Negative electrode material for lithium ion secondary battery, manufacturing method thereof, and negative electrode for lithium ion secondary battery using the same

The negative electrode material with a polymer-coated active material using carboxyl group-containing and imide-based polymers addresses the collapse issue in silicon-based electrodes, maintaining capacity and conductivity, thus enhancing the battery's cycle life.

JP2024141972APending Publication Date: 2024-10-10SUMITOMO RIKO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023053886
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing negative electrode materials for lithium ion secondary batteries using silicon-based active materials face issues with particle collapse due to expansion and contraction, leading to decreased capacity and shortened cycle life due to disconnection of conductive paths and inadequate lithium ion conductivity.

Method used

A negative electrode material is developed with a polymer-coated active material surface using a carboxyl group-containing polymer for lithium ion conductivity and a binder with an imide-based polymer for structural support, ensuring electronic conductivity and maintaining conductive paths despite material deformation.

Benefits of technology

The solution maintains high capacity and excellent cycle characteristics by preventing particle disintegration and ensuring smooth lithium ion movement, even after repeated charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141972000001_ABST
    Figure 2024141972000001_ABST
Patent Text Reader

Abstract

To provide a negative electrode material that can realize a lithium ion secondary battery whose capacity does not decrease even with repeated charging and discharging by suppressing breakage of the particles of a negative electrode active material and maintaining a conductive path, and a method for manufacturing the same.SOLUTION: A negative electrode material for a lithium ion secondary battery includes a polymer-coated active material including a negative electrode active material and a polymer layer having a carboxyl group-containing polymer and a conductive assistant and coating the surface of the negative electrode active material, and a binder having an imide-based polymer and a conductive assistant and binding the polymer-coated active materials together. A method for manufacturing the negative electrode material includes a step of dispersing the negative electrode active material in coating polymer liquid having a carboxyl group-containing polymer and a conductive assistant to prepare active material-containing liquid, a step of preparing binder liquid having an imide-based polymer and a conductive assistant, and a step of mixing the active material-containing liquid and the binder liquid to prepare negative electrode material liquid.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to negative electrodes for lithium ion secondary batteries, and in particular to negative electrode materials and methods for producing the same. [Background technology]

[0002] Lithium-ion secondary batteries have a relatively high energy density and are widely used as power sources for various electronic devices, electric vehicles, hybrid vehicles, etc. The negative electrode of a lithium-ion secondary battery is formed by mixing a powdered negative electrode active material with a binder, adding a solvent to make a paste of the negative electrode material, applying the paste to the surface of a current collector, and drying the paste. Carbon materials are known as negative electrode active materials, but from the viewpoint of increasing the battery capacity, the use of silicon materials with high capacity density is being investigated.

[0003] Silicon (Si) and silicon oxide (SiO x Silicon materials such as silicon carbide (SrAl2O3) expand and contract significantly as they absorb and release lithium ions during charging and discharging. Repeated expansion and contraction can cause the particles of the active material to break down or the connections between the active materials to be severed, resulting in a loss of conductive paths. As a result, the amount of silicon material that contributes to the absorption and release of lithium ions decreases, and the capacity decreases. Thus, when silicon materials are used, there is an issue that the capacity decreases significantly due to repeated charging and discharging, resulting in a short cycle life.

[0004] As a technique for improving the cycle characteristics of a lithium secondary ion battery, for example, Patent Document 1 describes a negative electrode material in which the particle surface of a negative electrode active material such as silicon oxide is coated with carbon, and carbon fibers are further attached to the surface with polyimide resin or the like. Patent Document 1 describes a negative electrode in which a layer containing the negative electrode material, a carbon material that occludes and releases lithium ions, and a binder is formed on a current collector. Patent Document 2 describes a binding agent (binder) in which polyamideimide and a carboxyl group-containing polymer are mixed. Patent Document 2 describes a method of manufacturing a negative electrode by applying a slurry, which is obtained by adding an organic solvent to a negative electrode mixture that is a mixture of a negative electrode active material made of a silicon material, the mixed binder, and a conductive assistant, to the surface of a current collector and drying the slurry. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2015 / 083262 [Patent Document 2] JP 2016-46151 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the negative electrode material of Patent Document 1, a conductive path is formed by carbon fibers adhered to the particle surface of the negative electrode active material. However, as described in paragraphs

[0029] and

[0032] of the same document, the carbon fibers merely form a conductive path between the negative electrode active material and the carbon material present around it. Therefore, even if the carbon fibers are adhered, it is difficult to suppress the collapse of particles due to the expansion and contraction of the negative electrode active material, or the disconnection between the active materials.

[0007] In Patent Document 2, the retention capacity of the negative electrode active material is improved by using a binder having different resin components, namely, polyamideimide and carboxyl group-containing polymer. As described in paragraphs

[0024] and

[0034] of the same document, polyamideimide and carboxyl group-containing polymer have different properties in terms of reactivity to lithium ions, strength, etc. However, according to Patent Document 2, polyamideimide and carboxyl group-containing polymer are mixed in advance to produce a binder, and then it is mixed with the negative electrode active material (paragraphs

[0054] -

[0059] ). In this case, since the polyamideimide and carboxyl group-containing polymer are arranged around the negative electrode active material in a mixed state, the characteristics of each component are not easily exhibited. For example, the carboxyl group-containing polymer has lithium ion conductivity, but the polyamideimide does not. Therefore, if there is little carboxyl group-containing polymer present in the vicinity of the negative electrode active material, it becomes difficult to supply lithium ions to the negative electrode active material.

[0008] In addition, in order to improve the electrical conductivity (electronic conductivity), a conductive assistant such as acetylene black is often mixed with the binder in the negative electrode. After repeated studies, the present inventor has found that since the conductive assistant is difficult to disperse in the carboxyl group-containing polymer, when the conductive assistant is mixed with the mixture of polyamideimide and the carboxyl group-containing polymer, the conductive assistant may be unevenly distributed on the polyamideimide side. Therefore, when the binder, which is a mixture of polyamideimide and the carboxyl group-containing polymer, is mixed with the conductive assistant and the negative electrode active material, even if the carboxyl group-containing polymer is present in the vicinity of the negative electrode active material, the conductive assistant contained therein is small, so that the electronic conductivity on the surface of the negative electrode active material may be reduced, and the absorption and release of lithium ions in the negative electrode active material may be inhibited.

