Paste composition for gas sealing, electrochemical module, and energy system
The gas sealing paste composition addresses issues of solvent recovery and void formation in SOFC and SOEC by using water-based, dispersible glass powder with vinyl polymer and polysaccharide, achieving high sealing performance and durability.
Patent Information
- Application Number
- JP2023053695
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing gas sealing compositions for solid oxide fuel cells (SOFC) and solid oxide electrolytic cells (SOEC) face issues such as increased manufacturing steps, yield reduction due to solvent recovery, void formation leading to gas leaks, and performance deterioration from volatilization of elements like silicon and phosphorus.
A gas sealing paste composition using water as a solvent, comprising glass powder, a vinyl polymer with a polyether structure, and a polysaccharide, with specific concentration ranges to ensure dispersibility, fluidity, and thermal stability, eliminating the need for solvent recovery equipment and preventing volatilization of inorganic binder elements.
The composition provides high gas sealing performance, reduces manufacturing complexity, and enhances durability by preventing voids and peeling, ensuring effective sealing even at high temperatures.
Smart Images

Figure 2024141847000002 
Figure 2024141847000003 
Figure 2024141847000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a paste composition for gas sealing, and an electrochemical module and an energy system including the paste composition for gas sealing. [Background technology]
[0002] In order to achieve the Sustainable Development Goals (SDG's), various energy devices are being developed. Among them, solid oxide fuel cells (SOFCs) are attracting attention because they can generate electricity using hydrogen and air as feed gases, and the generated heat can be used for heating and hot water in homes, making high-efficiency use of feed gases. In addition, energy devices that generate hydrogen from water vapor using solid oxide electrolysis cells (SOECs) are also attracting attention in order to build a hydrogen energy society.
[0003] These energy devices use materials such as metals and ceramics, but because they are exposed to high temperatures, each material expands according to its thermal expansion coefficient. In addition, the bonding material for bonding these materials together and preventing gas leakage also expands at high temperatures, so if the difference in thermal expansion coefficient between the bonding material and materials such as metals is large, there is a risk of gas leakage from the gas raw material due to peeling of the bonding material. Therefore, it is preferable to select materials so that the difference in thermal expansion coefficient between the bonding material and materials such as metals is as small as possible. In addition, the temperature range (operating temperature range) in which electrochemical reactions occur in SOFCs and SOECs is as high as 600 to 1000°C, and they are operated for a long period of time in this temperature range, so there is a possibility that the above-mentioned gas leakage may occur.
[0004] Conventionally, to prevent gas leakage, O-rings and other components made of elastomers have been mainly used, but when used at high temperatures, problems such as deformation and deterioration can occur. For this reason, various joining materials have been developed to prevent gas leakage in these energy devices.
[0005] For example, materials such as glass and mica have high melting points and are therefore unlikely to cause problems such as deformation or melting even at high temperatures. For this reason, gas leakage can be prevented by molding and using a sealing material made of glass, or by applying and baking a paste-like composition containing glass or mica to areas where gas leakage is likely to occur.
[0006] Patent Document 1 discloses a crystallizable glass composition containing SiO2 as a main component, an alkali metal, an alkaline earth metal, an oxide of zinc, and alumina. It describes that, in particular, when the molar ratio of zinc oxide to barium oxide is 1.9 to 10, it has an appropriate thermal expansion coefficient and can be suitably used as an adhesive material for metals such as SUS and Fe, and high-expansion ceramics such as ferrite and zirconia.
[0007] Patent Document 2 discloses a sealing material for solid oxide fuel cells, which is made of a mixed powder of glass powder containing silicon as a constituent element, magnesium oxide powder, and magnesium silicate powder. This sealing material is produced by mixing the mixed powder with an organic solvent such as turpentine oil and an organic dispersion material made of esters such as butyl acid ester to form a paste. It is described that by applying this paste between the single cells of an SOFC constructed by stacking multiple single cells and then firing it, gas leakage from the air intake path and exhaust path of the single cells can be prevented.
[0008] Patent Document 3 discloses a glass coating composition for fuel cell gaskets, which contains a glass component and a binder component effective for forming an alkaline solution in the presence of the same amount of water by weight, and in which the amount of water as a liquid carrier exceeds 50% by volume. This composition further contains a retarder effective for inhibiting hardening, so that the composition does not substantially harden even when stored for a long period of time and remains stable, and can be applied by either brush coating or spray coating, making it easy to handle. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2020-083662 A [Patent Document 2] JP 2007-149430 A [Patent Document 3] Patent No. 7136853 Summary of the Invention [Problem to be solved by the invention]
[0010] However, the inventions described in Patent Documents 1 and 2 use an organic solvent as the solvent for the composition. Therefore, when used as a gas sealing paste composition for SOFC or SOEC, local ventilation or a solvent recovery device is required when applying to these energy devices and drying. Therefore, there is a risk that the number of steps in the production of these energy devices will increase and the yield will decrease. The sealant for solid oxide fuel cells described in Patent Document 2 contains inorganic binders such as alumina, magnesium oxide, etc. Therefore, after the sealant is applied and fired, silicon, phosphorus, boron, etc. volatilize and accumulate in the seal portion and gas flow path, which may deteriorate the performance of the solid oxide fuel cell. The invention described in Patent Document 3 uses water as a solvent, but the water content in the composition is as high as 50% by volume, so that voids tend to form when the water evaporates after coating. Therefore, gas leaks tend to occur through the voids, and it is difficult to say that the invention is practical in terms of gas sealing properties.
[0011] Therefore, an object of the present invention is to provide a paste composition for sealing that has appropriate dispersibility and fluidity and exhibits high gas sealing properties after curing. [Means for solving the problem]
[0012] The characteristic configuration of the paste composition for sealing according to the present invention for achieving the above object is as follows: A paste composition for gas sealing containing water as a solvent, The composition comprises glass powder, a vinyl polymer having a polyether structure in the side chain, and a polysaccharide, The solid content is 73% by mass or more and 90% by mass or less, The combined content of the vinyl polymer and the polysaccharide is 0.50 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the glass powder.
[0013] According to this characteristic configuration, the glass powder particles are bonded to the vinyl polymer that functions as a dispersant, thereby increasing the dispersibility in the solvent. Furthermore, since the vinyl polymer has a polyether structure with bulky side chains, the glass particles bonded to the vinyl polymer are three-dimensionally repelled, thereby further increasing the dispersibility. As a result, even if the solid content concentration is high (73% by mass or more and 90% by mass or less), it is possible to provide an appropriate viscosity (fluidity) and form a paste. If the solid content concentration is less than 73% by mass, there will be many voids in the glass seal structure after the paste composition dries, and there is a risk of the sealability being reduced, and if the solid content concentration is more than 90% by mass, there is a risk of the dispersibility and fluidity of the glass powder in the paste composition being easily reduced, and the coatability being reduced.
[0014] Furthermore, by including a polysaccharide, the dispersion stability of the glass powder particles in the paste composition is improved, sedimentation can be suppressed (dispersibility can be increased), and good coatability can be obtained.
[0015] Furthermore, by setting the total content of the vinyl polymer and the polysaccharide to 0.50 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the glass powder, it is possible to impart an appropriate viscosity (fluidity) to the paste composition, improve the applicability, and improve the sealability. If the total content is less than 0.50 parts by mass, the dispersibility and fluidity of the glass powder in the paste composition are likely to decrease, and there is a risk of the applicability decreasing, whereas if it is more than 3.0 parts by mass, there is a risk of the glass seal structure having many voids when exposed to a high-temperature environment, and the sealability decreasing.
[0016] In addition, in the paste composition for sealing according to the present characteristic configuration, the solvent is water. Therefore, since it does not contain an organic solvent, solvent recovery equipment and ventilation equipment are not required when drying the paste composition. In addition, explosion-proof specifications are not required for each equipment, which is advantageous in terms of cost and productivity. In addition, the paste composition for gas sealing according to the present characteristic configuration does not contain an inorganic binder, and therefore, even when exposed to a high-temperature environment, it is possible to eliminate the possibility of volatilization and deposition of elements such as silicon and phosphorus derived from inorganic binders (silicic acid compounds, aluminum phosphate, etc.).
[0017] A further characteristic feature of the paste composition for sealing according to the present invention is that the main chain of the vinyl polymer has at least one unit selected from the group consisting of maleic anhydride units, maleic acid units and maleate units.
[0018] According to this characteristic configuration, the main chain has a structure that easily bonds with the glass powder particles, thereby improving the affinity between the glass powder particles and the vinyl polymer, thereby improving the dispersibility of the glass powder particles in the paste composition.
[0019] A further characteristic feature of the paste composition for sealing according to the present invention is that the content of the vinyl polymer is 0.10 parts by mass or more and 1.5 parts by mass or less based on 100 parts by mass of the glass powder.
