Polybutylene terephthalate resin composition, and molded article composed of the same

A PBT resin composition with controlled carboxyl group concentrations and specific additives addresses hydrolysis-induced degradation, ensuring stability and moldability, and facilitates recycling.

JP2024142470APending Publication Date: 2024-10-11TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023054615
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Polybutylene terephthalate resin (PBT) suffers from hydrolysis-induced degradation, leading to viscosity changes during melt retention, moldability issues, and insufficient hydrolysis resistance, particularly in high-temperature automotive and electronic applications, and recycled PBT lacks adequate hydrolysis resistance due to increased carboxyl group concentration from thermal history.

Method used

A PBT resin composition comprising specific ratios of PBT resin, dicyclopentadiene-type epoxy resin, and an ester compound of aliphatic alcohol and fatty acid, with controlled carboxyl group concentrations, inhibits crosslinking and maintains viscosity stability while enhancing hydrolysis resistance.

Benefits of technology

The composition achieves improved hydrolysis resistance and retention stability, reducing defects in molded products and enabling recycling of recycled PBT resin, with reduced energy consumption and carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142470000001
    Figure 2024142470000001
  • Figure 2024142470000002
    Figure 2024142470000002
Patent Text Reader

Abstract

To provide a polybutylene terephthalate resin composition which is excellent in hydrolysis resistance and retention stability, and a molded article composed of the same.SOLUTION: A polybutylene terephthalate resin composition is obtained by blending 0.5 to 4.0 pts.wt. of (B) a dicyclopentadiene type epoxy resin, and 0.05 to 1.5 pts.wt. of (C) an ester compound composed of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms, with respect to 100 pts.wt. of (A) a polybutylene terephthalate resin composed of 15 to 85 pts.wt. of (A-1) a polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less, and 15 to 85 pts.wt. of (A-2) a polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polybutylene terephthalate resin having excellent hydrolysis resistance and retention stability when heated and melted, and useful for applications such as electrical and electronic equipment parts, automobile parts, and machine parts, and to a molded article made of the same. [Background technology]

[0002] Polybutylene terephthalate resin (hereinafter sometimes abbreviated as PBT resin) has excellent heat resistance, chemical resistance, electrical properties, dimensional stability, etc., and is therefore widely used as a material for manufacturing various electrical and electronic equipment components, vehicle components for automobiles, trains, etc., and other general industrial products.

[0003] However, because PBT resin is susceptible to degradation due to hydrolysis, in order to be used as a component for various electrical and electronic devices, a component for vehicles such as automobiles and trains, and a material for manufacturing other general industrial products, it is required that the resin have a balance of general chemical and physical properties as well as long-term hydrolysis resistance.

[0004] In recent years, particularly with regard to the PBT resins used in automotive applications, there has been a strong demand for improved hydrolysis resistance in order to meet rising ambient temperatures associated with space-saving engine compartments, and to ensure the reliability of information and communication device parts used in advanced driver assistance systems for next-generation vehicles (EVs and HEVs).

[0005] There is also an increasing demand for smaller and lighter industrial molded products. Particularly in applications for thin-walled molded products such as in-vehicle connectors, if there is a large change in viscosity during molten retention, molding defects such as flash and short shots can occur during molding, so there is a demand for materials that have little viscosity change during molten retention and excellent retention stability.

[0006] Furthermore, in recent years, there has been an increasing demand for the recycling of polyester resins in preparation for a decarbonized society. There is also a demand to reduce waste by regenerating recycled polyester resins recovered from non-standard products in the production process or from products that were discarded after being used as specified products into polyester resin products again.

[0007] To date, methods for imparting hydrolysis resistance to polybutylene phthalate resin include blending an epoxy resin and a carbodiimide compound with polybutylene terephthalate resin, and blending a hindered amine compound with polybutylene terephthalate resin. As such resin compositions, PBT resin compositions (Patent Document 1) obtained by blending a specific hindered amine compound with PBT resin, polyester resin compositions (Patent Document 2) obtained by blending a carbodiimide compound, a nucleating agent, and an inorganic filler having a plate-shaped cross section with PBT resin, and PBT resin compositions (Patent Document 3) obtained by blending a polycarbonate resin, an inorganic filler, a pentaerythritol-based release agent, and a specific epoxy resin with PBT resin have been proposed.