[0009] The present disclosure has been made in consideration of the above-mentioned circumstances, and has an object to provide a negative electrode material that can realize a lithium-ion secondary battery whose capacity is not easily reduced even with repeated charging and discharging by suppressing the collapse of particles of the negative electrode active material and the disconnection of connections between negative electrode active materials and maintaining a conductive path, a method for producing the same, and a negative electrode for a lithium-ion secondary battery using the same. [Means for solving the problem]

[0010] (1) In order to solve the above problems, the negative electrode material for a lithium ion secondary battery disclosed herein is characterized by having a polymer-coated active material having a negative electrode active material, a polymer layer having a carboxy group-containing polymer and a conductive assistant and coating a surface of the negative electrode active material, and a binder having an imide-based polymer and a conductive assistant and binding the polymer-coated active materials together.

[0011] The negative electrode material for lithium ion secondary batteries of the present disclosure (hereinafter, sometimes simply referred to as the "negative electrode material of the present disclosure") has a polymer-coated active material in which the surface of the negative electrode active material is coated with a polymer layer. The carboxyl group-containing polymer constituting the polymer layer has lithium ion conductivity, and therefore the movement of lithium ions to the negative electrode active material is not easily hindered. The carboxyl group-containing polymer is relatively flexible and has high adhesion to the negative electrode active material, and therefore has excellent conformability to deformation of the negative electrode active material. Furthermore, the polymer layer has a conductive assistant. This maintains electronic conductivity on the surface of the negative electrode active material, and allows the negative electrode active material to smoothly absorb and release lithium ions.

[0012] The binder that bonds the polymer-coated active material to each other contains an imide-based polymer. The imide-based polymer has high strength, so it can suppress deformation due to expansion and contraction of the negative electrode active material (polymer-coated active material) and suppress separation of the active material particles. This makes it possible to maintain the conductive path even after repeated charging and discharging. Furthermore, the binder contains a conductive assistant, which also maintains the electronic conductivity of the binder.

[0013] The negative electrode material of the present disclosure has been developed based on the technical idea of ​​arranging two types of polymers with different properties, a carboxyl group-containing polymer and an imide-based polymer, in a location where their properties can be utilized. The conductive assistant is also reliably arranged in the polymer layer that covers the surface of the negative electrode active material, thereby maintaining the electronic conductivity of the surface of the negative electrode active material. According to the negative electrode material of the present disclosure, the carboxyl group-containing polymer (polymer layer) can maintain lithium ion conductivity, while the imide-based polymer, which has high strength, can suppress deformation of the negative electrode active material and maintain electronic conductivity. As a result, a lithium ion secondary battery with excellent cycle characteristics and a low capacity even when repeatedly charged and discharged can be realized.

[0014] (2) In the above configuration, the content of the carboxyl group-containing polymer may be 1.0% by mass or more and 4.0% by mass or less, based on 100% by mass of the negative electrode active material. With this configuration, an appropriate amount of polymer layer is formed on the surface of the negative electrode active material, and the effects of imparting electronic conductivity and lithium ion conductivity can be fully exhibited.

[0015] (3) In any of the above configurations, the content ratio of the imide-based polymer to the carboxyl group-containing polymer may be from 2 to 9, where the mass of the carboxyl group-containing polymer is taken as 1. With this configuration, it is possible to enhance the effect of the imide-based polymer in suppressing deformation of the negative electrode active material, while reducing irreversible reactions with lithium ions in the electrolyte when a lithium ion secondary battery is constructed, thereby suppressing a decrease in capacity.

[0016] (4) In any of the above configurations, the negative electrode material according to the present disclosure may have a volume resistivity of 0.5 Ω·cm or less. With this configuration, desired electronic conductivity can be achieved.

[0017] (5) In the above configuration (4), the content of the imide-based polymer may be 7.0% by mass or more when the mass of the negative electrode active material is taken as 100% by mass. This configuration has a high effect of suppressing deformation of the negative electrode active material, so that the initial high conductivity (before charging and discharging) can be maintained even after repeated charging and discharging, and a decrease in capacity can be suppressed.

[0018] (6) In any one of the above configurations, the negative electrode active material may contain silicon. With this configuration, a lithium ion secondary battery with a large capacity can be realized.

[0019] (7) In any of the above configurations, the carboxyl group-containing polymer may be one or more selected from polyacrylic acid, polymethacrylic acid, polyaspartic acid, polyglutamic acid, and carboxymethyl cellulose. According to this configuration, the carboxyl group-containing polymer covers the negative electrode active material and plays the role of SEI (Solid Electrolyte Interphase), which makes it difficult for the negative electrode active material to come into direct contact with the electrolyte, suppresses the decomposition reaction of the electrolyte, and suppresses deterioration of the cycle characteristics. In addition, since the polymer has sufficient reduction resistance against the negative electrode potential, deterioration of the polymer layer due to charging and discharging is unlikely to occur, and deterioration of the cycle characteristics can be suppressed.

[0020] (8) In any of the above configurations, the imide-based polymer may be one or more selected from the group consisting of polyamideimide and polyimide. The polymer of this configuration has high strength, so it is highly effective in suppressing deformation caused by expansion and contraction of the negative electrode active material, and it is easy to maintain the conductive path in the binder.

[0021] (9) A method for producing a negative electrode material for a lithium-ion secondary battery according to the present disclosure, which is one embodiment of the method for producing a negative electrode material according to the present disclosure (hereinafter, may be simply referred to as the “production method according to the present disclosure”), is characterized by comprising an active material-containing liquid preparation step of preparing an active material-containing liquid by dispersing a negative electrode active material in a coating polymer liquid having a carboxy group-containing polymer and a conductive assistant, a binder liquid preparation step of preparing a binder liquid having an imide-based polymer and a conductive assistant, and a negative electrode material liquid preparation step of mixing the active material-containing liquid and the binder liquid to prepare a negative electrode material liquid.