[0020] According to this characteristic configuration, the vinyl polymer is added in an amount of 0.10 parts by mass to 1.5 parts by mass based on 100 parts by mass of the glass powder, thereby improving the dispersibility and fluidity of the glass powder particles, and reducing the number of voids that occur in the glass seal structure when exposed to a high-temperature environment, thereby preventing a decrease in sealing performance. If the content of the vinyl polymer is less than 0.10 parts by mass, the fluidity may be poor and the coatability may be impaired, whereas if the content is more than 1.5 parts by mass, the voids in the gas seal part may become large when exposed to a high temperature, causing a decrease in gas sealing performance.
[0021] A further characteristic feature of the paste composition for sealing according to the present invention is that the content of the polysaccharide is 0.40 parts by mass or more and 1.5 parts by mass or less based on 100 parts by mass of the glass powder.
[0022] According to this characteristic configuration, the paste composition for gas sealing can have an appropriate viscosity, the dispersion stability of the glass powder particles in the paste composition can be improved, sedimentation can be suppressed (dispersibility can be increased), and good applicability can be obtained. If the content of the polysaccharide is less than 0.40 parts by mass, the viscosity is low, the dispersion stability of the glass powder particles in the paste composition is reduced, sedimentation (reduced dispersibility) is likely to occur, and the applicability may be reduced, whereas if the content is more than 1.5 parts by mass, there are many voids in the glass seal structure when exposed to a high-temperature environment, and the sealability may be reduced.
[0023] A further characteristic feature of the paste composition for gas sealing according to the present invention is that the polysaccharide is one or more of methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxybutyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose or a salt thereof, aminomethyl hydroxypropyl cellulose, aminoethyl hydroxypropyl cellulose, starch, tragacanth, pectin, glue, alginic acid or a salt thereof, carrageenan, xanthan gum, sodium hyaluronate, locust bean gum, tara gum, guar gum, and tamarind seed gum.
[0024] According to this characteristic configuration, the paste composition for sealing can have an appropriate viscosity and can be easily applied.
[0025] A further characteristic feature of the paste composition for sealing according to the present invention is that the glass powder is crystallized glass, and the thermal expansion coefficient of the glass powder is 8.0 ppm / K or more and 13 ppm / K or less.
[0026] According to this characteristic configuration, the paste composition for gas sealing is unlikely to expand and change in volume even in a high-temperature environment, and the occurrence of gas leakage can be suppressed. In addition, by setting the thermal expansion coefficient of the glass powder to 8.0 ppm / K or more and 13 ppm / K or less, the thermal expansion coefficient can be made similar to that of a metal member used in, for example, a solid oxide fuel cell (SOFC) or a solid oxide electrolysis cell (SOEC), and it is possible to prevent a large force from being applied to the paste composition for sealing due to the thermal expansion of the metal member, thereby preventing the paste composition for sealing from peeling off and suppressing the occurrence of gas leakage.
[0027] The electrochemical module according to the present invention for achieving the above object has the following characteristic configuration: A plurality of electrochemical elements each including an electrolyte layer and a first electrode and a second electrode disposed on either side of the electrolyte layer are stacked with metal substrates interposed between the electrochemical elements, and the above-mentioned paste composition for sealing is disposed between adjacent metal substrates.
[0028] According to this characteristic configuration, the gas sealing paste composition is disposed between adjacent metal members in the electrochemical module. Therefore, when the gas sealing paste composition is applied, the glass powder particles are well dispersed and the composition can be easily applied to the parts of the metal substrate that need to be joined (sealed). After the gas sealing paste composition is applied and then dried and fired, the fired body of the gas sealing paste composition can well seal (join) the metal substrates with high sealing properties. This makes it possible to well prevent the peeling of the fired body of the gas sealing paste composition even when exposed to a high-temperature environment, and well prevent the occurrence of gas leaks from the parts sealed (joined) by the fired body.
[0029] The electrochemical module according to the present invention for achieving the above object has the following characteristic configuration: A plurality of electrochemical elements, each of which has an electrolyte layer and a first electrode and a second electrode disposed on either side of the electrolyte layer, are stacked with metal substrates interposed between the electrochemical elements, annular sealing members having through holes are disposed between adjacent metal substrates, and the above-mentioned paste composition for sealing gas is disposed on at least a portion of the surface of the annular sealing member.
[0030] According to this characteristic configuration, an annular sealing member having a through hole is disposed between adjacent metal members in an electrochemical module, and a gas sealing paste composition is disposed on at least a part of the surface of the annular sealing member. Therefore, when the gas sealing paste composition is applied, the glass powder particles are well dispersed and the composition can be easily applied to the portion (at least a part of the surface of the annular sealing member) where bonding (sealing) is required between the metal substrate and the annular sealing member. After the gas sealing paste composition is applied and then dried and fired, the fired body of the gas sealing paste composition can well seal (bond) between the metal substrate and the annular sealing member in a state of high sealing performance. This makes it possible to well prevent the peeling of the fired body of the gas sealing paste composition even when exposed to a high-temperature environment, and well prevent the occurrence of gas leakage from the portion sealed (bonded) by the fired body.
[0031] A characteristic configuration of the energy system of the present invention for achieving the above-mentioned object is that it comprises an electrochemical device having the electrochemical module, a fuel converter that generates reducing components to be supplied to the electrochemical module or converts gas containing the reducing components generated in the electrochemical module, and a power converter that extracts electric power from the electrochemical module or distributes electric power to the electrochemical module, and is further comprises an exhaust heat utilization section that reuses heat discharged from the electrochemical device.
[0032] According to the above characteristic configuration, it is possible to realize an energy system that suppresses the occurrence of gas leaks and has excellent energy efficiency. [Brief description of the drawings]
[0033] [Figure 1] FIG. 1 is a schematic diagram of a solid oxide fuel cell including a fired body of a sealing paste composition according to an embodiment. [Diagram 2] FIG. 2 is an enlarged view of a region including a fired body of a sealing paste composition according to an embodiment. [Diagram 3] FIG. 1 is a schematic diagram of an energy system including a solid oxide fuel cell including a fired body of a paste composition for gas sealing according to an embodiment. [Figure 4] FIG. 1 is a schematic diagram of another energy system including a solid oxide electrolysis cell including a fired body of a sealing paste composition according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The paste composition 1 for gas sealing of the present invention (hereinafter sometimes abbreviated as paste composition 1) contains water as a solvent and glass powder, vinyl polymer, and polysaccharide as constituents.
[0035] <Glass powder> The glass powder is produced by pulverizing the bulk of raw glass. The paste composition 1 of the present invention is intended to be used in energy devices used at high temperatures, such as solid oxide fuel cells (SOFCs) and solid oxide electrolysis cells (SOECs), and therefore the raw glass is preferably crystallized glass. By using crystallized glass, the fired body of the paste composition 1 becomes physically strong and can be made more durable. As such raw glass, glass containing oxides of boron and barium as components, which is suitable for glass solder, is preferably used. Note that crystallized glass refers to a glass composition that has the property of precipitating crystals when heat-treated.
[0036] Such glass powder may expand in the temperature range of the energy device used. Therefore, cracks may occur at the location where gas is sealed with a paste containing glass powder, and gas may leak from the location. Therefore, it is preferable to use glass that is thermally stable and chemically resistant, easy to process, and has a thermal expansion coefficient that will not break even if it expands in the temperature range of the energy device used. As such glass, it is preferable to use glass that has a thermal expansion coefficient of 8.0 ppm / K to 13.0 ppm / K at a temperature of 20°C to 300°C, more preferably 8.5 ppm / K to 12.5 ppm / K, and even more preferably 9.0 ppm / K to 12.0 ppm / K. When the thermal expansion coefficient of the raw glass is within the above range, the paste composition 1 is unlikely to expand and change in volume even in a high-temperature environment, and the occurrence of gas leakage can be suppressed. In addition, for example, the thermal expansion coefficient can be made similar to that of a metal member used in an energy device, and the application of a large force to the paste composition 1 due to the thermal expansion of the metal member can be suppressed. This can prevent the paste composition 1 from peeling off, and suppress the occurrence of gas leakage. If the thermal expansion coefficient of the raw glass is less than 8.0 ppm / K, metal members are often used at the sealing portion, and when the paste composition 1 is applied to the sealing portion and fired, it cannot follow the thermal expansion of the metal members, and there is a risk that the fired paste composition 1 will be damaged. If the thermal expansion coefficient of the raw glass is more than 13.0 ppm / K, when the paste composition 1 is applied to the sealing portion and fired, it may be deformed too much due to temperature changes, and gas sealing may not be possible.
