Magnetic substrate, coil component including magnetic substrate, circuit module including coil component, and electronic device including circuit module
A magnetic substrate with distinct metal magnetic particle groups, featuring varying hematite and magnetite ratios in their insulating films, addresses uneven magnetic saturation, improving coil component performance by reducing flux concentration and eddy current loss.
Patent Information
- Application Number
- JP2023054406
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Magnetic saturation occurs unevenly in magnetic substrates containing multiple types of metal magnetic particles with different average particle sizes, leading to non-uniform magnetic properties and impaired electrical characteristics in coil components.
A magnetic substrate is designed with two distinct metal magnetic particle groups, each with a different average particle size, where the first group has a higher hematite content in its insulating film and a larger ratio of hematite to magnetite, while the second group has a lower hematite content in its insulating film, enhancing insulation and reducing magnetic flux concentration.
This configuration suppresses non-uniform magnetic saturation and improves electrical characteristics by reducing eddy current loss and magnetic resistance, thereby enhancing the performance of coil components.
Smart Images

Figure 2024142273000001_ABST
Abstract
Description
[Technical field]
[0001] The disclosure of this specification mainly relates to a magnetic base, a coil component including the magnetic base, a circuit module including the coil component, and an electronic device including the circuit module. [Background technology]
[0002] The coil component has a magnetic base made of a magnetic material, a coil conductor provided on the magnetic base, and an external electrode connected to an end of the coil conductor. A magnetic base made by bonding a large number of metallic magnetic particles made of a soft magnetic metal material that is unlikely to cause magnetic saturation even when a large current flows is known.
[0003] The magnetic base of the coil component is required to have high magnetic permeability. It is known that the magnetic permeability of the magnetic base can be increased by improving the filling rate of the metal magnetic particles in the magnetic base. For example, JP 2016-208002 A describes that the filling rate of the metal magnetic particles in the magnetic base is increased by configuring the magnetic base to include three or more types of metal magnetic particles having different average particle sizes. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-208002 A Summary of the Invention [Problem to be solved by the invention]
[0005] In a coil component having a magnetic base containing two or more types of metal magnetic particle groups with different average particle sizes, the magnetic flux generated when a current is applied preferentially passes through the large-diameter metal magnetic particles contained in the metal magnetic particle group with the large average particle size. Therefore, in such a coil component, magnetic saturation is likely to occur in the magnetic path where there are many large-diameter metal magnetic particles, and magnetic saturation occurs non-uniformly in the magnetic base. If magnetic saturation occurs non-uniformly in the magnetic base, it becomes difficult to improve the electrical characteristics of the coil component.
[0006] It is an object of the invention disclosed herein to solve or alleviate at least some of the above-mentioned problems. One of the more specific objects of the invention disclosed herein is to suppress the occurrence of non-uniform magnetic saturation in a magnetic substrate. The various inventions disclosed herein may be collectively referred to as "the present invention."
[0007] Objects of the present invention other than those mentioned above will become clear throughout the entire description of the specification. The invention disclosed in this specification may solve problems that are understood from other than the description in the "Problems to be Solved by the Invention" column. When the effects of an embodiment are described in this specification, the problems of the invention corresponding to the embodiment can be understood from the effects. [Means for solving the problem]
[0008] A coil component according to one embodiment of the present invention has a first metal magnetic particle group and a second metal magnetic particle. The first metal magnetic particle group includes a plurality of first metal magnetic particles and has a first average particle size. The first metal magnetic particles include a first metal portion and a first insulating film that covers the surface of the first metal portion and contains hematite. The second metal magnetic particle group includes a plurality of second metal magnetic particles and has a second average particle size. The second metal magnetic particles include a second metal portion and a second insulating film that covers the surface of the second metal portion and contains magnetite. In one embodiment, a Raman spectrum obtained by irradiating the first insulating film with an excitation laser having a wavelength of 488 nm has a wave number of 680 cm. -1 The wavenumber for the peak intensity of magnetite near 300 cm-1 The first HM ratio, which represents the ratio of the peak intensities of hematite present near the second insulating film, is calculated by irradiating the second insulating film with an excitation laser having a wavelength of 488 nm at a wave number of 680 cm. -1 The wavenumber for the peak intensity of magnetite near 300 cm -1 This is larger than the second HM ratio, which represents the ratio of the peak intensities of hematite present nearby. Effect of the Invention
[0009] According to one aspect of the invention disclosed in the specification, the occurrence of non-uniform magnetic saturation in the magnetic substrate can be suppressed. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a perspective view illustrating a coil component according to an embodiment. [Diagram 2] 2 is a cross-sectional view that illustrates a cross section of the coil device of FIG. 1 taken along line II. [Diagram 3] 3 is an enlarged schematic view of a region A of the magnetic substrate in FIG. 2. FIG. [Figure 4a] FIG. 2 is a cross-sectional view that typically shows a cross section of a first metal magnetic particle. [Figure 4b] FIG. 3 is a cross-sectional view that typically shows a cross section of a second metal magnetic particle. [Diagram 5] FIG. 4 is a flow diagram illustrating a method for manufacturing a coil component according to one embodiment. [Figure 6] FIG. 11 is a cross-sectional view of a coil component according to another embodiment. [Figure 7] 7 is an enlarged schematic view of a region B of the magnetic substrate in FIG. 6. FIG. [Figure 8] FIG. 11 is a cross-sectional view of a coil component according to another embodiment. [Figure 9] FIG. 9 is a plan view of the coil device of FIG. 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Various embodiments of the present invention will be described below with reference to the drawings as appropriate. Components common to multiple drawings are given the same or similar reference symbols throughout the multiple drawings. Please note that the drawings are not necessarily drawn to scale for the sake of convenience. The embodiments described below do not necessarily limit the invention according to the claims. Elements described in the following embodiments are not necessarily essential to the solution of the invention.
[0012] 1. First embodiment 1-1 Basic structure of coil component 1 Various embodiments disclosed in this specification relate to a magnetic base and a coil component including the magnetic base. A basic structure of a coil component 1 including a magnetic base 10 according to a first embodiment of the present invention will be described with reference to Fig. 1 and Fig. 2. Fig. 1 is a perspective view showing the coil component 1, and Fig. 2 is a schematic cross-sectional view of the coil component 1 cut along a plane along line II in Fig. 1.
[0013] 1 and 2 show a laminated inductor as an example of the coil component 1. The illustrated laminated inductor is an example of the coil component 1 including a magnetic base 10 to which the present invention can be applied, and the present invention can be applied to various types of coil components other than laminated inductors. The coil component 1 may be a wire-wound coil component, a planar coil, a bead inductor, or any other coil component. The coil component 1 may be a transformer, a filter, a reactor, an inductor array, or various other coil components. The coil component 1 may be a coupled inductor, a choke coil, or various other magnetically coupled coil components. The applications of the coil component 1 are not limited to those explicitly described in this specification.
[0014] As shown in the figure, the coil component 1 includes a magnetic base 10, a coil conductor 25 provided on the magnetic base 10, an external electrode 21 provided on the surface of the magnetic base 10, and an external electrode 22 provided on the surface of the magnetic base 10 at a position spaced apart from the external electrode 21. The external electrode 21 is electrically connected to one end of the coil conductor 25, and the external electrode 22 is electrically connected to the other end of the coil conductor 25.