[0022] In the manufacturing method of the present disclosure, in the active material-containing liquid preparation step, the negative electrode active material is dispersed in a coating polymer liquid. In this way, a polymer-coated active material is produced in which the surface of the negative electrode active material is coated with a polymer layer containing a carboxyl group-containing polymer and a conductive assistant. Separately from this, in the binder liquid preparation step, a binder liquid containing an imide-based polymer and a conductive assistant is prepared. Then, in the negative electrode material liquid preparation step, the active material-containing liquid containing the polymer-coated active material and the binder liquid are mixed.

[0023] In this manner, in the manufacturing method of the present disclosure, the carboxyl group-containing polymer and the imide-based polymer are used without being mixed in advance. Then, by disposing two types of polymers with different characteristics in a location where their characteristics can be utilized, each of the characteristics can be exhibited without impeding the other's characteristics. In addition, by blending a conductive assistant in both the active material-containing liquid and the binder liquid, uneven distribution of the conductive assistant in the imide-based polymer can be suppressed, and the conductive assistant can be reliably disposed in the polymer layer that covers the negative electrode active material. According to the manufacturing method of the present disclosure, the above-mentioned negative electrode material of the present disclosure that can realize a lithium ion secondary battery with excellent cycle characteristics can be easily manufactured.

[0024] (10) In the active material-containing liquid preparation step in the above configuration (9), the blending ratio of the conductive assistant to the carboxy group-containing polymer may be 0.3 or more and 1.0 or less, where the mass of the carboxy group-containing polymer is taken as 1. With this configuration, it is possible to impart a desired electronic conductivity to the polymer layer, while minimizing the effect on the flexibility of the polymer layer and suppressing embrittlement.

[0025] (11) In the active material-containing liquid preparation step in the above configuration (9) or (10), the coating polymer liquid may contain a dispersant for dispersing the conductive assistant. This configuration improves the dispersibility of the conductive assistant, allowing the conductive assistant to be more uniformly contained in the polymer layer.

[0026] (12) In the above (11), the dispersant may be one or more selected from an acrylic acid polymer, a styrene-acrylic acid copolymer, and a maleic acid-acrylic acid copolymer. The polycarboxylic acid of this configuration has a hydrophobic portion. Since the polycarboxylic acid having a hydrophobic portion has both a hydrophobic group and a hydrophilic group, in addition to the electrostatic dispersion effect due to the charge, a dispersion effect due to hydrophobicity and hydrophilicity is added. Therefore, the use of the polycarboxylic acid of this configuration can enhance the dispersion effect.

[0027] (13) The negative electrode for a lithium ion secondary battery according to the present disclosure (hereinafter, sometimes simply referred to as the "negative electrode according to the present disclosure") includes a negative electrode material layer having the negative electrode material according to the present disclosure, and a current collector. The negative electrode according to the present disclosure makes it possible to realize a lithium ion secondary battery having excellent cycle characteristics and in which the capacity is not easily reduced even after repeated charging and discharging. Effect of the Invention

[0028] In the negative electrode material of the present disclosure, the polymer layer of the polymer-coated active material maintains lithium ion conductivity and electronic conductivity, and the imide-based polymer of the binder suppresses deformation of the negative electrode active material to maintain the conductive path. As a result, a lithium ion secondary battery with excellent cycle characteristics that is less likely to decrease in capacity even when repeatedly charged and discharged can be realized. According to the manufacturing method of the present disclosure, by using a carboxyl group-containing polymer and an imide-based polymer without mixing them in advance, the respective characteristics can be exhibited in the resulting negative electrode material. In addition, by blending a conductive assistant in both the coating polymer liquid and the binder liquid that form the polymer layer, uneven distribution of the conductive assistant in the imide-based polymer can be suppressed, and the conductive assistant can be reliably arranged in the polymer layer that coats the negative electrode active material. According to the negative electrode of the present disclosure, a lithium ion secondary battery with excellent cycle characteristics can be realized. [Brief description of the drawings]

[0029] [Figure 1] FIG. 1 is a cross-sectional schematic diagram showing an example of a negative electrode material for a lithium ion secondary battery according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, the embodiments of the negative electrode material for lithium ion secondary batteries, the manufacturing method thereof, and the negative electrode for lithium ion secondary batteries using the same of the present disclosure will be described. Note that the embodiments are not limited to the following embodiments, and can be embodied in various modified and improved forms that can be implemented by those skilled in the art.

[0031] <Anode materials> First, an example of the negative electrode material for lithium ion secondary batteries of the present disclosure will be described with reference to a schematic diagram. FIG. 1 shows a schematic cross-sectional diagram of an example of the negative electrode material of the present disclosure. As shown in FIG. 1, the negative electrode material 1 has a polymer-coated active material 10 and a binder 20. The polymer-coated active material 10 has a negative electrode active material 11 and a polymer layer 12. The polymer layer 12 has a carboxyl group-containing polymer and a conductive assistant, and coats the surface of the negative electrode active material 11. The binder 20 has an imide-based polymer and a conductive assistant, and binds the polymer-coated active materials 10 together. In the polymer-coated active material 10, the polymer layer 12 maintains lithium ion conductivity and electronic conductivity. The polymer-coated active material 10 is bound by the binder 20, and deformation due to the absorption and release of lithium ions is suppressed. According to the negative electrode material 1, the conductive path is maintained even when charging and discharging are repeated, so that a lithium ion secondary battery with excellent cycle characteristics can be realized.

