Active energy ray-curable adhesive composition, adhesive using the same, adhesive sheet, and laminate

The active energy ray-curable adhesive composition addresses adhesion and plasticizer resistance issues by using a specific acrylic resin formulation, ensuring strong bonding to PVC and polyolefins with improved coating properties.

JP2024142334APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023054432
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing acrylic adhesive compositions exhibit poor adhesion to polyvinyl chloride (PVC) substrates and low plasticizer resistance, limiting their application in materials such as automobiles, and have high melt viscosity requiring high-temperature coating.

Method used

An active energy ray-curable adhesive composition comprising an acrylic resin with specific monomer units, including alkyl (meth)acrylates with 4 or more carbon atoms, alkoxyalkyl (meth)acrylates, and polar group-containing ethylenically unsaturated monomers, with a weight average molecular weight of 200,000 or less, and minimal thermal crosslinking agent content, ensuring low glass transition temperature and excellent adhesion to PVC.

Benefits of technology

The composition achieves high thermal stability, excellent adhesion to PVC substrates, and resistance to plasticizers, with improved hot-melt coating properties and adhesive strength to low-polarity materials like polyolefins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142334000001
    Figure 2024142334000001
  • Figure 2024142334000002
    Figure 2024142334000002
  • Figure 2024142334000003
    Figure 2024142334000003
Patent Text Reader

Abstract

To provide an active energy ray-curable adhesive composition from which an adhesive that is excellent in hot melt coating property, has high thermal stability of a resin, is excellent in adhesive characteristics of adhesive force, holding force or the like of an adhesive sheet using a PET base material, and is excellent in adhesion to a PVC base material, adhesive force to an adherend of an adhesive sheet using a PVC base material, and is excellent in plasticizer resistance can be obtained.SOLUTION: A composition contains an acrylic resin (A), wherein the acrylic resin (A) contains a constitutional unit derived from alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms, a constitutional unit derived from alkoxyalkyl (meth)acrylate (a2), a constitutional unit derived from a monomer (a3) having an active energy ray active site, and a constitutional unit derived from a polar group-containing ethylenic unsaturated monomer (a4), and a weight average molecular weight of the acrylic resin (A) is 200,000 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable pressure-sensitive adhesive composition and uses thereof. In particular, the present invention relates to an active energy ray-curable pressure-sensitive adhesive composition that can be used in pressure-sensitive adhesive sheets for hot melt coating, laminates, and the like, and to a pressure-sensitive adhesive, pressure-sensitive adhesive sheet, and laminate using the same. [Background technology]

[0002] Conventionally, rubber-based adhesives and acrylic-based adhesives have been known as adhesives used in adhesive layers of adhesive tapes, adhesive sheets, etc. As acrylic-based adhesives, (co)polymers having specific alkyl (meth)acrylates as essential constituent units have been developed.

[0003] In recent years, due to the growing concern about the environment, adhesive compositions that do not use organic solvents have been attracting attention. For example, Patent Document 1, Patent Document 2, etc. propose an acrylic hot-melt type adhesive composition characterized by coating a thermally melted resin on a substrate. For example, Patent Document 1 proposes crosslinking an acrylic adhesive composition that has been hot-melt coated by irradiation with active energy rays. However, the acrylic adhesive composition described in Patent Document 1 has a high melt viscosity and therefore requires high temperatures during coating.

[0004] Therefore, Patent Document 2 proposes a pressure-sensitive adhesive composition using an acrylic resin having a structural unit derived from a macromonomer, which has excellent low-temperature application properties, excellent retention even with low UV exposure, and reduces adhesive residue when peeled off. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2018-501397 [Patent Document 2] International Publication No. 2020 / 158475 Summary of the Invention [Problem to be solved by the invention]

[0006] The pressure-sensitive adhesive composition described in Patent Document 1 has adhesive strength to adherends such as stainless steel (SUS) and polyolefin, but its adhesion to polyvinyl chloride (PVC) substrates has not been examined.

[0007] Furthermore, the composition described in Patent Document 2 contains a large amount of structural units derived from alkyl acrylate as a constituent component of the acrylic resin, and has a small amount of structural units derived from monofunctional monomers that have a glass transition temperature of 0°C or higher and do not contain a polar group. As a result, the composition has poor adhesion to PVC substrates and low plasticizer resistance, and the adhesive strength decreases over time, making it difficult to apply the composition to PVC substrates used for automobiles, etc.

[0008] The present invention aims to provide an active energy ray-curable pressure-sensitive adhesive composition which not only has excellent hot melt coatability, high resin thermal stability, and excellent adhesive properties such as adhesive strength and holding power of a pressure-sensitive adhesive sheet using a polyethylene terephthalate (PET) substrate, but also provides a pressure-sensitive adhesive having excellent adhesion to a PVC substrate, adhesive strength of a pressure-sensitive adhesive sheet using a PVC substrate to an adherend, and plasticizer resistance. Another aim of the present invention is to provide a pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition, a pressure-sensitive adhesive sheet having an adhesive layer made of the pressure-sensitive adhesive, and a laminate in which the pressure-sensitive adhesive layer is laminated with another substrate. [Means for solving the problem]

[0009] The present inventors have found that the above-mentioned problems can be solved by specifying the weight average molecular weight of the acrylic resin (A) obtained by polymerizing a copolymerization component containing at least an alkyl (meth)acrylate and an alkoxyalkyl (meth)acrylate each having an alkyl group having 4 or more carbon atoms, and have thus completed the present invention.

[0010] That is, the present invention includes the following aspects. Aspect (1) of the present invention is an active energy ray-curable pressure-sensitive adhesive composition containing an acrylic resin (A), The acrylic resin (A) is A structural unit derived from an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms; A structural unit derived from an alkoxyalkyl (meth)acrylate (a2), A structural unit derived from a monomer (a3) ​​having an active energy ray active site, and a structural unit derived from a polar group-containing ethylenically unsaturated monomer (a4), The weight average molecular weight of the acrylic resin (A) is 200,000 or less.

[0011] In an embodiment (2) of the present invention, the pressure-sensitive adhesive composition of the embodiment (1) further contains a tackifier (B).

[0012] In an aspect (3) of the present invention, in the pressure-sensitive adhesive composition of the aspect (1) or (2), the acrylic resin (A) has a glass transition temperature of -30°C or lower.

[0013] A fourth aspect of the present invention is the pressure-sensitive adhesive composition according to any one of the first to third aspects, wherein the alkoxyalkyl (meth)acrylate (a2) is methoxyethyl (meth)acrylate.

[0014] Aspect (5) of the present invention is the pressure-sensitive adhesive composition according to any one of aspects (1) to (4), in which the content of the thermal crosslinking agent is less than 0.1% by weight of the total pressure-sensitive adhesive composition.