[0008] As a method for obtaining recycled polyester resin products, a thermoplastic resin composition obtained by blending a PBT resin with a polyethylene terephthalate resin and a crosslinked resin derived from a polyester film (Patent Document 4) has been proposed. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2019-147934 A [Patent Document 2] JP 2019-26842 A [Patent Document 3] Patent Publication No. 2021-25032 [Patent Document 4] International Publication No. 2013 / 108758 Summary of the Invention [Problem to be solved by the invention]

[0010] However, in Patent Document 1, the low molecular weight hindered amine compound was contained, which resulted in a large amount of gas generation during molding and insufficient moldability. In Patent Document 2, there was a problem that it was difficult to achieve high hydrolysis resistance by blending a carbodiimide compound. In Patent Document 3, there was a problem that when the amount of end-capping agent was increased to achieve higher hydrolysis resistance, viscosity increased during molten retention during molding, resulting in a significant decrease in moldability.

[0011] Furthermore, in Patent Document 4, there was a problem that the carboxyl group concentration increases due to decomposition of the polyester resin caused by heat history during processing of the recycled polyester resin, and the hydrolysis resistance performance significantly decreases.

[0012] In order to improve the hydrolysis resistance of PBT resin and maintain its durability for long-term use, in addition to the method of blending epoxy resins and hindered amine compounds, polyester resins with low carboxyl group concentrations are generally used. However, recycled polyester resins do not have good hydrolysis resistance because the carboxyl group concentration of the polyester resin obtained becomes high due to the heat history in the recycling process.

[0013] The present invention aims to provide a polybutylene terephthalate resin having excellent hydrolysis resistance and retention stability when heated and melted, which is useful for applications such as electrical and electronic equipment parts, automobile parts, and machine parts, and a molded article made from the same; and further to provide a polybutylene terephthalate resin composition that regenerates recycled polybutylene terephthalate resin and improves its quality, and a molded article made from the same. [Means for solving the problem]

[0014] As a result of repeated investigations to solve the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by blending specific amounts of (A) polybutylene terephthalate resin consisting of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t to 25 eq / t and (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t to 45 eq / t, (B) dicyclopentadiene type epoxy resin, and (C) ester compound consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms, thereby completing the present invention. That is, the present invention has the following configuration. 1. A polybutylene terephthalate resin composition comprising (A) 100 parts by weight of polybutylene terephthalate resin consisting of (A-1) 15 to 85 parts by weight of polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less and (A-2) 15 to 85 parts by weight of polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less, blended with (B) 0.5 to 4.0 parts by weight of a dicyclopentadiene type epoxy resin, and (C) 0.05 to 1.5 parts by weight of an ester compound consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms. 2. The polybutylene terephthalate resin composition according to item 1, wherein the (A) polybutylene terephthalate resin comprises 25 to 75 parts by weight of (A-1) a polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less, and 25 to 75 parts by weight of (A-2) a polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less. 3. The polybutylene terephthalate resin composition according to item 1 or 2, characterized in that the (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and not more than 45 eq / t is a recycled polybutylene terephthalate resin. 4. The polybutylene terephthalate resin composition according to any one of items 1 to 3, comprising 100 parts by weight of the polybutylene terephthalate resin (A) and 0.1 to 1.0 part by weight of the ester compound (C) consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms. 5. The polybutylene terephthalate resin composition according to any one of items 1 to 4, wherein the (C) ester compound composed of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms is pentaerythritol tetrastearate. 6. A molded article made of the polybutylene terephthalate resin composition according to any one of items 1 to 5. Effect of the Invention

[0015] According to the polybutylene terephthalate resin composition of the present invention, a molded article having excellent hydrolysis resistance and retention stability during heat melting can be obtained. Furthermore, by using recycled polybutylene terephthalate resin, the amount of energy consumed for production raw materials can be reduced, and carbon dioxide emissions can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, the polybutylene terephthalate resin composition of the present invention will be described in detail.

