Method for manufacturing plated article, and plated article
A controlled heat treatment process using a plating base paint with epoxy resin, conductive polymer, and inorganic filler addresses adhesion and plating precipitation issues, ensuring reliable plating even under high temperatures.
Patent Information
- Application Number
- JP2023053894
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for producing plated products face challenges in achieving both high adhesion between the base material and metal plating layer and maintaining plating precipitation, especially under high-temperature conditions, leading to issues such as peeling and poor deposition on fine patterns.
A specific heat treatment process is employed, using a plating base paint containing epoxy resin, conductive polymer, and inorganic filler, with controlled heat treatment temperatures to ensure both adhesion and plating depositability, optimizing the mass ratios of these components to enhance catalyst adsorption and crosslinking.
The method achieves high adhesion between the base material and metal plating layer, even under high-temperature conditions, with reliable plating precipitation, ensuring no peeling and maintaining fine pattern deposition quality.
Smart Images

Figure 2024141978000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a plated article which has excellent adhesion between a substrate and a metal plating layer even when exposed to a high-temperature environment and also has excellent plating deposition properties, and to a plated article produced by said method. [Background technology]
[0002] When plating various substrates, the plating layer must be able to withstand the intended use and environment and achieve the intended effect, and must not peel off from the substrate. Plating adhesion is the most important consideration when examining plating methods.
[0003] A plated article (flexible printed circuit board) in which copper foil is laminated on the surface of a polyimide resin film, which has high adhesion even after a heat load, has been reported. JP 2004-79660 A (Patent Document 1) discloses a plated article (flexible printed circuit board) that has high adhesion even after a heat load, by electrolessly plating nickel or a nickel alloy on the surface of a polyimide resin film and then electroplating copper on the surface of the plating layer. In order to physically (anchor effect due to roughening) and chemically (bonding to functional groups) increase the adhesive strength of the electroless plating layer of nickel or the like, and in turn the adhesive strength of the copper plating layer formed on the surface of the electroless plating layer, the polyimide resin film serving as the substrate had to be first plasma-treated and then activated with an alkali metal hydroxide.
[0004] In addition, Japanese Patent Laid-Open Publication No. 59-129489 (Patent Document 2) describes a method for plating substrates for printed wiring boards, in which the plating adhesion strength of electroless plating is improved by separating the steps of partially curing and completely curing polyimide resin.
[0005] Incidentally, in the composition for forming an electroless plating undercoat film disclosed in International Publication WO2015 / 019596 (Patent Document 3), a technique is known in which a base coat containing a conductive polymer and an epoxy resin is applied to a substrate to form a plating undercoat film, and then electroless plating is performed to form a metal plating film. However, when making a "plated item," the plating base paint may be treated with high heat to harden it, and this can result in a problem with the "plating base paint (layer)" after treatment, which reduces the ability of the metal film to deposit, i.e., the plating deposition properties. Furthermore, if the plating deposition properties of the "plating base paint (layer)" decrease, the plating will not deposit cleanly when plating high-precision fine patterns, resulting in problems such as increased resistance and disconnections.
[0006] On the other hand, when heat treatment is performed at a low temperature to ensure plating deposition, the required adhesion cannot be obtained. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-79660 A [Patent Document 2] Japanese Patent Application Publication No. 59-129489 [Patent Document 3] International Publication No. WO2015 / 019596 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention provides a hardening process for an electroless plating underlayer that can achieve both plating deposition property and adhesion by setting a specific heat treatment temperature in order to ensure plating deposition property, and a hardening process for an electroless plating underlayer manufactured by the process. We provide plated products that can be used for plating. [Means for solving the problem]
[0009] The present invention is intended to solve the above problems. That is, the present invention includes the following. The first embodiment of the present invention includes a step 1 of applying a plating undercoat paint on a substrate to form a plating undercoat layer, and a step of subjecting the plating undercoat layer to a heat treatment temperature T A a step 2 of heat-treating the substrate by electroless plating or electroless plating and electrolytic plating to form a metal plating film on the substrate; and a step 3 of heating the metal plating film at a heat treatment temperature T B a step 4 of heat-treating the plating undercoat by a method according to claim 1 to obtain a plated product having a metal plating film, the plating undercoat paint containing an epoxy resin, a conductive polymer, an inorganic filler and a solvent, the conductive polymer and the epoxy resin being in a mass ratio of 1:8 to 1:46, and the heat treatment