[0015] The coil component 1 can be mounted on a mounting board 2a. In the illustrated embodiment, the mounting board 2a is provided with land portions 3a and 3b. The coil component 1 is mounted on the mounting board 2a by joining the external electrode 21 to the land portion 3a and connecting the external electrode 22 to the land portion 3b. In this specification, the mounting board 2a on which the coil component 1 is mounted is called a circuit module 2. The circuit module 2 according to an embodiment of the present invention includes the coil component 1 and a mounting board 2a on which the coil component 1 is mounted. Various electronic components other than the coil component 1 can also be mounted on the circuit module 2. The circuit module 2 can be mounted on various electronic devices. Electronic devices on which the circuit module 2 can be mounted include smartphones, tablets, game consoles, automotive electrical equipment, servers, and various other electronic devices.
[0016] 1-2 Configuration of magnetic substrate 10 In one embodiment, the magnetic substrate 10 may be configured to have a rectangular parallelepiped shape. The length dimension of the magnetic substrate 10 is, for example, in the range of 1.0 mm to 6.0 mm, the width dimension is, for example, in the range of 0.5 mm to 4.5 mm, and the height dimension is, for example, in the range of 0.5 mm to 4.5 mm. The dimensions of the magnetic substrate 10 are not limited to the dimensions specifically described in this specification. In this specification, the term "rectangular parallelepiped" or "rectangular parallelepiped shape" does not mean only "rectangular parallelepiped" in the mathematically strict sense. The dimensions and shape of the magnetic substrate 10 are not limited to those explicitly described in this specification.
[0017] The magnetic base 10 has an upper surface 10a, a lower surface 10b, a first end surface 10c, a second end surface 10d, a first side surface 10e, and a second side surface 10f. The outer surface of the magnetic base 10 is defined by these six surfaces. The upper surface 10a and the lower surface 10b form the surfaces at both ends of the magnetic base 10 in the height direction, the first end surface 10c and the second end surface 10d form the surfaces at both ends of the magnetic base 10 in the length direction, and the first side surface 10e and the second side surface 10f form the surfaces at both ends of the magnetic base 10 in the width direction. The upper surface 10a and the lower surface 10b are spaced apart by the height dimension of the magnetic base 10, the first end surface 10c and the second end surface 10d are spaced apart by the length dimension of the magnetic base 10, and the first side surface 10e and the second side surface 10f are spaced apart by the width dimension of the magnetic base 10.
[0018] The magnetic substrate 10 has a body layer 20, a lower cover layer 19 provided on the lower surface of the body layer 20, and an upper cover layer 18 provided on the upper surface of the body layer 20. The upper cover layer 18, the lower cover layer 19, and the body layer 20 are components of the magnetic substrate 10.
[0019] 1-3 Coil conductor 2, the coil conductor 25 has a winding portion 25a wound around a coil axis Ax1 extending along the thickness direction (T-axis direction), a lead-out portion 25b1 extending from one end of the winding portion 25a to a first end face 10c of the magnetic base 10, and a lead-out portion 25b2 extending from the other end of the winding portion 25a to a second end face 10d of the magnetic base 10. The winding portion 25a has conductor patterns C11 to C17 extending in the circumferential direction around the coil axis Ax1. Adjacent ones of the conductor patterns C11 to C17 are connected to each other by vias (not shown).
[0020] 1-4 External electrode The external electrode 21 is provided on a first end surface 10c of the magnetic base 10. The external electrode 22 is provided on a second end surface 10d of the magnetic base 10. Each external electrode may extend to the lower surface of the magnetic base 10 as shown in the figure. The shape and arrangement of each external electrode are not limited to the example shown in the figure. For example, both the external electrodes 21 and 22 may be provided on the lower surface 10b of the magnetic base 10. In this case, the coil conductor 25 is connected to the external electrodes 21 and 22 provided on the lower surface 10b of the magnetic base 10 through a via conductor. The external electrodes 21 and 22 are arranged to be spaced apart from each other in the length direction.
[0021] 1-5 Metallic magnetic particles contained in the magnetic substrate 10 Next, the metal magnetic particles contained in the magnetic substrate 10 will be described with reference to Fig. 3, Fig. 4a, and Fig. 4b. Fig. 3 is an enlarged cross-sectional view showing a schematic enlargement of region A of the cross section shown in Fig. 2. Fig. 3 shows a schematic SEM image of region A of the cross section of the magnetic substrate 10 taken with a scanning electron microscope (SEM). Region A is an arbitrary region included in the cross section of the magnetic substrate 10 cut along the LT plane. Fig. 3 shows a schematic view of a portion of the numerous metal magnetic particles contained in the magnetic substrate 10.
[0022] The magnetic base 10 includes a plurality of first metal magnetic particles 31 and a plurality of second metal magnetic particles. In this specification, the plurality of first metal magnetic particles 31 included in the magnetic base 10 may be collectively referred to as a first metal magnetic particle group, and the plurality of second metal magnetic particles 32 included in the magnetic base 10 may be collectively referred to as a second metal magnetic particle group. In other words, the first metal magnetic particle group is composed of a plurality of first metal magnetic particles 31, and the second metal magnetic particle group is composed of a plurality of second metal magnetic particles 32.
[0023] In one embodiment, the average particle size of the plurality of first metal magnetic particles 31 (i.e., the average particle size of the first metal magnetic particle group) is in the range of 3 to 15 μm. In one embodiment, the average particle size of the plurality of second metal magnetic particles 32 (i.e., the average particle size of the second metal magnetic particle group) is, for example, in the range of 1 to 5 μm. In this specification, the average particle size of the plurality of first metal magnetic particles 31 may be referred to as the "first average particle size," and the average particle size of the plurality of second metal magnetic particles 32 may be referred to as the "second average particle size." The second average particle size is smaller than the first average particle size.
[0024] In one embodiment, the average particle size of the first metal magnetic particle group is in the range of 1.5 to 5 times the average particle size of the second metal magnetic particle group. By making the average particle size of the first metal magnetic particle group 1.5 to 5 times the average particle size of the second metal magnetic particle group, the second metal magnetic particles 32, which have a smaller diameter than the first metal magnetic particles 31, can easily enter between the first metal magnetic particles 31. In this way, by the magnetic base 10 including a plurality of first metal magnetic particles 31 and a plurality of second metal magnetic particles 32, the filling rate (density) of the metal magnetic particles in the magnetic base 10 can be increased.
[0025] The average particle size of the first metal magnetic particles 31 contained in the magnetic base 10 can be determined as follows. First, the magnetic base 10 is cut along its thickness direction (T-axis direction) to expose a cross section, and the cross section is photographed with a scanning electron microscope (SEM) at a magnification of about 1000 to 2000 times to obtain a circle-equivalent diameter (Heywood diameter) of each of the first metal magnetic particles 31 by image analysis. Next, the average value of the circle-equivalent diameters of each of the first metal magnetic particles 31 is calculated, and this average value can be used as the average particle size of the first metal magnetic particles 31. Since the average particle size of the first metal magnetic particles 31 is not significantly different from the average particle size of the raw material powder, the particle size distribution of the raw material powder of the first metal magnetic particles 31 can be measured by a laser diffraction scattering method according to JIS Z 8825, and the D50 value of the volume-based particle size distribution measured by this laser diffraction scattering method can be used as the average particle size of the first metal magnetic particles 31 contained in the magnetic base 10. The average particle size of the second metal magnetic particles 32 can be calculated in the same manner as the average particle size of the first metal magnetic particles 31 .
[0026] It can be confirmed that the magnetic base 10 has a first metal magnetic particle group and a second metal magnetic particle group with different average particle sizes as follows. First, the particle size of each of the metal magnetic particles contained in the magnetic base 10 is measured, and a particle size distribution showing the distribution of particle sizes is created based on the measurement results. The particle size distribution is a graph in which the horizontal axis indicates particle size and the vertical axis indicates the particle count. When peaks appear at two different positions on the horizontal axis in this particle size distribution, it can be determined that the magnetic base 10 has a first metal magnetic particle group and a second metal magnetic particle group with different average particle sizes.
