd. and 10 parts by mass of acrylic acid (AA) manufactured by Nippon Shokubai Co., Ltd. were dissolved in 45 parts by mass of methyl ethyl ketone (MEK) and 103 parts by mass of ethyl acetate, and 0.4 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) (AVN) was added as a polymerization initiator, and the mixture was reacted at 50°C for 24 hours under a nitrogen atmosphere to prepare a (meth)acrylic polymer solution. A nanoparticle dispersion (Nissan Chemical, Nanouse OZ-S40K-AC, solid content 40% by mass) was added to the obtained (meth)acrylic polymer solution, and the mixture was mixed and stirred so that the inorganic component content was 10% by mass, to prepare a (meth)acrylic polymer solution C2. The obtained (meth)acrylic polymer solution C2 became cloudy and precipitates were generated, so further investigation was not performed.

[0062] <Preparation of retroreflective sheet A1> The (meth)acrylic polymer solution A1 was applied to a 75 μm-thick polymethyl methacrylate (PMMA) film using a knife coater so that the thickness after drying would be 40 μm. After drying at 65° C. for 2 minutes and at 95° C. for 3 minutes, a PMMA overlaminate film with a (meth)acrylic adhesive was obtained. Printed prism sheet (3M TM Diamond Grade TM DG 3 A solid print was performed on the surface of a UV inkjet printer sold by MIMAKI ENGINEERING under the name "UJF-3042FX UV PRINTER" using ink sold by MIMAKI ENGINEERING under the name "LUS-200" (ink colors: yellow, white, magenta, cyan, black). The printer settings were resolution [720 x 600VD], other conditions [Pass8, Overprint 1 times], and print color setting [M100]. The resulting ink-attached printed prism sheet and the above-mentioned overlaminate film were attached to each other with a hand squeeze roller so that the printed layer and the adhesive layer of each were in contact with each other, to obtain retroreflective sheeting A1. The refractive index of the ink in the printed layer printed with the print color setting [M100] is 1.543.

[0063] <Production of retroreflective sheets A2 to A5 and B1 to B3> Retroreflective sheets A2 to A5 and B1 to B3 were obtained in the same manner as in the production of the retroreflective sheet A1, except that (meth)acrylic polymer solutions A2 to A5 and B1 to B3 were used instead of the (meth)acrylic polymer solution A1.

[0064] <Preparation of retroreflective sheet C3> As a PMMA overlaminate film with (meth)acrylic adhesive, 3M's "3M TM Electrocut TM A retroreflective sheet C3 was obtained in the same manner as in the production of the retroreflective sheet A1, except that the film ECF1170C was used.

[0065] (Evaluation of retroreflective sheeting) The retroreflective coefficient, the refractive index of the adhesive layer, and the inorganic component content of the retroreflective sheets A1 to A5, B1 to B2, and C3 obtained above were measured by the following methods. The results are shown in Table 1.

[0066] <Measurement of the retroreflection coefficient> Retroreflection coefficient (cd / lx / m 2 ) was obtained by measuring the retroreflection coefficient at an observation angle of 0.2 degrees and an incident angle of 5 degrees, i.e., 0.2° / 5°, using a retroreflection measuring device RetroSign GRX (manufactured by DELTA). Specifically, the measurement was performed by placing the handle of the measuring device parallel and perpendicular to the sheet winding direction. Measurements were performed at three appropriate points on the produced reflective sheet, and the average of the parallel and perpendicular measured values ​​was taken as the retroreflection coefficient of the reflective sheet.

[0067] <Refractive index measurement> The refractive index of the printed layer or the pressure-sensitive adhesive layer was measured for light having a wavelength of 633 nm at room temperature using a Metricon Model 2010 Prism Coupler (manufactured by Metricon).

[0068] <Measurement of inorganic component content> The obtained adhesive was heated for 10 minutes at 600° C. under air supply. The residue after heating was regarded as an inorganic component, and the inorganic component content was determined by subtracting the weight of the adhesive at the initial room temperature from the weight of the residue.

[0069] [Table 1]

[0070] <Preparation of (meth)acrylic polymer solution A6> 100 parts by mass of 2-(2-ethoxyethoxy)ethyl acrylate (EEEA) was dissolved in 45 parts by mass of methyl ethyl ketone (MEK) and 103 parts by mass of ethyl acetate, and 0.4 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) (AVN) was added as a polymerization initiator. The mixture was allowed to react at 50°C for 24 hours under a nitrogen atmosphere to prepare (meth)acrylic polymer solution A6.

[0071] <Preparation of (meth)acrylic polymer solution A7> A (meth)acrylic polymer solution was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A6. A nanoparticle dispersion (Nissan Chemical's Nanouse OZ-S40K-AC, solid content 40% by mass) was added to the obtained (meth)acrylic polymer solution, and the mixture was mixed and stirred so that the inorganic component content was 20% by mass, to prepare a (meth)acrylic polymer solution A7.

[0072] <Preparation of (meth)acrylic polymer solution A8> A (meth)acrylic polymer solution A8 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A6, except that the inorganic component content was adjusted to 30 mass %.