[0015] Aspect (6) of the present invention is a pressure-sensitive adhesive composition according to any one of aspects (1) to (5), wherein the acrylic resin (A) contains a structural unit derived from an alkyl (meth)acrylate (a5) having an alkyl group having 3 or less carbon atoms.

[0016] A seventh aspect of the present invention is an active energy ray-curable pressure-sensitive adhesive obtained by crosslinking the pressure-sensitive adhesive composition according to any one of the first to sixth aspects.

[0017] An embodiment (8) of the present invention is a pressure-sensitive adhesive sheet having an adhesive layer made of the active energy ray-curable pressure-sensitive adhesive of embodiment (7).

[0018] A ninth aspect of the present invention is a pressure-sensitive adhesive sheet having a polyvinyl chloride substrate and an adhesive layer made of the active energy ray-curable pressure-sensitive adhesive of the seventh aspect.

[0019] An embodiment (10) of the present invention is a laminate in which an adhesive layer made of the active energy ray-curable adhesive of embodiment (7) is laminated with another substrate.

[0020] In the present invention, the term "adhesive sheet" conceptually includes an adhesive sheet, an adhesive film, and an adhesive tape. Effect of the Invention

[0021] The adhesive obtained by crosslinking the adhesive composition of the present invention has excellent hot melt coatability, high thermal stability of the resin, and excellent adhesive properties such as adhesion and holding power to an adherend of an adhesive sheet using a PET substrate, particularly to an adherend with low polarity such as polyolefin. In addition, the adhesive of the present invention has excellent adhesion to a PVC substrate, adhesion to an adherend of an adhesive sheet using a PVC substrate, and plasticizer resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the embodiments of the present invention will be described in detail, however, these are merely examples of preferable embodiments and the present invention is not limited to these embodiments. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate, respectively. In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more, Y or less", as well as "preferably larger than X" or "preferably smaller than Y". Furthermore, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning that "it is preferably greater than X" or "it is preferably less than Y". Furthermore, "y and / or z (y and z are optional configurations)" means at least one of y and z, and means the following three cases: y only, z only, and y and z. In the present specification, in which multiple numerical ranges are described in stages, each upper limit and each lower limit can be the upper limit or lower limit of any combination of numerical ranges. For example, when the content of a certain component is described as "5-20 mass%, 10-15 mass%, "it can be each of the numerical ranges of "5-15 mass%, " "10-20 mass%, " "5-10 mass%, " and "15-20 mass%. Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical ranges can be replaced with values ​​shown in the examples or values ​​that are uniquely derived from the examples.

[0023] Active energy ray-curable adhesive composition The active energy ray-curable pressure-sensitive adhesive composition of the present invention (hereinafter, also simply referred to as "pressure-sensitive adhesive composition") contains at least an acrylic resin (A).

[0024] <Acrylic resin (A)> The acrylic resin (A) used in the present invention is produced by copolymerizing a copolymerization component (a). The copolymerization component (a) contains at least an alkyl (meth)acrylate (a1) having an alkyl group with 4 or more carbon atoms, an alkoxyalkyl (meth)acrylate (a2), a monomer (a3) ​​having an active energy ray active site, and a polar group-containing ethylenically unsaturated monomer (a4), and, if necessary, an alkyl (meth)acrylate (a5) having an alkyl group with 3 or less carbon atoms and other polymerizable monomers (a6). The acrylic resin (A) obtained by copolymerizing the copolymerization component (a) containing these monomers contains a structural unit derived from an alkyl (meth)acrylate (a1) having an alkyl group with 4 or more carbon atoms, a structural unit derived from an alkoxyalkyl (meth)acrylate (a2), a structural unit derived from a monomer (a3) ​​having an active energy ray active site, and a structural unit derived from a polar group-containing ethylenically unsaturated monomer (a4), and optionally contains a structural unit derived from an alkyl (meth)acrylate (a5) having an alkyl group with 3 or less carbon atoms and a structural unit derived from another polymerizable monomer (a6). In the acrylic resin (A) obtained by copolymerizing the copolymerization component (a), the content of the structural unit derived from each monomer relative to the total structural units is the same as the amount (content) of each monomer charged in the copolymerization component (a).

[0025] [Alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms] Examples of the alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms (hereinafter, sometimes simply referred to as "alkyl (meth)acrylate (a1)") include n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl (meth)acrylate, (iso)octyl acrylate, (iso)decyl acrylate, (iso)nonyl acrylate, lauryl (meth)acrylate, and isostearyl acrylate. Among these, n-butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are preferred from the viewpoint of low glass transition temperature. The alkyl (meth)acrylate (a1) preferably does not contain a polar group such as a hydroxyl group, a carboxyl group, or an amino group. The alkyl (meth)acrylate (a1) may be used alone or in combination of two or more. The alkyl (meth)acrylate (a1) is excluded from the monomer (a3) ​​having an active energy ray active site and the polar group-containing ethylenically unsaturated monomer (a4) described below.

[0026] The glass transition temperature when the homopolymer is formed is usually measured by a differential scanning calorimeter (DSC) and can be measured by a method in accordance with JIS K7121-1987 or JIS K6240.

[0027] The content of the alkyl (meth)acrylate (a1) is usually 1 to 99% by weight, preferably 30 to 97% by weight, more preferably 50 to 95% by weight, based on the copolymerization component (a). If the content is too low, the balance between adhesive strength and holding power tends to decrease, whereas if the content is too high, the adhesion to the PVC substrate and the plasticizer resistance tend to decrease.

[0028] [Alkoxyalkyl (meth)acrylate (a2)] Examples of the alkoxyalkyl (meth)acrylate (a2) include methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, and methoxypolyethylene glycol (meth)acrylate. Among these, methoxyethyl (meth)acrylate is preferred, and methoxyethyl acrylate is more preferred, because it has a low glass transition temperature, high polarity, and high versatility. The alkoxyalkyl (meth)acrylate (a2) preferably does not contain a polar group such as a hydroxyl group, a carboxyl group, or an amino group. The alkoxyalkyl (meth)acrylate (a2) may be used alone or in combination of two or more. The alkoxyalkyl (meth)acrylate (a2) is excluded from the monomer (a3) ​​having an active energy ray active site and the polar group-containing ethylenically unsaturated monomer (a4) described below.

[0029] The content of the alkoxyalkyl (meth)acrylate (a2) is preferably 1 to 99% by weight, more preferably 5 to 70% by weight, and particularly preferably 10 to 50% by weight, based on the copolymerization component (a). If the content is too low, the tack and adhesion to the PVC substrate tend to decrease, while if the content is too high, the adhesive strength, among other adhesive properties, tends to decrease.

