Decorative sheet
The decorative sheet achieves low gloss, scratch resistance, and three-dimensional formability by using a thermoplastic resin sheet with a urethane acrylate surface layer irradiated by excimer light to create wrinkles, addressing the limitations of previous technologies.
Patent Information
- Application Number
- JP2023053698
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing decorative sheets struggle to achieve a sufficient matte effect, scratch resistance, and three-dimensional formability due to inadequate incorporation of silica particles and excimer light irradiation, leading to insufficient low gloss and contradictory performance requirements.
A decorative sheet design featuring a base material with a surface layer that satisfies the condition Glossiness x (interface development area ratio Sdr+1)≧1.8, utilizing a thermoplastic resin sheet with a surface layer containing urethane acrylate and monofunctional acrylate, and irradiated with excimer light to create wrinkles for low gloss and enhanced scratch resistance and formability.
The solution results in a decorative sheet with low gloss due to a matte effect, excellent scratch resistance, and three-dimensional formability, balancing contradictory performance requirements.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative sheet. [Background technology]
[0002] Decorative sheets are used to enhance design by providing surface decoration in various applications such as wall materials, construction materials, building materials such as fittings, surface decoration of furniture, etc., automotive interiors, low-electricity electrical coverings, etc. Known decorative sheets include, for example, those having a layer with a low gloss (matte) effect provided on a substrate.
[0003] For example, a decorative sheet has been proposed that has a decorative layer containing a coloring material on a substrate, and a clear layer containing wet gel silica particles having an average particle size of 5 μm or less as measured by the Coulter Counter method (AP 50 μm) on the decorative layer. It is described that such a configuration can provide a decorative sheet that favorably maintains the color of the coloring layer and has a good matte surface even when it has a clear layer containing inorganic particles (see, for example, Patent Document 1).
[0004] Also, a decorative sheet has been proposed in which the surface of a coating film construction provided on a substrate is irradiated with excimer light from an excimer lamp, thereby reducing the gloss of the portion of the surface of the coating film construction irradiated with the electromagnetic waves compared to before the electromagnetic waves were irradiated. It is described that such a configuration can provide a decorative sheet having areas with different matte textures (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-77691 A [Patent Document 2] JP 2018-164901 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the decorative sheet described in Patent Document 1 above has the problem that, because silica particles are merely blended into the clear layer, a sufficient matte effect cannot be obtained and low gloss is difficult to achieve.
[0007] Furthermore, in the decorative sheet described in Patent Document 2, the clear layer does not contain silica particles or the like, and is simply irradiated with excimer light, so there is a problem that a sufficient matte effect is not obtained and low gloss is difficult to achieve.
[0008] Furthermore, in addition to the low gloss mentioned above, decorative sheets are required to have scratch resistance and three-dimensional formability that enables processing into molded products with complex shapes. However, scratch resistance and three-dimensional formability are contradictory properties, and it has been difficult to achieve both.
[0009] Therefore, the present invention has been made in consideration of the above problems, and has an object to provide a decorative sheet that has low gloss due to a matte effect, and is excellent in abrasion resistance and three-dimensional formability. [Means for solving the problem]
[0010] In order to achieve the above-mentioned object, the decorative sheet of the present invention comprises a substrate and a surface layer provided on the surface of the substrate, the surface layer having a glossiness of 2 or less, and characterized in that the relationship represented by the following formula (1) holds between the glossiness and the interfacial development area ratio Sdr of the surface layer on the side opposite to the substrate.
[0011] [Number 1] Glossiness × (interface development area ratio Sdr + 1) ≧ 1.8 (1) Effect of the Invention
[0012] According to the present invention, it is possible to provide a decorative sheet that has low gloss due to a matte effect, and is excellent in abrasion resistance and three-dimensional formability. [Brief description of the drawings]
[0013] [Figure 1] 1 is a cross-sectional view showing a decorative sheet according to an embodiment of the present invention. [Diagram 2] 2 is a laser microscope photograph showing the surface state of the surface layer in the decorative sheet of Example 1. [Diagram 3] 3 is a laser microscope photograph showing the surface state of the surface layer in the decorative sheet of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The decorative sheet of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0015] <Decorative sheet> As shown in FIG. 1, the decorative sheet 1 of the present invention comprises a substrate 2 and a surface layer 3 provided on a surface 2a of the substrate 2.