[0037] <Vinyl polymer> The vinyl polymer improves the dispersibility of the glass powder particles in the paste composition 1. Examples of the vinyl polymer include those that adhere to the surfaces of the glass powder particles and maintain dispersibility by generating electrical repulsion between the glass powder particles due to the ionic nature of the vinyl polymer, and those that prevent the glass powder particles from approaching each other less than a certain distance due to steric hindrance of the side chains bonded to the main chain. Vinyl polymers have a vinyl group as a repeating unit constituting the main chain and a polyether structure in the side chain. The main chain of the vinyl polymer preferably has an ionic group. With this configuration, the ionic group functions as an adsorption group to the particle surface of the glass powder, and an electric repulsive force acts between the particles of the glass powder, so that even if the proportion of solids other than the solvent in the paste composition 1 (mainly glass powder, but also including vinyl polymers and polysaccharides) is relatively high (i.e., even if the solid concentration is high), it is possible to make it into a paste, and the applicability can be improved. In this embodiment, the main chain of the vinyl polymer has one or more units of maleic anhydride units, maleic acid units, or maleate units. The side chain of the vinyl polymer is a relatively long carbon chain such as a long-chain alkyl. With such a structure, the glass powder particles can be appropriately dispersed in the paste composition 1 due to the steric repulsion effect of the side chain. In this embodiment, a vinyl polymer having a polyether structure in the side chain is preferably used. In this embodiment, the polyether structure in the side chain has a polyoxyalkylene group, which is a derivative of alkylene oxide.
[0038] The content of the vinyl polymer in the paste composition 1 of this embodiment is 0.10 parts by mass or more and 1.5 parts by mass or less, more preferably 0.20 parts by mass or more and 1.2 parts by mass or less, and even more preferably 0.30 parts by mass or more and 1.0 parts by mass or less, based on 100 parts by mass of the glass powder. This makes it possible to increase the dispersibility and fluidity of the glass powder particles in the paste composition 1, and also to reduce the number of voids that occur in the glass seal structure when exposed to a high-temperature environment, thereby preventing a decrease in sealing performance. If the content of the vinyl polymer is less than 0.10 parts by mass, the fluidity may be poor and the coating properties may be impaired, and if it is more than 1.5 parts by mass, the voids in the gas seal part may become large when exposed to a high temperature, and the gas sealability may be reduced.
[0039] <Polysaccharide> The paste composition 1 contains a polysaccharide. This composition improves the dispersion stability of the glass powder particles in the paste composition, suppresses sedimentation (increases dispersibility), and provides good applicability. Examples of polysaccharides include methylcellulose, ethylcellulose, hydroxymethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, hydroxybutylmethylcellulose, hydroxyethylcellulose, carboxymethylcellulose or a salt thereof, aminomethylhydroxypropylcellulose, aminoethylhydroxypropylcellulose, starch, tragacanth, pectin, glue, alginic acid or a salt thereof, carrageenan, xanthan gum, sodium hyaluronate, locust bean gum, tara gum, guar gum, and tamarind seed gum.
[0040] The content of the polysaccharide is in the range of 0.40 parts by mass to 1.5 parts by mass, more preferably 0.70 parts by mass to 1.4 parts by mass, and even more preferably 0.80 parts by mass to 1.3 parts by mass, based on 100 parts by mass of the glass powder. This allows the paste composition 1 to have a suitable viscosity, improves the dispersion stability of the glass powder particles in the paste composition 1, and suppresses sedimentation (increases dispersibility), resulting in good applicability. If the content of the polysaccharide is less than 0.40 parts by mass, the viscosity is reduced, the dispersion stability of the glass powder particles in the paste composition 1 is reduced, sedimentation (reduction in dispersibility) is likely to occur, and there is a risk of reduced applicability. If the content of the polysaccharide is more than 1.5 parts by mass, there is a risk of increased voids in the glass seal structure when exposed to a high-temperature environment, resulting in reduced sealability.
[0041] The total content of the vinyl polymer and the polysaccharide is preferably in the range of 0.50 parts by mass to 3.0 parts by mass, more preferably 0.70 parts by mass to 2.5 parts by mass, and even more preferably 0.90 parts by mass to 2.0 parts by mass, based on 100 parts by mass of the glass powder. This provides the paste composition 1 with an appropriate viscosity (fluidity), improves the coating property, and improves the sealing property. If the total content is less than 0.50 parts by mass, the dispersibility and fluidity of the glass powder in the paste composition 1 are likely to decrease, and there is a risk of the coating property decreasing, and if it is more than 3.0 parts by mass, there is a risk of the glass sealing structure having many voids when exposed to a high-temperature environment, and the sealing property decreasing.
[0042] <Solvent> The solvent of the paste composition 1 is water, and the solvent does not include anything other than water. That is, the solvent does not include an organic solvent. With this configuration, a solvent recovery facility or a ventilation facility is not required when drying the paste composition, and the process is simplified. Furthermore, explosion-proof specifications are not required for each facility, which is advantageous in terms of cost and productivity.
[0043] The lower limit of the solid content concentration of the paste composition 1 is preferably 73% by mass or more, more preferably 75% by mass or more, and more preferably 78% by mass or more. The upper limit of the solid content concentration of the paste composition 1 is preferably 90% by mass or less, more preferably 87% by mass or less, and more preferably 85% by mass or less. If the solid content concentration is less than 73% by mass, there may be many voids in the glass seal structure after the paste composition 1 is dried, and the sealability may be reduced. If the solid content concentration is more than 90% by mass, the dispersibility and fluidity of the glass powder in the paste composition 1 may be easily reduced, and the coatability may be reduced. The solid content concentration is defined by the following formula. (Solid content concentration)=(mass of paste composition after removing water) / (mass of paste composition)×100 The mass of the paste composition 1 after removing water may be the value obtained by measuring the mass of the residue after evaporating water from the composition, or the sum of the masses of the raw materials before constituting the paste composition 1.
[0044] The paste composition 1 does not contain an inorganic binder. Examples of the inorganic binder include silicic acid compounds and aluminum phosphate. Even when exposed to a high-temperature environment, it is possible to eliminate the possibility of volatilization and deposition of elements such as silicon and phosphorus derived from the inorganic binder (silicic acid compounds, aluminum phosphate, etc.).
[0045] FIG. 1 shows an electrochemical module M including a fired body 1A of a paste composition 1. In this specification, a solid oxide fuel cell will be described as an example of an electrochemical module M including an electrochemical element A, but the electrochemical module M is not limited to a solid oxide fuel cell. In addition, although preferred embodiments are described below, each of these embodiments is described to more specifically exemplify the present invention, and various modifications are possible within the scope of the present invention, and the present invention is not limited to the following description. In addition, when expressing the positional relationship of layers, for example, the electrolyte layer side as viewed from the electrode layer is called "upper" or "upper side", and the first plate-like body side is called "lower" or "lower side". The electrochemical element A, electrochemical element stack S, and electrochemical module M will be described below with reference to Figs. 1 and 2.
[0046] <Electrochemical element> As shown in Figures 1 and 2, the electrochemical element A includes a metal support (an example of a metal member) 10 having an internal flow path A1 formed between opposing surfaces of a conductive first plate-like body 11 and a conductive second plate-like body 12. The metal support 10 includes, in at least a portion of the first plate-like body 11 and the second plate-like body 12 constituting the metal support 10, a gas flow-permitting portion 11A that allows gas to pass between the internal flow path A1, which is inside the metal support 10, and the outside, and an electrochemical reaction portion 30 that has, in the stated order, a membrane-like electrode layer (an example of a first electrode) 31, a membrane-like electrolyte layer 32, and a membrane-like counter electrode layer (an example of a second electrode) 33, in a state covering all or a portion of the gas flow-permitting portion 11A. The metal support 10 is provided at one end with a first through-portion 41 for passing a first gas, which is one of a reducing component gas such as a fuel gas and an oxidizing component gas such as air, from the outside in the surface-penetrating direction to the internal flow passage A1, and at the other end with a second through-portion 51 for passing the first gas that has passed through the internal flow passage A1 outward in the surface-penetrating direction of the metal support 10. It will be understood that the first through-portion 41 and the second through-portion 51 are symmetrical and have the same structure.
[0047] <Metal support> The metal support 10 includes a first plate-shaped body 11 and a second plate-shaped body 12 . The first plate-like body 11 supports an electrochemical reaction section 30 having an electrode layer 31, an electrolyte layer 32, and a counter electrode layer 33. The material of the first plate-like body 11 is a material having excellent electronic conductivity, heat resistance, oxidation resistance, and corrosion resistance. For example, ferritic stainless steel, austenitic stainless steel, nickel-based alloys, etc. are used. In particular, alloys containing chromium are preferably used.