temperature T A is between the temperature at which the solvent evaporates and the temperature at which the catalyst adsorption of the plating underlayer decreases, and B The present invention relates to a method for producing a plated article, characterized in that the temperature is between the temperature at which the epoxy resin hardens and the temperature at which copper damage occurs. A second aspect of the present invention relates to the method for producing a plated article according to the first aspect, wherein the plating undercoat contains 0.3 to 1.0 part by mass of the inorganic filler per 1 part by mass of epoxy resin. A third aspect of the present invention relates to the method for producing a plated article according to the first aspect, wherein the conductive polymer and the epoxy resin have a mass ratio of 1:9 to 1:14. The fourth aspect of the present invention is the heat treatment temperature T A is 80°C to 140°C, and the heat treatment temperature T B The method for producing a plated article according to the first embodiment relates to a method for producing a plated article according to the first embodiment, wherein the heating temperature is 120°C to 150°C. A fifth aspect of the present invention relates to a plated article produced by the method for producing a plated article according to any one of the first to fourth aspects. Effect of the Invention
[0010] The present invention provides a method for producing a plated article which exhibits high adhesion between a substrate and a metal plating layer even when exposed to a high-temperature environment and also exhibits excellent plating deposition properties, and a plated article produced by said method. Specifically, in terms of plating deposition properties, the performance is achieved such that even dense areas where continuous patterns with wiring widths of 100 μm or more are densely packed can be plated reliably, and adhesion with a peel strength of 0.35 N / mm or more is also achieved. [Brief description of the drawings]
[0011] [Figure 1] Figure 1 shows the criteria for judging plating deposition properties for plating objects with a pattern that includes dense areas, sparse areas, and fine lines. If there are no missing parts in the dense areas, sparse areas, or fine lines by visual inspection, it is judged as OK, but if there are missing parts, it is judged as NG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Plating base paint> The present invention uses a plating undercoat paint capable of forming a metal plating film by electroless plating, and the plating undercoat paint contains conductive or reducing polymer particles, a synthetic resin, and an inorganic filler. Each component of the plating undercoat paint will be described in detail below.
[0013] (Conductive or reducing polymer particles) The reducing polymer microparticles of the present invention are not particularly limited as long as they are polymers having π-conjugated double bonds and have a conductivity of less than 0.01 S / cm, preferably 0.005 S / cm or less. Examples of the reducing polymer microparticles include polyacetylene, polyacene, polyparaphenylene, polyparaphenylenevinylene, polypyrrole, polyaniline, polythiophene, and various derivatives thereof, and preferably polypyrrole. Reducible polymer particles can be synthesized from monomers that have π-conjugated double bonds. However, commercially available reducing polymer fine particles can also be used. The reducible polymer microparticles are used as a dispersion liquid in which they are dispersed in an organic solvent, and in order to maintain dispersion stability in the dispersion liquid, the reducible polymer microparticles are made to have a solid content of 16 mass% or less (solid content ratio) of the mass of the dispersion liquid. Examples of organic solvents for dispersing reducing polymer microparticles include aliphatic esters such as butyl acetate, aromatic solvents such as toluene, ketones such as methyl ethyl ketone, cyclic saturated hydrocarbons such as cyclohexane, chain saturated hydrocarbons such as n-octane, chain saturated alcohols such as methanol, ethanol, and n-octanol, aromatic esters such as methyl benzoate, aliphatic ethers such as diethyl ether, and mixtures thereof.
[0014] The conductive polymer fine particles of the present invention are not particularly limited as long as they are polymers having conductive π-conjugated double bonds, and examples thereof include polyacetylene, polyacene, polyparaphenylene, polyparaphenylenevinylene, polypyrrole, polyaniline, polythiophene, and various derivatives thereof, and preferably polypyrrole. The conductive polymer fine particles can be synthesized from a monomer having a π-conjugated double bond, but commercially available conductive polymer fine particles can also be used. The conductive polymer microparticles are used as a dispersion liquid in which they are dispersed in an organic solvent, and in order to maintain dispersion stability in the dispersion liquid, the conductive polymer microparticles are made to account for 16 mass % or less (solid content ratio) of the mass of the dispersion liquid as solid content. As the organic solvent in which the conductive polymer fine particles are dispersed, the same organic solvent as that in which the reducing polymer fine particles are dispersed can be used.
[0015] (Synthetic resin) The synthetic resin of the present invention is an epoxy resin having an epoxy equivalent of 875 to 9,200. The epoxy resin may be any one having two or more epoxy groups in the molecule, and various epoxy resins can be used, such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, dicyclopentadiene type epoxy resin, and epoxy resins obtained by modifying these resins. These can be used alone or as a mixture of two or more types.