[0030] [Monomer (a3) ​​having an active energy ray active site] As the monomer (a3) ​​having an active energy ray active site, a (meth)acrylic acid ester having a site capable of forming a crosslink with another site in the acrylic resin (A) molecule or with another acrylic resin molecule by irradiation with active energy rays can be used. When irradiating with active energy rays, light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, electromagnetic waves such as X-rays and gamma rays, as well as electron beams, proton beams, neutron beams, etc. can be used, but curing by ultraviolet irradiation is advantageous in terms of curing speed, ease of obtaining irradiation equipment, cost, etc. Examples of active energy ray active sites include a benzophenone structure, a benzyl structure, an o-benzoylbenzoic acid ester structure, a thioxanthone structure, a 3-ketocoumarin structure, a 2-ethylanthraquinone structure, and a camphorquinone structure. Each of these structures can be excited by ultraviolet irradiation, and in the excited state, it can extract hydrogen radicals from the acrylic resin (A) molecule. In this way, radicals are generated on the acrylic resin (A). Various reactions are caused in the system, such as the formation of a crosslinked structure by the generated radicals bonding with each other, the generation of peroxide radicals by reaction with oxygen molecules, the formation of a crosslinked structure via the generated peroxide radicals, and the extraction of another hydrogen radical by the generated radical, and the acrylic resin (A) is finally crosslinked.

[0031] Among the above-mentioned structures, the benzophenone structure is preferred in consideration of transparency, reactivity, etc. Examples of (meth)acrylates having such a benzophenone structure include, but are not limited to, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and mixtures thereof. The monomer (a3) ​​having an active energy ray active site is excluded from the alkyl (meth)acrylate (a1), the alkoxyalkyl (meth)acrylate (a2) and the polar group-containing ethylenically unsaturated monomer (a4). The monomer (a3) ​​having an active energy ray active site can be used alone or in combination of two or more kinds.

[0032] The content of the monomer (a3) ​​having an active energy ray active site is usually 0.1 to 10% by weight, preferably 0.2 to 5% by weight, more preferably 0.3 to 3% by weight, based on the copolymerization component (a). If the content is too low, the curability upon irradiation with active energy rays tends to be low, whereas if the content is too high, the curability is good but the gel fraction increases too much, so that the adhesive strength tends to decrease.

[0033] [Polar Group-Containing Ethylenically Unsaturated Monomer (a4)] Examples of the polar group-containing ethylenically unsaturated monomer (a4) include hydroxyl group-containing monomers, carboxyl group-containing monomers, amino group-containing monomers, amide group-containing monomers, and cyano group-containing monomers. These may be used alone or in combination of two or more. Among them, carboxyl group-containing monomers are preferred because they have excellent adhesive strength as copolymerized acrylic resins.

[0034] Examples of the hydroxyl group-containing monomer include (meth)acrylic acid hydroxyalkyl ester monomers such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; and primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, N-methylol (meth)acrylamide, and hydroxyethyl acrylamide; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro 2-hydroxypropyl (meth)acrylate; and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate. Among these, (meth)acrylic acid hydroxyalkyl ester monomers are preferred, and 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are more preferred, and 4-hydroxybutyl acrylate is particularly preferred, in that they contain less impurities such as di(meth)acrylates and are easy to produce.

[0035] Examples of the carboxy group-containing monomer include (meth)acrylic acid, β-carboxyethyl (meth)acrylate, crotonic acid, maleic acid, maleic anhydride, fumaric acid, citraconic acid, glutaconic acid, itaconic acid, N-glycolic acid, and cinnamic acid.

[0036] Examples of the amino group-containing monomer include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and quaternary products thereof.

[0037] Examples of the amide group-containing monomer include (meth)acrylamide, N-(n-butoxyalkyl)(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, vinylpyrrolidone, and acryloylmorpholine.

[0038] Examples of the cyano group-containing monomer include acrylonitrile and methacrylonitrile.

[0039] The content of the polar group-containing ethylenically unsaturated monomer (a4) is usually less than 15% by weight, preferably 0.1% by weight or more and less than 13.5% by weight, more preferably 0.5 to 12% by weight, particularly preferably 1 to 11% by weight, and even more preferably 2 to 10% by weight, based on the copolymerization component (a) in terms of achieving both thermal stability and adhesive properties of the resin. If the content is too high, the thermal stability of the copolymerized acrylic resin tends to decrease. If the content is too low, the adhesive strength tends to decrease and the adhesion to the PVC substrate tends to decrease.

[0040] [Alkyl (meth)acrylate (a5) having an alkyl group having 3 or less carbon atoms] Examples of the alkyl (meth)acrylate (a5) having an alkyl group having 3 or less carbon atoms include methyl (meth)acrylate and ethyl (meth)acrylate. Methyl acrylate is preferred because of its high polarity and good adhesion to PVC substrates.

[0041] [Other polymerizable monomers (a6)] The other polymerizable monomer (a6) may be any other polymerizable monomer other than the above (a1), (a2), (a3), (a4) and (a5), and examples thereof include alicyclic structure-containing monomers, aromatic monomers, vinyl monomers, etc. These may be used alone or in combination of two or more.

[0042] Examples of the alicyclic structure-containing monomer include (meth)acrylates having an alicyclic structure, such as cyclohexyl (meth)acrylate, isobornyl acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and 2-adamantyl (meth)acrylate.

[0043] Examples of the aromatic monomer include (meth)acrylates having one aromatic ring, such as phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxydipropylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, phenoxypolypropylene glycol-(meth)acrylate, and (meth)acrylates having two aromatic rings, such as phenoxybenzyl (meth)acrylate and ethoxylated o-phenylphenol (meth)acrylate.

[0044] Examples of the vinyl monomer include monomers such as vinyl propionate, vinyl stearate, vinyl acetate, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyl toluene, vinyl pyridine, vinyl pyrrolidone, methyl vinyl ketone, and dimethyl allyl vinyl ketone.

[0045] The other polymerizable monomer (a6) can be contained within a range that does not impair the effects of the present invention. The content is preferably 20% by weight or less, more preferably 15% by weight or less, based on the copolymerization component (a), with the lower limit being 0% by weight.

[0046] [Method for producing acrylic resin (A)] The acrylic resin (A) can be produced by a conventional method such as solution radical polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc., using the copolymerization component (a). For example, a method of mixing or dropping appropriately selected polymerization components and a polymerization initiator into an organic solvent and polymerizing under predetermined polymerization conditions can be mentioned. Among them, solution radical polymerization and bulk polymerization are preferred, and solution radical polymerization is particularly preferred in that the acrylic resin (A) can be stably obtained.

[0047] Examples of the organic solvent used in the polymerization reaction include aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as hexane, esters such as ethyl acetate and butyl acetate, aliphatic alcohols such as n-propyl alcohol and isopropyl alcohol, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc. These organic solvents may be used alone or in combination of two or more.