[0048] The first plate-like body 11 is generally plate-shaped and has a gas flow-permitting portion 11A in the center thereof, which is made up of a large number of through-holes that penetrate from the front surface to the back surface. The through-holes can be provided in the first plate-like body 11 by, for example, laser processing. The through-holes have the function of allowing gas to pass from the back surface to the front surface of the first plate-like body 11. The gas flow-permitting portion 11A is preferably provided in an area of the first plate-like body 11 that is smaller than the area in which the electrode layer 31 is provided.
[0049] A metal oxide layer (not shown) is provided on the surface of the first plate-like body 11 as a diffusion suppression layer. That is, the diffusion suppression layer is formed between the first plate-like body 11 and the electrode layer 31 described below. The metal oxide layer is provided not only on the surface of the first plate-like body 11 exposed to the outside, but also on the contact surface (interface) with the electrode layer 31. It can also be provided on the inner surface of the through hole. This metal oxide layer can suppress interdiffusion of elements between the first plate-like body 11 and the electrode layer 31.
[0050] The metal oxide layer can be formed by various methods, but a method of oxidizing the surface of the first plate-like body 11 to form a metal oxide is preferably used. The metal oxide layer may be formed on the surface of the first plate-like body 11 by a spray coating method (such as a thermal spray method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method such as a sputtering method or a PLD method, a CVD method, or by plating and oxidation treatment. Furthermore, the metal oxide layer may contain a highly conductive spinel phase, etc.
[0051] When a ferritic stainless steel material is used for the first plate-like body 11, the thermal expansion coefficient is close to that of YSZ (yttria-stabilized zirconia) and GDC (gadolinium-doped ceria, also called CGO), which are the materials for the electrode layer 31 and the electrolyte layer 32. Therefore, even when a temperature cycle of low and high temperatures is repeated, the first plate-like body 11, the electrode layer 31, and the electrolyte layer 32 are deformed and expanded to the same extent, so that the electrochemical element A is unlikely to be damaged. This is preferable because it allows the realization of an electrochemical element A with excellent long-term durability.
[0052] The second plate-like body 12 is overlapped with the first plate-like body 11 and integrated with the peripheral edge portion 10a by welding to form the metal support body 10. The material of the second plate-like body 12 is preferably a heat-resistant metal, and is more preferably the same material as that of the first plate-like body 11 from the viewpoints of reducing the difference in thermal expansion with the first plate-like body 11 and ensuring the reliability of joining such as welding. The second plate-like body 12 forms an internal flow path A1 from one end side to the other end side in a region facing the gas flow permissible portion 11A of the first plate-like body 11, i.e., in a region between the first plate-like body 11 and the second plate-like body 12. The internal flow path A1 constitutes a first gas flow path 40 through which a first gas, which is either an oxidizing gas or a reducing gas, flows. The upstream side of the first gas flow path 40 provided in the electrochemical module M is fluidically connected to an external first gas supply device (not shown) that supplies the first gas via a first gas supply unit 61 of the housing B described later, and the downstream side of the first gas flow path 40 is fluidically connected to the outside via a first gas exhaust unit 62 of the housing B described later.
[0053] <Electrochemical reaction section> The electrochemical reaction section 30 is formed on the metal support 10, and includes an electrode layer 31, an electrolyte layer 32, and a counter electrode layer 33 in this order from the bottom in the stacking direction of the electrochemical device A. (electrode layer) 1 and 2, the electrode layer 31 can be provided as a thin layer on the surface of the first plate-like body 11 in an area larger than the area in which the through-holes are provided. When the electrode layer 31 is a thin layer, the thickness can be, for example, about 1.0 μm to 100 μm, and preferably 5.0 μm to 50 μm. With such a thickness, it is possible to reduce the amount of expensive electrode layer material used to cut costs while ensuring sufficient electrode performance.
[0054] The electrode layer 31 is formed as a porous layer having a plurality of pores in its interior and on its surface, and has gas permeability. The electrode layer 31 is formed, for example, so that its density is 30% or more and less than 80%. The size of the pores can be appropriately selected so that the electrochemical reaction proceeds smoothly. The density is the ratio of the material constituting the layer to the space, and can be expressed as (1-porosity), and is equivalent to the relative density.
[0055] The material of the electrode layer 31 may be, for example, a composite material such as NiO-GDC, Ni-GDC, NiO-YSZ, Ni-YSZ, CuO-CeO2, or Cu-CeO2. There is no particular limitation on the method of forming the electrode layer 31, but it is preferable to form it by a low-temperature firing method (for example, a wet method using firing in a low-temperature range without firing in a high-temperature range higher than 1100°C), a spray coating method (such as a thermal spray method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method (such as a sputtering method or a pulse laser deposition method), or a CVD method. These processes that can be used in a low-temperature range eliminate the need to use firing in a high-temperature range higher than, for example, 1100°C.
[0056] (electrolyte layer) 1 and 2, the electrolyte layer 32 is a thin film layer that covers the electrode layer 31. The electrolyte layer 32 can be formed in a thin film state with a thickness of 10 μm or less. The electrolyte layer 32 is provided on the surface of the first plate-like body 11 in an area larger than the area in which the through-holes are provided. In other words, the through-holes are formed inside the area in the first plate-like body 11 in which the electrolyte layer 32 is formed.
[0057] The electrolyte layer 32 has ion conductivity for conducting ions derived from the first gas or the second gas generated in the electrode layer 31 to the counter electrode layer 33, and also has gas barrier properties for preventing the first gas or the second gas from being transmitted to the counter electrode layer 33.
[0058] The electrolyte layer 32 may be made of an electrolyte material that conducts oxygen ions, such as YSZ (yttria-stabilized zirconia), SSZ (scandium-stabilized zirconia), GDC (gadolinium-doped ceria), YDC (yttrium-doped ceria), SDC (samarium-doped ceria), or LSGM (strontium-magnesium-doped lanthanum gallate), or an electrolyte material that conducts hydrogen ions, such as perovskite-type oxides. In particular, zirconia-based ceramics are preferably used. There is no particular limitation on the method for forming the electrolyte layer 32, but it is preferable to form it by a low-temperature firing method (for example, a wet method using firing in a low-temperature range without firing in a high-temperature range exceeding 1100°C), a spray coating method (such as a thermal spray method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method (such as a sputtering method or a pulse laser deposition method), or a CVD (chemical vapor deposition) method. By using these film formation processes that can be used in a low-temperature range, it is possible to obtain an electrolyte layer 32 that is dense and has high airtightness and gas barrier properties without firing in a high-temperature range exceeding 1100°C. Therefore, damage to the first plate-like body 11 can be suppressed, and interdiffusion of elements between the first plate-like body 11 and the electrode layer 31 can be suppressed, thereby realizing an electrochemical element A with excellent performance and durability. In particular, it is preferable to use a low-temperature firing method or a spray coating method, since it is possible to realize a low-cost element. Furthermore, the spray coating method is more preferable because it is easy to obtain a dense electrolyte layer that has high airtightness and gas barrier properties in a low temperature range.
[0059] The electrolyte layer 32 is formed in a state where it covers the electrode layer 31. Therefore, it is possible to suppress gas leakage from the electrode layer 31. When the electrochemical element A is used as a component of an SOFC, gas is supplied to the electrode layer 31 from the back side of the first plate-like body 11 through the through-holes during operation of the SOFC. In the portion where the electrolyte layer 32 contacts the first plate-like body 11, gas leakage can be suppressed without providing a separate member such as a gasket. Note that, although the electrolyte layer 32 covers the entire periphery of the electrode layer 31 in this embodiment, a configuration in which the electrolyte layer 32 is provided on the upper part of the electrode layer 31 and a gasket or the like is provided around it may also be adopted.
[0060] (Counter electrode layer) The counter electrode layer 33 is a thin film layer formed on the electrolyte layer 32. The thickness of the thin film layer can be, for example, about 1.0 μm to 100 μm, preferably 5.0 μm to 50 μm. With such a thickness, it is possible to reduce the amount of expensive counter electrode layer material used to cut costs while ensuring sufficient electrode performance. The counter electrode layer 33 is formed as a porous layer having a plurality of pores in its interior and on its surface, and has gas permeability. The counter electrode layer 33 is formed, for example, so that its density is 30% or more and less than 80%. The size of the pores can be appropriately selected so that the electrochemical reaction proceeds smoothly.
[0061] The material of the counter electrode layer 33 may be, for example, a composite oxide such as LSCF or LSM, a ceria-based oxide, or a mixture thereof. In particular, the counter electrode layer 33 preferably contains a perovskite-type oxide containing two or more elements selected from the group consisting of La, Sr, Sm, Mn, Co, and Fe. The counter electrode layer 33 formed using the above materials functions as a cathode.