[0017] The polybutylene terephthalate resin composition of the present invention is obtained by blending 100 parts by weight of (A) polybutylene terephthalate resin, which is composed of (A-1) 15-85 parts by weight of polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less and (A-2) 15-85 parts by weight of polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less, (B) 0.5-4.0 parts by weight of dicyclopentadiene type epoxy resin, and (C) 0.05-1.5 parts by weight of an ester compound composed of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms. (A) Polybutylene terephthalate resin is excellent in injection molding and mechanical properties, but the ester bond is easily decomposed by hydrolysis, resulting in an increase in the carboxyl group concentration. As the carboxyl group concentration increases, the molecular weight of the polybutylene terephthalate resin (A) is reduced, mechanical properties are reduced, and during molding, the viscosity is reduced, causing defects due to burrs in the molded product. In the present invention, by blending the polybutylene terephthalate resin (A) with the dicyclopentadiene type epoxy resin (B), the carboxyl end groups of the polybutylene terephthalate resin (A) generated by hydrolysis react with the epoxy groups of the dicyclopentadiene type epoxy resin (B), suppressing the increase in the carboxyl groups. In addition, during melt kneading to obtain the polybutylene terephthalate resin composition of the present invention, the reaction between the carboxyl end groups of the polybutylene terephthalate resin (A) and the epoxy groups of the dicyclopentadiene type epoxy resin (B) progresses, and the initial carboxyl group concentration of the obtained polybutylene terephthalate resin composition decreases. As a result, the obtained polybutylene terephthalate resin composition can maintain the high mechanical properties of the polybutylene terephthalate resin (A). However, when the carboxyl terminal group of (A) the polybutylene terephthalate resin reacts with the epoxy group of (B) the dicyclopentadiene-type epoxy resin, a crosslinking reaction between the molecular chains is simultaneously induced.The crosslinking here refers to a network structure in which compounds are entangled, which is generated by the reaction between the carboxyl end group of (A) polybutylene terephthalate resin and the epoxy group of (B) dicyclopentadiene type epoxy resin and the epoxy group of dicyclopentadiene type epoxy resin. When such a crosslinking structure is formed, the viscosity of the polybutylene terephthalate resin composition increases, which is undesirable because short shots occur during injection molding and continuous molding becomes impossible. Therefore, by blending (B) dicyclopentadiene-type epoxy resin and (C) an ester compound consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms with (A) polybutylene terephthalate resin consisting of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less and (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less, it is possible to suppress the reaction between epoxy groups that leads to an increase in viscosity during melt retention and make it difficult to form a crosslinked structure, while selectively promoting the reaction between the carboxyl groups of (A) polybutylene terephthalate resin and the epoxy groups of (B) dicyclopentadiene-type epoxy resin, thereby improving hydrolysis resistance and maintaining viscosity stability during melt retention.

[0018] Here, the polybutylene terephthalate resin composition of the present invention contains a reaction product of (A) polybutylene terephthalate resin and (B) dicyclopentadiene type epoxy resin, but the reaction product is produced by a complicated reaction, and there are circumstances in which it is not practical to specify its structure. Therefore, the present invention is specified by the components to be blended.

[0019] (A) Polybutylene terephthalate resin The polybutylene terephthalate resin (A) constituting the present invention is a polymer obtained by a normal polymerization method such as polycondensation reaction of terephthalic acid or its ester-forming derivative and 1,4-butanediol or its ester-forming derivative as the main components, and may contain other copolymerization components within a range that does not impair the properties, for example, about 20 parts by weight or less. Note that the main component here means that, for the dicarboxylic acid component and the diol component, terephthalic acid or its ester-forming derivative, or 1,4-butanediol or its ester-forming derivative, independently accounts for more than 50 parts by weight of each of the components. Preferred examples of these polymers and copolymers include polybutylene terephthalate, polybutylene (terephthalate / isophthalate), polybutylene (terephthalate / adipate), polybutylene (terephthalate / sebacate), polybutylene (terephthalate / decanedicarboxylate), polybutylene (terephthalate / naphthalate), poly(butylene / ethylene) terephthalate, and the like, which may be used alone or in combination of two or more kinds.

[0020] The polybutylene terephthalate resin (A) used in the present invention is not particularly limited as long as it can be melt-kneaded, but from the viewpoint of fluidity, it is preferable that the melt flow rate (MFR) measured at 250°C and 1000 gf is 1 to 100 g / 10 min, and from the viewpoint of mechanical properties, it is more preferable that the MFR is 1 to 75 g / 10 min.

[0021] The method for producing the polybutylene terephthalate resin (A) used in the present invention is not particularly limited, and known polycondensation methods and ring-opening polymerization methods can be used. Either a batch polymerization method or a continuous polymerization method can be used, and either a method involving transesterification and polycondensation reactions, or a method involving polycondensation by direct polymerization (direct polymerization method) can be applied. The direct polymerization method is preferred because it is easy to control the amount of carboxyl terminal groups and is economical. In order to effectively promote the esterification reaction or the transesterification reaction and the polycondensation reaction, it is preferable to add a catalyst during these reactions. Specific examples of the catalyst include organotitanium compounds such as methyl ester, tetra-n-propyl ester, tetra-n-butyl ester, tetraisopropyl ester, tetraisobutyl ester, tetra-tert-butyl ester, cyclohexyl ester, phenyl ester, benzyl ester, tolyl ester, or mixed esters of titanic acid, dibutyltin oxide, methylphenyltin oxide, tetraethyltin, hexaethylditin oxide, cyclohexahexylditin oxide, didodecyltin oxide, and triethyltin hydride. Examples of the catalyst include tin compounds such as tin oxide, triphenyltin hydroxide, triisobutyltin acetate, dibutyltin diacetate, diphenyltin dilaurate, monobutyltin trichloride, dibutyltin dichloride, tributyltin chloride, dibutyltin sulfide, butylhydroxytin oxide, alkylstannoic acids such as methylstannoic acid, ethylstannoic acid, and butylstannoic acid, zirconia compounds such as zirconium tetra-n-butoxide, and antimony compounds such as antimony trioxide and antimony acetate. Two or more of these catalysts can be used in combination. From the viewpoint of the carboxyl group concentration of (A) polybutylene terephthalate resin, among these polymerization catalysts, organic titanium compounds and tin compounds are preferred, and tetra-n-butyl ester of titanic acid is more preferred. The amount of the polymerization catalyst added is preferably in the range of 0.01 to 0.2 parts by weight relative to 100 parts by weight of polybutylene terephthalate resin.