[0048] Among these organic solvents, from the standpoint of ease of polymerization reaction, chain transfer effect, ease of drying when applying the pressure-sensitive adhesive composition, and safety, it is preferable to use a combination of esters such as ethyl acetate and butyl acetate; ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone; and aliphatic alcohols such as n-propyl alcohol and isopropyl alcohol, and in particular, from the standpoint of the chain transfer effect, it is preferable to use a combination of methyl ethyl ketone and isopropanol. The amount of the organic solvent used is usually 10 to 900 parts by weight based on 100 parts by weight of the copolymerization component (a).

[0049] Examples of polymerization initiators used in such solution radical polymerization include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis(methylpropionic acid), which are normal radical polymerization initiators; organic peroxides such as benzoyl peroxide, lauroyl peroxide, di-t-butyl peroxide, and cumene hydroperoxide; and the like, which can be appropriately selected and used according to the monomer to be used. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used is usually 0.01 to 10 parts by weight based on 100 parts by weight of the copolymerization component (a).

[0050] By the above method, an acrylic resin (A) can be obtained which contains a structural unit derived from an alkyl (meth)acrylate (a1) having an alkyl group with 4 or more carbon atoms, a structural unit derived from an alkoxyalkyl (meth)acrylate (a2), a structural unit derived from a monomer (a3) ​​having an active energy ray active site, and a structural unit derived from a polar group-containing ethylenically unsaturated monomer (a4), and which may, if necessary, contain a structural unit derived from an alkyl (meth)acrylate (a5) having an alkyl group with 3 or less carbon atoms and a structural unit derived from another polymerizable monomer (a6).

[0051] [Physical properties of acrylic resin (A)] The glass transition temperature (Tg) of the acrylic resin (A) is preferably −30° C. or lower, more preferably −30 to −70° C., particularly preferably −31 to −60° C., still more preferably −32 to −50° C., and particularly preferably −33 to −47° C. If the glass transition temperature is too low, the adhesion to the PVC substrate tends to decrease, whereas if it is too high, the tack before curing tends to decrease.

[0052] The above glass transition temperature is calculated by the following Fox formula.

[0053]

number

[0054] That is, it is a value calculated by applying the glass transition temperature and weight fraction of a homopolymer prepared from each of the monomers constituting the acrylic resin (A) to the Fox formula. The glass transition temperature of a homopolymer prepared from each of the monomers constituting the acrylic resin (A) is usually measured by a differential scanning calorimeter (DSC) and can be measured by a method in accordance with JIS K7121-1987 or JIS K6240.

[0055] The weight average molecular weight (Mw) of the acrylic resin (A) is preferably 200,000 or less, more preferably 10,000 to 200,000, particularly preferably 20,000 to 190,000, even more preferably 30,000 to 180,000, especially preferably 40,000 to 150,000, furthermore 50,000 to 100,000, and particularly preferably 60,000 to 80,000. If the weight average molecular weight is too small, the cohesive force tends to be low and the adhesive properties tend to be reduced, whereas if it is too large, the melt viscosity tends to be too high, making it unsuitable for hot melt coating.

[0056] The dispersity of the acrylic resin (A) [weight average molecular weight (Mw) / number average molecular weight (Mn)] is preferably 10 or less, more preferably 7 or less. If the dispersity is too high, the cohesive force tends to decrease. The lower limit of the dispersity is usually 1.

[0057] The weight-average molecular weight of the acrylic resin (A) is the weight-average molecular weight calculated based on the molecular weight of standard polystyrene. The weight-average molecular weight was measured using a high-performance liquid chromatograph (manufactured by Japan Waters, "Waters 2695 (main body)" and "Waters 2414 (detector)") with a column: Shodex GPC KF-806L (exclusion limit molecular weight: 2 × 10 7 , Separation range: 100~2×10 7 The molecular weight can be measured by connecting three of these in series (theoretical plate number: 10,000 plates / unit, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm), and the number average molecular weight can be measured in the same manner. The degree of dispersion can be determined from the measured values ​​of the weight average molecular weight and the number average molecular weight.

[0058] The viscosity of the acrylic resin (A) diluted with an organic solvent is preferably 100 to 30,000 mPa·s / 25° C., and more preferably 400 to 10,000 mPa·s / 25° C. If the viscosity is too low, when a component with a high specific gravity is used, the component tends to settle, and the concentration of the component in the acrylic resin (A) tends to be non-uniform. The viscosity of the acrylic resin (A) is generally measured by a B-type viscometer.

[0059] The acrylic resin (A) is the main component of the pressure-sensitive adhesive composition of the present invention, and its content is preferably 50% by weight or more, more preferably 60 to 98% by weight, particularly preferably 70 to 95% by weight, and even more preferably 75 to 93% by weight, relative to the pressure-sensitive adhesive composition. If the content is outside this range, the effects of the present invention tend to be difficult to obtain.

[0060] <Tackifier (B)> In the present invention, a tackifier (B) may be appropriately contained. Examples of such tackifiers (B) include rosin-based resins (B1), phenol-based resins, terpene-based resins, modified terpene-based resins, hydrocarbon-based resins, epoxy-based resins, polyamide-based resins, elastomer-based resins, and ketone-based resins. From the viewpoint of compatibility with the acrylic resin (A), rosin-based resins (B1) are preferred. These may be used alone or in combination of two or more.

[0061] Examples of the rosin resin (B1) include modified rosin resins such as hydrogenated rosin, disproportionated rosin, and polymerized rosin, and rosin esters obtained by esterifying unmodified rosin with alcohols. Among these, rosin esters are preferred from the viewpoint of forming a hot melt composition because they have high thermal stability at high temperatures when mixed with the solvent-free acrylic resin (A).

[0062] The softening point of the tackifier (B) is preferably from 20 to 180° C., more preferably from 50 to 170° C., and particularly preferably from 70 to 160° C. If it is too high or too low, the adhesiveness tends to decrease. The softening point of the tackifier (B) is generally measured in accordance with the method described in JIS K-5902 or JIS K-5903.

[0063] The content of the tackifier (B) is preferably 50 parts by weight or less, more preferably 35 parts by weight or less, and even more preferably 20 parts by weight or less, based on 100 parts by weight (solid content) of the acrylic resin (A). It is particularly preferably 15 parts by weight or less. If the content is too high, the effects of the present invention tend to be difficult to obtain.

[0064] <Optional ingredients> In addition to the acrylic resin (A) and tackifier (B), the pressure-sensitive adhesive composition of the present invention may contain various additives as optional components, such as conductive agents such as carbon and metal, inorganic fillers such as metal particles and glass particles, bulking agents, antioxidants, ultraviolet absorbers, crosslinking accelerators such as ionic compounds, peroxides, silane coupling agents, and urethane catalysts, crosslinking retarders such as acetylacetone, monofunctional monomers, and polyfunctional monomers. These may be used alone or in combination of two or more.