[0062] There is no particular limitation on the method for forming the counter electrode layer 33, and for example, a low-temperature firing method (for example, a wet method using firing in a low-temperature range without firing in a high-temperature range exceeding 1100°C), a spray coating method (thermal spraying, aerosol deposition, aerosol gas deposition, powder jet deposition, particle jet deposition, cold spray, etc.), a PVD method (sputtering, pulse laser deposition, etc.), a CVD method, etc.) can be appropriately used. In each formation method, a treatment temperature of 1100°C or less is preferable because it can suppress damage to the first plate-like body 11 and also suppress interdiffusion of elements between the first plate-like body 11 and the electrode layer 31, thereby realizing an electrochemical element A with excellent performance and durability. In particular, it is preferable to use a low-temperature firing method or a spray coating method, etc., because it can realize a low-cost element. Furthermore, it is even more preferable to use a low-temperature firing method because it makes it easier to handle raw materials.
[0063] In the electrochemical reaction section 30, a chemical reaction between the first gas and the second gas progresses. For example, a case will be described in which a fuel gas containing hydrogen as the first gas is circulated from the rear surface of the first plate-like body 11 through the through-holes to the electrode layer 31, and air as the second gas is circulated to the counter electrode layer 33, which is the counter electrode of the electrode layer 31. In such a case, the electrochemical reaction section 30 is maintained at an operating temperature of 500°C or higher and 900°C or lower. When an electrolyte material that conducts oxide ions is used for the electrolyte layer 32, oxygen molecules contained in the air are converted into electrons e in the counter electrode layer 33. - reacts with to produce oxide ions O 2- The oxide ion O 2- The hydrogen molecules contained in the flowing fuel gas are converted into oxide ions O 2- reacts with water molecules and electrons e - In the electrolyte layer 32, protons H + When an electrolyte material that conducts electrons is used, hydrogen molecules contained in the fuel gas flowing through the electrode layer 31 are converted into electrons e - Proton H + The proton H + moves through the electrolyte layer 32 to the counter electrode layer 33. In the counter electrode layer 33, oxygen molecules and protons H + , electronic e - react to generate water molecules. The above reaction generates an electromotive force as an electrochemical output between the electrode layer 31 and the counter electrode layer 33. In this case, the electrode layer 31 functions as the fuel electrode (anode) of the fuel cell, and the counter electrode layer 33 functions as the air electrode (cathode).
[0064] The electrochemical reaction section 30 may be configured to include an intermediate layer 34 between the electrode layer 31 and the electrolyte layer 32 , and a reaction prevention layer 35 between the electrolyte layer 32 and the counter electrode layer 33 .
[0065] <Electrochemical module> As shown in FIG. 1, the electrochemical module M includes a housing B that houses an electrochemical element stack S described later, a first gas supply unit 61 that flows a first gas from the outside of the housing B to an internal flow path A1, a first gas exhaust unit 62 that flows the first gas after the reaction, a second gas supply unit 71 that flows a second gas from the outside of the housing B to the flow unit A2, a second gas exhaust unit 72 that flows the second gas after the reaction, and an output unit 8 that obtains an output associated with the electrochemical reaction in the electrochemical reaction unit 30. The electrochemical module M includes a distribution chamber 90 within the housing B that distributes the second gas flowing from the second gas supply unit 71 to the flow unit A2. The distribution chamber 90 is a space located on the side (lateral side) of the electrochemical element stack S that serves as the inlet or outlet of the flow section A2 of the electrochemical element stack S, and the flow section A2 has an opening formed on the space side and is connected to the space.
[0066] The housing B may have a buffer section 300 disposed between the housing B and the periphery of the electrochemical element A. Specifically, as shown in Fig. 1, the electrochemical element stack S is mounted inside the housing B such that the buffer section 300 is in contact with the periphery of each electrochemical element A of the electrochemical element stack S. A support part B1 is provided integrally with the housing B. The support part B1 is provided so as to protrude from the inner surface of the housing B. The buffer part 300 is disposed at a predetermined position inside the housing B in the longitudinal direction by being supported by the support part B1. Meanwhile, the buffer part 300 is disposed at a predetermined position inside the housing B in the lateral direction by being supported by the inner wall of the housing B. 1, the buffer unit 300 has a second gas supply port 301 for supplying a second gas from the second gas supply unit 71 through the distribution chamber 90 to the flow section A2 of each electrochemical element A surrounded by the buffer unit 300, and a second gas exhaust port 302 for exhausting the second gas from the flow section A2 of each electrochemical element A through the distribution chamber 90 to the second gas exhaust section 72. The buffer unit 300 air-tightly surrounds the electrochemical element stack S with respect to the housing B, except for the second gas supply port 301 and the second gas exhaust port 302.
[0067] Examples of materials for the case B include ferritic stainless steel, martensitic stainless steel, and composites of these with ceramics. The material of the electrochemical element A is preferably the same as that of the housing B. In other words, the materials of the electrochemical element A and the housing B preferably have the same thermal expansion coefficient as that of the housing B. The housing B and the electrochemical element A each thermally expand due to heat generated during use of the electrochemical module M. Since the electrochemical element A is built into the housing B, if the thermal expansion coefficients of the housing B and the electrochemical element A differ significantly, there is a risk of defects such as deformation and damage occurring in the electrochemical element A. In contrast, as described above, the housing B and the electrochemical element A have approximately the same thermal expansion coefficients, and therefore thermally expand to the same extent. Therefore, the difference in thermal expansion between the electrochemical element A and the housing B is kept small, and the risk of defects such as deformation and damage occurring in the electrochemical element A can be suppressed.
[0068] The electrochemical element stack S is housed within a housing B in a state where it is sandwiched between a pair of current collectors 81, 82 at both ends in the stacking direction of the electrochemical elements A of the electrochemical element stack S, and an output section 8 is extended from the current collectors 81, 82 so as to be freely connected to a power supply destination outside the housing B, and the current collectors 81, 82 may be arranged to hermetically accommodate the electrochemical element stack S in the housing B and to function as a buffer section for each electrochemical element A.
[0069] As a result, the electrochemical module M distributes fuel gas from the first gas supply unit 61 and air from the second gas supply unit 71, so that the fuel gas enters as indicated by the dashed arrows in Fig. 1 and Fig. 2 and air enters as indicated by the solid arrows. The fuel gas distributed from the first gas supply unit 61 is guided to the first gas flow path 40 from the first penetration portion 41 of the uppermost electrochemical element A of the electrochemical element stack S, and flows through the internal flow paths A1 of all the electrochemical elements A from the first gas flow path 40 partitioned by the first annular seal member 43. The air distributed from the second gas supply unit 71 temporarily flows into the distribution chamber 90, and then flows through the flow paths A2 formed between the electrochemical elements A. Incidentally, when the second plate-like body 12 is used as a reference, the portion of the second plate-like body 12 that bulges out from the first plate-like body 11 forms an internal flow path A1 between the first plate-like body 11 and the second plate-like body 12, and contacts the counter electrode layer 33 of the electrochemical reaction unit 30 of the adjacent electrochemical element A to enable electrical connection. On the other hand, the portion of the second plate-like body 12 that contacts the first plate-like body 11 is electrically connected to the first plate-like body 11, and forms a flow section A2 between the second plate-like body 12 and the electrochemical reaction unit 30 of the adjacent electrochemical element A.
[0070] The electricity generated in the electrochemical reaction section 30 in accordance with the flow of this fuel gas and air is connected in series between the current collectors 81, 82 through contact between the electrochemical reaction section 3 of the adjacent electrochemical element A and the second plate-like body 12, and the combined output is taken out from the output section 8.
[0071] <Electrochemical element stack> As shown in FIG. 1, the electrochemical element stack S of the electrochemical module M is configured such that a plurality of electrochemical elements A, each of which includes an electrolyte layer 32, and an electrode layer 31 and a counter electrode layer 33 disposed on either side of the electrolyte layer 32, are stacked with metal supports 10 interposed between the electrochemical elements A, and an annular sealing member having a through hole is disposed between adjacent metal supports 10. Specifically, in the electrochemical module M, a plurality of electrochemical elements A are stacked and arranged such that, with respect to adjacent electrochemical elements A, the metal support 10 constituting one electrochemical element A faces the metal support 10 constituting the other electrochemical element A, the outer surface of a second plate-like body 12 other than the first plate-like body 11 on which the electrochemical reaction section 30 in the metal support 10 constituting one electrochemical element A is arranged is electrically connected to the outer surface of the first plate-like body 11 in the metal support 10 constituting the other electrochemical element A (which actually comes into contact with the upper surface of the counter electrode layer 33), and a flow section A2 through which the second gas flows along both outer surfaces is formed between the adjacent outer surfaces. To achieve electrical connection, in addition to simply contacting the electrically conductive surface parts, it is possible to employ a method of applying a surface pressure to the contact surface, interposing a highly electrically conductive material to reduce the contact resistance, etc. Specifically, the rectangular electrochemical elements A are aligned with the first through-hole 41 at one end and the second through-hole 51 at the other end, with the electrochemical reaction part 30 of each electrochemical element A facing upward, and the first annular seal member (an example of an annular seal member) 43 and the second annular seal member (an example of an annular seal member) 53 are interposed between the first through-hole 41 and the second through-hole 51, and stacked (assembled) to form the above configuration.