[0022] In terms of hydrolysis resistance and viscosity stability during melt retention, the polybutylene terephthalate resin (A) used in the present invention contains 15 to 85 parts by weight of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less, and 15 to 85 parts by weight of (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less, out of 100 parts by weight of the polybutylene terephthalate resin (A). As mentioned above, polybutylene terephthalate resin tends to deteriorate due to hydrolysis, and although the incorporation of a dicyclopentadiene type epoxy resin is expected to improve hydrolysis resistance, viscosity increase due to the formation of a crosslinked structure during melting and viscosity decrease due to thermal decomposition occur, making it difficult to stabilize the viscosity during melt retention. Therefore, 15 to 85 parts by weight of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t to 25 eq / t and 15 to 85 parts by weight of (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t to 45 eq / t are blended out of 100 parts by weight of (A) polybutylene terephthalate resin. If the blending amount of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t to 25 eq / t is less than 15 parts by weight, the viscosity reduction and physical property reduction due to the decomposition of the polybutylene terephthalate resin become significant. If the blending amount of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t to 25 eq / t exceeds 85 parts by weight, the viscosity increase becomes significant due to the formation of a crosslinked structure with the epoxy resin. It is more preferable to blend 25 to 75 parts by weight of (A-1) polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less, and 25 to 75 parts by weight of (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less, out of 100 parts by weight of (A) polybutylene terephthalate resin.

[0023] (A-2) Polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and not more than 45 eq / t may be a virgin resin, but from the viewpoint of economic efficiency and environmental performance, it is more preferable that it is a recycled polybutylene terephthalate resin. Note that, a virgin resin refers to a resin obtained by polymerization reaction from a resin raw material and that has never been recycled.

[0024] The recycled polybutylene terephthalate resin in the present invention refers to a resin derived from a pre-consumer recycled product obtained from a non-standard product in the manufacturing process, or a post-consumer recycled product obtained by recovering a resin product using a polybutylene terephthalate resin distributed in the city. The recycled polybutylene terephthalate resin can be suitably used when obtaining the polybutylene terephthalate resin composition of the present invention, since it can obtain a high-quality polybutylene terephthalate resin composition while reducing the amount of waste and carbon dioxide emissions.

[0025] Recycled polybutylene terephthalate resins are derived from, for example, nonstandard pellets generated during the manufacture of polybutylene terephthalate resins, nonstandard products generated during the manufacture of resin products such as bottles, films, fibers, and injection molded products, pre-consumer products such as sprues, runners, and pellet waste generated during molding, and post-consumer products obtained by recovering products containing polybutylene terephthalate resin from the market. Examples of recycled polybutylene terephthalate resins include chemical recycled products obtained by depolymerizing resin products containing polybutylene terephthalate resin recovered from the market, decomposing the polybutylene terephthalate resin, and repolymerizing the depolymerized resin, as well as flake-shaped recycled products obtained by crushing the recovered polybutylene terephthalate resin, and material recycled products such as pellet-shaped recycled products obtained by cutting the molten resin discharged from a die after heating and melting during the manufacture of a resin composition containing polybutylene terephthalate resin.

[0026] (B) Dicyclopentadiene type epoxy resin The dicyclopentadiene-type epoxy resin (B) used in the present invention has a structure represented by the following general formula (1) and contains an epoxy group in the molecule.

[0027] [ka]

[0028] In the above general formula (1), n ​​indicates the number of repeating units of the dicyclopentadiene epoxy resin (B). n represents a range of 0 to 10. The dicyclopentadiene epoxy resin (B) used in the present invention is in the form of brown pellets, and if the number of repeating units n is small, the pellets melt together and cause blocking, which is undesirable as it cannot be fed. If the number of repeating units n is large, the reaction between the dicyclopentadiene epoxy resins (B) tends to proceed easily, and a crosslinked structure is easily formed, which tends to deteriorate the retention stability of the polybutylene terephthalate resin composition. From the viewpoint of blocking property and retention stability, the number of repeating units n of the dicyclopentadiene epoxy resin is preferably 1 to 4, more preferably 1 to 3.