[0065] In addition to the above-mentioned optional components, the pressure-sensitive adhesive composition of the present invention may contain impurities contained in the raw materials for producing the components of the pressure-sensitive adhesive composition, to the extent that the effects of the present invention are not impaired.

[0066] When the optional components are used, the content is preferably 5 parts by weight or less, more preferably 1 part by weight or less, and particularly preferably 0.5 parts by weight or less, based on 100 parts by weight of the acrylic resin (A). If the content is too high, the effects of the present invention tend to be impaired.

[0067] [Method for preparing pressure-sensitive adhesive composition] The pressure-sensitive adhesive composition of the present invention can be obtained by mixing the acrylic resin (A) with a tackifier (B) and / or optional components as required. The method for mixing these components is not particularly limited, and various methods can be used, such as a method in which the components are mixed together at once, or a method in which any component is mixed and then the remaining components are mixed together or sequentially.

[0068] The total content of the acrylic resin (A) and the tackifier (B) in the pressure-sensitive adhesive composition is preferably 90% by weight or more, more preferably 95% by weight or more, and particularly preferably 98% by weight or more.

[0069] The active energy ray-curable adhesive composition of the present invention is useful as an adhesive component, particularly as an adhesive component for hot melts. When used for hot melts, the above components are blended to obtain an adhesive composition solution, and the solvent is then distilled off.

[0070] The step of distilling off the solvent from the blended PSA composition solution can be carried out by a known general method. Examples of the method for distilling off the solvent include a method for distilling off the solvent by heating, a method for distilling off the solvent by reducing pressure, and the like. From the viewpoint of efficiently distilling off the solvent, the method for distilling off the solvent by heating under reduced pressure is preferred.

[0071] The temperature when the solvent is distilled off by heating is preferably 60 to 150° C., and in particular, it is preferable to hold the reaction solution after polymerization of the acrylic resin (A) at 60 to 80° C. to distill off the solvent, and then distill off the solvent at 80 to 150° C., in order to extremely reduce the amount of remaining solvent. Note that, in order to suppress gelation of the acrylic resin (A), it is preferable not to distill off the solvent at a temperature of 150° C. or higher.

[0072] The pressure when distilling off the solvent under reduced pressure is preferably 20 to 101.3 kPa, and in particular, it is preferable to maintain the pressure in the range of 50 to 101.3 kPa to distill off the solvent in the reaction solution, and then distill off the remaining solvent at 0 to 50 kPa, in order to extremely reduce the amount of remaining solvent. In this manner, the active energy ray-curable pressure-sensitive adhesive composition used in the present invention can be produced.

[0073] The pressure-sensitive adhesive composition of the present invention preferably contains substantially no solvent, more preferably the solvent content of the pressure-sensitive adhesive composition is 2 wt% or less, particularly preferably 0.00001 to 2 wt%, further preferably 0.0001 to 1 wt%, and most preferably 0.001 to 0.1 wt%. If the solvent content is too high, bubbles are generated and the physical properties after curing with active energy rays tend to decrease.

[0074] The pressure-sensitive adhesive composition of the present invention preferably contains substantially no thermal crosslinking agent, more preferably the content of the thermal crosslinking agent is less than 0.1 wt % of the total pressure-sensitive adhesive composition, particularly preferably 0.00001 to 0.05 wt %, and even more preferably 0.0001 to 0.01 wt %. By being substantially free of a thermal crosslinking agent, the usefulness as a hot melt pressure-sensitive adhesive component becomes even more remarkable. Examples of the thermal crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a metal chelate-based crosslinking agent, and an aziridine-based crosslinking agent.

[0075] The melt viscosity of the pressure-sensitive adhesive composition of the present invention is preferably 1 to 1500 Pa·s, more preferably 2 to 500 Pa·s, and particularly preferably 5 to 100 Pa·s. If the melt viscosity of the pressure-sensitive adhesive composition is too high, the coatability during hot melt coating tends to decrease. If the melt viscosity of the pressure-sensitive adhesive composition is too low, the adhesive properties after curing with active energy rays tend to decrease due to a decrease in molecular weight.

[0076] The melt viscosity of the pressure-sensitive adhesive composition is measured using a solvent-free pressure-sensitive adhesive composition with a rotational rheometer under the following conditions. Measuring equipment: MCR301 (manufactured by Anton Paar) Cone plate diameter: 25mm Measurement distance: 0.5mm Measurement shear rate: 0.002 (1 / S) Measurement temperature: 130℃ or 160℃

[0077] <Active energy ray-curable adhesive, adhesive sheet, and laminate> The adhesive composition of the present invention can be made into an active energy ray-curable adhesive by crosslinking the acrylic resin (A). In addition, by laminating an adhesive layer containing this adhesive on a substrate sheet such as a plastic film, an adhesive sheet having a substrate sheet / adhesive layer laminate structure can be obtained. Furthermore, by laminating this adhesive layer on an adherend, a laminate having an adherend / adhesive layer laminate structure can be obtained. In the following, the substrate and the adherend are collectively referred to as "members".

[0078] The pressure-sensitive adhesive sheet is preferably a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer laminated on a substrate sheet, or a substrate-less double-sided pressure-sensitive adhesive sheet having separators (release sheets) laminated on both sides of the pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer may be the pressure-sensitive adhesive composition of the present invention itself, or may be the pressure-sensitive adhesive composition of the present invention cured (crosslinked). The curing method may be a method in which the pressure-sensitive adhesive composition is cured by crosslinking using a crosslinking agent, or a combination of the method.

[0079] The pressure-sensitive adhesive sheet can be produced, for example, as follows. First, a pressure-sensitive adhesive layer is formed on one or both sides of a substrate sheet to a predetermined thickness by a method in which the pressure-sensitive adhesive composition is applied in a molten state by heating to one or both sides of the substrate sheet and then cooled, a method in which the pressure-sensitive adhesive composition is melted by heating and extruded and laminated onto the substrate sheet using a T-die or the like, a method in which a solvent is applied and then dried, etc. Next, a release sheet can be attached to the surface of the pressure-sensitive adhesive layer as necessary to produce a pressure-sensitive adhesive sheet.

[0080] In addition, after forming the adhesive layer on the base sheet, an active energy ray irradiation treatment may be carried out as necessary, and then an aging treatment may be carried out to produce an adhesive sheet having an adhesive layer in which the adhesive composition is cured (crosslinked).

[0081] A substrate-less double-sided pressure-sensitive adhesive sheet can also be produced by forming a pressure-sensitive adhesive layer on a release sheet and laminating a release sheet onto the opposite side of the pressure-sensitive adhesive layer. When the obtained pressure-sensitive adhesive sheet or double-sided pressure-sensitive adhesive sheet is used, the release sheet is peeled off from the pressure-sensitive adhesive layer.

