Deoxidation method of molten steel

By adjusting the Al addition rate and dissolved oxygen concentration in relation to molten steel circulation flow rate, the method stabilizes Al loss during molten steel deoxidation, overcoming equipment complexity and heat generation challenges.

JP2024141873AInactive Publication Date: 2024-10-10JFE STEEL CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023053729
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for deoxidizing molten steel using Al or Al alloy in a vacuum degassing device are complicated, require specialized equipment, and do not account for heat generation and reflux during deoxidation, leading to unstable Al loss.

Method used

A method for deoxidizing molten steel by adding Al or Al alloy based on the relationship between the addition rate, dissolved oxygen concentration, and molten steel circulation flow rate, using the formula F/(C/10^6 × Q) ≥ 24, where F is the Al addition rate, C is the dissolved oxygen concentration, and Q is the molten steel reflux flow rate, to stabilize Al loss at a low level without specialized equipment.

Benefits of technology

The method minimizes Al loss by stabilizing it at a low level, eliminating the need for specialized equipment and addressing heat generation and reflux issues, ensuring efficient deoxidation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141873000001_ABST
    Figure 2024141873000001_ABST
Patent Text Reader

Abstract

To provide a deoxidation method of molten steel that does not need dedicated equipment for adding Al or an Al alloy and can stabilize a loss Al amount to a low level when adding the Al or the Al alloy in the deoxidation method of the molten steel conducted by adding the Al or the Al alloy.SOLUTION: A deoxidation method of molten steel to deoxidize molten steel by adding Al or an Al alloy with a vacuum degasser includes adding the Al or the Al alloy into the molten steel on the basis of the relation among an addition rate of the Al or the Al alloy, dissolved oxygen concentration in the molten steel, and a molten steel circulation flow amount.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for removing oxygen in molten steel using a vacuum degassing device, and more particularly to a method for deoxidizing molten steel by adding Al or an Al alloy to the molten steel.

Background Art

[0002] Deoxidation of molten steel performed using a vacuum degassing device is carried out by adding Al or an Al alloy (hereinafter simply referred to as "Al") to the molten steel. The addition amount of Al added to the molten steel is determined based on the amount required to deoxidize the dissolved oxygen in the molten steel and the amount required for adjusting the components of the molten steel.

[0003] Here, Al added to the molten steel has a smaller specific gravity compared to various elements in the molten steel. Therefore, during the refining process using a vacuum degassing device, when Al is added to the molten steel, reactions between Al and the atmosphere and between Al and slag occur, and evaporation of Al also occurs. Therefore, it is necessary to increase the addition amount of Al to the molten steel on the premise of the specific gravity and evaporation of Al. Regarding the method for deoxidizing molten steel by adding Al to the molten steel, the following has been conventionally studied.

[0004] Patent Document 1 discloses a method of charging a container containing a specific gravity adjusting material and a deoxidizing agent (Al) into molten steel. Further, regarding the form of Al to be added, Non-Patent Document 1 discloses a method of pushing a wire-shaped Al wire at a high speed, Non-Patent Document 2 discloses a method of blowing powdered Al powder, and Non-Patent Document 3 discloses a method of injecting molten Al.

[0005] Also, in a vacuum degassing device which is secondary refining after primary refining, it is considered that the evaporation amount of Al further increases due to the deoxidation treatment under high vacuum. For this reason, Patent Document 2 discloses, as a solution, a method in which the pressure V when adding Al to the molten steel is set to 20 Torr < V ≤ 760 Torr.

Prior Art Documents

Patent Documents

[0006] [Patent Document 1] Japanese Patent Application Publication No. 53-64613 [Patent Document 2] Japanese Patent Application Publication No. 11-172322 [Non-patent literature]

[0007] [Non-Patent Document 1] "Tetsu to Hagane", vol.56, No.11, (1970), S430 [Non-Patent Document 2] "Tetsu to Hagane", vol.66, No.4, (1980), S267 [Non-Patent Document 3] "Tetsu to Hagane", vol.69, No.4, (1983), S189 [Non-Patent Document 4] "Tetsu to Hagane", vol.73, No.4, (1987), S176 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the method disclosed in Patent Document 1 requires the placement of a specific gravity adjuster and a deoxidizer (Al) in a container and the adjustment of the specific gravity, making the process of adding Al to molten steel more complicated. In addition, the methods disclosed in Non-Patent Documents 1 to 3 require dedicated equipment for adding Al. The method disclosed in Patent Document 2 does not take into account the heat generated by the reaction between Al and the oxygen dissolved in the molten steel, and the disclosed pressure range includes a range in which it becomes difficult to reflux the molten steel during the deoxidation treatment of the molten steel.