[0029] Particularly preferred dicyclopentadiene type epoxy resins (B) are available under the names HP-7200H from DIC Corporation and XD-1000L from Nippon Kayaku Co., Ltd.

[0030] The dicyclopentadiene type epoxy resin (B) must be blended in an amount of 0.5 to 4.0 parts by weight per 100 parts by weight of the polybutylene terephthalate resin (A). If it is less than 0.5 parts by weight, hydrolysis resistance is not sufficiently exhibited. If it exceeds 4.0 parts by weight, the viscosity increases during melt retention. From the viewpoint of moldability, it is more preferably 1.0 to 3.5 parts by weight, and even more preferably 1.0 to 3.0 parts by weight.

[0031] (C) Ester compounds consisting of fatty alcohols and fatty acids having 5 to 24 carbon atoms In the present invention, (C) an ester compound composed of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms (hereinafter sometimes abbreviated as (C) fatty acid ester compound) is used.

[0032] The aliphatic alcohol is preferably an aliphatic alcohol having 2 to 20 carbon atoms and 1 to 10 hydroxyl groups, such as lauryl alcohol, stearyl alcohol, behenyl alcohol, ethylene glycol, propylene glycol, butylene glycol, glycerol, diglycerol, erythritol, pentaerythritol, sorbitol, triglycerol, dipentaerythritol, and tetraglycerol. These aliphatic alcohols can be used alone or in combination of two or more. Preferred aliphatic alcohols are pentaerythritol and dipentaerythritol. Pentaerythritol is particularly preferred.

[0033] The fatty acid is preferably a linear or branched saturated fatty acid having 5 to 24 carbon atoms, such as pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid, arachidic acid, behenic acid, and lignoceric acid, with stearic acid being particularly preferred.

[0034] In order to avoid an ester exchange reaction with the polybutylene terephthalate resin (A), the fatty acid ester compound (C) is preferably a full ester substantially free of free hydroxyl and carboxyl groups. Specifically, behenyl behenate, glycerin tristearate, pentaerythritol tetrastearate, pentaerythritol tetrabehenate, and dipentaerythritol hexastearate are preferred, with pentaerythritol tetrastearate being more preferred.

[0035] From the viewpoint of suppressing hydrolysis of the (A) polybutylene terephthalate resin, the acid value of the fatty acid ester compound is preferably from 0.1 to 15 mgKOH / g, and more preferably from 0.1 to 10 mgKOH / g.

[0036] The (C) fatty acid ester compound may be used alone or in combination of two or more kinds.

[0037] (C) Fatty acid ester compounds are available, for example, from Emery Oleochemicals Japan Co., Ltd. under the trade name "Roxiol", from ADEKA Corporation under the trade name "Adeka Cizer" (registered trademark), and from Riken Vitamin Co., Ltd. under the trade name "Likestar" (registered trademark).

[0038] In the present invention, the fatty acid ester compound (C) is blended in an amount of 0.05 to 1.5 parts by weight per 100 parts by weight of the polybutylene terephthalate resin (A). If the amount is less than 0.05 parts by weight, the mold releasability decreases. If the amount is more than 1.5 parts by weight, gas generation during molding and mold fouling become significant. From the viewpoint of moldability, the amount is preferably 0.1 to 1.0 parts by weight.

[0039] [Other ingredients] The polybutylene terephthalate resin composition of the present invention may contain other resin components, flame retardants, fillers, stabilizers, crystal nucleating agents, colorants, lubricants, and other conventional additives, as long as the effects of the present invention are not impaired. Two or more of these may be contained.

[0040] The other resin components may be any melt-moldable resin, and examples thereof include AS resin (acrylonitrile / styrene copolymer), hydrogenated or unhydrogenated SBS resin (styrene / butadiene / styrene triblock copolymer), hydrogenated or unhydrogenated SIS resin (styrene / isoprene / styrene triblock copolymer), polyethylene resin, polypropylene resin, polymethylpentene resin, cyclic olefin resin, cellulose resin such as cellulose acetate, polycarbonate resin, polyethylene terephthalate resin, polytrimethylene terephthalate resin, polyamide resin, polyacetal resin, polysulfone resin, polyphenylene sulfide resin, polyether ether ketone resin, polyimide resin, polyetherimide resin, and the like.

[0041] In particular, amorphous resins such as AS resin (acrylonitrile / styrene copolymer) can be easily melt-kneaded with polybutylene terephthalate resin, and by blending them, molded articles with excellent dimensional stability can be produced.