[0016] <Base material> The substrate 2 is made of, for example, a thermoplastic resin sheet, and as this thermoplastic resin sheet, any of those typically used for substrates in decorative sheets 1 can be used. Specific examples include polyvinyl chloride (PVC) sheets, glycol-modified polyethylene terephthalate (PETG) sheets, amorphous crystalline polyester resin (APET) sheets, polyolefin sheets (polyethylene sheets, polypropylene sheets, etc.), acrylonitrile-butadiene-styrene resin (ABS) sheets, polycarbonate sheets, etc. Furthermore, an example of an amorphous crystalline polyester resin (APET) sheet used for the substrate 2 is a recycled polyethylene terephthalate (RPET) sheet made from raw materials such as PET bottles.
[0017] As the thermoplastic resin sheet, a glycol-modified polyethylene terephthalate sheet is preferred from the viewpoint of ease of processing into a quadratic curved surface and excellent three-dimensional moldability. The glycol-modified polyethylene terephthalate sheet is a type of polyethylene terephthalate, and is a non-crystalline polyester that contains, as a glycol component, ethylene glycol and a diol other than ethylene glycol (1,4-cyclohexanedimethanol), whereas the glycol component of polyethylene terephthalate is ethylene glycol.
[0018] The thermoplastic resin sheet may be a stretched sheet or an unstretched sheet. The thermoplastic resin sheet may contain additives such as colorants, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, storage stabilizers, lubricants, and fillers, as necessary. The thermoplastic resin sheet is preferably colored from the viewpoint of design.
[0019] The thickness of the substrate 2 is not particularly limited, but is preferably 50 to 800 μm, and more preferably 250 to 500 μm. If the thickness of the substrate 2 is 50 μm or more, the mechanical strength and the concealing property can be sufficiently improved. If the thickness of the substrate 2 is 800 μm or less, the three-dimensional moldability is more excellent, and it is easy to ensure the flexibility and printability.
[0020] <Surface layer> The surface layer 3 is a coating film of a paint mainly composed of urethane acrylate. The surface layer 3 can be formed by applying the paint onto the surface 2a of the substrate 2 and curing it, and the surface layer 3 is formed of a cured paint. As shown in FIG. 1, wrinkles are formed on the surface 3a of the surface layer 3 (i.e., the surface opposite to the substrate 2 side).
[0021] The urethane acrylate used may have a functionality of 2 to 10, and examples thereof include phenyl glycidyl ether acrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer. In addition, EBECRYL8402, KRM8452, EBECRYL210, EBECRYL220, EBECRYL4500, EBECRYL230, EBECRLY270, EBECRYL4858, EBECRYL8804, EBECRYL8807, EBECRYL9270, EBECRYL4100, EBECRYL4666, EBECRYL4513, EBECRYL8311, EBECRYL8465, EBECRYL9260, EBECRYL Commercially available products such as 8606, EBECRYL8701, KRM8452, KRM8667, EBECRYL4265, EBECRYL4587, EBECRYL4200, EBECRYL8210, EBECRYL1290, EBECRYL5129, EBECRYL8254, EBECRYL8301R, KRM8200, KRM8904, U-6LPA, UA-1100H, U-200PA, and UA-160TM (all trade names) can be used. These urethane acrylates may be used alone or in combination of two or more.