[0009] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for deoxidizing molten steel by adding Al or an Al alloy, which does not require any dedicated facility for adding Al or an Al alloy, and which can stabilize the amount of Al loss when adding Al or an Al alloy at a low level. [Means for solving the problem]

[0010] The gist of the present invention is as follows.

[0011] [1] A method for deoxidizing molten steel using a vacuum degassing apparatus to add Al or an Al alloy to deoxidize the molten steel, the method comprising adding the Al or Al alloy to the molten steel based on the relationship between the addition rate of the Al or Al alloy, the dissolved oxygen concentration in the molten steel, and the amount of molten steel circulated. [2] The method for deoxidizing molten steel according to [1], wherein the Al or Al alloy is added to molten steel so as to satisfy the following formula (1): F / (C / 10 6 × Q)≧24 (1) Q = 7438 x G 1 / 3 ×D 4 / 3 ×(ln(101325 / P)) 1 / 3 / W···(2) where F is the rate of addition of Al or Al alloy (kg / s t), C is the dissolved oxygen concentration in the molten steel (ppm), Q is the amount of circulated molten steel (kg / s t), and G is the amount of circulated gas (Nm 3 / s), D is the diameter of the immersion tube (m), P is the degree of vacuum in the vacuum chamber (Pa), and W is the amount of molten steel (tons). Effect of the Invention

[0012] According to the present invention, in a method for deoxidizing molten steel by adding Al or an Al alloy, it is possible to stabilize the amount of Al loss that occurs when adding Al or an Al alloy at a low level without requiring any dedicated equipment for adding Al or an Al alloy. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic vertical cross-sectional view of an example of a vacuum degassing apparatus. [Diagram 2] FIG. 13 is a graph showing the relationship between the adjustment ratio and the amount of Al loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail. Fig. 1 shows a schematic vertical cross-sectional view of an example of a vacuum degassing apparatus 1. The vacuum degassing apparatus 1 may be an RH vacuum degassing apparatus. The vacuum degassing apparatus 1 has a ladle 2, a vacuum tank 5, an ascending side immersion tube 6, a descending side immersion tube 7, a reflux gas blowing pipe 8, a duct 9, and a raw material inlet 10.

[0015] First, molten iron is decarburized and refined in a converter, and the molten steel 3 and slag 4 obtained by the decarburization are tapped into a ladle 2. The molten steel 3 may be in an undeoxidized state. If necessary, an Al-containing slag modifier may be added onto the slag 4 covering the molten steel 3 in the ladle 2. As long as the Al-containing slag modifier can be added in a dispersed manner from above the slag 4, there is no need to use dedicated equipment for adding the Al-containing slag modifier.

[0016] In the vacuum degassing apparatus 1, the ladle 2 containing the molten steel 3 is raised by a lifting device (not shown), and the upflow side immersion tube 6 and the downflow side immersion tube 7 are immersed in the molten steel 3 in the ladle 2. The inside of the vacuum chamber 5 is then evacuated by an exhaust device (not shown) connected to a duct 9 to reduce the pressure inside the vacuum chamber 5, and reflux gas is blown into the upflow side immersion tube 6 from the reflux gas blowing tube 8. When the pressure inside the vacuum chamber 5 is reduced, the molten steel 3 in the ladle 2 rises in proportion to the difference between the atmospheric pressure and the pressure (degree of vacuum) inside the vacuum chamber 5, and flows into the vacuum chamber 5. The molten steel 3 in the ladle 2 rises up the upflow side immersion tube 6 together with the reflux gas bubbles 11 due to the gas lift effect caused by the reflux gas bubbles 11 blown from the reflux gas blowing tube 8, and flows into the vacuum chamber 5. Argon gas is generally used as the reflux gas.

[0017] The molten steel 3 that flows into the vacuum vessel 5 due to the pressure difference and the gas lift effect returns to the ladle 2 via the downflow side immersion pipe 7. This flow of the molten steel 3 flowing from the ladle 2 to the vacuum vessel 5 and then returning from the vacuum vessel 5 to the ladle 2 is called the "reflux flow." In this way, the molten steel 3 forms a reflux flow, and the molten steel 3 is subjected to vacuum degassing refining.