[0042] As the flame retardant, any of those used as flame retardants for polyester resin compositions can be used. For example, organic halogen-based flame retardants, specifically, high molecular weight organic halogen compounds such as halogenated polycarbonates (e.g., carbonate oligomers of tetrabromobisphenol A), halogenated acrylic resins, halogenated epoxy resins, halogenated phenoxy resins, halogenated polystyrenes, tetrabromobisphenol A·ethyl ether oligomers, and halogenated polyphenylene ethers (e.g., polydibromophenylene oxide); decabromodiphenyl ether, hexabromophenol, and tetrabromobisphenol A·bis(2,3-dibromopropionyl) are available. Examples of suitable flame retardants include low molecular weight organic halogen compounds such as brominated bisphenol A such as tetrabromobisphenol A·bis(allyl ether), tetrabromobisphenol A·2-hydroxyethyl ether, hexabromobenzene, tetrabromophthalic anhydride, tribromophenol, bis(tribromophenoxy)ethane, bis(pentabromophenoxy)ethane, ethylene bistetrabromophthalimide, brominated styrene, tetrabromobisphenol S, and bis(2,3-dibromopropyl ether) of tetrabromobisphenol S. These organic halogen flame retardants may be used alone or in combination of two or more. Phosphorus-based and inorganic flame retardants may also be used.

[0043] As the filler, any filler such as fibrous, plate-like, powdery, or granular filler can be used. As the fibrous filler, glass fiber, carbon fiber, metal fiber, and organic fiber (nylon, polyester, aramid, polyphenylene sulfide, liquid crystal polymer, acrylic, etc.) can be used, and they can be used alone or in combination of two or more. As the fibrous filler, glass fiber is preferable from the viewpoint of reducing the molding shrinkage rate and linear expansion coefficient of the molded product and easy availability. For example, glass fiber is available from Nippon Electric Glass Co., Ltd. under the trade name T-187. In addition, the diameter of the fibrous filler is preferably 4 to 25 μm, and more preferably 6 to 20 μm. In order to improve the adhesion of the interface with the polybutylene terephthalate resin, it is preferable to treat the surface of the fibrous filler with a surface treatment agent such as a binder. As the surface treatment agent, preferred are glass fibers treated with a silane coupling agent such as an aminosilane compound or an epoxysilane compound, urethane, a copolymer made of acrylic acid such as an acrylic acid / styrene copolymer, a copolymer made of maleic anhydride such as a methyl acrylate / methyl methacrylate / maleic anhydride copolymer, vinyl acetate, or a sizing agent containing one or more epoxy compounds such as a bisphenol-type epoxy or a novolac-type epoxy, and from the viewpoint of hydrolysis resistance and mechanical properties, it is preferable to use a fibrous filler that has been surface-treated with a bisphenol-type epoxy compound and / or a novolac-type epoxy compound. Specific examples of plate-like, powdery, and granular fillers include whisker-like fillers such as rock wool, potassium titanate whiskers, barium titanate whiskers, aluminum borate whiskers, and silicon nitride whiskers; and powdery, granular, or plate-like fillers such as mica, talc, kaolin, silica, calcium carbonate, glass beads, glass flakes, glass microballoons, clay, molybdenum disulfide, wollastonite, montmorillonite, titanium oxide, zinc oxide, calcium polyphosphate, graphite, and barium sulfate. These may be used alone or in combination of two or more kinds.

[0044] As the stabilizer, any of those used as stabilizers for polyester resin compositions can be used. For example, antioxidants, light stabilizers, catalyst deactivators, etc. can be mentioned. Two or more of these may be blended.

[0045] As the crystal nucleating agent, either an inorganic crystal nucleating agent or an organic crystal nucleating agent can be used, and these may be used alone or in combination of two or more kinds.

[0046] Examples of colorants include organic dyes, organic pigments, inorganic pigments, etc. Two or more of these may be mixed together.

[0047] The polybutylene terephthalate resin composition of the present invention is preferably one in which the above-mentioned (A) to (C) and, if necessary, other components are uniformly dispersed. Examples of the method for producing the polybutylene terephthalate resin composition of the present invention include a method in which each component is melt-kneaded using a known melt-kneader such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader, or a mixing roll. Each component may be mixed together in advance and then melt-kneaded. The moisture content of each component is preferably low, and it is desirable to dry the components in advance if necessary.

[0048] As a method for feeding each component into the melt kneader, for example, a single-screw or twin-screw extruder is used, and the components (A) to (C) and other components are fed through a main feeding port provided at the base of the screw, and an inorganic filler is fed through a sub-feed port provided between the main feeding port and the tip of the extruder, and then melt-mixed.