[0082] Examples of the base sheet include polyester-based resins such as polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, and polyethylene terephthalate / isophthalate copolymers; polyolefin-based resins such as polyethylene, polypropylene, and polymethylpentene; polyethylene fluoride resins such as polyvinyl fluoride, polyvinylidene fluoride, and polyethylene fluoride; polyamides such as nylon 6 and nylon 6,6; vinyl polymers such as polyvinyl chloride, polyvinyl chloride / vinyl acetate copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, and vinylon; cellulose-based resins such as cellulose triacetate and cellophane; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; polystyrene; polycarbonate; polyarylate; and synthetic resin sheets such as polyimide; metal foils such as aluminum, copper, and iron; paper such as fine paper and glassine paper; and woven fabrics and nonwoven fabrics made of glass fiber, natural fibers, synthetic fibers, and the like. These substrate sheets can be used as a single layer or as a multi-layered body in which two or more types are laminated together. Among these, synthetic resin sheets are preferred from the viewpoint of weight reduction and the like.

[0083] Furthermore, as the release sheet, for example, various synthetic resin sheets, paper, cloth, nonwoven fabric, etc. exemplified as the base material sheet can be used which have been subjected to a release treatment. As the release sheet, it is preferable to use a silicone-based release sheet.

[0084] The method for applying the pressure-sensitive adhesive composition is not particularly limited as long as it is a common application method, and examples thereof include roll coating, die coating, gravure coating, comma coating, and screen printing.

[0085] By irradiating with active energy rays, the acrylic resin (A) in the active energy ray-curable pressure-sensitive adhesive composition forms intramolecular and / or intermolecular crosslinked structures.

[0086] The gel fraction of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is preferably 5 to 95% from the viewpoint of adhesive strength and durability, more preferably 7 to 90%, and even more preferably 10 to 85%. If the gel fraction is too low, the cohesive strength tends to decrease, leading to a decrease in holding power. On the other hand, if the gel fraction is too high, the cohesive strength tends to increase, leading to a decrease in adhesive strength.

[0087] The gel fraction can be adjusted to fall within the above range, for example, by adjusting the amount of active energy ray irradiation or the type and amount of the monomer (a3) ​​having an active energy ray-active site, or, in the case of using a crosslinking agent, by adjusting the type and amount of the crosslinking agent.

[0088] The gel fraction is a measure of the degree of crosslinking (degree of curing) and is calculated, for example, by the following method. That is, an adhesive sheet (without a separator) in which an adhesive layer is formed on a polymer sheet (e.g., a PET film, etc.) serving as a substrate is wrapped in a 200-mesh SUS wire net and immersed in toluene at 23°C for 24 hours. The weight of the adhesive layer is measured before and after immersion in toluene, and the difference between the two weights is the weight of the insoluble adhesive component remaining in the wire net. The weight percentage of the insoluble adhesive component remaining in the wire net relative to the weight of the adhesive layer before immersion in toluene is the gel fraction. However, the weight of the substrate is subtracted.

[0089] The thickness of the adhesive layer of the adhesive sheet is usually preferably 5 to 2000 μm, more preferably 10 to 100 μm, and particularly preferably 20 to 60 μm. If the thickness of the adhesive layer is too thin, the adhesiveness tends to decrease, whereas if it is too thick, the adhesive tends to overflow when used as an adhesive label.

[0090] The thickness of the adhesive layer in the present invention is a value determined by subtracting the measured thickness of the components other than the adhesive layer from the measured thickness of the entire laminate including the adhesive layer using a Mitutoyo ID-C112B.

[0091] Furthermore, in a laminate in which a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive is laminated with another substrate, i.e., a laminate having a laminate structure of adherend / pressure-sensitive adhesive layer / other member, the pressure-sensitive adhesive layer has high adhesion before curing and exhibits high adhesive strength after curing, so that the other member is unlikely to easily shift or peel off from the adherend. Therefore, by using the pressure-sensitive adhesive of the present invention, a laminate with high adhesion reliability and excellent quality in appearance can be obtained.

[0092] The active energy ray-curable pressure-sensitive adhesive composition of the present invention not only exhibits excellent adhesive properties such as adhesive strength and holding power to adherends with low polarity such as polyolefins, but also exhibits excellent hot-melt coatability and high thermal stability of the resin, and further exhibits adhesion to polyvinyl chloride substrates and plasticizer resistance. Therefore, the pressure-sensitive adhesive composition of the present invention is useful for various applications, particularly for hot melt coating, such as adhesive applications for cautions, frozen foods, building materials, automobiles, electronic parts, FPC manufacturing, semiconductor manufacturing processes, component sealing, aircraft parts, and sporting goods, and is particularly suitable for use in automobiles and marking films (pressure-sensitive adhesive sheets and pressure-sensitive adhesive tapes). EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are by weight. In the following examples, the viscosity, weight average molecular weight, dispersity, glass transition temperature (Tg) and other physical properties of the acrylic resin (A) were measured according to the methods described above. First, prior to the examples, the following components were prepared.

[0094] <Acrylic resin (A)> The following were used as raw material monomers for the acrylic resin. Alkyl (meth)acrylate having an alkyl group with 4 or more carbon atoms (a1) BA: normal butyl acrylate (Tg = -55°C, manufactured by Mitsubishi Chemical Corporation) Alkoxyalkyl (meth)acrylate (a2) MEA: Methoxyethyl acrylate (Tg = -50°C, manufactured by Osaka Organic Chemical Industry Co., Ltd.) Monomers having active energy ray-active sites (a3) MBP: 4-methacryloyloxybenzophenone (Shinryo Corporation) Polar group-containing ethylenically unsaturated monomer (a4) Aac: Acrylic acid (manufactured by Nippon Shokubai Co., Ltd.) Alkyl (meth)acrylates having an alkyl group with 3 or less carbon atoms (a5) MA: methyl acrylate (Tg = 8°C, manufactured by Mitsubishi Chemical Corporation)

[0095] [Preparation of acrylic resin (A-1) solution] A four-necked round-bottom flask equipped with a reflux condenser, a stirrer, a nitrogen gas inlet, and a thermometer was charged with 47 parts of methyl ethyl ketone (MEK), 8.3 parts of isopropyl alcohol (IPA), and 0.017 parts of azobis(2,4-dimethylvaleronitrile) (ADVN) as a polymerization initiator. The mixture was heated to reflux in the flask, and then a mixed solution of 57 parts of BA, 17.5 parts of MEA, 0.50 parts of MBP, 7.5 parts of Aac, 17.5 parts of MA, 3.3 parts of methyl ethyl ketone (MEK), and 0.12 parts of ADVN was added dropwise over 2 hours. One hour after the completion of the monomer dropwise addition, 0.067 parts of polymerization initiator (ADVN) and 3.3 parts of MEK were added and reacted for 1 hour, after which 0.067 parts of polymerization initiator (ADVN) and 3.3 parts of MEK were further added and reacted for 1 hour, after which 0.067 parts of polymerization initiator (ADVN) and 3.3 parts of MEK were further added and reacted for 2 hours to obtain an acrylic resin (A-1) solution [solid concentration 59.3%, viscosity 570 mPa s, weight average molecular weight (Mw) 60,700, dispersity 2.26 (Mw / Mn), calculated Tg = -36.8°C].