[0027] In addition to the first metal magnetic particle group and the second metal magnetic particle group, the magnetic base 10 may include a third metal magnetic particle group having an average particle size smaller than that of the second metal magnetic particle group. The magnetic base 10 may include three or more types of metal magnetic particles having different average particle sizes.
[0028] As shown in FIG. 4a, the first metal magnetic particle 31 has a first metal part 31a that exhibits magnetism and a first insulating film 31b that covers the surface of the first metal part 31a. Also, as shown in FIG. 4b, the second metal magnetic particle 32 has a second metal part 32a that exhibits magnetism and a second insulating film 32b that covers the surface of the second metal part 32a. The first insulating film 31b can be distinguished from the first metal part 31a based on the difference in brightness in a scanning electron microscope (SEM) image at about 10,000 times magnification. Similarly, the second insulating film 32b can be distinguished from the second metal part 32a based on the difference in brightness in the SEM image.
[0029] In one embodiment, the first metal part 31a is made of a soft magnetic metal material containing Fe. In one embodiment, the first metal part 31a contains Fe in an amount of 93.5 wt% or more. The first metal part 31a can contain Fe in a range of 93.5 to 97 wt%. The first metal part 31a can contain at least one additive element selected from the group consisting of Si, Cr, Al, Zr, Ti, Ni, and Si, in addition to Fe. The first metal part 31a is made of, for example, Fe-Cr-Al, Fe-Si-Cr-Al, or a mixture of these materials. The soft magnetic metal material for the first metal part 31a is not limited to those mentioned above.
[0030] In one embodiment, the first insulating film 31b contains an oxide of Fe. The first insulating film 31b contains insulating hematite (Fe2O3). The first insulating film 31b may contain magnetite (Fe3O4) in addition to hematite. Hematite has better insulating properties than magnetite but does not exhibit soft magnetic properties. On the other hand, magnetite has poorer insulating properties than hematite but exhibits soft magnetic properties. In one embodiment, the content ratio of magnetite in the first insulating film 31b is lower than the content ratio of hematite. In one embodiment, the content ratio of hematite in the first insulating film 31b is higher than the content ratio of magnetite. In one embodiment, the difference between the content ratio of hematite and the content ratio of magnetite in the first insulating film 31b is determined by the difference in wave number of 300 cm in a Raman spectrum obtained by irradiating the first insulating film 31b with an excitation laser having a wavelength of 488 nm. -1 Peak intensity and wave number of hematite near 680 cm -1 In this specification, the peak intensity of the magnetite at a wave number of 680 cm is determined by comparing it with the peak intensity of magnetite present in the vicinity of the first insulating film 31b. -1 The wavenumber for the peak intensity of magnetite near 300 cm -1The ratio of the peak intensities of hematite present in the vicinity of the first insulating film 31b may be referred to as the "first HM ratio". In one embodiment, the first HM ratio is greater than 1. By making the content ratio of hematite in the first insulating film 31b higher than the content ratio of conductive magnetite (in other words, by making the first HM ratio greater than 1), the insulating properties of the first insulating film 31b can be improved. By improving the insulating properties of the first insulating film 31b, electrical connection between the first metal portions 31a and between the first metal portion 31a and the second metal portion 32a can be prevented, and thus eddy current loss in the magnetic base 10 can be suppressed.
[0031] The first insulating film 31b may further contain chromite (FeCr2O4). In the first insulating film 31b, the content ratio of magnetite may be lower than the content ratio of chromite. In the first insulating film 31b, the content ratio of chromite may be higher than the content ratio of magnetite. In one embodiment, the difference between the content ratio of magnetite and the content ratio of chromite in the first insulating film 31b is determined based on the difference between the wave number of 680 cm in a Raman spectrum obtained by irradiating the first insulating film 31b with an excitation laser having a wavelength of 488 nm. -1 The peak intensity and wave number of magnetite present near 730 cm -1 For example, in a Raman spectrum obtained by irradiating the first insulating film 31b with an excitation laser having a wavelength of 488 nm, the peak intensity at the wave number of 680 cm -1 The wavenumber for the magnetite peak intensity near 730 cm -1When the ratio of the peak intensities of chromite present in the vicinity is greater than 1, it can be determined that the content ratio of chromite in the first insulating film 31b is higher than the content ratio of magnetite. Chromite has better insulating properties than magnetite, but does not exhibit soft magnetic properties. By making the content ratio of chromite in the first insulating film 31b higher than the content ratio of conductive magnetite, the insulating properties of the first insulating film 31b can be improved. By improving the insulating properties of the first insulating film 31b, electrical connections between the first metal parts 31a and between the first metal part 31a and the second metal part 32a can be prevented, so that eddy current loss in the magnetic base 10 can be suppressed.
[0032] In one embodiment, the second metal part 32a is made of a soft magnetic metal material containing Fe. In one embodiment, the second metal part 32a contains Fe in an amount of 93.5 wt% or more. The second metal part 32a can contain Fe in a range of 93.5 to 96 wt%. The first metal part 31a can contain at least one element selected from the group consisting of Si, Cr, Al, Zr, Ti, Ni, and Si, in addition to Fe. As the soft magnetic metal material for the second metal part 32a, for example, Fe-Si, Fe-Si-Cr, Fe-Si-Mn, or a mixture of these materials can be used. The soft magnetic metal material for the second metal part 32a is not limited to those mentioned above.
[0033] In one embodiment, the second insulating film 32b contains an oxide of Fe. The second insulating film 32b contains magnetite exhibiting soft magnetism. The second insulating film 32b may contain hematite in addition to magnetite. In one embodiment, the content ratio of magnetite in the second insulating film 32b is higher than the content ratio of hematite. In one embodiment, the difference between the content ratio of hematite and the content ratio of magnetite in the second insulating film 32b is determined based on a wave number of 300 cm in a Raman spectrum obtained by irradiating the second insulating film 32b with an excitation laser having a wavelength of 488 nm. -1 Peak intensity and wave number of hematite near 680 cm -1In this specification, the peak intensity of the magnetite at a wave number of 680 cm is determined by comparing it with the peak intensity of magnetite present in the vicinity of the second insulating film 32b. -1 The wavenumber for the peak intensity of magnetite near 300 cm -1 The ratio of the peak intensities of nearby hematite may be referred to as the “second HM ratio.” In one embodiment, the second HM ratio is less than 1.
[0034] The second insulating film 32b may further contain chromite. The content ratio of magnetite in the second insulating film 32b may be higher than the content ratio of chromite. In one embodiment, the difference between the content ratio of magnetite and the content ratio of chromite in the second insulating film 32b is determined based on the wave number of 680 cm in a Raman spectrum obtained by irradiating the second insulating film 32b with an excitation laser having a wavelength of 488 nm. -1 The peak intensity and wave number of magnetite present near 730 cm -1 For example, in a Raman spectrum obtained by irradiating the second insulating film 32b with an excitation laser having a wavelength of 488 nm, the peak intensity of chromite at a wave number of 680 cm -1 The wavenumber for the magnetite peak intensity near 730 cm -1 When the ratio of the peak intensities of chromite present in the vicinity is smaller than 1, it can be determined that the content ratio of magnetite in the second insulating film 32b is higher than the content ratio of chromite.
[0035] In the magnetic base 10, the first metal magnetic particles 31 are bonded to adjacent first metal magnetic particles or second metal magnetic particles 32 via at least one of the first insulating film 31b and the second insulating film 32b. Thus, the first metal portions 31a are electrically insulated from each other, and the first metal portion 31a and the second metal portion 32a are electrically insulated from each other.