[0018] When the molten steel 3 is not yet deoxidized, a decarburization reaction of the molten steel 3 proceeds by vacuum degassing refining. After the decarburization is completed, the concentration of dissolved oxygen in the molten steel 3 is measured. Based on the measured concentration of dissolved oxygen in the molten steel, a total amount of Al is calculated, which is the amount of Al added (stoichiometric amount) required for deoxidation, the amount of Al added required for adjusting the composition of the molten steel 3, and the amount of Al added corresponding to the amount of Al lost due to evaporation of Al (hereinafter referred to as the "lost Al amount"). Based on the calculated total amount of Al, Al is added to the molten steel 3 in the vacuum tank 5 through the raw material inlet 10. As a result, the deoxidization of the molten steel 3 proceeds. After that, the composition of the molten steel 3 is adjusted as a cast slab after casting, the temperature is adjusted, and inclusions (alumina, etc.) in the molten steel are removed. The lost Al amount includes the amount lost due to a reaction with the atmosphere, the amount lost due to a reaction with the slag 4, and the amount lost due to evaporation.

[0019] The inventors considered that the amount of Al added to the molten steel 3 (total Al amount) can be roughly divided into the amount of Al added (stoichiometric amount) required for deoxidation, the amount of Al added required for adjusting the composition of the molten steel 3, and the amount of Al lost due to evaporation of Al, etc. Furthermore, they came to the conclusion that the amount of Al lost is due to oxidation accompanying a reaction with oxides contained in the slag 4, oxidation accompanying contact with the air, and evaporation of Al inside the vacuum tank 5. Then, in order to reduce the amount of Al lost due to evaporation (hereinafter referred to as "Al evaporation loss"), they focused on the degree of vacuum inside the vacuum tank 5, the temperature of the molten steel 3 flowing into the vacuum tank 5, and the concentration of Al in the molten steel 3 (hereinafter referred to as "Al concentration").

[0020] The degree of vacuum inside the vacuum chamber 5 can be made low by lowering the exhaust output of the exhaust device connected to the duct 9. The present inventors considered that by making the inside of the vacuum chamber 5 low vacuum, it is possible to reduce the amount of Al evaporation loss.

[0021] The temperature of the molten steel 3 flowing into the vacuum vessel 5 decreases as the amount of Al added increases due to the sensible heat of the added Al. On the other hand, when the concentration of dissolved oxygen in the molten steel is high, the temperature of the molten steel 3 increases because the reaction with the added Al (deoxidation) is an exothermic reaction. That is, the temperature of the molten steel 3 is determined by the balance between the sensible heat of the added Al and the exothermic reaction due to deoxidation. For this reason, the inventors considered that the temperature of the molten steel 3 in the vacuum vessel 5 is determined by the balance between the addition rate of Al added to the molten steel 3, the concentration of dissolved oxygen in the molten steel 3 flowing from the ladle 2, and the amount of molten steel refluxed from the molten steel 3. Then, the inventors considered that it is possible to reduce the amount of Al evaporation loss by lowering the temperature of the molten steel 3 inside the vacuum vessel 5. Furthermore, the inventors considered that it is effective to increase the addition rate of Al, lower the concentration of dissolved oxygen in the molten steel 3, and reduce the amount of molten steel refluxed from the molten steel 3 in order to lower the temperature of the molten steel 3.

[0022] On the other hand, the Al concentration in the molten steel 3 increases as the rate of addition of Al increases, and the amount of Al evaporation loss increases. For this reason, the present inventors also considered that there is a possibility that the increase in the Al concentration can be suppressed and the amount of Al evaporation loss can be reduced by slowing down the rate of addition of Al.

[0023] Based on these results, in order to reduce the amount of Al evaporation loss, the ratio of the Al addition rate, which can be increased or decreased to have any effect, to the dissolved oxygen concentration in molten steel and the molten steel reflux rate, which can be decreased to be effective (hereinafter referred to as the "adjustment ratio") was calculated, and the relationship with the amount of Al evaporation loss was investigated. The ratio [-(dimensionless number)] (adjustment ratio) of the Al addition rate F to the dissolved oxygen concentration in molten steel C and the molten steel reflux rate Q was calculated using the following formula (3).