[0016] Furthermore, in the case of epoxy resins with an epoxy equivalent of less than 875, it becomes difficult for the catalyst metal to be adsorbed, and as a result, it becomes difficult to obtain a metal plating film, i.e., plating deposition properties are poor. In addition, even if a metal plating film is obtained, it is presumed that crosslinking of the epoxy resin is likely to be insufficient when polypyrrole fine particles and epoxy resins with an epoxy equivalent of less than 875 are used, and when exposed to a high-temperature environment, oxidized copper (copper oxide) and copper diffuse through the coating layer and reach the substrate, and high adhesion, specifically, 180-degree peel strength of 0.35 N / mm or more, cannot be obtained. In the case of epoxy resins with an epoxy equivalent of over 9200, there is no loss in adhesion when exposed to high heat environments, but there is a risk that they cannot be used as paints.
[0017] From the viewpoint of a coating material for fine line printing, an epoxy equivalent of 2,400 to 8,500 is more preferable. The term "equivalent" used herein means the molecular weight (Mw) divided by the number of functional groups (n), and means equivalent [g / eq] = Mw / n.
[0018] (Inorganic filler) The inorganic filler of the present invention can be a powder of a metal oxide such as titanium oxide (titania), aluminum oxide (alumina) or silicon oxide (silica), and has hydrophilic properties. . In general, inorganic fillers of metal oxides often have hydrophilic groups on the surface, and exhibit hydrophilicity. A filler in which almost all of the hydrophilic groups have been replaced with hydrophobic groups such as alkyl groups and amino groups by surface hydrophobization treatment is called a hydrophobic inorganic filler, and is distinguished from a hydrophilic inorganic filler that has not been surface hydrophobized. Therefore, the hydrophilic inorganic filler of the present invention is one that has not been surface hydrophobized. In addition, a hydrophilic inorganic filler containing a hydrophobic inorganic filler may be used as long as it does not impair the effects of the present invention. In particular, silica particles are preferred because they contain many hydrophilic groups and the particle size can be easily adjusted. This is because a high proportion of hydrophilic groups on the surface of the plating underlayer can increase the amount of catalytic metal adsorbed, resulting in excellent plating deposition properties.
[0019] In the present invention, the average primary particle size of the inorganic filler is preferably from 1 nm to 5 μm, and more preferably from 1 nm to 1 μm. The smaller the average primary particle size of the inorganic filler, i.e., the larger the specific surface area, the greater the surface area of the coating film and the greater the amount of catalytic metal adsorbed, thereby improving plating deposition properties. However, when the average primary particle size is less than 1 nm, even a small amount of addition increases the filler density in the paint, making it easy to increase the initial viscosity of the paint. However, a certain amount must be added to improve plating deposition properties, and this increases the viscosity too much, making printing itself difficult. In addition, when the average primary particle size exceeds 1 μm, the proportion of paint in contact with the filler surface decreases, the swelling of the filler becomes insufficient, and the initial viscosity of the paint tends to be difficult to increase. Therefore, it is difficult to adjust the viscosity to a level suitable for various printing methods, and printing of fine patterns becomes even more difficult. The average primary particle size is determined by photographing inorganic particles at 50,000x magnification using a conventional scanning electron microscope, then measuring the particle sizes of at least 50 randomly selected inorganic particles in the photograph and calculating the average.
[0020] In the plating undercoat of the present invention, the mass ratio of the synthetic resin (epoxy resin) to the inorganic filler is epoxy resin:inorganic filler=1:0.3 to 1.0. If the inorganic filler exceeds 1.0 part by mass per part by mass of epoxy resin, the crosslinking of the epoxy resin becomes insufficient, and peeling between the substrate and the metal plating film is likely to occur. Also, if the inorganic filler is less than 0.3 part by mass, the surface area of the coating film does not increase, the effect of increasing the amount of adsorbed catalytic metal becomes insufficient, and plating deposition property decreases. From the viewpoint of a coating material for continuous printing, the inorganic filler is more preferably 0.3 to 0.6, that is, epoxy resin:inorganic filler=1:0.3 to 0.6.
[0021] In the plating undercoat coating of the present invention, the mass ratio of reducing or conductive polymer fine particles to epoxy resin (polymer fine particles:epoxy resin) is 1:8 to 1:46. If the amount of epoxy resin exceeds 46 parts by mass per part by mass of reducing or conductive polymer fine particles, the proportion of reducing or conductive polymer fine particles to which the catalytic metal can adhere decreases, resulting in poor plating deposition properties. Furthermore, if the epoxy resin is less than 8 parts by mass, self-aggregation of reducing or conductive polymer particles in the coating material is promoted, making it difficult to suppress thickening over time, and crosslinking of the epoxy resin becomes insufficient, which makes it easy for peeling to occur between the substrate and the metal plating film. From the viewpoint of plating deposition speed, it is preferable that the epoxy resin is 9 to 14 parts by mass per 1 part by mass of reducing or conductive polymer fine particles.