[0072] The metal support 10 has a first through portion 41 provided at one end of the metal support 10 and a second through portion 51 provided at the other end of the metal support 10, with the first through portion 41 forming the upstream side of an internal flow path A1 formed between the first plate-like body 11 and the second plate-like body 12, and the second through portion 51 forming the downstream side of the internal flow path A1. When multiple electrochemical elements A are stacked (assembled) as described above, in the first through-hole 41, the upper opening 42 on the upper side of the electrochemical element A in the stacking direction is in contact with the lower end of the first annular sealing member 43 to maintain airtightness and form the first gas flow path 40 together with the first annular sealing member 43, and in the first through-hole 41, the lower opening 44 on the lower side of the electrochemical element A in the stacking direction is in contact with the upper end of the other first annular sealing member 43 to maintain airtightness and form the first gas flow path 40 together with the other first annular sealing member 43. Similarly, when multiple electrochemical elements A are stacked (assembled) as described above, in the second through-hole 51, the upper opening 52 on the upper side of the electrochemical element A in the stacking direction is in contact with the lower end of the second annular sealing member 53 to maintain airtightness and form the first gas flow path 40 together with the second annular sealing member 53, and in the second through-hole 51, the lower opening 54 on the lower side of the electrochemical element A in the stacking direction is in contact with the upper end of the other second annular sealing member 53 to maintain airtightness and form the first gas flow path 40 together with the other second annular sealing member 53. In this way, multiple electrochemical elements A are stacked (assembled) with the first annular sealing member 43 and the second annular sealing member 53 interposed between the outer surface of the second plate-like body 12, which is different from the first plate-like body 11 in which the electrochemical reaction section 30 in the metal support 10 constituting one electrochemical element A is arranged, and the outer surface of the first plate-like body 11 in the metal support 10 constituting another electrochemical element A.
[0073] The first annular sealing member 43 and the second annular sealing member 53 are composed of an annular flat plate with a through hole formed in the center, and are made of insulating ceramic material such as alumina, metal coated with this, or materials such as mica fiber and glass, and function as an insulating seal part that electrically insulates adjacent electrochemical elements A from each other. The planar outer shape of the first annular sealing member 43 and the second annular sealing member 53 is not limited to annular, and may be any shape as long as it is annular. Annular includes any shape such as circular, elliptical, rectangular, and polygonal.
[0074] The electrochemical module M has the above-mentioned configuration, and thus includes, at one longitudinal end side of the rectangular metal support 10, a first through-portion 41 for flowing a first gas, which is one of a reducing component gas and an oxidizing component gas, from the outside in the surface penetration direction to the internal flow path A1, and a first annular sealing member 43 for separating the first through-portions 41 formed on both outer surfaces of the metal support 10 from the flow path A2 within the flow path A2, and these first through-portions 41 and first annular sealing member 43 form a first gas flow path 40 for flowing the first gas to the internal flow path A1. In addition, the other longitudinal end side of the rectangular metal support 10 is provided with a second penetration portion 51 that flows the first gas that has passed through the internal flow path A1 outward in the surface penetration direction of the metal support 10, and a second annular sealing member 53 that separates the second penetration portions 51 formed on both outer surfaces of the metal support 10 from the flow portion A2 within the flow portion A2, and these second penetration portions 51 and second annular sealing member 53 form a first gas flow path 40 that flows the first gas that has passed through the internal flow path A1. In addition, around the abutting portion of the first plate-like body 11 where the first annular sealing member 43 and the second annular sealing member 53 are provided on the side of the first plate-like body 11 opposite the internal flow path A1, to facilitate positioning of the first annular sealing member 43 and the second annular sealing member 53 in the direction along the surface of the first plate-like body 11.
[0075] In addition, since the electrochemical module M has the above-mentioned configuration, a flow passage A2 that intersects with the first annular sealing member 43 and the second annular sealing member 53 is provided in the adjacent electrochemical element A to form a second gas flow passage 50. A counter electrode layer 33 is disposed in the middle of the flow passage A2 so as to come into contact with the second gas and cause an electrochemical reaction. The second gas flow passage 50 can be fluidly connected to an external second gas supply device (not shown) that supplies the second gas via a second gas supply part 71 in the case B. The second gas that has passed through the second gas flow passage 50 is discharged to the outside through a second gas discharge part 72 provided in the case B.
[0076] <Fired body> The paste composition 1 according to this embodiment is applied to the electrochemical module M where airtightness is required, and fired at a predetermined temperature. As a result, the fired body 1A of the paste composition 1 is mainly composed of glass powder and functions as a gas seal part. The firing temperature of the paste composition 1 is preferably 500°C or more and 1100°C or less, and more preferably 500°C or more and 800°C or less. If fired at less than 500°C, components other than the glass powder may remain, and there is a risk that the gas sealability is not fully exhibited. If it exceeds 1100°C, there is a possibility that it may have an adverse effect on the components of the electrochemical module M, and may lead to a decrease in durability. The paste composition 1 can be applied and fired at the timing when a plurality of electrochemical elements A are stacked (assembled) to form an electrochemical element stack S, which is then fired.
[0077] In this embodiment, when electrochemical elements A are stacked with a first annular sealing member 43 and a second annular sealing member 53 interposed therebetween, a paste composition 1 is applied to the outer peripheries of the first annular sealing member 43 and the second annular sealing member 53 and to the contact points between the first annular sealing member 43 and the second annular sealing member 53 and the metal support 10, and then fired to form a fired body 1A, as shown in FIG. 1. In FIG. 1, the paste composition 1 is also applied to the contact points between the current collector (an example of a metal member) 81 and the first annular sealing member 43 and the second annular sealing member 53, and then fired to form a fired body 1A.
[0078] The sintered body 1A of the paste composition 1 can be formed by applying it to areas of the electrochemical module M where airtightness is required and then firing it. For example, the sintered body 1A can be formed by applying it to the contact areas between the upper and lower surfaces of the first annular sealing member 43 and the second annular sealing member 53 and the metal support 10 and then firing it.
[0079] Using the electrochemical module M described above, an energy system Z, which will be described later, can be constructed.
[0080] <Energy system> Figures 3 and 4 show an overview of Energy System Z. The energy system Z includes an electrochemical device 100 and a heat exchanger 200 serving as a waste heat utilization section for reusing heat discharged from the electrochemical device 100. The electrochemical device 100 has an electrochemical module M, a desulfurizer 101, and a reformer 102, which is a type of fuel converter, as well as a fuel supply unit 103 that circulates fuel gas containing a reducing component to the electrochemical module M, and an inverter 104, which is a type of power converter, as an output unit that extracts electricity from the electrochemical module M.
[0081] More specifically, the electrochemical device 100 includes an inverter 104, a desulfurizer 101, a reforming water tank 105, a vaporizer 106, a reformer 102, a blower 107, a combustion unit 108, a control unit 110, and an electrochemical module M.
[0082] The desulfurizer 101 removes (desulfurizes) sulfur compounds contained in a hydrocarbon-based raw fuel such as city gas. When sulfur compounds are contained in the raw fuel, the provision of the desulfurizer 101 can suppress contamination of the reformer 102 or the electrochemical element A by the sulfur compounds. The vaporizer 106 generates steam from the reforming water flowing from the reforming water tank 105. The reformer 102 uses the steam generated by the vaporizer 106 to steam reform the raw fuel desulfurized by the desulfurizer 101, and generates a reformed gas containing hydrogen.
[0083] The electrochemical module M generates power by electrochemical reaction using the reformed gas circulated from the reformer 102 and the air circulated from the blower 107. The combustion section 108 mixes the reaction exhaust gas circulated from the electrochemical module M with air, and combusts combustible components in the reaction exhaust gas.
[0084] The inverter 104 adjusts the output power of the electrochemical module M to have the same voltage and frequency as the power received from a commercial grid (not shown).
[0085] The reformer 102 performs a reforming process of the raw fuel using the combustion heat generated by the combustion of the reaction exhaust gas in the combustion section 108 .
[0086] The raw fuel is circulated to the desulfurizer 101 through a raw fuel supply passage 112 by the operation of a boost pump 111. The reforming water in the reforming water tank 105 is circulated to the vaporizer 106 through a reforming water supply passage 114 by the operation of a reforming water pump 113. The raw fuel supply passage 112 merges with the reforming water supply passage 114 at a location downstream of the desulfurizer 101, and the reforming water and raw fuel that have been merged outside the casing B are circulated to the vaporizer 106.