[0036] In one embodiment, the first insulating film 31b and the second insulating film 32b contain an oxide of at least one additional element selected from the group consisting of Si, Cr, Al, Zr, Ti, Ni, and Si. In one embodiment, at least one of the first insulating film 31b and the second insulating film 32b may contain a nitride of the additional element. In the first insulating film 31b and the second insulating film 32b, the oxide of Fe is formed radially outside the oxide and nitride of the additional element.
[0037] In one embodiment, the first insulating film 31b is irradiated with an excitation laser having a wavelength of 488 nm, and the Raman spectrum obtained shows a wave number of 680 cm -1 The wavenumber for the peak intensity of magnetite near 300 cm -1 The first HM ratio, which represents the ratio of the peak intensities of hematite present in the vicinity of the second insulating film 32b, is obtained by irradiating the second insulating film 32b with an excitation laser having a wavelength of 488 nm at a wave number of 680 cm. -1 The wavenumber for the peak intensity of magnetite near 300 cm -1 This is larger than the second HM ratio, which represents the ratio of the peak intensities of hematite present nearby.
[0038] As described above, the content ratio of hematite, magnetite, and chromite in the first insulating film 31b and the second insulating film 32b can be determined based on the peak intensity by Raman spectroscopy. In one embodiment, the analysis of the Raman spectroscopy intensity in the first insulating film 31b can be performed using a Raman spectrum obtained by identifying two adjacent first metal magnetic particles 31 in a cross section of the magnetic substrate 10 cut along the T axis (for example, a cross section of the magnetic substrate 10 cut along the LT plane) and measuring the scattered light by a spectrometer when an excitation laser having a wavelength of 488 nm is irradiated onto the first insulating film 31b interposed between the two adjacent first metal magnetic particles 31. The Raman spectroscopic intensity of the first insulating film 31b can be analyzed by identifying the triple junction of the first metal magnetic particle 31 in a cross section of the magnetic substrate 10 cut along the T axis, and using the Raman spectrum obtained by measuring the scattered light when an excitation laser with a wavelength of 488 nm is irradiated onto the first insulating film 31b present at this triple junction using a spectrometer.
[0039] In the Raman spectrum obtained as described above, the peak intensities of the peaks derived from hematite, magnetite, and chromite are obtained, and the content ratios of hematite, magnetite, and chromite in the first insulating film 31b can be determined according to the magnitude of the peak intensities of the hematite, magnetite, and chromite. For example, when the peak intensity of the peak derived from hematite is greater than the peak intensity of the peak derived from magnetite in the obtained Raman spectrum, it can be determined that the content ratio of hematite is higher than the content ratio of magnetite. In the Raman spectrum, the peak intensity at a wave number of 300 cm is -1 The peak near 680 cm is due to hematite (Fe2O3). -1 The peak near 730 cm is due to magnetite (Fe3O4). -1 The peak near the 270 cm wavenumber in the Raman spectrum is due to chromite (FeCr2O4).-1 ~330cm -1 The peak due to magnetite (Fe3O4) can appear in the range of 665 cm in the Raman spectrum. -1 ~695cm -1 The peak due to chromite (FeCr2O4) can appear in the wavenumber range of 700 cm in the Raman spectrum. -1 ~760cm -1 The scattered light in the Raman spectroscopic analysis can be measured using a Raman spectrophotometer (NRS-3300) manufactured by JASCO Corporation.
[0040] The magnitude of the content ratio of hematite, magnetite, and chromite in the second insulating film 32b can be determined in the same manner as the method for determining the magnitude of the content ratio of hematite, magnetite, and chromite in the first insulating film 31b.
[0041] The first HM ratio, which represents the ratio of the hematite content ratio to the magnetite content ratio in the first insulating film 31b, is calculated by obtaining the peak intensity of hematite and the peak intensity of magnetite in a Raman spectrum obtained from scattered light generated when an excitation laser is irradiated to the first insulating film 31b exposed on the cross section of the magnetic base 10, and dividing the peak intensity of hematite thus obtained by the peak intensity of magnetite. The second HM ratio, which represents the ratio of the hematite content ratio to the magnetite content ratio in the second insulating film 32b, is calculated by obtaining the peak intensity of hematite and the peak intensity of magnetite in a Raman spectrum obtained from scattered light generated when an excitation laser is irradiated to the second insulating film 32b exposed on the cross section of the magnetic base 10, and dividing the peak intensity of hematite thus obtained by the peak intensity of magnetite.
[0042] In one embodiment, the Fe content in the first metal portion 31a is higher than the Fe content in the second metal portion 32a. Since Fe has high saturation magnetization, by making the Fe content in the first metal portion 31a higher than the Fe content in the second metal portion 32a, magnetic saturation can be prevented from occurring in the magnetic path passing through the first metal magnetic particle 31. The Fe content in the first metal portion 31a and the Fe content in the second metal portion 32a are measured by exposing a cross section of the magnetic base 10 by cutting the magnetic base 10 along the coil axis Ax1 and performing an energy dispersive X-ray spectroscopy (EDS) analysis on the cross section. The Fe content can be measured using a scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectroscopy (EDS) detector. An EDS analysis using an SEM equipped with an EDS detector is called an SEM-EDS analysis. The Fe content is measured at an acceleration voltage of 5 kV using, for example, a scanning electron microscope SU7000 manufactured by Hitachi High-Tech Corporation and an energy dispersive X-ray spectrometer Octane Elite manufactured by Ametec Co., Ltd. The contents of elements other than Fe contained in the first soft magnetic metal particles 30a are also measured by SEM-EDS analysis in the same manner as the Fe content.
[0043] The first insulating film 31b and the second insulating film 32b may be oxide films formed by oxidizing elements such as Fe contained in the raw material powder by performing a heat treatment on a molded body containing the raw material powder of the first metal magnetic particles 31 and the second metal magnetic particles 32. As described in detail later, the magnetic base 10 can be produced by mixing raw material powder made of a soft magnetic material with a resin to generate a mixed resin composition and heating this mixed resin composition. The elements contained in the raw material powder may be diffused to the surface of the raw material powder by the heat treatment in the manufacturing process of the magnetic base 10, and oxidized on the surface of the raw material powder to form the first insulating film 31b and the second insulating film 32b. The first insulating film 31b and the second insulating film 32b may be formed by heating a coating layer formed on the surface of the raw material powder of the first metal part 31a containing Fe and the raw material powder of the second metal part 32a containing Fe.
[0044] In one embodiment, the thickness of the first insulating film 31b and the second insulating film 32b is 100 nm or less. The thickness of the first insulating film 31b and the second insulating film 32b can be changed depending on the average particle size of the soft magnetic metal particles.
[0045] 1-6 Manufacturing method of coil component 1 Next, an example of a method for manufacturing the coil component 1 will be described with reference to FIG. 5. Since the magnetic base 10 is produced in the process of manufacturing the coil component 1, the method for manufacturing the magnetic base 10 will also be described with reference to FIG. 5. FIG. 5 is a flow diagram showing a method for manufacturing the coil component 1 according to an embodiment of the present invention. In the following description, it is assumed that the coil component 1 is manufactured by a sheet lamination method. The coil component 1 may be manufactured by a known method other than the sheet lamination method. For example, the coil component 1 can be manufactured by a lamination method such as a print lamination method, a thin film process method, or a slurry build method.