[0032] [Polymer-coated active material] The negative electrode active material constituting the polymer-coated active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions, and examples thereof include carbon materials, silicon (Si), tin (Sn), germanium (Ge), and oxides and nitrides thereof. Silicon, tin, germanium, and the like have a high capacity density compared to carbon materials, but also have a large volume change associated with the absorption and release of lithium ions. In this regard, the effect of the negative electrode material of the present disclosure is more pronounced in the case of a material that has a large volume change associated with the absorption and release of lithium ions. Therefore, it is desirable to adopt a silicon material having silicon with a high capacity density as the negative electrode active material. Examples of silicon materials include Si, SiO x (silicon oxide, 0.3≦x≦1.6), SiN x (silicon nitride), etc.

[0033] When the negative electrode active material is a silicon material, it is desirable that the particle surface is coated with carbon in order to improve the electronic conductivity on the particle surface of the silicon material and to reinforce the particles. That is, it is desirable that the negative electrode active material is composed of silicon material particles and a carbon layer covering at least a part of the silicon material particles. In this case, the thickness of the carbon layer is preferably 1 nm or more and 100 nm or less. If the carbon layer is too thin, the effect of improving the electronic conductivity and the effect of reinforcing cannot be obtained, and conversely, if the carbon layer is too thick, the capacity density of the active material decreases. As a method for coating the silicon material particles with carbon, for example, a method of growing a carbon film on the particle surface by chemical vapor deposition using a hydrocarbon gas, a method of coating the particles with a compound containing carbon and then carbonizing them, etc. can be used.

[0034] The polymer layer constituting the polymer-coated active material may cover the entire surface of the negative electrode active material or may cover only a part of it. The polymer layer has a carboxyl group-containing polymer and a conductive assistant. Examples of the carboxyl group-containing polymer include polyacrylic acid, polymethacrylic acid, polyaspartic acid, polyglutamic acid, and carboxymethyl cellulose. One of these may be used alone or in combination of two or more. Among them, polyacrylic acid is preferred because it has sufficient reduction resistance against the negative electrode potential and can maintain its strength without softening even at a high temperature of about 60°C.

[0035] From the viewpoint of forming an appropriate amount of polymer layer on the surface of the negative electrode active material and fully exerting the effects of imparting electronic conductivity and lithium ion conductivity, the content of the carboxyl group-containing polymer is desirably 1.0% by mass or more when the mass of the negative electrode active material is 100% by mass. It is more preferable that it is 1.2% by mass or more. On the other hand, if the formed polymer layer is too thick, the reinforcing effect of the binder decreases, the resistance to lithium ion migration increases, and the capacity density of the active material decreases, so the content of the carboxyl group-containing polymer is desirably 4.0% by mass or less when the mass of the negative electrode active material is 100% by mass. It is more preferable that it is 3.9% by mass or less.

[0036] As the conductive assistant, a carbon material such as carbon black, acetylene black, graphite, vapor-grown carbon fiber, etc. may be used, and one of these may be used alone or in combination of two or more. The content of the conductive assistant may be any content that can impart electronic conductivity to the polymer layer, and as described later, the amount of the conductive assistant in the coating polymer liquid may be adjusted in the step of forming the polymer layer.

[0037] [binder] The binder binds the polymer-coated active material together and has an imide-based polymer and a conductive assistant. Examples of the imide-based polymer include polyamideimide and polyimide. One of these may be used alone or in combination of two or more. Among them, polyamideimide is preferable because it has high strength and is relatively flexible.

[0038] In order to fully exert the effect as a binder of binding polymer-coated active materials to each other and suppressing deformation due to expansion and contraction, the content ratio of the imide-based polymer to the carboxyl group-containing polymer should be 2 or more when the mass of the carboxyl group-containing polymer is 1. On the other hand, from the viewpoint of reducing irreversible reactions with lithium ions in the electrolyte when a lithium ion secondary battery is constructed and suppressing a decrease in capacity, the content ratio of the imide-based polymer to the carboxyl group-containing polymer should be 9 or less when the mass of the carboxyl group-containing polymer is 1. In addition, from the viewpoint of increasing the effect of suppressing deformation of the negative electrode active material, the content of the imide-based polymer should be 7.0 mass% or more when the mass of the negative electrode active material is 100 mass%.

[0039] The conductive assistant may be one or more selected from carbon materials such as carbon black, acetylene black, graphite, and vapor-grown carbon fiber. The conductive assistant may be the same as or different from the conductive assistant contained in the polymer layer. The content of the conductive assistant may be any amount that can impart electronic conductivity to the binder, and as described below, the amount of the conductive assistant may be adjusted in the binder liquid for forming the binder.

[0040] [Volume resistivity] The volume resistivity of the negative electrode material for lithium ion secondary batteries according to the present disclosure is desirably 0.5 Ω·cm or less in order to maintain high electronic conductivity. The volume resistivity in this specification is a value measured using an electrode resistance measurement system ("RM2610" manufactured by Hioki E.E. Corporation).

[0041] <Method of manufacturing negative electrode material for lithium-ion secondary batteries> The method for producing a negative electrode material for a lithium ion secondary battery according to the present disclosure includes an active material-containing liquid preparation step, a binder liquid preparation step, and a negative electrode material liquid preparation step. Each step will be described below.

[0042] [Active material-containing liquid preparation process] This step is a step of preparing an active material-containing liquid by dispersing a negative electrode active material in a coating polymer liquid having a carboxyl group-containing polymer and a conductive assistant. This step produces a polymer-coated active material in which the surface of the negative electrode active material is coated with a polymer layer having a carboxyl group-containing polymer and a conductive assistant. The active material-containing liquid may be prepared by adding a carboxyl group-containing polymer, a conductive assistant, a negative electrode active material, etc. to a predetermined solvent, or may be prepared by adding a negative electrode active material to a coating polymer liquid prepared in advance. In the former case, the liquid composition excluding the negative electrode active material becomes the coating polymer liquid. In the latter case, this step includes a coating polymer liquid preparation step of preparing a coating polymer liquid having a carboxyl group-containing polymer and a conductive assistant, and a dispersion step of dispersing a negative electrode active material in the coating polymer liquid to prepare an active material-containing liquid. The solvent used for the coating polymer liquid and the active material-containing liquid may be an organic solvent such as N-methyl-2-pyrrolidone (NMP). The active material-containing liquid may be prepared at room temperature.