[0087] The reforming water is vaporized in the vaporizer 106 to become water vapor. The raw fuel containing water vapor produced in the vaporizer 106 is circulated to the reformer 102 through a water vapor-containing raw fuel supply passage 115. The raw fuel is steam reformed in the reformer 102 to produce a reformed gas (a first gas having a reducing component) mainly composed of hydrogen gas. The reformed gas produced in the reformer 102 is circulated to the electrochemical module M through a fuel supply unit 103.
[0088] The reaction exhaust gas is combusted in the combustion section 108 to become a combustion exhaust gas, which is sent from the combustion exhaust gas discharge passage 116 to the heat exchanger 200. A combustion catalyst section 117 (e.g., a platinum-based catalyst) is arranged in the combustion exhaust gas discharge passage 116, and reduces the carbon monoxide, hydrogen, and other reducing components contained in the combustion exhaust gas by combustion.
[0089] The heat exchanger 200 exchanges heat between the combustion exhaust gas generated by the combustion in the combustion section 108 and the cold water passing through it, thereby generating hot water. That is, the heat exchanger 200 operates as a waste heat utilization section that reuses the heat discharged from the electrochemical module M.
[0090] Instead of the exhaust heat utilization section, a reaction exhaust gas utilization section may be provided that utilizes the reaction exhaust gas circulating (without being combusted) from the electrochemical module M. Also, at least a part of the reaction exhaust gas circulating from the first gas discharge section 62 to the outside of the housing B may be recycled by merging with any of the locations 101, 103, 106, 112, 113, and 115 in FIG. 3. The reaction exhaust gas contains residual hydrogen gas that was not used in the reaction in the electrochemical element A. In the reaction exhaust gas utilization section, the residual hydrogen gas is utilized for heat utilization by combustion or for power generation by a fuel cell or the like, thereby making effective use of energy.
[0091] 4 shows an example of the energy system Z in which the electrochemical reaction unit 30 operates as an electrolysis cell. In this energy system Z, supplied water and carbon dioxide are electrolyzed in the electrochemical reaction unit 30 to generate hydrogen, carbon monoxide, and the like. Furthermore, hydrocarbons and the like are synthesized in the fuel converter 25. By configuring the heat exchanger 24 in FIG. 4 to operate as an exhaust heat utilization unit that exchanges heat between the reaction heat generated by the reaction in the fuel converter 25 and water to vaporize it, and the heat exchanger 23 in FIG. 4 to operate as an exhaust heat utilization unit that exchanges heat between the exhaust heat generated by the electrochemical element A and the water vapor and carbon dioxide supplied by the boost pump 111 to preheat them, energy efficiency can be improved. Furthermore, the power converter supplies power to the electrochemical device A. This allows the electrochemical device A to function as an electrolysis cell as described above. Therefore, according to the above configuration, it is possible to provide an energy system Z or the like that can improve the efficiency of converting electrical energy into chemical energy such as fuel.
[0092] Examples of the present invention will be described below, but the present invention is not limited to these.
[0093] Example 1 5.0 g of glass powder (GM31107, Schott Aktiengesellschaft), 0.025 g of Marialim (SC-0505K, NOF Corp.) as a vinyl polymer, and 0.050 g of hydroxypropylcellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.) as a polysaccharide were weighed and placed in a container of a mixer (Awatori Rentaro, Thinky Corp.), and then water was added to a solid content of 85% by mass. The mixture was then stirred and kneaded at 2000 rpm for 5 minutes to obtain a paste composition. The paste composition was applied to the outer peripheral surface of a solid oxide fuel cell gasket (Thermiculite 866LS, Tokyo Kogyo Boeki Shokai Co., Ltd.) to evaluate the applicability and measure the leak rate. The settling property (dispersibility) of the paste composition was also evaluated.
[0094] Example 2 A paste composition was prepared under the same conditions as in Example 1, except that the glass powder was G018-311 (manufactured by Schott Aktiengesellschaft), and the coating property was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0095] Example 3 A paste composition was prepared under the same conditions as in Example 1, except that the glass powder was G018-311 (manufactured by Schott Aktiengesellschaft), the vinyl polymer was 0.050 g of Marialim (SC-0505K, NOF Corporation), and the polysaccharide was 0.050 g of hydroxypropyl cellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.), and the coatability was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0096] Example 4 A paste composition was prepared under the same conditions as in Example 1, except that the glass powder was G018-311 (manufactured by Schott Aktiengesellschaft), the vinyl polymer was 0.015 g of Marialim (SC-0505K, NOF Corporation), and the polysaccharide was 0.075 g of hydroxypropyl cellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.), and the coatability was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0097] Example 5 A paste composition was prepared under the same conditions as in Example 1, except that the glass powder was G018-311 (manufactured by Schott Aktiengesellschaft), the vinyl polymer was 0.050 g of Marialim (SC-0505K, NOF Corporation), and the polysaccharide was 0.035 g of hydroxypropyl cellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.), and the coatability was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0098] Comparative Example 1 A paste composition was prepared under the same conditions as in Example 1, except that the vinyl polymer and polysaccharide were not added, and water was added so that the solid concentration was 75 mass %. The paste composition was then applied to the upper and lower surfaces of a metal ring, and the application property was evaluated and the leak rate was measured.
[0099] Comparative Example 2 A paste composition was prepared under the same conditions as in Example 1, except that no polysaccharide was added, 0.025 g of Marialim (SC-0505K, NOF Corporation) was used as the vinyl polymer, and water was added so that the solid content concentration was 80 mass %, and the coating property was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0100] Comparative Example 3 A paste composition was prepared under the same conditions as in Example 1, except that no polysaccharide was added, 0.025 g of Marialim (SC-0505K, NOF Corporation) was used as the vinyl polymer, and water was added so that the solid content concentration was 80 mass %. The paste composition was then applied to the upper and lower surfaces of a metal ring, and the application property was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0101] Comparative Example 4 A paste composition was prepared under the same conditions as in Example 1, except that no vinyl polymer or polysaccharide was added, and water was added so that the solid content concentration was 68% by mass. The paste composition was then applied to the upper and lower surfaces of a metal ring, and the application property was evaluated and the leak rate was measured. The sedimentation property (dispersibility) of the paste composition was also evaluated.
[0102] Comparative Example 5 A paste composition was prepared under the same conditions as in Example 1, except that no vinyl polymer was added and 0.050 g of hydroxypropyl cellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.) was used as the polysaccharide, and the coatability was evaluated.
[0103] Comparative Example 6 A paste composition was prepared under the same conditions as in Example 1, except that no vinyl polymer was added, 0.050 g of hydroxypropyl cellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.) was used as the polysaccharide, and water was added so that the solid concentration was 75 mass %, and the coatability was evaluated.
[0104] Comparative Example 7 Each component was weighed out so that the total amount was 5.0 g of glass powder (G018-311, Schott Aktiengesellschaft), 0.15 g of Marialim (SC-0505K, NOF Corp.) as a vinyl polymer, and 0.15 g of hydroxypropylcellulose (NISSO HPC Grade.SL, Nippon Soda Co., Ltd.) as a polysaccharide, and placed in the container of a mixer (Awatori Rentaro, Thinky Corp.). Water was then added so that the solid content concentration was 75% by mass. A paste composition was prepared under the same conditions as in Example 1, and the applicability was evaluated and the leak rate was measured. The settling property (dispersibility) of the paste composition was also evaluated.
[0105] Evaluation of Dispersibility of Paste Composition The paste compositions obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were allowed to stand for 1 hour in a separate container. Thereafter, the presence or absence of deposits of glass powder on the bottom of the container (below the paste composition) was confirmed to evaluate dispersibility. The results are shown in Table 1. In Table 1, the case where no glass powder was observed is indicated as ◯, and the case where deposits of glass powder were observed is indicated as ×. Evaluation of Coating Properties of Paste Composition The paste compositions obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were evaluated as follows: ◯ if application to a solid oxide fuel cell gasket or metal ring was possible with a dispenser or a brush; △ if application with a dispenser or a brush was not possible but application with a spatula was possible; and × if application with a dispenser, a brush, or a spatula was impossible. The results are shown in Table 1. <Leak rate measurement> The paste compositions obtained in Examples 1 to 5 and Comparative Examples 1 to 7 were applied to the side (outer periphery) of a solid oxide fuel cell gasket (Thermiculite 866LS, Tokyo Kogyo Boeki Shokai Co., Ltd.) and to the upper and lower surfaces of a metal ring, and the solid oxide fuel cell gasket and metal ring were placed between test flanges and fired at 750°C with both flanges fastened. Thereafter, pressure gauges were connected to the inside of the gasket and the metal ring, hydrogen gas was added, and the pressure was increased to 5.0 to 10 kPa and the pressure was recorded when the pressure was maintained. After 10 minutes, the pressure in the gasket and the metal ring was measured, and the leak rate was calculated according to the following formula. The results are shown in Table 1. (Leak rate) = 100 x {(Pressure inside the gasket or metal ring immediately after holding) - (Pressure inside the gasket or metal ring after 10 minutes)} / Pressure inside the gasket or metal ring immediately after holding) As a reference example, Table 1 shows the leakage rate when no paste composition was applied to a gasket for a solid oxide fuel cell.