[0046] First, in step S1, a magnetic sheet is produced. The magnetic sheet is produced from a magnetic material paste obtained by kneading soft magnetic metal powder (raw material powder) that is the raw material of soft magnetic metal particles with a binder resin and a solvent. The raw material powder is a mixed powder produced by mixing a first raw material powder that is the raw material powder of the first metal magnetic particles 31 and a second raw material powder that is the raw material powder of the second metal magnetic particles 32. The average particle size of the second raw material powder is smaller than the average particle size of the first raw material powder. Both the first raw material powder and the second raw material powder are mainly composed of Fe. The raw material powder may contain 93.5 t% or more of Fe. The first raw material powder and the second raw material powder may contain at least one element selected from the group consisting of Si, Cr, Al, Zr, Ti, Ni, and Si as an additive element. All of the additive elements are elements that are more easily oxidized than oxygen in the heating process of step S12. The content ratio of Cr in the first raw material powder may be higher than the content ratio of Cr in the second raw material powder. The second raw material powder may have a higher Al content than the first raw material powder, and the second raw material powder may have a higher Si content than the first raw material powder.
[0047] A coating layer containing the above-mentioned additive element may be formed on the surfaces of the first and second raw material powders. The coating layer is formed, for example, by a sol-gel method.
[0048] The binder resin for the magnetic material paste is, for example, an acrylic resin. The binder resin for the magnetic material paste may be an epoxy resin, a polyimide resin, a resin known as a binder resin other than the above, or a mixture thereof. The solvent is, for example, toluene. This magnetic material paste is applied to the surface of a plastic base film by a doctor blade method or other general method. A sheet-shaped molded body is obtained by drying the magnetic material paste applied to the surface of the base film. A plurality of magnetic sheets are produced by pressurizing and molding this sheet-shaped molded body in a mold at a molding pressure of about 10 to 100 MPa.
[0049] Next, in step S2, a conductive paste is applied to some of the magnetic sheets prepared in step S1. The conductive paste is produced by kneading a conductive powder made of a conductive material with excellent conductivity, such as Ag, Pd, Cu, Al, or an alloy thereof, with a binder resin and a solvent. The binder resin for the conductive paste may be the same type of resin as the binder resin for the magnetic material paste. Both the binder resin for the conductive paste and the binder resin for the magnetic material paste may be acrylic resin.
[0050] By applying a conductive paste to the magnetic sheet, an unfired conductive pattern is formed on the magnetic sheet, which will become the conductive patterns C11 to C17 after firing. A through hole penetrating in the stacking direction is formed in a part of the magnetic sheet. When the conductive paste is applied to the magnetic sheet having the through hole, the conductive paste is also embedded in the through hole. In this way, an unfired via is formed in the through hole of the magnetic sheet. The conductive paste is applied to the magnetic sheet by, for example, a screen printing method.
[0051] Next, in step S3, the magnetic sheets prepared in step S1 are stacked to prepare an upper laminate that will become the upper cover layer 18, an intermediate laminate that will become the main body layer 20, and a lower laminate that will become the lower cover layer 19. The upper laminate and the lower laminate are each formed by stacking four of the magnetic sheets prepared in step S1 that do not have an unfired conductor pattern formed thereon. The intermediate laminate is formed by stacking seven magnetic sheets on which an unfired conductor pattern is formed in a predetermined order. The intermediate laminate prepared as described above is sandwiched between the upper laminate and the lower laminate from above and below, and the upper laminate and the lower laminate are thermocompressed to the intermediate laminate to obtain a main laminate. Next, the main laminate is divided into pieces of a desired size using a cutting machine such as a dicing machine or a laser processing machine to obtain a chip laminate. The chip laminate is an example of a molded body including an element that will become the magnetic base 10 after heat treatment and an unfired conductor pattern that will become the coil conductor 25 after heat treatment. The green compact including the base material that will become the magnetic substrate 10 after heat treatment and the unsintered conductor pattern that will become the coil conductor 25 after heat treatment may be produced by a method other than the sheet lamination method.
[0052] Next, in step S4, the molded body produced in step S3 is degreased. When a thermally decomposable resin is used as the binder resin for the magnetic material paste and the conductive paste, the molded body can be degreased in a non-oxygen atmosphere such as a nitrogen atmosphere. By performing the degreasing in a non-oxygen atmosphere, it is possible to prevent Fe contained in the raw material powder from being oxidized in the degreasing. The degreasing is performed at a temperature higher than the thermal decomposition start temperature of the binder resin for the magnetic material paste. When an acrylic resin is used as the binder resin for the magnetic material paste, the degreasing is performed at a temperature higher than the thermal decomposition start temperature of the acrylic resin, for example, 300 to 500°C. The thermally decomposable resin contained in the molded body is decomposed by the degreasing, so that no thermally decomposable resin remains in the molded body after the degreasing is completed. By using the same thermally decomposable resin as the binder resin for the magnetic material paste for the binder resin for the conductive paste, the thermally decomposable resin contained in the unsintered conductor pattern is also thermally decomposed in the degreasing in step S4. In this manner, in step S4, both the magnetic sheets and the unsintered conductor patterns constituting the compact are degreased.
[0053] Next, in step S5, the degreased compact is subjected to a first heating treatment. The first heating treatment is performed at a first heating temperature of 750°C to 900°C in a low oxygen concentration atmosphere containing oxygen in the range of 5 to 1000 ppm. The first heating treatment may be performed in a low oxygen concentration atmosphere of about 5 to 10 ppm. By heating the raw material powder at 750 to 900°C, the additive elements (e.g., Cr, Al, and Si) in each raw material powder are diffused to the surface vicinity by thermal diffusion and bonded with oxygen in the atmosphere. In the first heating treatment, oxides of Al, Cr, and Si, which are easily oxidized among the additive elements that have moved to the surface of each raw material powder, are generated. By the first heating treatment, oxides of the additive elements (e.g., Al2O3, Cr2O3, SiO2) are formed on the surfaces of the heated first raw material powder and second raw material powder. The first heating time for which the first heating treatment is performed can be between 1 hour and 6 hours. In addition to the additive elements, Fe may also be slightly oxidized in the first heating treatment. Since the first heat treatment is performed in a low oxygen concentration atmosphere, when Fe is oxidized, magnetite (Fe3O4) is generated more as the oxide of Fe than hematite (Fe2O3). In the first heat treatment, the oxide of Fe is generated radially outward from the oxide of the additive element.
[0054] Next, in step S6, the compact after being heated in the first heat treatment is subjected to a second heat treatment at an oxygen concentration higher than that in the first heat treatment. The second heat treatment may be performed in a low-oxygen atmosphere of more than 1000 ppm and not more than 10000 ppm. Since the second heat treatment is performed at an oxygen concentration higher than that in the first heat treatment, a part of the magnetite formed on the surface of the first raw material powder is further oxidized to generate hematite in the second heat treatment. On the other hand, since the content ratio of Al and Si in the second raw material powder is higher than that in the first raw material powder, most of the oxygen supplied to the periphery of the second raw material powder is consumed for the oxidation of Al and Si. Therefore, the change from magnetite to hematite is less likely to proceed on the surface of the second raw material compared to the reaction occurring on the surface of the first raw material powder. Also, in the second heat treatment, the magnetite generated in the first heat treatment is combined with Cr to generate chromite (FeCr2O4). Since the first raw material powder contains Cr at a higher content ratio than the second raw material powder, more chromite is generated on the surface of the first raw material powder than the second raw material powder.