[0022] (solvent) The plating undercoat coating of the present invention may contain a solvent in addition to the conductive or reducing polymer fine particles, the epoxy resin, and the inorganic filler. The solvent is not particularly limited as long as it can dissolve the epoxy resin. However, even if a solvent dissolves a substrate to a large extent, it is possible to use the solvent by lowering the solubility by mixing it with another solvent having low solubility. Examples of the solvent include aliphatic esters such as butyl acetate, aromatic solvents such as toluene and benzyl alcohol, ketones such as methyl ethyl ketone, cyclic saturated hydrocarbons such as cyclohexane, chain saturated hydrocarbons such as n-octane, chain saturated alcohols such as methanol, ethanol and n-octanol, aromatic esters such as methyl benzoate, aliphatic ethers such as diethyl ether, and mixtures thereof. In addition, when an epoxy resin and an inorganic filler are mixed into a dispersion liquid of polymer microparticles dispersed in an organic solvent, the organic solvent used in the dispersion liquid can be used as part or all of the solvent for the plating undercoat paint.
[0023] (Other Ingredients) Depending on the application and the object to be coated, the plating undercoat of the present invention may contain resins such as an epoxy resin curing agent or curing catalyst, a dispersion stabilizer, a thickener, an ink binder, etc. Furthermore, as long as the effect of the present invention is not impaired, inorganic fillers other than the inorganic filler of the present invention, such as carbon black, may be added. The amount of the other components added is preferably within the range of 0.1 to 2% by mass relative to the total mass of the base coating.
[0024] (hardening agent or hardening catalyst) The curing agent that can be used here may be at least one selected from the group consisting of isocyanates, carbodiimides, oxazolines, epoxies, acid anhydrides, phenols, thiols, polyanilines, and dicyandiamides. Examples of the curing catalyst that can be used herein include imidazoles, tertiary amines, and tertiary phosphines.
[0025] Specific examples of the imidazoles include 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2,4-dimethylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-vinyl-2-methylimidazole, 1-propyl-2-methylimidazole, 2-isopropylimidazole, 1-cyanomethyl-2-methyl-imidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, and masked imidazoles.
[0026] Specific examples of tertiary amines include trimethylamine, triethylamine, tripropylamine, tributylamine, tetramethylbutanediamine, tetramethylpentanediamine, tetramethylhexadiamine, triethylenediamine, N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, N,N-dimethylanisidine, pyridine, picoline, quinoline, N,N'-dimethylaminopyridine, N-methylpiperidine, N,N'-dimethylpiperazine, 1,8-diazabicyclo-[5,4,0]-7-undecene (DBU), and the like.
[0027] Specific examples of tertiary phosphines include trimethylphosphine, triethylphosphine, tripropylphosphine, tributylphosphine, triphenylphosphine, dimethylphenylphosphine, methyldiphenylphosphine, etc. Among these, tertiary amines are preferred because they provide a cured product with higher heat resistance.
[0028] The plating undercoat paint of the present invention can be obtained by, for example, adding a binder in which an epoxy resin and an inorganic filler are mixed in advance to a dispersion of conductive or reducing polymer microparticles, thereby obtaining a plating undercoat paint in which the solids are uniformly dispersed without agglomeration.
[0029] <Method of manufacturing plated items> Usually, in order to maintain high adhesion between the plating underlayer and the plating layer, the underlayer is cured by heating or drying and curing by exposure to light or electron beams before plating. Drying is performed at room temperature or under heating conditions, and the heating temperature is not limited as long as it is lower than the glass transition temperature of the substrate, and is generally 160°C or higher. The method for producing a plated product of the present invention includes a step 1 of applying a plating undercoat paint onto a substrate to form a plating undercoat layer, and a step of subjecting the plating undercoat layer to a heat treatment temperature T A a step 2 of heat-treating the metal plating film by electroless plating or electroless plating and electrolytic plating; and a step 3 of heating the metal plating film at a heat treatment temperature T B and a step 4 of subjecting the plated product to a heat treatment by the above method to obtain a plated product. Heat treatment temperature T in step 2 A is between the temperature at which the solvent evaporates and the temperature at which the catalyst adsorption of the plating underlayer decreases, and the heat treatment temperature T B is between the temperature at which the epoxy resin hardens and the temperature at which copper damage occurs. The specific explanation is as follows.