[0096] [Preparation of acrylic resin (A-2, A'-1 to A'-2) solutions] In the production of the acrylic resin (A-1) solution, the ratio of each copolymerization component (a) was changed as shown in Table 1, and polymerization was carried out to obtain acrylic resins (A-2, A'-1 to A'-2). The copolymerization ratio (content) of the structural unit derived from each monomer in the obtained acrylic resin (A) was the same as the amount of the monomer charged.

[0097] [Table 1]

[0098] <Tackifier (B)> As the tackifier (B), the following was prepared. (B-1) Rosin ester (Arakawa Chemical Industries, Ltd., Super Ester A-75, softening point: 70 to 80°C) (B-2) Rosin ester (Arakawa Chemical Industries, Ltd., Super Ester A-100, softening point: 95 to 105°C)

[0099] <Examples 1 to 4, Comparative Examples 1 to 2> The acrylic resin solution (A) and the tackifier resin (B) were blended according to Table 2. The blending amounts are all amounts of solids. The blended solution was placed in a flask equipped with a U-shaped connecting tube so that the solvent could be distilled out of the system, and the mixture was left at a jacket temperature of 80°C for 1 hour, and then reduced to 10 kPa and left at a jacket temperature of 90°C for 2 hours to distill off the solvent, thereby obtaining active energy ray-curable pressure-sensitive adhesive compositions as described in Examples 1 to 4 and Comparative Examples 1 and 2.

[0100] [Table 2]

[0101] <Hot melt coatability> The melt viscosity was measured using the rotational rheometer and evaluated according to the following criteria. The results are shown in Table 3.

[0102] (Evaluation Criteria) ◎··40Pa·s or less ○ More than 40 Pa s and less than 80 Pa s △: Greater than 80 Pa s and less than 400 Pa s × 400 Pa s or greater

[0103] <Thermal stability> The melt viscosity was measured using the rotational rheometer at 130° C. for 8 hours under nitrogen flow conditions, and the melt viscosity after heating at 130° C. for 8 hours was evaluated according to the following evaluation criteria. The results are shown in Table 3.

[0104] (Evaluation Criteria) ◎··40Pa·s or less ○ More than 40 Pa s and less than 80 Pa s △: Greater than 80 Pa s and less than 400 Pa s × 400 Pa s or greater

[0105] [Table 3]

[0106] [Preparation of adhesive sheet (PET substrate)] Each of the active energy ray-curable adhesive compositions of Examples 1 to 4 and Comparative Examples 1 to 2 was mixed with ethyl acetate and diluted to a solid content concentration of 50%, and then coated on a 38 μm-thick light release silicone separator (Mitsui Chemicals Tohcello, Inc., "SPPET01 38BU") using an applicator so that the thickness after drying would be 25 μm, forming an adhesive layer. A UV irradiation device using a high-pressure mercury lamp was used to apply the composition at a prescribed dose (140 mW / cm 2 , 900mJ / cm 2 ) was irradiated with ultraviolet light, and then the surface of the adhesive layer was laminated to a 50 μm thick PET film (Toray Industries, Inc., "Lumirror #50-T60") to produce an adhesive sheet (a laminate of PET film / adhesive layer / light release silicone separator).

[0107] <Initial adhesive strength> A test piece measuring 25 mm wide x 200 mm wide was prepared from the PET-based adhesive sheet obtained above, and after removing the separator, the piece was pressed and attached to the adherend (SUS304-BA plate, polyethylene (PE) plate) by rolling a 2 kg rubber roller back and forth twice in an atmosphere of 23°C and 50 RH%, and left to stand at 23°C for 30 minutes. After that, the 180° peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min in accordance with JIS Z 0237, and evaluated as follows. The results are summarized in Table 4.

[0108] (Evaluation criteria, versus SUS-BA plate) ◎ 15.0N / 25mm or more and peeling occurs at the interface with the adherend ○ 15.0N / 25mm or more and cohesive peeling or substrate interface peeling △ 8.0N / 25mm or more, less than 15.0N / 25mm × Less than 8.0N / 25mm

[0109] (Evaluation criteria, against PE board) 〇 6.0N / 25mm or more △ 4.0N / 25mm or more, less than 6.0N / 25mm × Less than 4.0N / 25mm

[0110] <Gel fraction> The adhesive was picked from the PET-based adhesive sheet obtained above, wrapped in a 200-mesh SUS wire net, and immersed in toluene adjusted to 23°C for 24 hours. The weight of the adhesive layer was measured before and after immersion in toluene, and the difference between the two weights was taken as the weight of the insoluble adhesive component remaining in the wire net. The weight percentage of the insoluble adhesive component remaining in the wire net relative to the weight of the adhesive layer before immersion in toluene was taken as the gel fraction (%). The results are summarized in Table 4.

[0111] <Holding force> A test piece measuring 25mm wide x 25mm wide was prepared from the PET-based adhesive sheet obtained above, and after removing the separator, it was pressed and attached (attached area 25mm x 25mm) to a stainless steel plate (SUS304) polished with sandpaper by reciprocating a 2kg roller. The holding power was measured for 24 hours under a 40°C atmosphere with a load of 1kg using a creep tester (Tester Sangyo Co., Ltd., Holding Power Tester BE-501, with High Temperature and Humidity Chamber). The evaluation criteria for holding power are as follows. The results are summarized in Table 4. In the table, "NC" indicates that there was no change after 24 hours.

[0112] (Evaluation Criteria) ◎ Maintained for 1440 minutes or more without deviation 〇··Retained for 1440 minutes or more, but there was a discrepancy △: 30 minutes or more, less than 1440 minutes × Held for less than 30 minutes

[0113] [Table 4]

[0114] [Preparation of adhesive sheet (PVC substrate)] Each of the active energy ray-curable adhesive compositions of Examples 1 to 4 and Comparative Examples 1 to 2 was mixed with ethyl acetate and diluted to a solid content concentration of 50%, and then coated on a 38 μm-thick light release silicone separator (Mitsui Chemicals Tohcello, Inc., "SPPET01 38BU") using an applicator so that the thickness after drying would be 25 μm, forming an adhesive layer. A UV irradiation device using a high-pressure mercury lamp was used to apply the composition at a prescribed dose (140 mW / cm 2 , 60mJ / cm 2 ,300mJ / cm 2 or 900mJ / cm 2 After irradiating the adhesive layer with ultraviolet light (see Table 2), the surface of the adhesive layer was laminated to a soft PVC film having a thickness of 80 μm to produce an adhesive sheet (a laminate of PVC film / adhesive layer / light release silicone separator).