[0024] F / (C / 10 6 ×Q) ···(3) Here, F is the addition rate of Al or Al alloy (kg / s t), C is the dissolved oxygen concentration in molten steel (ppm), and Q is the amount of molten steel returned to the steel (kg / s t).

[0025] The amount of molten steel circulated Q was calculated using the following formula (2) (see Non-Patent Document 4). As shown in formula (2), the degree of vacuum P in the vacuum vessel was used as a factor that influences the amount of molten steel circulated Q. The degree of vacuum P in the vacuum vessel was used as a factor that determines the amount of molten steel circulated Q, taking into consideration the relationship between the degree of vacuum in the vacuum vessel 5 and the change in the amount of molten steel 3 circulated, and due to the commonality of the effect in reducing the amount of Al evaporation loss.

[0026] Q = 7438 x G 1 / 3 ×D 4 / 3 ×(ln(101325 / P)) 1 / 3 / W···(2) Here, G is the reflux gas flow rate (Nm 3 / s), D is the diameter of the immersion tube (m), P is the degree of vacuum in the vacuum chamber (Pa), and W is the amount of molten steel (tons).

[0027] Next, the operating conditions in the vacuum degassing equipment 1 were changed to investigate the relationship between the value calculated by formula (3) (adjustment ratio) and the amount of Al loss (kg / t). In the investigation, first, the dissolved oxygen concentration in the molten steel was measured before adding Al, and then Al was added to the molten steel 3 inside the vacuum tank 5 at a predetermined addition rate, and a sample of the molten steel 3 was taken and the Al concentration was analyzed. The amount obtained by subtracting the amount of Al added required for deoxidation (stoichiometric ratio calculation) and the amount of dissolved Al calculated from the Al concentration in the sample (corresponding to the amount of Al added required for component adjustment) from the amount of Al added was determined as the amount of Al loss (kg / t).

[0028] As a result, it was found that the amount of Al loss decreases with an increase in the value of the adjustment ratio. And, it was found that the amount of Al loss shows a constant value when the value of the adjustment ratio is 24 or more. That is, as shown in the following formula (1), when the relationship of the ratio of the Al addition rate F to the dissolved oxygen concentration C in the molten steel and the molten steel reflux amount Q is 24 or more is satisfied, it was found that the amount of Al loss can be stabilized at a low level, that is, the fluctuation of the value of the amount of Al loss can be suppressed. In other words, by adjusting the operating conditions so that the ratio of the Al addition rate F to the oxygen concentration C in the molten steel and the molten steel reflux amount Q is 24 or more, the amount of Al loss can be minimized. In this case, the amount of Al evaporation loss included in the amount of Al loss is also minimized. The amount of Al loss includes not only the amount of Al evaporation loss, but also the amount consumed by oxidation accompanying the reaction with oxides contained in the slag 4 and oxidation accompanying contact with the air.

[0029] F / (C / 10 6 × Q)≧24 (1)

[0030] Therefore, in the deoxidation method for deoxidizing molten steel 3 using a vacuum degassing apparatus 1, when adding Al to the molten steel 3 inside the vacuum tank 5, the amount of Al lost can be minimized by adjusting the operating conditions so that the ratio of the Al addition rate F to the oxygen concentration C in the molten steel and the molten steel reflux amount Q is 24 or more.

[0031] That is, in a method for deoxidizing molten steel 3 by adding Al or an Al alloy using a vacuum degassing apparatus 1, the amount of Al loss can be minimized by adding Al to the molten steel 3 based on the relationship between the Al addition rate F, the dissolved oxygen concentration C in the molten steel, and the molten steel circulation amount Q. That is, the amount of Al added to the molten steel 3 does not require any dedicated equipment for adding Al or an Al alloy, and it is possible to stabilize the amount of Al loss when adding Al or an Al alloy at a low level.

[0032] Although it is not necessary to set an upper limit value on the left side of equation (1), a value may be set within a range that does not adversely affect the operation of the vacuum degassing equipment 1. The Al addition rate F and the degree of vacuum P in the vacuum chamber need to be adjusted as follows.

[0033] If the addition rate F is increased so fast that the sensible heat of Al causes the temperature of the molten steel to fall below the liquidus temperature of the molten steel components, the fluidity of the molten steel 3 will decrease, affecting operation. For this reason, it is necessary to maintain the temperature of the molten steel 3 at or above the liquidus temperature of the molten steel components, by combining the heat generated by deoxidation and the heat removed by the sensible heat of the additives. Specifically, it is preferable to set the addition rate F at a value that ensures a liquidus temperature of 10°C or higher.