[0030] (Process 1)
[0031] The method for applying the plating undercoat paint of the present invention to a substrate is not particularly limited, and for example, it can be printed or coated using a screen printer, a gravure printer, a flexographic printer, an offset printer, a spin coater, a roll coater, or the like. Among these, in order to form a fine pattern with a line width of 100 μm or less, it is preferable to use a screen printer, a gravure offset printer, a flexographic printer, or a roll coater. From the viewpoint of continuous printing, the viscosity increase rate is preferably 100% or more and less than 200%, and more preferably less than 100%.
[0032] The thickness of the plating underlayer formed is preferably 10 nm to 10 μm (0.01 to 10 μm), and more preferably 1.0 μm to 10 μm. If the thickness is less than 10 nm, the plating is difficult to deposit, whereas if the thickness exceeds 10 μm, it is difficult to obtain adhesion between the substrate and the metal plating film. Furthermore, by setting the thickness in the range of 1.0 μm to 10 μm, the deposition properties of the plating are improved.
[0033] The substrate of the present invention is not particularly limited, but examples thereof include polyethylene naphthalate (PEN) resin, polyethylene terephthalate (PET) resin, polypropylene (PP) resin, polycarbonate (PC) resin, polyamide (PA) resin, polyimide (PI) resin, cycloolefin polymer (COP) resin, polyether ether ketone (PEEK) resin, liquid crystal polymer (LCP) resin, fluororesin, epoxy resin, phenolic resin, glass, and the like. The shape of the substrate is not particularly limited, but may be, for example, a plate or a film. Other examples of substrates include resin molded products obtained by molding resin by injection molding, etc. By providing the plating material of the present invention on such resin molded products, decorative plated products for automobiles, for example, can be produced, or by providing the plating material of the present invention over the entire surface or in a pattern on a film made of polyimide resin, for example, electric circuit products can be produced. The substrate used in the present invention is preferably a polyimide (PI) resin film or a liquid crystal polymer (LCP) resin film.
[0034] (Process 2) The applied plating undercoat is heat-treated at temperature T A By this treatment, the solution containing the metal is evaporated and a plating underlayer is formed. In a normal plating process, a heat treatment at a high temperature of 160°C to 200°C is required before plating to harden the undercoat. In the present invention, the expected adhesion can be obtained even in the heat treatment after plating while ensuring plating deposition, so the heat treatment temperature T A Set the temperature to 150°C or lower. However, if the heat treatment temperature before plating exceeds 140°C, the plating deposition property decreases, and when plating high-precision fine patterns, the plating does not deposit cleanly, causing problems such as an increase in resistance value and disconnection. A If the temperature is too low, the solvent contained in the plating underlayer cannot be completely evaporated, and sufficient adhesion cannot be obtained even if heat treatment is performed after plating. From the viewpoint of mass production, the heat treatment temperature T A It is more preferable that the temperature is 80°C to 140°C.
[0035] (Step 3) A metal plating film is formed on the plating underlayer by electroless plating or by electroless plating and electrolytic plating.
[0036] In the case of electroless plating, the substrate on which the plating underlayer has been formed is immersed in a catalytic solution for adhering a catalytic metal such as palladium chloride, and then washed with water, and then immersed in an electroless plating bath to form a metal plating film.
[0037] The catalyst solution is a solution containing a precious metal (catalytic metal) having catalytic activity for electroless plating. Examples of the catalytic metal include palladium, gold, platinum, rhodium, etc. These metals may be in the form of a single metal or a compound. From the viewpoint of stability containing the catalytic metal, palladium compounds are preferred, and among these, palladium chloride is particularly preferred. A specific preferred catalyst solution is 0.05% palladium chloride-0.005% hydrochloric acid aqueous solution (pH 3). The treatment temperature is 20 to 50° C., preferably 30 to 40° C., and the treatment time is 0.1 to 20 minutes, preferably 1 to 10 minutes. Through the above-mentioned operations, the polymer particles in the plating underlayer ultimately become conductive polymer particles.
[0038] The substrate treated as described above is immersed in a plating solution for depositing metal, thereby forming an electroless plating film. The plating solution is not particularly limited as long as it is a plating solution that is usually used for electroless plating. That is, all metals that can be used for electroless plating, such as copper, gold, silver, nickel, etc., can be used, with copper being preferred. A specific example of the electroless copper plating bath is ATS Addcopper IW bath (manufactured by Okuno Chemical Industries Co., Ltd.). The treatment temperature is 20° C. to 50° C., preferably 30° C. to 40° C., and the treatment time is 1 minute to 30 minutes, preferably 5 minutes to 15 minutes. The resulting plated product is preferably aged for several hours or more, for example, 2 hours or more, in a temperature range lower than the Tg of the base material used.