[0115] <Adhesion to substrate> The PVC-based adhesive sheet obtained above was left to cure for one day, the separator was removed, and the adhesive adhered to the PVC film was rubbed with a silicon plug 10 times to check the condition and evaluate it as follows. The results are summarized in Table 5.

[0116] (Evaluation Criteria) 〇 No peeling △ Peeling occurs, but the amount of peeling is small × Peeling occurs and the amount of peeling is large

[0117] <Initial adhesive strength> An adherend was prepared by backing a PVC film with a stainless steel plate. A test piece measuring 25 mm wide x 200 mm wide was prepared from the PVC-based pressure-sensitive adhesive sheet obtained above, and after removing the separator, the PVC film side of the adherend was pressed and attached by rolling a 2 kg rubber roller back and forth twice under an atmosphere of 23°C and 50 RH%, and left to stand at 23°C for 30 minutes. Thereafter, the 180° peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min in accordance with JIS Z 0237, and evaluated as follows. The results are summarized in Table 5.

[0118] (Evaluation criteria, against PVC film) ◎ 15.0N / 25mm or more and peeling occurs at the interface with the adherend ○ 15.0N / 25mm or more and cohesive peeling or substrate interface peeling △ 8.0N / 25mm or more, less than 15.0N / 25mm × Less than 8.0N / 25mm

[0119] <Adhesive strength over time> A test piece with a width of 25 mm x 200 mm was prepared from the PVC-based adhesive sheet obtained above, and placed in a dryer adjusted to 60 ° C. and left to stand for 7 days. After heating at 60 ° C. for 7 days, the adhesive sheet was air-cooled to 23 ° C. Then, the separator was peeled off, and the PVC film-backed adherend was pressed and attached by rolling a 2 kg rubber roller back and forth twice under an atmosphere of 23 ° C. and 50 RH%, and left to stand for 30 minutes at 23 ° C. Then, the 180 ° peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min according to JIS Z 0237, and evaluated as follows. The results are summarized in Table 5.

[0120] (Evaluation criteria, against PVC film) ◎ 15.0N / 25mm or more and peeling occurs at the interface with the adherend ○ 15.0N / 25mm or more and cohesive peeling or substrate interface peeling △ 8.0N / 25mm or more, less than 15.0N / 25mm × Less than 8.0N / 25mm

[0121] <Plasticizer resistance> The adhesive strength retention rate was calculated using the following formula to calculate the plasticizer resistance, and the results were evaluated according to the following criteria. The results are shown in Table 5. [Formula 1] Adhesive strength retention rate (%) = (adhesive strength over time / initial adhesive strength) x 100

[0122] (Evaluation Criteria) ○ 75% or more △: 60% or more but lower than 75% × Less than 60%

[0123] [Table 5]

[0124] The acrylic resin (A) contained in the adhesive composition of Examples 1 to 4 contains a structural unit derived from an alkyl (meth)acrylate (a1) having an alkyl group with 4 or more carbon atoms, a structural unit derived from an alkoxyalkyl (meth)acrylate (a2), a structural unit derived from a monomer (a3) ​​having an active energy ray active site, and a structural unit derived from a polar group-containing ethylenically unsaturated monomer (a4), so that the resin as a whole has a low glass transition temperature, but also contains a structural unit derived from a highly polar monomer, so that it is considered to have excellent adhesion to low polarity adherends such as polyolefins, and also excellent adhesion to PVC substrates and resistance to plasticizer migration from PVC substrates. Furthermore, since the weight average molecular weight of the acrylic resin (A) is 200,000 or less, it is considered to have excellent hot melt coatability and thermal stability of the resin.

[0125] On the other hand, the acrylic resin contained in the pressure-sensitive adhesive composition of Comparative Example 1 had a weight-average molecular weight of more than 200,000, and therefore was inferior in hot melt coatability and thermal stability compared to the Examples. In addition, the adhesion to substrates, adhesive strength over time, plasticizer resistance, and adhesive strength to low-polarity adherends were also inferior. The acrylic resin contained in the pressure-sensitive adhesive composition of Comparative Example 2 did not contain a structural unit derived from alkoxyalkyl (meth)acrylate (a2), and therefore the adhesive strength to a PE plate, which is a low-polarity adherend, was inferior to that of the Examples.

Claims

1. An active energy ray-curable pressure-sensitive adhesive composition containing an acrylic resin (A), The acrylic resin (A) is A structural unit derived from an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms; A structural unit derived from an alkoxyalkyl (meth)acrylate (a2), A structural unit derived from a monomer (a3) ​​having an active energy ray active site, and a structural unit derived from a polar group-containing ethylenically unsaturated monomer (a4), The active energy ray-curable pressure-sensitive adhesive composition, wherein the acrylic resin (A) has a weight average molecular weight of 200,000 or less.

2. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1 , further comprising a tackifier (B).

3. 3. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, wherein the acrylic resin (A) has a glass transition temperature of −30° C. or lower.

4. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1 or 2, wherein the alkoxyalkyl (meth)acrylate (a2) is methoxyethyl (meth)acrylate.

5. 3. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, wherein the content of the thermal crosslinking agent is less than 0.1% by weight of the total pressure-sensitive adhesive composition.

6. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1 or 2, wherein the acrylic resin (A) contains a structural unit derived from an alkyl (meth)acrylate (a5) having an alkyl group having 3 or less carbon atoms.

7. 3. An active energy ray-curable pressure-sensitive adhesive obtained by crosslinking the active energy ray-curable pressure-sensitive adhesive composition according to claim 1 or 2.

8. A pressure-sensitive adhesive sheet having an adhesive layer comprising the active energy ray-curable pressure-sensitive adhesive according to claim 7.

9. 8. An adhesive sheet comprising a polyvinyl chloride substrate and an adhesive layer comprising the active energy ray-curable adhesive according to claim 7.

10. A laminate comprising an adhesive layer comprising the active energy ray-curable adhesive according to claim 7 and another substrate.

Citation Information

Patent Citations

  • Mixture consisting of polyacrylate and polyvinyl ether, use thereof as an adhesive, method for producing pressure-sensitive article, and article of this kind

    JP2002317090A

  • Adhesive sheet

    JP2003292910A

  • Optical pressure-sensitive adhesive sheet

    JP2013522393A

  • Radiation curable hot-melt adhesive

    JP2015214601A

  • (METH)acrylic polymer and adhesive

    JP2023009641A

Cited By

  • LIGHT SOURCE DEVICE

    DE102025131655A1

  • Hot-melt adhesive, adhesive sheet, and article

    JP2026059423A