[0055] In this way, the second heat treatment produces more hematite and chromite on the surface of the first raw material powder than on the surface of the second raw material powder. Also, because magnetite is consumed to produce hematite and chromite, the amount of magnetite decreases on the surface of the first raw material powder. Therefore, the second heat treatment can make the content ratio of hematite and chromite higher than the content ratio of magnetite on the surface of the first raw material powder. Also, because magnetite produced in the first heat treatment is less likely to change to hematite or chromite on the surface of the second raw material powder, the content ratio of magnetite on the surface of the second raw material powder can be made higher than the content ratio of hematite and chromite.
[0056] In the second heat treatment, in addition to the oxidation of the raw material powder, the conductor powder in the unsintered conductor pattern is also sintered. The conductor powder in the unsintered conductor pattern is sintered to obtain the coil conductor 25. When copper powder is used as the conductor powder, the copper crystals are densely sintered to become the coil conductor 25.
[0057] The second heating process is performed at the second heating temperature for only the second heating time. The second heating temperature and the second heating time are determined so that an insulating film having a sufficient thickness to ensure insulation is formed on the surface of the raw material powder. The second heating temperature can be, for example, between 500 and 700°C. The higher the second heating temperature, the faster the oxidation progresses, so the second heating time varies depending on the second heating temperature. When the second heating temperature is 500°C, the second heating time can be between 1 hour and 6 hours. When the second heating temperature is 700°C, the second heating time can be between 30 minutes and 1 hour.
[0058] In this way, the first and second raw powders contained in the compact are oxidized by the first and second heat treatments, so that the first metal magnetic particles 31 are produced from the first raw powder, and the second metal magnetic particles 32 are produced from the second raw powder. In the second heat treatment, a first insulating film 31b is formed on the surface of the first metal magnetic particles 31, and a second insulating film 32b is formed on the surface of the second metal magnetic particles 32. By the second heat treatment, adjacent metal magnetic particles are bonded to each other via the insulating films formed on their surfaces. In this way, a magnetic base 10 in which soft magnetic metal particles are bonded is obtained.
[0059] Next, in step S7, the external electrodes 21 and 22 are formed on the surface of the magnetic base 10 obtained in step S6. The external electrode 21 is connected to one end of the coil conductor 25, and the external electrode 22 is connected to the other end of the coil conductor 25. Before forming the external electrodes 21 and 22, the molded body after the second heat treatment may be impregnated with a resin. The molded body is impregnated with a thermosetting resin such as an epoxy resin. This allows the resin to permeate into the gaps between the soft magnetic metal particles in the magnetic base 10. Then, by hardening the resin impregnated in the magnetic base 10, the mechanical strength of the magnetic base 10 can be improved.
[0060] Through the above steps, the coil component 1 is manufactured.
[0061] 1-7 Example of Effects of the First Embodiment In the first embodiment, the first HM ratio in the first insulating film 31b formed on the surface of the first metal magnetic particle 31 constituting the first metal magnetic particle group having a large average particle size is larger than the second HM ratio in the second insulating film 32b formed on the surface of the second metal magnetic particle 32 constituting the second metal magnetic particle group having a small average particle size. In other words, when the first insulating film 31b and the second insulating film 32b are compared in terms of the content ratio of hematite and magnetite, the content ratio of hematite to magnetite in the first insulating film 31b is higher than the content ratio of hematite to magnetite in the second insulating film 32b. Since hematite is non-magnetic, the concentration of magnetic flux on the first metal magnetic particle 31 can be alleviated by covering the surface of the large-diameter first metal magnetic particle 31 with the first insulating film 31b having a higher content ratio of hematite than the second insulating film 32b. Therefore, it is possible to suppress magnetic saturation in the magnetic path passing through the first metal magnetic particle 31, and as a result, it is possible to alleviate the non-uniformity of magnetic saturation in the magnetic base 10.
[0062] Furthermore, by covering the surface of the first metal magnetic particle 31 with the first insulating film 31b having a high hematite content, it is possible to improve the insulating properties of the first metal magnetic particle 31. This makes it possible to suppress the occurrence of large eddy current loss caused by electrical connection between the first metal magnetic particle 31 and another adjacent metal magnetic particle (another first metal magnetic particle 31 or second metal magnetic particle 32).
[0063] In one embodiment, the magnetite content in the first insulating film 31b is lower than the hematite content (i.e., the first HM ratio is greater than 1), so that the first insulating film 31b can further reduce the concentration of magnetic flux on the first metal magnetic particles 31 and further improve the insulating properties of the first metal magnetic particles 31.
[0064] In one embodiment, the content ratio of magnetite in the first insulating film 31b is lower than the content ratio of non-magnetic chromite. Such a first insulating film 31b can further reduce the concentration of magnetic flux on the first metal magnetic particles 31.
[0065] In one embodiment, the content ratio of magnetite in the second insulating film 32b is higher than the content ratio of non-magnetic hematite, so that the second insulating film 32b can reduce the magnetic resistance of the magnetic path passing through the second metal magnetic particles 32. This can suppress the concentration of magnetic flux on the first metal magnetic particles 31, so that the non-uniformity of magnetic saturation in the magnetic base 10 can be further alleviated.
[0066] In one embodiment, the content ratio of magnetite in the second insulating film 32b is higher than the content ratio of non-magnetic chromite, so that the second insulating film 32b can reduce the magnetic resistance of the magnetic path passing through the second metal magnetic particles 32. This can suppress the concentration of magnetic flux on the first metal magnetic particles 31, so that the non-uniformity of magnetic saturation in the magnetic base 10 can be further alleviated.
[0067] In one embodiment, the Fe content in the first metal portion 31a is higher than the Fe content in the second metal portion 32a. Since Fe has high saturation magnetization, by increasing the Fe content in the first metal portion 31a, it is possible to suppress the occurrence of magnetic saturation due to the magnetic flux passing through the first metal magnetic particles 31 (first metal portion 31a). This makes it possible to further reduce the non-uniformity of magnetic saturation in the magnetic base 10.
[0068] 2. Second embodiment Next, a coil component 1 according to a second embodiment will be described with reference to Fig. 6 and Fig. 7. Fig. 6 is a cross-sectional view showing a cross section of the coil component 1 according to the second embodiment cut along the LT plane, and Fig. 7 is an enlarged cross-sectional view showing a schematic enlargement of region B of the cross section shown in Fig. 6. The second embodiment differs from the first embodiment in that the magnetic base 10 is partitioned into a first region 50a and a second region 50b.
[0069] As shown in FIG. 6, the magnetic base 10 is divided into a first region 50a and a second region 50b. In the illustrated embodiment, the magnetic base 10 has a plurality of second regions 50b. Each of the second regions 50b is disposed between adjacent conductor patterns among the conductor patterns C11 to C17. The second region 50b is a plate-like member extending parallel to the LW plane from the first end face 10c to the second end face 10d and from the first side face 10e to the second side face 10f. The first region 50a is a region of the magnetic base 10 other than the second region 50b.
[0070] 7, the first region 50a is composed of the first metal magnetic particles 31. The first region 50a does not include the second metal magnetic particles 32. The second region 50b is composed of the second metal magnetic particles 32. The second region 50b does not include the first metal magnetic particles 31.
[0071] 6 shows a magnetic path MP through which magnetic flux passes, which is generated when the current flowing between the external electrodes 21 and 22 through the coil conductor 25 changes. The entire length of the magnetic path MP passes through the magnetic base 10 made of a magnetic material, so the magnetic path MP is a closed magnetic path. The magnetic flux flows around the coil conductor 25 along the magnetic path MP. In FIG. 6, the flow of the magnetic flux is shown diagrammatically by arrows.