[0039] In addition, in the case of a plating underlayer formed by applying a plating undercoat paint containing conductive polymer microparticles to a substrate, a dedoping process can then be carried out and a plated product can be produced by the same operations as described above. The dedoping treatment may be carried out using a reducing agent, for example, a borohydride compound such as sodium borohydride or potassium borohydride, dimethylamine borane, diethylamine borane, or trimethylamine borane. For example, a method of immersing a substrate provided with a plating underlayer containing conductive polypyrrole fine particles and a binder in a solution containing an alkylamine borane such as alkylamine borane or triethylamine borane, and hydrazine, or in an alkaline solution, is used. From the viewpoints of operability and economy, immersion treatment in an alkaline solution is preferred. In particular, since the plating underlayer containing conductive polymer particles, epoxy resin, and inorganic filler can be made thin, it is possible to achieve dedoping by alkali treatment for a short period of time under mild conditions. For example, it is treated in a 1M aqueous sodium hydroxide solution at a temperature of 20 to 50° C., preferably 30 to 40° C., for 1 to 30 minutes, preferably 3 to 10 minutes. The substrate on which the plating underlayer has been formed and which has been subjected to the above-mentioned dedoping treatment is subjected to electroless plating to form a plated product, and the electroless plating method can be carried out by the same procedure as described above.
[0040] In addition, the above-mentioned plated product may be further plated with the same or a different metal by electrolytic plating on the formed metal plating film. The metal plating film may be formed on both sides of the substrate.
[0041] (Step 4) In step 4, the substrate after plating is heated to a temperature of T B The heat treatment temperature T B is basically set to 160°C or less. Heat treatment temperature T B However, if the temperature exceeds 150°C to 160°C, copper damage will occur, and copper ions oxidized from the metal plating layer will diffuse through the plating underlayer and reach the substrate, decomposing the substrate and causing a problem of reduced adhesion between the plating underlayer and the substrate. In addition, if the epoxy resin and hardener used are heated below the reaction initiation temperature (110°C to 120°C), sufficient adhesion cannot be obtained even if the heat treatment is performed. B The temperature is preferably 110°C to 160°C. From the viewpoint of mass production, the heat treatment temperature T B It is more preferable that the temperature is 120°C to 150°C. EXAMPLES
[0042] The present invention will be described based on the embodiments, but is not limited thereto.
[0043] Base paint 1 1.5 mmol of anionic surfactant Pelex OT-P (Kao Corporation), 10 mL of toluene, and 100 mL of ion-exchanged water were added and stirred until emulsified while maintaining the temperature at 20° C. to obtain an emulsion. Next, 21.2 mmol of pyrrole monomer was added to the resulting emulsion and stirred for 1 hour, and then 6 mmol of ammonium persulfate was added and the polymerization reaction was carried out for 2 hours. After the reaction was completed, the organic phase was recovered and washed several times with ion-exchanged water to obtain conductive polypyrrole fine particles dispersed in toluene. Next, 1 part by mass of conductive polypyrrole microparticles was mixed with 10 parts by mass of epoxy resin (epoxy equivalent 3000-5000) as a binder and 3 parts by mass of inorganic filler, and a dilution solvent, isophorone (boiling point 215°C), was added to prepare primer 1 (filler:epoxy = 0.3:1).
[0044] Base paint 2 Undercoat 2 (filler:epoxy=0.3:1) was obtained by carrying out the same procedure as for undercoat 1, except that a dilution solvent, methyl ethyl ketone (MEK) (boiling point: 79° C.), was added.
[0045] Base paint 3 Undercoat coating 3 (filler:epoxy=0.3:1) was obtained by carrying out the same operation as for undercoat coating 1, except that 10 parts by mass of an epoxy resin (epoxy equivalent weight 2400 to 3300) was added.
[0046] Base paint 4 Undercoat coating 4 (filler:epoxy=0.3:1) was obtained by carrying out the same operation as for undercoat coating 1, except that 10 parts by mass of epoxy resin (epoxy equivalent weight 7500 to 8500) was added.
[0047] Base paint 5 Undercoat paint 5 (filler:epoxy=1:1) was obtained by carrying out the same operations as for undercoat paint 1, except that 8 parts by mass of epoxy resin (epoxy equivalent 3000-5000) and 8 parts by mass of inorganic filler were added.