[0022] The surface layer 3 may also contain a monofunctional acrylate. Examples of the monofunctional acrylate include ethyl carbitol acrylate, methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, β-(meth)acryloyloxyethyl hydrogen phthalate, β-(meth)acryloyloxyethyl hydrogen succinate, nonylphenoxyethyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, phenoxyethyl (meth)acrylate, and phenoxypolyethylene glycol. (Meth)acrylate, butoxy polyethylene glycol (meth)acrylate, alkyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate , 3-acryloyloxyglycerin mono(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 2-hydroxy-1-(meth)acryloxy-3-(meth)acryloxypropane, polypropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, poly-ε-caprolactone mono(meth)acrylate, dialkylaminoethyl(meth)acrylate, glycidyl(meth)acrylate, mono[2-(meth)acryloyloxyethyl] ... acrylate, trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 2,2,3,4,4,4-hexafluorobutyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, dicyclopentenyloxyalkyl (meth)acrylate, dicyclopentenyl (meth)acrylate, tricyclodecanyl (meth)acrylate, tricyclodecanyloxyethyl (meth)acrylate, and isobornyloxyethyl (meth)acrylate. These monofunctional acrylates may be used alone or in combination of two or more.
[0023] Furthermore, the compounding ratio of the urethane acrylate to the monofunctional acrylate in the surface layer 3 is not particularly limited as long as it does not impair the characteristics of the decorative sheet 1 of the present invention, and can be, for example, in the range of urethane acrylate:monofunctional acrylate = 1:0.5 to 1:4 by mass ratio.
[0024] In addition, since the crosslinking distance of urethane acrylate is longer than that of monofunctional acrylate, flexibility is improved, and wrinkle formation and three-dimensional moldability tend to be improved, but if the mass ratio of urethane acrylate is large, the coating film may have poor scratch resistance. In addition, since the crosslinking distance of monofunctional acrylate is short, crosslinking density is improved and scratch resistance is improved, but if the mass ratio of monofunctional acrylate is large, wrinkle formation and three-dimensional moldability may be reduced.
[0025] Furthermore, the thickness of the surface layer 3 is not particularly limited, but is preferably 1 to 10 μm. If the thickness of the surface layer 3 is 10 μm or more, the surface roughness of the surface 3a of the surface layer 3 increases, improving fingerprint resistance but decreasing tactile sensation.
[0026] From the viewpoint of improving scratch resistance and three-dimensional formability, the thickness of the surface layer 3 is more preferably 3 to 8 μm.
[0027] Furthermore, the coating material may contain components other than the urethane acrylate and the monofunctional acrylate, as long as the effects of the invention are not impaired. Examples of the other components include multifunctional acrylates, vinyl chloride-vinyl acetate copolymers, photopolymerization initiators, colorants, UV absorbers, light stabilizers, antioxidants, antistatic agents, storage stabilizers, plasticizers, lubricants, and fillers.
[0028] Examples of the polyfunctional acrylate include dipropylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, EBECRYL145, EBECRYL150, IRR214K, EBECRYL130, trimethylolpropane triacrylate, EBECRYL160S, OTA480, PETIA, PETRA, EBECRYL40, PETA, EBECRYL140, EBECRL1140, EBECRYL1142, DPHA, EBECRYL895, EBECRYL896, ethoxybisphenol A diacrylate, and glycerin triacrylate. These polyfunctional acrylates may be used alone or in combination of two or more.
[0029] As the photopolymerization initiator, for example, an alkylphenone-based, an acylphosphine oxide-based, or a cationic initiator can be used.
[0030] <Manufacturing method> When producing the decorative sheet 1 of the present invention, first, for example, a substrate 2 made of the above-mentioned thermoplastic resin sheet is prepared. This thermoplastic resin sheet may be a commercially available one, or may be one produced by a known production method such as a calendar method or an extrusion molding method.
[0031] Next, a coating material containing, for example, urethane acrylate, monofunctional acrylate, polyfunctional acrylate, vinyl chloride-vinyl acetate copolymer, and a photopolymerization initiator added to a solvent such as methyl ethyl ketone is applied onto the surface 2a of the substrate 2, to form a coating film that will become the surface layer 3 on the surface 2a of the substrate 2.
[0032] For example, when a difunctional to decafunctional urethane acrylate containing a photopolymerization initiator is used, the use of a monofunctional acrylate can be omitted.