[0043] From the viewpoint of imparting the desired electronic conductivity to the formed polymer layer, the blending ratio of the conductive assistant to the carboxyl group-containing polymer is desirably 0.3 or more when the mass of the carboxyl group-containing polymer is 1. On the other hand, if the blending amount of the conductive assistant is too large, the polymer layer becomes brittle or the flexibility of the polymer layer decreases. As a result, the conductive path may be broken by repeated charging and discharging, leading to a deterioration in cycle characteristics. Therefore, the blending ratio of the conductive assistant is desirably 1.0 or less when the mass of the carboxyl group-containing polymer is 1. Also, as described above, from the viewpoint of forming an appropriate amount of polymer layer on the surface of the negative electrode active material, the blending amount of the carboxyl group-containing polymer is desirably 1.0 part by mass or more with respect to 100 parts by mass of the negative electrode active material. It is more preferable that it is 1.2 parts by mass or more. On the other hand, if the formed polymer layer is too thick, the reinforcing effect of the binder decreases, the migration resistance of lithium ions increases, and the capacity density of the active material decreases, so the blending amount of the carboxyl group-containing polymer is desirably 4.0 parts by mass or less with respect to 100 parts by mass of the negative electrode active material. It is more preferable that the amount is 3.9 parts by mass or less.

[0044] In order to improve the dispersibility of the conductive assistant, a dispersant may be used. In other words, the coating polymer liquid may have a dispersant for dispersing the conductive assistant. Examples of the dispersant include acrylic acid polymer, styrene-acrylic acid copolymer, and maleic acid-acrylic acid copolymer.

[0045] [Binder liquid preparation process] This step is a step of preparing a binder liquid having an imide-based polymer and a conductive assistant. The order of carrying out this step and the above-mentioned active material-containing liquid preparation step may be any order, or they may be carried out simultaneously. The binder liquid may be prepared by adding an imide-based polymer, a conductive assistant, etc. to a predetermined solvent. The binder liquid may be prepared at room temperature. The solvent used in the binder liquid may be the same as or different from the active material-containing liquid, and an organic solvent such as NMP may be used.

[0046] From the viewpoint of imparting the desired electronic conductivity to the binder, the blending ratio of the conductive assistant to the imide-based polymer is desirably 0.3 or more when the mass of the imide-based polymer is 1. On the other hand, if the blending amount of the conductive assistant is too large, the binder becomes brittle or the adhesiveness of the binder decreases. This may reduce the effect of suppressing the deformation of the negative electrode active material, which may lead to a decrease in cycle characteristics. Therefore, the blending ratio of the conductive assistant is desirably 1.0 or less when the mass of the imide-based polymer is 1.

[0047] [Negative electrode material liquid preparation process] This step is a step of preparing a negative electrode material liquid by mixing the active material-containing liquid and the binder liquid. This step may also be performed at room temperature. The solvent is then removed from the prepared negative electrode material liquid to obtain a negative electrode material. The solvent may be removed by drying the negative electrode material liquid by heating or the like. The heating temperature may be appropriately determined depending on the type of solvent.

[0048] In order to fully exert the effect as a binder when mixing the active material-containing liquid with the binder liquid, the blending ratio of the imide-based polymer to the carboxyl group-containing polymer should be 2 or more when the mass of the carboxyl group-containing polymer is 1. On the other hand, from the viewpoint of reducing irreversible reactions with lithium ions in the electrolyte and suppressing a decrease in capacity when a lithium ion secondary battery is constructed, the blending ratio of the imide-based polymer should be 9 or less. Also, from the viewpoint of enhancing the effect of suppressing deformation of the negative electrode active material, the blending amount of the imide-based polymer should be 7.0 mass% or more when the mass of the negative electrode active material is 100 mass%.

[0049] <Negative electrode> The negative electrode for lithium ion secondary batteries of the present disclosure includes a negative electrode material layer having the negative electrode material of the present disclosure and a current collector. The negative electrode material layer can be formed, for example, by applying the negative electrode material liquid prepared in the manufacturing method of the present disclosure to the surface of the current collector, drying it, and compressing it to increase the electrode density as necessary. The material of the current collector is not particularly limited as long as it has electronic conductivity, and for example, copper, nickel, stainless steel, etc. are suitable. The shape of the current collector is also not particularly limited, and for example, a foil having a thickness of 1 μm or more and 100 μm or less is suitable. Examples of the method for applying the negative electrode material liquid include a doctor blade method, a roll coating method, a dipping method, and a spray method. For drying, a dryer such as a hot air dryer or an infrared heater may be used. In order to suppress oxidation of the current collector, it is desirable to perform drying in a vacuum or an inert gas atmosphere.

[0050] <Lithium-ion secondary battery> When a lithium ion secondary battery is constructed using the negative electrode for lithium ion secondary batteries of the present disclosure, the configuration other than the negative electrode may follow the configuration of a known lithium ion secondary battery. That is, the negative electrode of the present disclosure, the positive electrode, a separator sandwiched between the two electrodes, and an electrolyte may be housed in a sealed case to construct a lithium ion secondary battery. The positive electrode is formed by mixing a positive electrode active material and a binder, adding a solvent to make a paste-like positive electrode material, applying the paste to the surface of a current collector, and drying it. The positive electrode active material may be any compound that can absorb and release lithium ions, and from the viewpoint of being able to construct a 4V class battery, a lithium transition metal composite oxide having Co, Ni, or the like as its main constituent elements is suitable. The binder may be any binder that can bind the positive electrode active materials together, and examples of such binder include fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride, and thermoplastic resins such as polypropylene and polyethylene. The positive electrode material preferably further contains a conductive assistant, and like the conductive assistant of the negative electrode, carbon materials such as carbon black, acetylene black, graphite, vapor-grown carbon fiber, etc. can be used. In addition, as a solvent for dispersing these materials, an organic solvent such as NMP can be used, and as a current collector, like the current collector of the negative electrode, a metal foil or the like is suitable.