[0048] Base Coat 6 Undercoat paint 6 (filler:epoxy=0.3:1) was obtained by carrying out the same operations as for undercoat paint 1, except that 46 parts by mass of epoxy resin (epoxy equivalent weight 3000-5000) and 14 parts by mass of inorganic filler were added.
[0049] Comparison Base Coat 1 Comparative primer coating 1 (filler:epoxy=0) was obtained by carrying out the same procedure as for primer coating 1, except that 16 parts by mass of epoxy resin (epoxy equivalent: 3000-5000) was added and no inorganic filler was added.
[0050] Comparison Base Coat 2 Comparative primer 2 (filler:epoxy = 1.5:1) was obtained by carrying out the same operations as for primer 1, except that 6.4 parts by mass of epoxy resin (epoxy equivalent 3000-5000) and 9.6 parts by mass of inorganic filler were added.
[0051] Comparison Base Coat 3 Comparative primer 3 (filler:epoxy = 0.3:1) was obtained by carrying out the same operations as for primer 1, except that 54 parts by mass of epoxy resin (epoxy equivalent 3000-5000) and 16 parts by mass of inorganic filler were added.
[0052] For the components of the base coat, please also refer to Tables 1 and 2. [Table 1] [Table 2]
[0053] <Examples 1 to 11 and Comparative Examples 1 to 6> (Step 1 and Step 2) A screen printer was used to coat one side of a polyimide film substrate (manufactured by Toray DuPont Co., Ltd., product name "Kapton 200H") with a primer coating, and the coating was applied at a temperature T ABy subjecting the sample to heat treatment for a period of time, the contained solvent was volatilized, and a sample for confirming the plating deposition was prepared, which was a substrate on which a plating underlayer with a thickness of 2 μm was formed and which had a pattern including dense areas, sparse areas, and fine lines. Thereafter, the plating deposition properties of the above-mentioned plating deposition confirmation samples were evaluated by the following method.
[0054] <Examples 21 to 31, Comparative Examples 11, 14, and 16> (Step 1 and Step 2) A primer was applied to one side of a polyimide film substrate (manufactured by Toray DuPont Co., Ltd., product name "Kapton 200H") using a screen printing machine, and the substrate was heated at a temperature T A The substrate was prepared by subjecting the substrate to a heat treatment for 10 minutes, and the solvent contained therein was evaporated to form a plating undercoat layer having a thickness of 2 μm. The undercoat paint and the first heat treatment conditions of Examples 21 to 31 were the same as those of Examples 1 to 11. The undercoat paint and the first heat treatment conditions of Comparative Examples 11, 14, and 16 were the same as those of Comparative Examples 1, 4, and 6. (Steps 3 and 4) The substrate on which the underlayer was formed was immersed in a 1M sodium hydroxide aqueous solution at 35°C for 5 minutes, then rinsed with ion-exchanged water, and then immersed in a 0.02% palladium chloride-0.01% hydrochloric acid aqueous solution at 35°C for 5 minutes, followed by rinsing with ion-exchanged water to adhere a catalytic metal to the plating underlayer. The substrate was then immersed in an electroless plating bath (manufactured by Okuno Chemical Industries Co., Ltd., product name "ATS Addcopper IW Bath") for 10 minutes at 35°C to deposit copper with a film thickness of 0.3 μm. Further, electrolytic plating was performed in a copper sulfate plating bath to thicken the substrate to 30 μm, and the substrate was then subjected to a second heat treatment at a temperature T B A sample for checking adhesion having a plating layer was completed by heat treatment at . Next, the adhesion confirmation samples that had been subjected to the above treatment were further evaluated for plating adhesion by the following method.
[0055] (Plating Deposition Properties) The area where copper was deposited was visually observed, and the plating deposition property was evaluated as follows. Note that dense plated areas are areas where the wiring width is 100μm or more and where continuous patterns are densely packed. Sparse plated areas are areas where the wiring width is 100μm or more but the patterns are independent. Fine plated line areas are areas where the wiring width is less than 100μm. The ease of plating deposition is dense plated areas > sparse plated areas ≒ fine plated line areas. ◯: The plating film has grown in all areas, including densely plated areas, sparsely plated areas, and finely plated areas. △: A plating film has grown in the densely plated area, but there are areas in either the sparsely plated area or the finely plated area where the plating film has not grown. ×: There are areas where the plating film has not grown in all of the densely plated areas, sparsely plated areas, and finely plated areas.