[0033] The coating method is not particularly limited, and examples thereof include cast coating, die coating, gravure coating, roll knife coating, reverse roll coating, roll coating, and comma coating.
[0034] Next, excimer light is irradiated onto the coating film formed on the surface 2a of the substrate 2. More specifically, excimer light having a short peak wavelength (within a range of 120 to 230 nm) is irradiated onto the coating film.
[0035] When excimer light is irradiated using an excimer lamp, the peak wavelength of the electromagnetic wave can be changed by changing the discharge gas filled in the excimer lamp. The discharge gas for irradiating excimer light with the above peak wavelength can be, for example, Ar. 2 , Kr 2 , Xe 2 etc. can be used.
[0036] Then, by irradiating the coating with ultraviolet light (350 to 450 nm) to cure the coating, a surface layer 3 is formed on the surface of the substrate 2, and a decorative sheet 1 is produced in which wrinkles are formed on the surface 3a of the surface layer 3, as shown in Figure 1.
[0037] Even if the coating film is irradiated with excimer light having a short peak wavelength (within the range of 120 to 230 nm) instead of the ultraviolet light (350 to 450 nm), the coating film does not cure completely.
[0038] By irradiating the coating film with the above-mentioned excimer light, hardening occurs only on the outermost surface of the coating film, resulting in unevenness between the surface and the interior of the coating film, and coating components migrate from the unreacted parts inside the coating film to the surface, resulting in wrinkles being formed on the surface of the coating film.As a result, it becomes possible to control the gloss level of the surface layer 3.
[0039] Furthermore, in the decorative sheet 1 of the present invention, the gloss level of the surface 3a of the surface layer 3 is 2 or less due to the matting effect caused by the wrinkles described above, making it possible to achieve low gloss.
[0040] From the viewpoint of improving low gloss, the gloss of the surface 3a of the surface layer 3 is preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.5 or less.
[0041] Additionally, the term "glossiness" as used herein is an index of low glossiness, and refers to the 60° glossiness measured in accordance with a method conforming to JIS Z 8741:1997, which refers to the glossiness calculated based on the results of measurement using a photodetector installed in the direction of the reflection angle when light is incident at an incident angle of 60° on the measurement surface (surface 3a of the surface layer 3) of the decorative sheet 1.
[0042] Furthermore, in the decorative sheet 1 of the present invention, due to the formation of wrinkles by irradiation with excimer light as described above, the relationship represented by the following formula (2) is established between the gloss level described above and the interfacial development area ratio Sdr on the surface 3a of the surface layer 3, making it possible to achieve both the opposing properties of scratch resistance and three-dimensional formability, and as a result, it is possible to obtain a decorative sheet with excellent scratch resistance and three-dimensional formability.
[0043] [Number 2] Glossiness × (interface development area ratio Sdr + 1) ≧ 1.8 (2)
[0044] The "interfacial developed area ratio Sdr" referred to here is a parameter focusing on the planar direction and the height direction, and is used to evaluate the "three-dimensional surface quality (surface roughness)" specified in ISO 25178, and represents the rate at which the developed area (surface area) of the defined area increases relative to the area of the defined area. For example, in the case of a completely flat surface, the area of the defined area and the developed area (surface area) of the defined area are the same, so the interfacial developed area ratio Sdr is 0, but if the surface (defined area) is inclined, the developed area (surface area) of the defined area increases, so the interfacial developed area ratio Sdr becomes greater than 0.
[0045] As described above, the interface development area ratio Sdr indicates how much the development area (surface area) of the defined region has increased relative to the area of the defined region, so the value of the "interface development area ratio Sdr+1" indicates the ratio of the entire development area (surface area) of the defined region to the area of the defined region. For example, if the area of the defined region is S and the development area (surface area) of the defined region is 1.5S (i.e., 1.5 times the area of the defined region), the interface development area ratio Sdr is 0.5, and the ratio of the entire development area (surface area) of the defined region to the area of the defined region (i.e., the value of the interface development area ratio Sdr+1) is 1.5.