[0051] The separator separates the positive electrode and the negative electrode and holds the electrolyte. As the separator, an insulating microporous film such as polyethylene or polypropylene is used. The electrolyte is a lithium salt dissolved in an organic solvent. Examples of the organic solvent include aprotic organic solvents such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethoxyethane, and tetrahydrofuran. Examples of the electrolyte include lithium salts such as LiClO4, LiAsF6, LiBF4, LiPF6, LiCF3SO3, and LiN(CF3SO2)2. Also, instead of the electrolyte, a polymer gel electrolyte such as polyethylene oxide can be used. EXAMPLES

[0052] Next, the present disclosure will be described in more detail with reference to examples. First, various negative electrode materials were manufactured and their volume resistivities were measured. Next, the capacity retention rate of a lithium ion secondary battery including a negative electrode using the negative electrode material was measured.

[0053] <Production of negative electrode materials> [Negative electrode active material] Carbon-coated silicon oxide (SiO) particles used as the negative electrode active material were produced as follows. First, Si powder and SiO2 powder were mixed in a predetermined ratio and granulated, and then heated under vacuum and cooled to precipitate SiO particles. Next, the obtained SiO particles were pulverized to an average particle size of 5 μm, and heat-treated at 850° C. for 15 minutes in a hydrocarbon gas atmosphere using a rotary kiln. This resulted in SiO particles whose surfaces were coated with carbon. The heat treatment was performed so that the carbon layer on the surface of the SiO particles had a thickness of about 30 nm.

[0054] [Imide polymer] Polyamideimide (PAI) was produced as an imide-based polymer constituting the binder as follows. First, tolidine diisocyanate (TODI) ("TODI / R203" manufactured by Nippon Soda Co., Ltd.) and the same mole of trimellitic anhydride ("TMA" manufactured by Mitsubishi Gas Chemical Co., Ltd.) were dissolved in N-methyl-2-pyrrolidone (NMP). The solid content concentration in the NMP solution was set to 20 mass%. Next, the NMP solution was heated to 130°C over 1 hour while stirring under a nitrogen stream, and reacted at 130°C for about 5 hours to obtain polyamideimide.

[0055] [Example 1] The negative electrode material of Example 1 was manufactured as follows. The blending amounts of the materials used are shown in Table 1 below. First, NMP was added to polyacrylic acid (PAA) ("20CLPAH" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a carboxyl group-containing polymer and acetylene black (AB) ("Denka Black (registered trademark)" manufactured by Denka Co., Ltd.) as a conductive assistant, and the mixture was stirred to prepare a coating polymer liquid. Next, carbon-coated SiO particles as a negative electrode active material were added to the coating polymer liquid and stirred to prepare an active material-containing liquid (active material-containing liquid preparation step). Separately from this, NMP was added to the manufactured polyamideimide and acetylene black (same as above) as a conductive assistant, and the mixture was stirred to prepare a binder liquid (binder liquid preparation step). Then, the active material-containing liquid and the binder liquid were mixed to prepare a slurry-like negative electrode material liquid. Mixing and stirring in the manufacturing process of the negative electrode material was performed using a planetary centrifugal mixer “THINKY MIXER (registered trademark), ARE-310” manufactured by Thinky Corporation in all of the Examples and the Reference Examples and Comparative Examples described below.

[0056] A 10 μm thick electrolytic copper foil was prepared as a current collector. The negative electrode material solution was applied to the surface of the electrolytic copper foil using a doctor blade, and then dried at 80° C. for 15 minutes to form a pre-dried negative electrode material layer with a coating thickness of 24 μm. The pre-dried negative electrode material layer was then dried at 200° C. for 2 hours under vacuum to obtain a negative electrode material layer. The obtained negative electrode material layer is referred to as the negative electrode material of Example 1. The negative electrode material layer is included in the concept of the negative electrode material of the present disclosure. In this manner, a negative electrode in which a negative electrode material layer was formed on the surface of the current collector was obtained.

[0057] [Examples 2 to 4 and Reference Examples 1 to 6] Except for changing the amounts of the materials used, the negative electrode materials of Examples 2 to 4 and Reference Examples 1 to 6 were produced in the same manner as in Example 1. The amounts of the materials used are shown in Table 1 below. For the negative electrode material of Reference Example 3, acetylene black was not used when preparing the coating polymer solution, and NMP was added to only polyacrylic acid and stirred.

[0058] Regarding the blending amounts of materials, the main differences between the negative electrode material of Example 1 and the negative electrode materials of Examples 2 to 4 are as follows. In the negative electrode material of Example 2, the blending ratio of the imide-based polymer to the carboxyl group-containing polymer (PAI / PAA) was increased. Conversely, in the negative electrode material of Example 3, the blending ratio was decreased. In the negative electrode material of Example 4, the blending ratios of the conductive assistant to the carboxyl group-containing polymer (PAA:AB) and the blending ratio of the conductive assistant to the imide-based polymer (PAI:AB) were increased.

[0059] Similarly, the main differences between the negative electrode material of Example 1 and the negative electrode materials of Reference Examples 1 to 6 are as follows. In the negative electrode materials of Reference Examples 1 and 2, the blending amount of the imide-based polymer to the negative electrode active material was reduced, and the blending ratio (PAI / PAA) of the imide-based polymer to the carboxyl group-containing polymer was reduced. In the negative electrode material of Reference Example 3, no conductive assistant was blended in the coating polymer liquid. That is, the blending ratio (PAA:AB) of the conductive assistant to the carboxyl group-containing polymer was set to 1:0. In the negative electrode material of Reference Example 4, the blending amount of the imide-based polymer to the negative electrode active material was reduced. In the negative electrode material of Reference Example 5, the blending ratio (PAA:AB) of the conductive assistant to the carboxyl group-containing polymer and the blending ratio (PAI:AB) of the conductive assistant to the imide-based polymer were reduced. Conversely, in the negative electrode material of Reference Example 6, the compounding ratio of the conductive assistant to the carboxyl group-containing polymer (PAA:AB) and the compounding ratio of the conductive assistant to the imide-based polymer (PAI:AB) were increased.