[0072] The magnetic flux path MP is divided into a first magnetic flux path passing through the first region 50a and a second magnetic flux path passing through the second region 50b. The first magnetic flux path indicates a region where the magnetic flux path MP overlaps with the first region 50a. The second magnetic flux path indicates a region where the magnetic flux path MP overlaps with the second region 50b. In one aspect, the first region 50a and the second region 50b are arranged so that a first magnetic flux path length representing the length of the first magnetic flux path is longer than a second magnetic flux path length representing the length of the second magnetic flux path. In the illustrated embodiment, a little less than half of the region of the magnetic flux path MP extending along the T axis overlaps with the second region 50b, but the remaining region of the magnetic flux path MP extending along the T axis and the region of the magnetic flux path MP extending along the L axis all overlap with the first region 50a. Thus, the length of the first magnetic flux path overlapping with the first region 50a of the magnetic flux path MP is longer than the length of the second magnetic flux path overlapping with the second region 50b of the magnetic flux path MP. A plurality of magnetic paths are generated around the coil conductor 25. When determining the lengths of the first and second magnetic paths, the region where the magnetic path that goes around the coil conductor 25 in the shortest distance overlaps with the first region 50a may be defined as the first magnetic path, and the region where the magnetic path overlaps with the second region 50b may be defined as the second magnetic path. The magnetic path that goes around the coil conductor 25 in the shortest distance is a path that is shortened so as to pass through the upper surface of the conductor pattern C11, the lower surface of the conductor pattern C17, and both ends of each of the conductor patterns C11 to C17 in the L-axis direction from the magnetic path MP shown in FIG. 6.
[0073] The magnetic base 10 is divided into the first region 50a and the second region 50b, and may not include other regions. That is, in one embodiment, the magnetic base 10 does not have any region other than the first region 50a and the second region 50b.
[0074] The magnetic base 10 and the coil component 1 according to the second embodiment can achieve the same effect as the magnetic base 10 and the coil component 1 according to the first embodiment. According to the second embodiment, the majority of the magnetic path MP passes through the first region 50a composed of the first metal magnetic particle group having a large average particle size, so that the magnetic resistance of the magnetic path MP can be reduced more than that of the first metal magnetic particles 31 in which the first metal magnetic particles 31 and the second metal magnetic particles 32 are mixed, and the inductance of the coil component 1 can be improved. In order to further improve the inductance, it is desirable that the length of the first magnetic path overlapping the first region 50a of the magnetic path MP is at least twice the length of the second magnetic path overlapping the second region 50b of the magnetic path MP.
[0075] 3. Third embodiment Next, a coil device 101 according to another embodiment of the present invention will be described with reference to Fig. 8 and Fig. 9. Fig. 8 is a cross-sectional view showing a cross section of the coil device 101 cut along the LT plane, and Fig. 9 is a plan view of the coil device 101. In Fig. 9, the coil conductor is drawn through the substrate. The coil device 101 differs from the coil device 1 in that it includes a magnetic substrate 110 instead of the magnetic substrate 10, and includes a coil conductor 125 instead of the coil conductor 25. The following description will focus on the differences between the coil device 101 and the coil device 1.
[0076] 10, the coil conductor 125 extends linearly from the external electrode 21 to the external electrode 22 in a plan view (when viewed from the T-axis). In this way, the coil conductor 125 does not have any parts that are arranged opposite to each other within the magnetic base 10 in a plan view. In this way, the coil conductor 125 does not have any parts that are arranged opposite to each other within the magnetic base 10 in a plan view, and therefore it is possible to increase the insulation reliability (voltage resistance) without changing the volume resistivity of the magnetic base 10, compared to a conventional inductor having an internal conductor with parts that are opposed to each other in a plan view.
[0077] The magnetic base 110 is divided into a first region 150a and a second region 150b. As shown in Fig. 9, the second region 150b is a plate-like member extending parallel to the LT plane from the upper surface 110a to the lower surface 110b and from the first end surface 110c to the second end surface 10d. The first region 150a is the region of the magnetic base 110 other than the second region 150b.
[0078] The first region 150a is composed of the first metal magnetic particles 31, similar to the first region 50a of the second embodiment. The second region 150b is composed of the second metal magnetic particles 32, similar to the second region 50b of the second embodiment. The magnetic base 110 is partitioned into the first region 150a and the second region 150b, and may not include other regions. That is, in one aspect, the magnetic base 110 does not have any region other than the first region 150a and the second region 150b.
[0079] 9 shows a magnetic path MP through which magnetic flux passes, which is generated when the current flowing between the external electrodes 21 and 22 through the coil conductor 25 changes. The entire length of the magnetic path MP passes through the magnetic base 10 made of a magnetic material, so the magnetic path MP is a closed magnetic path. The magnetic flux flows around the coil conductor 25 along the magnetic path MP. In FIG. 9, the flow of the magnetic flux is shown diagrammatically by arrows.
[0080] The magnetic flux path MP is divided into a first magnetic flux path passing through the first region 150a and a second magnetic flux path passing through the second region 150b. The first magnetic flux path indicates a region where the magnetic flux path MP overlaps with the first region 150a. The second magnetic flux path indicates a region where the magnetic flux path MP overlaps with the second region 150b. In one aspect, the first region 150a and the second region 150b are arranged such that a first magnetic flux path length representing the length of the first magnetic flux path is longer than a second magnetic flux path length representing the length of the second magnetic flux path. In the illustrated embodiment, a little less than half of the region of the magnetic flux path MP extending along the W axis overlaps with the second region 150b, but the remaining region of the magnetic flux path MP extending along the W axis and the region of the magnetic flux path MP extending along the L axis all overlap with the first region 50a. Therefore, the length of the first magnetic path that overlaps with the first region 150a of the magnetic path MP is longer than the length of the second magnetic path that overlaps with the second region 150b of the magnetic path MP.
[0081] According to the third embodiment, the magnetic base 110 is configured so that the first magnetic path overlapping the first region 150a of the magnetic path MP is longer than the second magnetic path overlapping the second region 150b. Therefore, the majority of the path of the magnetic path MP passes through the first region 150a composed of the first metal magnetic particle group having a large average particle size, so that the magnetic resistance of the magnetic path MP can be reduced more than when the first metal magnetic particles 31 and the second metal magnetic particles 32 are mixed, and the inductance of the coil component 1 can be improved. In order to further improve the inductance, it is desirable that the length of the first magnetic path overlapping the first region 150a of the magnetic path MP is at least twice the length of the second magnetic path overlapping the second region 150b of the magnetic path MP.
[0082] 4 Notes The dimensions, materials, and arrangements of each component described in the various embodiments above are not limited to those explicitly described in each embodiment, and each component can be modified to have any dimensions, materials, and arrangements that may fall within the scope of the present invention.
[0083] Components not explicitly described in this specification may be added to each of the above-described embodiments, and some of the components described in each embodiment may be omitted.
[0084] The designations "first," "second," "third," and the like in this specification are given to identify components, and do not necessarily limit the number, order, or content. Furthermore, numbers for identifying components are used in different contexts, and a number used in one context does not necessarily indicate the same configuration in another context. Furthermore, a component identified by a certain number does not prevent the component from also having the function of a component identified by another number.
[0085] In this specification, when a certain component is referred to as "including" or "having," it does not mean that other components are excluded, but rather that other components may be further included, unless this is inconsistent with the content of the present invention.
[0086] 5. Supplementary Notes The embodiments disclosed herein also include the following.