[0046] Furthermore, as the gloss level decreases, the number of wrinkles on the surface 3a of the surface layer 3 increases, and therefore the developed area (surface area) of the above-mentioned defined region increases, and the interfacial developed area ratio Sdr increases; however, when the gloss level is 2 or less and the relationship of the above formula (2) is established, it is possible to achieve low gloss while also achieving a balance between scratch resistance and three-dimensional formability, which are contradictory properties.
[0047] Similarly, as the gloss level increases, wrinkles on the surface 3a of the surface layer 3 decrease, and the developed area (surface area) of the above-mentioned defined region decreases, resulting in a smaller interfacial developed area ratio Sdr. However, when the gloss level is 2 or less and the relationship of the above formula (2) is established, it is possible to achieve low gloss while simultaneously achieving the opposing properties of scratch resistance and three-dimensional formability.
[0048] As described above, the present invention makes it possible to provide a decorative sheet that has low gloss due to a matte effect, and is also excellent in abrasion resistance and three-dimensional formability.
[0049] The wettability of the surface is correlated with the interfacial development area ratio Sdr, and the higher the interfacial development area ratio Sdr, the higher the wettability. Also, high wettability makes it easier for dirt to adhere. Therefore, from the viewpoint of improving the contamination resistance by lowering the wettability of the surface, the interfacial development area ratio Sdr of the surface 3a of the surface layer 3 is preferably 10 or less, more preferably 2 or less, and even more preferably 1 or less. EXAMPLES
[0050] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.
[0051] The materials used in producing the decorative sheet are shown below. (1) Urethane acrylate-1: Bifunctional urethane acrylate (manufactured by Mitsubishi Chemical Corporation, product name: UV-6630B) (2) Urethane acrylate-2: Bifunctional urethane acrylate (manufactured by Mitsubishi Chemical Corporation, product name: UV-6640B) (3) Urethane acrylate-3: Bifunctional urethane acrylate (manufactured by Mitsubishi Chemical Corporation, product name: UV-3300B) (4) Urethane acrylate-4: 4-functional urethane acrylate (manufactured by Daicel Allnex Co., Ltd., product name: EBECRYL8606) (5) Urethane acrylate - 5:9 functional urethane acrylate (manufactured by Mitsubishi Chemical Corporation, product name: UV-7620EA) (6) Urethane acrylate-6:10 functional urethane acrylate (manufactured by Daicel Allnex Co., Ltd., product name: KRM8452) (7) Multifunctional acrylate-1:3-functional acrylate (manufactured by Daicel Allnex Co., Ltd., product name: trimethylolpropane triacrylate (TMPTA)) (8) Multifunctional acrylate-2:4 functional acrylate (manufactured by Daicel Allnex Co., Ltd., product name: EBECRYL140) (9) Multifunctional acrylate-3:6-functional acrylate (manufactured by Daicel Allnex Co., Ltd., product name: dipentaerythritol hexaacrylate (DPHA)) (10) Monofunctional acrylate: tetrahydrofurfuryl acrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name: Light Acrylate THF-A) (11) Vinyl chloride-vinyl acetate copolymer: (manufactured by Nissin Chemical Industry Co., Ltd., product name: Solvine CL) (12) Initiator: alkylphenone-based photopolymerization initiator (manufactured by IGM Resins BV, product name: Omnirad1173)
[0052] Example 1 <Preparation of decorative sheet> First, a PVC substrate having a thickness of 350 μm was prepared. Next, the materials shown in Table 1 were mixed to prepare a coating material of Example 1 having the composition (parts by mass) shown in Table 1. This coating material was applied onto the surface of the substrate using a bar coater to form a coating film that would become a surface layer on the surface of the substrate.
[0053] Next, the above coating film was dried using a hot air dryer at a temperature of 50° C. for 20 seconds.