[0049] The melt-kneading temperature is preferably from 190 to 340°C, more preferably from 210 to 310°C, and even more preferably from 240 to 290°C, in that excellent fluidity and mechanical properties are obtained.

[0050] The resin composition of the present invention can be molded by any method such as commonly known injection molding, extrusion molding, blow molding, press molding, spinning, etc., and can be processed into various molded products and used. The molded products can be injection molded products, extrusion molded products, blow molded products, films, sheets, fibers, etc., the films can be various films such as unstretched, uniaxially stretched, and biaxially stretched films, and the fibers can be various fibers such as unstretched yarns, stretched yarns, and ultra-stretched yarns.

[0051] In the present invention, the above-mentioned various molded products can be used for various applications such as automobile parts, electric and electronic parts, building materials, various containers, daily necessities, household goods, and sanitary products. In particular, the polybutylene terephthalate resin composition of the present invention has excellent retention stability when heated and melted, and therefore can provide good small, thin-walled molded products, and is particularly suitable as connector parts for electric and electronic equipment parts. In addition, since the polybutylene terephthalate resin composition of the present invention has excellent hydrolysis resistance and retention stability even after being used as a molded product, the molded products used for various applications can be recycled and circulated to be used as various molded products. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Raw materials used in each example and comparative example are shown below. (A) Polybutylene terephthalate A-1: Polybutylene terephthalate (MFR: 28g / 10min (250℃, 1kgf), carboxyl group concentration: 15eq / t) A-2: Recycled polybutylene terephthalate (MFR: 32g / 10min (250℃, 1kgf), carboxyl group concentration: 35eq / t) (B) Epoxy resin B-1: Dicyclopentadiene type epoxy resin having an epoxy equivalent of 290 g / eq represented by general formula (1) (manufactured by DIC Corporation, "HP-7200H"). Note that n in general formula (1) is a value of 1 to 3. B'-1: Bisphenol A type epoxy resin with an epoxy equivalent of 925 g / eq ("jER1004" manufactured by Mitsubishi Chemical Corporation) (C) Fatty acid ester compound C-1: Pentaerythritol tetrastearate obtained from pentaerythritol (carbon number 5, hydroxyl group number 4) and stearic acid (oxygen number 18) (manufactured by Emeryoleochemicals Japan Co., Ltd., "Roxiol" VPG861 (trade name), acid value 1 mgKOH / g) C-2: Pentaerythritol tetrastearate obtained from pentaerythritol (carbon number 5, hydroxyl group number 4) and stearic acid (oxygen number 18) (manufactured by Riken Vitamin Co., Ltd., "Likestar" EW-400 (trade name), acid value 9 mg KOH / g) C'-1: Montanic acid ester obtained from an aliphatic alcohol and montanic acid (having 28 carbon atoms) ("Licowax OP" (trade name) manufactured by Clariant Japan Co., Ltd.) D-1: Chopped strand (manufactured by Nippon Electric Glass Co., Ltd., T-187 (product name), 3 mm length, average fiber width: 13.0 μm).

[0053] The evaluation methods used in the examples and comparative examples are summarized below.

[0054] (1) Tensile properties The pellets obtained in each of the Examples and Comparative Examples were dried in a hot air dryer at 130° C. for 3 hours, and then injection molded into multipurpose test pieces Type A (total length 150 mm, test section width 10 mm, thickness 4 mm) specified in ISO3167:2002 using an SE50DUZ injection molding machine manufactured by Sumitomo Heavy Industries, Ltd. under molding conditions of a cylinder temperature of 260° C. and a mold temperature of 80° C. Using the obtained test pieces, tensile properties were measured according to ISO527-1, -2:2012.

[0055] (2) Hydrolysis resistance The pellets obtained in each of the Examples and Comparative Examples were used to mold test pieces in the same manner as described in (1) above. The test pieces were subjected to hydrolysis treatment (PCT treatment) at 121°C and 100% RH for 50 hours using a HAST CHAMBER EHS-221M manufactured by TABAI ESPEC Co., Ltd. The tensile properties of the test pieces were measured in the same manner as described in (1), and the tensile strength retention was calculated using the following calculation formula to evaluate the hydrolysis resistance. Tensile strength retention rate (%) = (tensile strength (after hydrolysis treatment) (MPa) / tensile strength (before hydrolysis treatment) (MPa) x 100

[0056] (3) Retention stability The melt flow rate (MFR) of the polybutylene terephthalate resin composition obtained in each of the Examples and Comparative Examples was measured using G-02 manufactured by Toyo Seiki Co., Ltd. under conditions of a temperature of 270° C. and a load of 2160 gf in accordance with ISO1133.