[0034] The larger the degree of vacuum P in the vacuum tank (lower the degree of vacuum), the smaller the amount of molten steel circulating Q. In this case, the left side of equation (1) becomes larger, which is preferable, but the molten steel will not circulate unless the molten steel 3 is sucked up to the inside of the vacuum tank 5 at a low degree of vacuum. For this reason, it is preferable to set in advance a degree of vacuum that allows the molten steel 3 to circulate using an inside-tank observation camera or the like, and to ensure that the degree of vacuum does not exceed the set degree of vacuum when Al is added.

[0035] Furthermore, when an Al alloy is used for addition to the molten steel 3, if the Al purity is low, the sensible heat of the alloy increases, and it is not possible to increase the addition rate F of the Al alloy. For this reason, it is desirable to use Al or a high-purity Al alloy. EXAMPLES

[0036] Approximately 315 to 330 tons of molten steel with a carbon concentration of 0.02 to 0.06 mass% was tapped from the converter into a ladle with an inner diameter of 3.2 m without being deoxidized, and vacuum treatment was performed in an RH vacuum degassing device to reduce the carbon concentration to a specified concentration. Then, the addition rate was changed and the amount of Al required for deoxidation treatment was added to the molten steel. After addition, a reflux treatment was performed for 2 minutes in the RH vacuum degassing device, after which a sample of the molten steel was taken and submitted for analysis.

[0037] Table 1 shows the operating conditions in the examples, the "ratio (adjustment ratio) between the rate of addition of Al and the oxygen concentration in molten steel and the amount of molten steel returned" obtained from the operating conditions, and the amount of Al loss. FIG. 2 shows the relationship between the adjustment ratio and the amount of Al loss. Comparative Examples 1 to 14 show examples in which the adjustment ratio was set to a value smaller than 24. Invention Examples 1 to 14 show examples in which the adjustment ratio was set to a value of 24 or more.

[0038] [Table 1]

[0039] As shown in Table 1 and FIG. 2, in Comparative Examples 1 to 14, the smaller the adjustment ratio, the larger the amount of Al loss. On the other hand, it was confirmed that in Inventive Examples 1 to 14, regardless of whether the adjustment ratio was increased or decreased, the amount of Al loss was almost constant and showed the minimum value. That is, it was confirmed that the amount of Al loss can be minimized by setting the operating conditions such that the ratio of the Al addition rate to the oxygen concentration in the molten steel and the amount of molten steel reflux is 24 or more. That is, it was confirmed that by adding Al to molten steel based on the relationship between the Al addition rate, the dissolved oxygen concentration in the molten steel, and the amount of molten steel reflux, it is possible to stabilize the amount of Al loss at a low level when adding Al or an Al alloy without requiring a dedicated facility for adding Al or an Al alloy. [Explanation of symbols]

[0040] 1 Vacuum degassing equipment 2 ladle 3. Molten Steel 4. Slug 5 Vacuum chamber 6. Upward dip tube 7 Descending dip tube 8. Circulation gas inlet pipe 9 Duct 10 Raw material input port 11 Gas Bubbles

Claims

1. A method for deoxidizing molten steel using a vacuum degassing apparatus to add Al or an Al alloy to deoxidize the molten steel, the method comprising adding the Al or Al alloy to the molten steel based on a relationship between an addition rate of the Al or Al alloy, a dissolved oxygen concentration in the molten steel, and a circulation amount of the molten steel.

2. The method for deoxidizing molten steel according to claim 1 , wherein the Al or Al alloy is added to the molten steel so as to satisfy the following formula (1): F / (C / 10 6 ×Q)≧24 ・・・(1) Q=7438×G 1/3 ×D 4/3 ×(ln(101325 / P)) 1/3 / W・・・(2) Here, F is the rate of addition of Al or Al alloy (kg / s.t), C is the dissolved oxygen concentration in molten steel (ppm), Q is the amount of molten steel returned (kg / s.t), and G is the amount of returned gas (Nm 3 / s), D is the diameter of the immersion tube (m), P is the degree of vacuum in the vacuum chamber (Pa), and W is the amount of molten steel (tons).

Citation Information

Patent Citations

  • Molten steel deoxidation and alloy adding method

    JP1978064613A

  • Method for aluminum-deoxidizing molten steel

    JP1999172322A