[0060] [Comparative Example 1] The negative electrode material of Comparative Example 1 was produced as follows. 85 parts by mass of carbon-coated SiO particles as the negative electrode active material, 5 parts by mass of acetylene black (same as above) as the conductive assistant, and 10 parts by mass of polyacrylic acid (same as above) as the binder were added to NMP and stirred to prepare a slurry-like negative electrode material solution. Using this negative electrode material solution, a negative electrode material layer was formed on the surface of the electrolytic copper foil in the same manner as in the negative electrode production method of Example 1 described above.

[0061] [Comparative Example 2] The negative electrode material of Comparative Example 2 was produced as follows. 85 parts by mass of carbon-coated SiO particles as the negative electrode active material, 5 parts by mass of acetylene black (same as above) as the conductive assistant, and 10 parts by mass of polyamideimide (same as above) as the binder were added to NMP and stirred to prepare a slurry-like negative electrode material solution. Using this negative electrode material solution, a negative electrode material layer was formed on the surface of the electrolytic copper foil in the same manner as in the negative electrode production method of Example 1 described above.

[0062] [Comparative Example 3] The negative electrode material of Comparative Example 3 was produced as follows. 2.5 parts by mass of polyacrylic acid (same as above) and 7.5 parts by mass of polyamideimide (same as above) as binders were mixed to produce a binder mixture. 85 parts by mass of carbon-coated SiO particles as the negative electrode active material, 5 parts by mass of acetylene black (same as above) as the conductive assistant, and NMP were added to 10 parts by mass of the binder mixture and stirred to prepare a slurry-like negative electrode material liquid. Using this negative electrode material liquid, a negative electrode material layer was formed on the surface of the electrolytic copper foil in the same manner as in the negative electrode production method of Example 1 described above.

[0063] <Manufacturing lithium-ion secondary batteries> In order to evaluate the characteristics of a lithium-ion secondary battery using the manufactured negative electrode, a half-cell coin-type battery was manufactured as follows. First, the manufactured negative electrode was punched into a circular shape with a diameter of 12 mm to prepare an evaluation electrode, and a metal lithium plate was punched into a circular shape with a diameter of 14 mm to prepare a counter electrode. Next, a glass filter and a resin sheet were prepared as separators. The resin sheet was a three-layered microporous film made of polypropylene / polyethylene / polypropylene. Then, the resin sheet and the glass filter were stacked in this order on the negative electrode material layer of the evaluation electrode, and the electrolyte was impregnated. The electrolyte used was a mixed solvent in which ethylene carbonate and diethyl carbonate were mixed in a volume ratio of 1:1, and LiPF6 was dissolved at a concentration of (1 mol / L). Then, the counter electrode was stacked on the glass filter to prepare an electrode body, which was then housed in a coin-type battery case ("CR2032" manufactured by Hosen Co., Ltd.) and pressure was applied using a crimping machine to produce a sealed coin-type battery.

[0064] <Evaluation method> [Volume resistivity] The volume resistivity of the negative electrode material layer formed on the surface of the current collector was measured using an electrode resistance measuring system ("RM2610" manufactured by Hioki E.E. Corporation).

[0065] [Capacity maintenance rate] The manufactured coin-type battery was subjected to a charge-discharge cycle test at 30°C, and the capacity retention rate after a predetermined number of cycles was calculated. In the charge-discharge cycle test, the absorption of Li in the evaluation electrode is called discharging, and the release of Li from the evaluation electrode is called charging. First, a constant current discharge was performed at a 0.1C rate until the voltage of the evaluation electrode relative to the counter electrode became 0.01V, and a 10-minute pause was given after the discharge was completed. Next, a constant current charge was performed at a 0.1C rate until the voltage of the evaluation electrode relative to the counter electrode became 1.5V, and a 10-minute pause was given after the charge was completed. The discharge capacity at this time was taken as the initial discharge capacity, and the charge capacity was taken as the initial charge capacity. The "1C rate" is the current value at which the theoretical capacity of the battery is completely charged or discharged in one hour in the case of constant current charging and discharging. This charge and discharge was considered as one cycle, and the charge-discharge cycle test was performed up to 100 cycles. The capacity retention rates after 30, 50, and 100 cycles were calculated by the following formula (I). In this test, a capacity retention rate of 80% or more after 30 cycles and a capacity retention rate of 70% or more after 100 cycles were evaluated as having good cycle characteristics. Capacity retention rate (%) = (charge capacity after a certain number of cycles / initial charge capacity) × 100 (I)

[0066] <Evaluation Results> Table 1 shows the materials and amounts used in producing the negative electrode material, the volume resistivity of the negative electrode material, and the measurement results of the capacity retention rate of the lithium-ion secondary battery. [Table 1]

[0067] The negative electrode materials of Examples 1 to 4 are manufactured by mixing polyacrylic acid (carboxyl group-containing polymer), polyamideimide (imide-based polymer) and the negative electrode active material separately, and further adding a conductive assistant to each of the two polymers. As shown in Table 1, the capacity retention rate after 30 cycles is larger for the negative electrode materials of Examples 1 to 4 than for the negative electrode material of Comparative Example 3 manufactured by mixing the negative electrode active material with the mixture of the two polymers. After 100 cycles, the difference in the capacity retention rate is larger. That is, it was confirmed that the capacity of the lithium ion secondary battery is less likely to decrease even after repeated charging and discharging when the negative electrode materials of Examples 1 to 4 are used. In addition, when the negative electrode materials of Examples 1 to 3, which have the same amount of conductive assistant in the negative electrode material, are compared with the negative electrode material of Comparative Example 3, the volume resistivity of the negative electrode materials of Examples 1 to 3 is smaller than that of Comparative Example 3. That is, it was confirmed that the electronic conductivity is also improved in the negative electrode materials of Examples 1 to 3.