[0057] Furthermore, after the polybutylene terephthalate resin composition was allowed to reside in the cylinder for 30 minutes, the melt flow rate was measured again under the same conditions, and the ratio of the melt flow rate after residence to the melt flow rate before residence (change rate (%)) was calculated by the following calculation formula. Melt flow rate retention rate (%) = (MFR after retention (g / 10 min) / MFR before retention (g / 10 min)) x 100

[0058] From the viewpoint of retention stability during molding, it is favorable if the melt flow rate retention is within the range of 50 to 150%, and more preferably within the range of 75 to 125%.

[0059] (4) Low gas emission The pellets obtained in each of the Examples and Comparative Examples were heat-treated at 260°C for 2 hours using a Perfect Oven manufactured by TABAI ESPEC Co., Ltd., and the weight loss rate due to heating was calculated using the following calculation formula to evaluate the low gassing properties. Weight loss rate (%) = {1-(weight after heat treatment (g) / weight before heat treatment (g)} x 100

[0060] If the weight loss rate is less than 0.5%, the low gassing property of the resin composition is good, and if it is less than 0.3%, it is more preferable. A weight loss rate of less than 0.3% was judged as ○, a weight loss rate of 0.3% to less than 0.5% was judged as △, and a weight loss rate of 0.5% or more was judged as ×.

[0061] [Examples 1 to 7, Comparative Examples 1 to 7] According to the compounding composition shown in Table 1, the (A), (B), and (C) components, as well as all other additives, were fed from the base of a twin-screw extruder, and the (D) component was fed from a sub-feed port installed between the main inlet and the tip of the extruder, and melt-kneaded in a twin-screw extruder (TEM37SS (trade name) manufactured by Toshiba Machine Co., Ltd.) with a screw diameter of 37 mm and a cylinder temperature set at 260°C. The strand discharged from the die was cooled in a cooling bath and then pelletized with a strand cutter to obtain a resin composition. The results of evaluation of the obtained resin composition by the above-mentioned method are shown in Table 1.

[0062] [Table 1]

[0063] The following is clear from Table 1.

[0064] From the comparison of Examples 1 to 7 and Comparative Examples 1 to 7, it can be seen that a polybutylene terephthalate resin composition obtained by blending 100 parts by weight of polybutylene terephthalate resin consisting of (A-1) 15 to 85 parts by weight of polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t to 25 eq / t and (A-2) 15 to 85 parts by weight of (A) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t to 45 eq / t, (B) 0.5 to 4.0 parts by weight of dicyclopentadiene type epoxy resin, and (C) 0.05 to 1.5 parts by weight of an ester compound consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms, is excellent in the balance of hydrolysis resistance, mechanical properties, retention stability, and low gas properties. Furthermore, by using recycled polybutylene terephthalate resin as (A-2), it can be said that it is excellent in economical efficiency and environmental performance.

Claims

1. A polybutylene terephthalate resin composition comprising (A) 100 parts by weight of a polybutylene terephthalate resin consisting of (A-1) 15 to 85 parts by weight of a polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less and (A-2) 15 to 85 parts by weight of a polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less, (B) 0.5 to 4.0 parts by weight of a dicyclopentadiene-type epoxy resin, and (C) 0.05 to 1.5 parts by weight of an ester compound consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms.

2. The polybutylene terephthalate resin composition according to claim 1, wherein the polybutylene terephthalate resin (A) is composed of 25 to 75 parts by weight of (A-1) a polybutylene terephthalate resin having a carboxyl group concentration of 5 eq / t or more and 25 eq / t or less and 25 to 75 parts by weight of (A-2) a polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and 45 eq / t or less.

3. The polybutylene terephthalate resin composition according to claim 1 or 2, characterized in that the (A-2) polybutylene terephthalate resin having a carboxyl group concentration of more than 25 eq / t and not more than 45 eq / t is a recycled polybutylene terephthalate resin.

4. The polybutylene terephthalate resin composition according to claim 1 or 2, comprising 0.1 to 1.0 parts by weight of the ester compound (C) consisting of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms, based on 100 parts by weight of the polybutylene terephthalate resin (A).

5. 3. The polybutylene terephthalate resin composition according to claim 1, wherein the (C) ester compound composed of an aliphatic alcohol and a fatty acid having 5 to 24 carbon atoms is pentaerythritol tetrastearate.

6. A molded article comprising the polybutylene terephthalate resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polyester resin composition and molded article produced from that composition

    JP2019026842A

  • Polybutylene terephthalate resin composition, and molding made thereof

    JP2019147934A

  • Polybutylene phthalate resin composition, molded article and composite structure

    JP2021025032A

  • Thermoplastic resin composition and method for producing thermoplastic resin composition

    WO2013108758A1