[0056] The plating deposition results are summarized in Table 3. In Example 3, the primer 1 was used, but the temperature T A The temperature was 150°C, exceeding 140°C. There were some areas where the plating film had not grown in either the sparsely plated areas or the finely plated wire areas, but the plating film had grown in the densely plated areas. In Example 11, the temperature T of the first heat treatment A Since the temperature range is within the preferred range of 80°C to 140°C, and the mass ratio of the polymer particles polypyrrole:epoxy resin used in the undercoat 6 is also at the limit of the optimum range of 1:46, the plating deposition performance is slightly reduced. In Comparative Example 2, the primer 1 was used, but the temperature T A Because the plating temperature was 160°C, which exceeded 140°C, there were areas where the plating film had not grown in the densely plated areas, sparsely plated areas, and finely plated areas, and the plating deposition performance was reduced. In Comparative Examples 3 and 5, Comparative Primer Coatings 1 and 3 were used. The plating deposition properties were reduced because Comparative Primer Coating 1 did not contain any inorganic filler and the mass ratio of polymeric microparticle polypyrrole:epoxy resin used in Comparative Primer Coating 1 exceeded the optimum range. There were areas where the plating film had not grown in each of the dense plating areas, sparse plating areas, and fine plating line areas. In the other Examples 1 to 2, 4 to 10 and Comparative Examples 1, 4, and 6, the plating film grew in all of the densely plated portions, sparsely plated portions, and finely plated portions.
[0057] [Table 3]
[0058] (Plating adhesion) The 180 degree peel strength [N / mm] of each of the plated products of Examples 21 to 31 and Comparative Examples 11, 14, and 16 produced above was measured. ○: Peel strength 0.5N / mm or more △: Peel strength 0.35N / mm or more ×: Peel strength less than 0.35N / mm
[0059] The plating adhesion results are summarized in Table 4. Temperature T of the second heat treatment in Example 24 B is 160° C., and the temperature T of the second heat treatment in Example 26 B The temperature was 110° C., which is just at the upper and lower limits of the preferred range of 110° C. to 160° C. The adhesion was slightly weaker than in the other examples. In Example 30, the mass ratio of the polymeric particulate polypyrrole to epoxy resin used in the base coat 5 was at the limit of the optimum range of 1:8, and the mass ratio of the polymeric particulate polypyrrole to epoxy resin used in the base coat 6 was also at the limit of the optimum range of 1:1, so that the plating adhesion was slightly reduced. In Comparative Examples 11 and 16, the temperature T B were 180° C. and 100° C., respectively, which are outside the preferred range of 110° C. to 160° C., and therefore the expected adhesion was not obtained. In Comparative Example 14, both the mass ratio of the filler to the epoxy resin and the mass ratio of the polypyrrole to the epoxy resin in the comparative primer 2 used are outside the optimum range. The other Examples 21 to 23, 25, 27 to 29, and 31 all had a 180 degree peel strength of 0.5 N / mm or more.
[0060]
Table 4
Claims
1. Step 1: applying a plating undercoat paint onto a substrate to form a plating undercoat layer; The plating underlayer is heat-treated at temperature T A Step 2: heat-treating the Step 3 of forming a metal plating film on the substrate by electroless plating or electroless plating and electrolytic plating; and The metal plating film is heat-treated at temperature T B A method for producing a plated article, comprising the steps of: the plating undercoat paint includes an epoxy resin, a conductive polymer, an inorganic filler, and a solvent, the conductive polymer and the epoxy resin being in a mass ratio of 1:8 to 1:46; The heat treatment temperature T A is between the temperature at which the solvent evaporates and the temperature at which the catalyst adsorption of the plating underlayer decreases, The heat treatment temperature T B A method for producing plated objects, characterized in that the temperature is between the temperature at which the epoxy resin hardens and the temperature at which copper damage occurs.
2. 2. The method for producing a plated product according to claim 1, wherein the plating undercoat contains 0.3 to 1.0 part by mass of the inorganic filler per 1 part by mass of the epoxy resin.
3. 2. The method for producing a plated article according to claim 1, wherein the conductive polymer and the epoxy resin have a mass ratio of 1:9 to 1:
14.
4. The heat treatment temperature T A is 80° C. to 140° C., and the heat treatment temperature T B The method for producing a plated article according to claim 1, wherein the temperature is 120°C to 150°C.
5. A plated article produced by the method for producing a plated article according to any one of claims 1 to 4.
Citation Information
Patent Citations
Method of plating board for printed circuit
JP1984129489A
Method of manufacturing flexible printed board
JP2004079660A
Composition for forming electroless plating underlayer film
WO2015019596A1