[0068] On the other hand, the negative electrode material of Comparative Example 1 contains only polyacrylic acid as a polymer. Therefore, the dispersibility of the conductive assistant is poor, and the volume resistivity is large. In addition, the effect of suppressing the expansion and contraction of the negative electrode active material is small, so the conductive path is cut off when charging and discharging are repeated, and the capacity is significantly reduced. In addition, the negative electrode material of Comparative Example 2 contains only polyamideimide as a polymer. Since polyamideimide has poor lithium ion conductivity, the capacity is significantly reduced when charging and discharging are repeated.

[0069] In the negative electrode materials of Reference Examples 1 and 2, the amount of imide-based polymer blended was small, so the volume resistivity was larger than that of the negative electrode materials of Examples 1 to 3, which had the same blend ratio (PAA:AB) of the conductive assistant in the binder. In addition, the capacity decreased when charging and discharging were repeated. The reason for this is thought to be that the blend ratio (PAI / PAA) of the imide-based polymer to the carboxyl group-containing polymer was small, so the effect of suppressing deformation of the negative electrode active material by the imide-based polymer was not fully exhibited. In addition, in the negative electrode material of Reference Example 3, since the conductive assistant was not blended in the coating polymer liquid, it is presumed that the conductive assistant is not contained in the polymer layer. The surface of the negative electrode active material was covered with the carboxyl group-containing polymer that does not have electronic conductivity, the supply of electrons to the surface of the negative electrode active material was reduced, and the negative electrode active material that can contribute to the charge and discharge reaction was reduced, so the capacity retention rate after 100 cycles was small. In the negative electrode material of Reference Example 4, although the volume resistivity was small, the capacity decreased when charging and discharging was repeated. The reason for this is that the amount of imide-based polymer blended with respect to the negative electrode active material is small, and therefore the effect of suppressing deformation of the negative electrode active material by the imide-based polymer is not fully exerted. The negative electrode material of Reference Example 5 has a smaller blend ratio of conductive assistant to carboxyl group-containing polymer than the negative electrode material of Example 1. For this reason, it is considered that the electronic conductivity of the surface of the negative electrode active material is insufficient, and the capacity is reduced by repeated charging and discharging. On the other hand, the negative electrode material of Reference Example 6 has a larger blend ratio of conductive assistant to carboxyl group-containing polymer than the negative electrode material of Example 1. It is considered that this makes the polymer layer brittle, and the capacity is reduced by repeated charging and discharging. [Explanation of symbols]

[0070] 1: negative electrode material, 10: polymer-coated active material, 11: negative electrode active material, 12: polymer layer, 20: binder.

Claims

1. a polymer-coated active material having a negative electrode active material and a polymer layer having a carboxyl group-containing polymer and a conductive assistant and coating a surface of the negative electrode active material; a binder having an imide-based polymer and a conductive assistant and binding the polymer-coated active materials together; A negative electrode material for a lithium ion secondary battery, comprising:

2. 2. The negative electrode material for lithium ion secondary batteries according to claim 1, wherein the content of the carboxyl group-containing polymer is 1.0% by mass or more and 4.0% by mass or less, where the mass of the negative electrode active material is 100% by mass.

3. 2. The negative electrode material for lithium ion secondary batteries according to claim 1, wherein a content ratio of the imide polymer to the carboxyl group-containing polymer is 2 to 9, where the mass of the carboxyl group-containing polymer is taken as 1.

4. 2. The negative electrode material for a lithium ion secondary battery according to claim 1, wherein the volume resistivity is 0.5 Ω·cm or less.

5. 5. The negative electrode material for lithium ion secondary batteries according to claim 4, wherein the content of the imide-based polymer is 7.0 mass % or more when the mass of the negative electrode active material is taken as 100 mass %.

6. The negative electrode material for a lithium ion secondary battery according to claim 1 , wherein the negative electrode active material contains silicon.

7. 2. The negative electrode material for a lithium ion secondary battery according to claim 1, wherein the carboxyl group-containing polymer is at least one selected from the group consisting of polyacrylic acid, polymethacrylic acid, polyaspartic acid, polyglutamic acid, and carboxymethyl cellulose.

8. 2. The negative electrode material for a lithium ion secondary battery according to claim 1, wherein the imide-based polymer is at least one selected from the group consisting of polyamide-imide and polyimide.

9. A method for producing a negative electrode material for a lithium ion secondary battery according to claim 1, an active material-containing liquid preparation step of preparing an active material-containing liquid by dispersing a negative electrode active material in a coating polymer liquid having a carboxyl group-containing polymer and a conductive assistant; A binder liquid preparation step of preparing a binder liquid having an imide-based polymer and a conductive assistant; a negative electrode material liquid preparation step of mixing the active material-containing liquid with the binder liquid to prepare a negative electrode material liquid; 2. A method for producing a negative electrode material for a lithium ion secondary battery, comprising:

10. 10. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 9, wherein in the active material-containing liquid preparation step, a blending ratio of the conductive assistant to the carboxyl group-containing polymer is 0.3 or more and 1.0 or less, where the mass of the carboxyl group-containing polymer is 1.

11. 10. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 9, wherein in the active material-containing liquid preparation step, the coating polymer liquid contains a dispersant for dispersing the conductive assistant.

12. The method for producing a negative electrode material for a lithium ion secondary battery according to claim 11, wherein the dispersant is at least one selected from the group consisting of an acrylic acid polymer, a styrene-acrylic acid copolymer, and a maleic acid-acrylic acid copolymer.

13. A negative electrode for a lithium ion secondary battery comprising: a negative electrode material layer having the negative electrode material for a lithium ion secondary battery according to claim 1; and a current collector.

Citation Information

Patent Citations

  • Binding agent for negative electrode for secondary battery, negative electrode for secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery

    JP2016046151A

  • Negative electrode material for lithium ion secondary batteries, method for producing same, negative electrode for lithium ion secondary batteries, method for producing negative electrode for lithium ion secondary batteries, and lithium ion secondary battery

    WO2015083262A1