[0073] <Preparation of (meth)acrylic polymer solution A9> A (meth)acrylic polymer solution A9 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A6, except that the inorganic component content was adjusted to 40 mass %.

[0074] <Preparation of (meth)acrylic polymer solution A10> A (meth)acrylic polymer solution A10 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A6, except that the inorganic component content was adjusted to 50 mass %.

[0075] <Preparation of (meth)acrylic polymer solution A11> A (meth)acrylic polymer solution A11 was prepared in the same manner as in the preparation of the (meth)acrylic polymer solution A6, except that the inorganic component content was adjusted to 60 mass %.

[0076] <Production of retroreflective sheet A6> The (meth)acrylic polymer solution A6 was applied to a 75 μm-thick polymethyl methacrylate (PMMA) film using a knife coater so that the thickness after drying would be 40 μm. After drying at 65° C. for 2 minutes and at 95° C. for 3 minutes, a PMMA overlaminate film with a (meth)acrylic adhesive was obtained. Printed prism sheet (3M TM Diamond Grade TM DG 3 A solid print was made on the surface of a sheet of ultra-high brightness reflective sheeting (manufactured and sold under the product name "Ultra-brightness reflective sheeting wide-angle prism type (full cube) DG4090") using a UV inkjet printer sold by Durst under the product name "Rho 163 TS". The printer settings were resolution [600 x 600 dpi], other conditions [Pass 2], print color settings [M100, Y100, and traffic colors (Red, Yellow, Brown, Purple)]. The ink used for printing was 3M TMPiezo Inkjet Series 8900UV Ink (ink colors: Blue, Black, Red, Yellow, Magenta, Cyan) was used. The resulting ink-attached printed prism sheet and the above-mentioned overlaminate film were attached together with a hand squeeze roller so that the printed layer and the adhesive layer of each were in contact with each other, to obtain retroreflective sheeting A6. The refractive indices of red and yellow output by the traffic color setting of the UV inkjet printer are 1.519 and 1.532, respectively.

[0077] <Production of retroreflective sheets A7 to A11> Retroreflective sheets A7 to A11 were obtained in the same manner as in the production of the retroreflective sheet A6, except that the (meth)acrylic polymer solutions A7 to A11 were used instead of the (meth)acrylic polymer solution A6.

[0078] <Production of retroreflective sheet C4> As a PMMA overlaminate film with (meth)acrylic adhesive, 3M's "3M TM Electrocut TM A retroreflective sheet C4 was obtained in the same manner as in the production of the retroreflective sheet A6, except that the film ECF1170C was used.

[0079] (Evaluation of retroreflective sheeting) The retroreflective coefficient, the refractive index of the adhesive layer, and the inorganic component content of the retroreflective sheets A6 to A11 and C4 obtained above were measured by the methods described above. The results are shown in Table 2.

[0080] [Table 2]

[0081] (Weather resistance test) The retroreflective sheets A1 and A3 were subjected to a weather resistance test using JIS Z 9117:2011_8.5.1 Sunshine carbon arc lamp accelerated weather resistance test (SWOM). The results are shown in Table 3. If ΔE is 5 or less, yellowing is sufficiently suppressed and the sheet is evaluated as having excellent weather resistance.

[0082] [Table 3] [Explanation of symbols]

[0083] Reference Signs List: 1... retroreflective layer, 3... printed layer, 5... adhesive layer (adjacent layer), 5a... acrylic resin, 5b... inorganic nanoparticles, 7... protective film layer (transparent substrate layer), 10... retroreflective sheet, 20... overlaminate film.

Claims

1. A retroreflective sheet having multiple layers, The printing layer has at least a printing layer and an adjacent layer in contact with the printing layer, the adjacent layer contains an acrylic resin having structural units derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol and inorganic nanoparticles; A retroreflective sheeting in which the refractive index of adjacent layers is 1.50 to 1.

55.

2. 2. The retroreflective sheet according to claim 1, wherein the adjacent layer is a pressure-sensitive adhesive layer, and the retroreflective sheet has a retroreflective layer, a printed layer, a pressure-sensitive adhesive layer, and a protective film layer in this order.

3. 3. The retroreflective sheeting according to claim 1, wherein the ester of (meth)acrylic acid and an ethoxylated alkyl alcohol is 2-(2-ethoxyethoxy)ethyl acrylate or poly(ethylene glycol) methyl ether acrylate.

4. The retroreflective sheeting according to claim 1 or 2, wherein the inorganic nanoparticles are zirconia particles.

5. A pressure-sensitive adhesive composition comprising an acrylic resin having structural units derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles.

6. An overlaminate film having a transparent substrate layer and a pressure-sensitive adhesive layer, An overlaminate film, the adhesive layer of which contains an acrylic resin having a structural unit derived from an ester of (meth)acrylic acid and an ethoxylated alkyl alcohol, and inorganic nanoparticles.

Citation Information

Patent Citations

  • Method for manufacturing marked reflective sheet

    WO2013145946A1