[0087] [Appendix 1] a first metal magnetic particle group including a first metal magnetic particle having a first average particle size, the first metal magnetic particle group including a first insulating film covering a surface of the first metal portion and containing hematite; a second metal magnetic particle including a second metal portion and a second insulating film covering a surface of the second metal portion and containing magnetite, the second metal magnetic particle having a second average particle size smaller than the first average particle size; having In the Raman spectrum obtained by irradiating the first insulating film with an excitation laser having a wavelength of 488 nm, -1 The wavenumber for the peak intensity of magnetite near 300 cm -1 The first HM ratio, which represents the ratio of the peak intensity of hematite present in the vicinity of the second insulating film, is determined by irradiating the second insulating film with an excitation laser having a wavelength of 488 nm at a wave number of 680 cm. -1The wavenumber for the peak intensity of magnetite near 300 cm -1 It is larger than the second HM ratio, which represents the ratio of the peak intensities of hematite present nearby. Magnetic substrate. [Appendix 2] The first insulating film further includes magnetite, the first HM ratio is greater than 1; The magnetic substrate according to [Appendix 1]. [Appendix 3] The first insulating film further includes chromite, In the Raman spectrum obtained by irradiating the first insulating film with an excitation laser having a wavelength of 488 nm, -1 The wavenumber for the magnetite peak intensity near 730 cm -1 The ratio of the peak intensities of the chromites present nearby is greater than 1. The magnetic substrate according to [Appendix 1] or [Appendix 2]. [Appendix 4] The second insulating film further includes hematite, the second HM ratio is less than 1; The magnetic substrate according to any one of [Appendix 1] to [Appendix 3]. [Appendix 5] The second insulating film further includes chromite, In the Raman spectrum obtained by irradiating the second insulating film with an excitation laser having a wavelength of 488 nm, -1 The wavenumber for the magnetite peak intensity near 730 cm -1 The ratio of the peak intensities of the chromites present nearby is less than 1. The magnetic substrate according to any one of [Appendix 1] to [Appendix 4]. [Appendix 6] The Fe content in the first metal portion is higher than the Fe content in the second metal portion. The magnetic substrate according to any one of [Appendix 1] to [Appendix 5]. [Appendix 7] a magnetic substrate comprising: a first metal magnetic particle group including a first metal magnetic particle group having a first average particle size, the first metal magnetic particle group including a first metal portion and a first insulating film covering the surface of the first metal portion and containing hematite; and a second metal magnetic particle group including a second metal portion and a second insulating film covering the surface of the second metal portion and containing magnetite, the second metal magnetic particle group having a second average particle size smaller than the first average particle size; a coil conductor embedded in the magnetic substrate; Equipped with a first HM ratio representing a ratio of a hematite content ratio to a magnetite content ratio in the first insulating film is greater than a second HM ratio representing a ratio of a hematite content ratio to a magnetite content ratio in the second insulating film; Coil parts. [Appendix 8] the substrate is partitioned into a first region composed of the plurality of first metal magnetic particles and a second region composed of the plurality of second metal magnetic particles; The closed magnetic path in the base body is divided into a first magnetic path passing through the first region and a second magnetic path passing through the second region, A first magnetic path length representing the length of the first magnetic path is longer than a second magnetic path length representing the length of the second magnetic path. A coil component described in [Appendix 7]. [Appendix 9] The closed magnetic path passes through only the first magnetic path and the second magnetic path. The coil component according to claim 7 or 8. [Appendix 10] A circuit module comprising the coil component according to any one of [Appendix 7] to [Appendix 9]. [Appendix 11] An electronic device including the circuit module according to [Appendix 10]. [Explanation of symbols]
[0088] 1, 101 Coil parts 10, 110 Magnetic substrate 25, 125 coil conductor 31 First metal magnetic particles 31a 1st metal part 31b First insulating film 32 Second metal magnetic particles 32a 2nd metal part 32b Second insulating film
Claims
1. a first metal magnetic particle group including a plurality of first metal magnetic particles having a first metal portion and a first insulating film covering a surface of the first metal portion and containing hematite, the first metal magnetic particle group having a first average particle size; a second metal magnetic particle including a second metal portion and a second insulating film covering a surface of the second metal portion and containing magnetite, the second metal magnetic particle having a second average particle size smaller than the first average particle size; having In the Raman spectrum obtained by irradiating the first insulating film with an excitation laser having a wavelength of 488 nm, the wave number is 680 cm -1 The wave number for the peak intensity of magnetite present near 300 cm -1 The first HM ratio, which represents the ratio of peak intensities of hematite present in the vicinity of the second insulating film, is a ratio of the peak intensities of hematite present in the vicinity of the second insulating film at a wave number of 680 cm in a Raman spectrum obtained by irradiating the second insulating film with an excitation laser having a wavelength of 488 nm. -1 The wave number for the peak intensity of magnetite present near 300 cm -1 is greater than a second HM ratio representing the ratio of peak intensities of hematite present in the vicinity, Magnetic substrate.
2. The first insulating film further includes magnetite, the first HM ratio is greater than 1; The magnetic substrate according to claim 1 .
3. The first insulating film further includes chromite, In the Raman spectrum obtained by irradiating the first insulating film with an excitation laser having a wavelength of 488 nm, the wave number is 680 cm -1 The wave number for the peak intensity of magnetite present near 730 cm -1 The ratio of the peak intensities of the chromites present nearby is greater than 1.
3. The magnetic substrate according to claim 1 or 2.
4. The second insulating film further includes hematite, the second HM ratio is less than 1; 3. The magnetic substrate according to claim 1 or 2.
5. The second insulating film further includes chromite, In the Raman spectrum obtained by irradiating the second insulating film with an excitation laser having a wavelength of 488 nm, the wave number is 680 cm -1 The wave number for the peak intensity of magnetite present near 730 cm -1 The ratio of the peak intensities of the chromites present in the vicinity is less than 1.
3. The magnetic substrate according to claim 1 or 2.
6. The Fe content in the first metal portion is higher than the Fe content in the second metal portion.
3. The magnetic substrate according to claim 1 or 2.
7. a first metal magnetic particle group including a first metal magnetic particle having a first average particle size, the first metal magnetic particle group including a first metal portion and a first insulating film covering the surface of the first metal portion and containing hematite; and a second metal magnetic particle group including a second metal portion and a second insulating film covering the surface of the second metal portion and containing magnetite, the second metal magnetic particle group having a second average particle size smaller than the first average particle size; a coil conductor embedded in the magnetic substrate; Equipped with In the Raman spectrum obtained by irradiating the first insulating film with an excitation laser having a wavelength of 488 nm, the wave number is 680 cm -1 The wave number for the peak intensity of magnetite present near 300 cm -1 The first HM ratio, which represents the ratio of peak intensities of hematite present in the vicinity of the second insulating film, is a ratio of the peak intensities of hematite present in the vicinity of the second insulating film at a wave number of 680 cm in a Raman spectrum obtained by irradiating the second insulating film with an excitation laser having a wavelength of 488 nm. -1 The wave number for the peak intensity of magnetite present near 300 cm -1 is greater than a second HM ratio representing the ratio of peak intensities of hematite present in the vicinity, Coil parts.
8. the substrate is partitioned into a first region composed of a plurality of first metal magnetic particles and a second region composed of a plurality of second metal magnetic particles; a closed magnetic path in the base body is divided into a first magnetic path passing through the first region and a second magnetic path passing through the second region, A first magnetic path length representing the length of the first magnetic path is longer than a second magnetic path length representing the length of the second magnetic path. The coil component according to claim 7.
9. The closed magnetic path passes through only the first magnetic path and the second magnetic path. The coil component according to claim 8.
10. A circuit module comprising the coil component according to claim 7 or 8.
11. An electronic device comprising the circuit module according to claim 10.
Citation Information
Patent Citations
Coil electronic component and method of manufacturing the same
JP2016208002A