[0106] [Table 1]
[0107] The paste compositions obtained in Examples 1 to 5 were considered to be paste compositions in which the constituent components were stably dispersed even over a long period of time, since the constituent components did not settle. In addition, the paste compositions can be applied with a dispenser or a brush, so that they can be applied around the gasket and without small gaps. Therefore, it is considered possible to use the paste compositions in the manufacturing process of actual fuel cells. Furthermore, the leak rate after 10 minutes was 0 in all cases, which fully demonstrated the gas sealing function. On the other hand, the paste composition obtained in Comparative Example 1 had a leakage rate of 0 after 10 minutes, but the constituent components accumulated when left to stand, and it is difficult to say that it has excellent dispersibility. Furthermore, since it was not possible to apply it with a dispenser or a brush, the application properties were inferior to the paste compositions obtained in Examples 1 to 5. Therefore, it is considered that it is difficult to handle in the actual fuel cell manufacturing process and is not suitable for practical use. Although the paste compositions obtained in Comparative Examples 2 to 4 all have excellent applicability, when left to stand, the constituent components accumulate, so that remixing is required before use, and firing is required immediately after application, so that it is difficult to say that they are suitable for practical use. In particular, the paste compositions of Comparative Examples 2 and 4 have a higher leakage rate than the paste compositions of Examples 1 to 5, and from this point of view as well, they are unsuitable for use as paste compositions for fuel cells. The paste compositions of Comparative Examples 5 and 6 were inferior to the paste compositions of Examples 1 to 5 in both dispersibility and coatability, and it is difficult to say that they are suitable for practical use. In Comparative Example 7, the dispersibility and coatability were comparable to those of the paste compositions obtained in Examples 1 to 5. However, since the leakage rate was 10.4%, it is considered difficult to use the paste composition as a fuel cell paste composition.
[0108] (Another embodiment) (1) In the above embodiment, an example was described in which the paste composition 1 (sintered body 1A) was placed at a location where gas sealing was required in an electrochemical module M equipped with a metal-supported electrochemical element A, but the electrochemical module M may be an electrochemical module M of another form.
[0109] For example, although not shown, the electrochemical module M may be a solid oxide fuel cell stack formed by stacking a plurality of flat solid oxide fuel cells (electrochemical elements) each having a first electrode (electrode layer) facing one side of a flat solid electrolyte membrane and a second electrode (counter electrode layer) facing the other side of the membrane, with separators (an example of a metal member) sandwiched between the fuel cells. In this configuration, a groove (first gas flow path) through which a first gas can flow is formed on the surface of one separator facing the electrode layer, and a groove (second gas flow path) through which a second gas can flow is formed on the surface of the separator facing the counter electrode layer, and the first gas and the second gas flowing through these grooves are supplied to the electrode layer and the counter electrode layer. In addition, the stacked separators have a distribution structure that supplies the first gas and the second gas to each groove, and the distribution structure is formed in an outer region than the central region in which the grooves are formed in a plan view of the separator. For this reason, it is necessary to gas-seal between the separators between the gas flowing through the grooves and the outside, and it is also necessary to gas-seal between the gas flowing through the distribution structure and the outside. Therefore, in the electrochemical module M, a plurality of fuel cell units each having a flat solid electrolyte membrane and an electrode layer and a counter electrode layer respectively disposed on either side of the solid electrolyte membrane are stacked with separators interposed between the fuel cell units, and a paste composition (sintered body) is disposed between adjacent separators.
[0110] Furthermore, for example, although not shown, the electrochemical module M may be a cylindrical flat plate type solid oxide fuel cell stack having a plurality of cylindrical flat plate type fuel cells (electrochemical elements) and a manifold into which the first gas is introduced. In this configuration, a plurality of cylindrical flat-plate type fuel cells are arranged in parallel with each other via current collecting members and are provided to stand upright from the manifold. Each fuel cell is formed in a cylindrical flat-plate shape and has a conductive member, a first electrode (electrode layer), an electrolyte layer, a second electrode (counter electrode layer), an adhesion layer, and an interconnector. The conductive member is provided with a first gas flow path that penetrates the conductive member along the direction in which the fuel cells are arranged, and a first gas supplied from the manifold flows through the first gas flow path. In the cylindrical flat plate type electrochemical module M as described above, the paste composition (sintered body) can be placed at the joint between the manifold and the fuel cell arranged upright so as to communicate with the manifold, thereby making the joint gas-sealed.
[0111] In the above embodiment, the electrochemical device 100 includes an electrochemical module M including a plurality of electrochemical elements A. However, the electrochemical device 100 of the above embodiment is also applicable to a configuration including one electrochemical element A.
[0112] In addition, the configurations disclosed in the above-mentioned embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided that no contradiction arises. Furthermore, the embodiments disclosed in this specification are illustrative, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Industrial Applicability]
[0113] The present invention can be used as a gas sealing paste composition for sealing locations that require gas sealing in solid oxide fuel cells and solid oxide electrolysis cells. [Explanation of symbols]
[0114] 1: Paste composition 1A: Sintered body 10: Metal support 31: Electrode layer 32: Electrolyte layer 33: Counter electrode layer 43: First annular seal member 53: Second annular seal member 100: Electrochemical equipment 102: Reformer 104: Inverter 200: Heat exchanger A: Electrochemical element M: Electrochemical module Z: Energy System
Claims
1. A paste composition for gas sealing containing water as a solvent, The composition comprises glass powder, a vinyl polymer having a polyether structure in the side chain, and a polysaccharide, The solid content is 73% by mass or more and 90% by mass or less, a total content of the vinyl polymer and the polysaccharide is 0.50 parts by mass or more and 3.0 parts by mass or less per 100 parts by mass of the glass powder.
2. 2. The paste composition for sealing according to claim 1, wherein the main chain of the vinyl polymer has at least one unit selected from the group consisting of maleic anhydride units, maleic acid units and maleate units.
3. 2. The paste composition for sealing according to claim 1, wherein the content of the vinyl polymer is from 0.10 parts by mass to 1.5 parts by mass, based on 100 parts by mass of the glass powder.
4. 2. The paste composition for sealing according to claim 1, wherein the content of the polysaccharide is 0.40 parts by mass or more and 1.5 parts by mass or less, based on 100 parts by mass of the glass powder.
5. 2. The paste composition for sealing according to claim 1, wherein the polysaccharide is one or more of methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxybutyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose or a salt thereof, aminomethyl hydroxypropyl cellulose, aminoethyl hydroxypropyl cellulose, starch, tragacanth, pectin, glue, alginic acid or a salt thereof, carrageenan, xanthan gum, sodium hyaluronate, locust bean gum, tara gum, guar gum, and tamarind seed gum.
6. 2. The paste composition for sealing according to claim 1, wherein the glass powder is crystallized glass, and the thermal expansion coefficient of the glass powder is 8.0 ppm / K or more and 13 ppm / K or less.
7. 13. An electrochemical module comprising: a plurality of electrochemical elements each including an electrolyte layer and a first electrode and a second electrode disposed on either side of the electrolyte layer, the electrochemical elements being stacked with metal substrates interposed between the electrochemical elements; and the paste composition for sealing according to claim 1 being disposed between adjacent metal substrates.
8. 13. An electrochemical module comprising: a plurality of electrochemical elements, each of which includes an electrolyte layer and a first electrode and a second electrode disposed on either side of the electrolyte layer, stacked with metal substrates interposed between the electrochemical elements; annular sealing members each having a through hole disposed between adjacent metal substrates; and the paste composition for sealing according to claim 1 disposed on at least a portion of a surface of the annular sealing member.
9. 9. An electrochemical device comprising the electrochemical module according to claim 7 or 8, a fuel converter which generates a reducing component to be supplied to the electrochemical module or converts a gas containing the reducing component generated in the electrochemical module, and a power converter which extracts electric power from the electrochemical module or passes electric power to the electrochemical module, An energy system comprising a waste heat utilization section that reuses heat discharged from the electrochemical device.
Citation Information
Patent Citations
Green sheet for solid oxide fuel cell and manufacturing method therefor
JP2014216119A
Fuel cell gasket
JP2016511506A
Green sheet for sealing
JP2020167093A
Glass coating composition
JP2020191295A
Glass composition for sealing
WO2016129543A1