[0054] Next, using an excimer irradiation device (manufactured by Ushio Inc., product name: 172 nm Light Emission Unit, model: SUS1000), Xe 2 The coating was irradiated with excimer light (peak wavelength: 172 nm) using as the discharge gas. The cumulative light amount was 11 mJ / cm 2 , the irradiation intensity is 25mW / cm 2 The irradiation was performed so that
[0055] Then, the coating film was irradiated with ultraviolet light (dominant wavelength: 365 nm) using an ultraviolet light irradiation device (4 kW high-pressure mercury lamp for ultraviolet curing (ECS-401GX) manufactured by Eye Graphics Co., Ltd.) to photo-cure the coating film, thereby forming a surface layer on the surface of the substrate and producing a decorative sheet. Note that the ultraviolet light irradiation distance was 150 cm, and the lamp movement speed was 7.8 m / min, and the ultraviolet light irradiation (illuminance: 170 mW / cm 2 ) and the irradiation dose (accumulated light amount) was set to 200 mJ / cm 2 It was decided.
[0056] A laser microscope photograph showing the surface condition of the surface layer is shown in Figure 2. As shown in Figure 2, it can be seen that a large number of wrinkles are formed on the surface of the surface layer by irradiating the coating film that will become the surface layer with excimer light.
[0057] <Thickness measurement> Next, the thickness of the surface layer (coating film) of the prepared decorative sheet was measured using a digital microscope (Keyence Corporation, product name: VHX-5000) or a field emission scanning electron microscope (SEM) (Hitachi High-Technologies Corporation, product name: S-4800).
[0058] More specifically, the sheet was cut to expose the cross section, and the cross section was observed with a digital microscope (measurement magnification: 500x) or a field emission scanning electron microscope (measurement magnification: 1000x). Five locations with high and low coating film heights were selected, the thickness was measured, and the average value was calculated. The above measurement was performed three times, and the average value of the three coating film heights was calculated to be the thickness of the surface layer. The results are shown in Table 1.
[0059] <Gloss measurement> Next, the 60° gloss of the surface of the surface layer of the decorative sheet prepared above was measured using a gloss meter (manufactured by Horiba Ltd., product name: Gloss Checker IG-320) in accordance with JIS Z 8741:1997. The above measurement was performed five times, and the average value of the five gloss values was calculated to be the surface gloss of the surface layer. The results are shown in Table 1.
[0060] <Evaluation of three-dimensional formability> Next, an MDF substrate (a substrate having an approximately rectangular prism shape with a width of 100 mm, a length of 150 mm, and a thickness of 15 mm, all corners of which were chamfered with a radius of 2 mm) was prepared, and the decorative sheet prepared above was placed on the MDF substrate, and a vacuum forming machine (manufactured by Seibu Co., Ltd., product name: STN-40-600-800) was used to cover the top surface and four side surfaces of the MDF substrate, a total of five surfaces, with the decorative sheet, under a heating temperature of 110°C. Vacuum forming was performed on the top surface and four side surfaces of the MDF substrate, a total of five surfaces, so that the decorative sheet conformed to the MDF substrate, and the decorative sheet was adhered to the top surface and four side surfaces of the MDF substrate, a total of five surfaces. The state of the surface layer of the decorative sheet covering the top surface, sides, and corners of the MDF substrate was visually confirmed with the naked eye and with a 10x magnifying glass, and the three-dimensional formability was evaluated based on the following evaluation criteria. The results are shown in Table 1.
[0061] The decorative sheet is molded to fit the MDF base material, and there are no cracks or changes in gloss on the surface layer of the decorative sheet: ◎ The decorative sheet is molded to fit the MDF base material, but the surface layer of the decorative sheet has fine cracks that can be seen with a magnifying glass, or gloss changes that can be seen with the naked eye: Yes Cracks visible to the naked eye on the surface layer of the decorative sheet: ×
[0062] <Evaluation of abrasion resistance (resistance to fingernail scratches)> Next, the decorative sheet prepared above was placed on a glass plate, and the surface layer of the decorative sheet was rubbed five times at a speed of about 300 mm / sec with the nail of the index finger at an angle of about 90° to the surface layer of the decorative sheet (i.e., five different parts of the surface layer of the decorative sheet were rubbed once each). Then, the condition of the surface layer of the decorative sheet was visually confirmed, and the scratch resistance was evaluated based on the following evaluation criteria. The results are shown in Table 1.
[0063] No scratches found on the surface layer of the decorative sheet: ◎ There are thin scratches that can be seen depending on the angle at which the surface layer of the decorative sheet is observed: Yes There are thin scratches that can be seen regardless of the angle at which the surface layer of the decorative sheet is observed: △ There is a clearly recognizable large scratch on the surface layer of the decorative sheet: ×
[0064] <Measurement of interface development area ratio Sdr> Next, the interfacial development area ratio Sdr of the surface layer of the prepared decorative sheet was measured using a shape analysis laser microscope (Keyence Corporation, product name: VK-X1050) in accordance with ISO 25178. Note that a 661 nm semiconductor laser was used as the laser type, and in surface shape mode (high-speed mode), a standard objective lens of 50x was used, and a measurement range of 1024 pixels x 768 pixels (area of measurement area (defined area): 57567 μm 2 ) the developed area (surface area) of the defined region was measured, and the interfacial developed area ratio Sdr was measured. The above-mentioned measurements were also carried out at six arbitrary positions on the surface of the surface layer of the decorative sheet, and the average of the six interfacial developed area ratios Sdr was calculated, which was taken as the interfacial developed area ratio Sdr of the surface layer. The results are shown in Table 1.
[0065] (Examples 2 to 7, Comparative Examples 1 to 8) A decorative sheet was produced in the same manner as in Example 1 above, except that the composition of the coating components was changed to the composition shown in Table 1 (parts by mass).
[0066] Then, the thickness, gloss, three-dimensional moldability, and scratch resistance (nail scratch resistance) were measured, and the interfacial development area ratio Sdr was measured in the same manner as in Example 1. The results are shown in Tables 1 and 2.
[0067] Moreover, Fig. 3 shows a laser microscope photograph showing the surface state of the surface layer of the decorative sheet of Example 2. As shown in Fig. 3, it can be seen that a large number of wrinkles are formed on the surface of the surface layer by irradiating the coating film that becomes the surface layer with excimer light.
[0068] [Table 1]
[0069] [Table 2]
[0070] As shown in Table 1, the decorative sheets of Examples 1 to 7, in which the gloss of the surface layer is 2 or less, have low gloss due to the matte effect. Furthermore, in the decorative sheets of Examples 1 to 7, the relationship of the above formula (2) is established between the gloss and the interfacial development area ratio Sdr at the surface of the surface layer, so it is possible to achieve both scratch resistance and three-dimensional formability, which are contradictory properties, and it is possible to obtain decorative sheets with excellent scratch resistance and three-dimensional formability. [Industrial Applicability]
[0071] As described above, the present invention is suitable for decorative sheets. [Explanation of symbols]
[0072] 1 Decorative sheet 2 Base material 2a Surface of the substrate 3 Surface layer 3a Surface of the surface layer
Claims
1. A substrate; a surface layer provided on the surface of the substrate; Equipped with The gloss level of the surface layer is 2 or less, A decorative sheet characterized in that the relationship between the glossiness and the interfacial development area ratio Sdr of the surface layer on the surface opposite the substrate side satisfies the following formula (1): [Equation 1] Glossiness × (interface development area ratio Sdr + 1) ≧ 1.8 (1)
2. 2. The decorative sheet according to claim 1, wherein the surface layer is an excimer irradiated product.
3. 3. The decorative sheet according to claim 1, wherein the surface layer contains a di- to deca-functional urethane acrylate and a monofunctional acrylate.
Citation Information
Patent Citations
Matte article and method for manufacturing same
JP2022008024A
Decorative sheet
JP2024049531A
Decorative sheet, decorative sheet set and method of constructing decorative sheet
JP2015077691A
Method of manufacturing building material
JP2018164901A
Cited By
Decorative sheet
US12735602B2
Decorative sheet
US20250179325A1