Metal material for contact point, as well as, contact point therewith, switch and connector

The metal material for contacts, with controlled KAM values and elastic modulus, addresses wear resistance issues in silver-plated contacts by enhancing durability and maintaining low resistance.

JP2024142527APending Publication Date: 2024-10-11FURUKAWA ELECTRIC CO LTD +1

Patent Information

Application Number
JP2023054686
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing metal materials for contacts, such as those with silver plating, suffer from inadequate wear resistance due to insufficient consideration of elastic deformation, leading to increased contact resistance and wear during sliding.

Method used

A metal material for contacts comprising a conductive base material with a silver-containing layer, where the average KAM value is 0.20° to 2.00° and the elastic modulus in the thickness direction is 1.0 GPa to 60.0 GPa, with specific elastic modulus ratios and thickness ranges to enhance wear resistance.

Benefits of technology

The solution provides improved wear resistance and maintains low contact resistance, ensuring durability and reliability of contacts, switches, and connectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142527000001_ABST
    Figure 2024142527000001_ABST
Patent Text Reader

Abstract

To provide a metal material for contact points having excellent wear resistance, as well as a contact point therewith, a switch and a connector.SOLUTION: A metal material for contact points comprises a conductive substrate and a silver-containing layer containing silver provided on at least a portion of a surface of the conductive substrate, wherein in a cross-section of the metal material for contact points, an average KAM value of the silver-containing layer is 0.20° or more and 2.00°or less, and the elastic modulus in a thickness direction of a portion from the surface of the silver-containing layer to one-fifth the thickness of the silver-containing layer is 1.0 GPa or more and less than 60.0 GPa.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a metal material for contacts, and to a contact, a switch, and a connector using the same. [Background technology]

[0002] Contacts and connectors, which are used for connecting terminals and electronic devices in consumer and automotive applications, are becoming more and more popular as vehicle drive systems become more electrified in order to achieve the fuel economy that has been required in recent years. For example, the amount of current passing through the wires between the battery, inverter, and motor is increasing dramatically. As a result, heat generation during current flow has become an issue.

[0003] To address these issues, materials are used that have a Ni undercoat plated on the surface of a highly conductive base material such as pure copper, dilute copper alloy, or Corson alloy, and then Ag or Ag alloy plated on top of that.

[0004] However, Ag is a metal that is susceptible to adhesive wear, and is therefore prone to being scraped off during sliding. Furthermore, wear increases the contact resistance.

[0005] For example, Patent Document 1 describes a method for producing a silver-plated product by forming a surface layer made of silver on a material by electroplating in a silver plating solution consisting of an aqueous solution containing potassium silver cyanide or silver cyanide, potassium cyanide or sodium cyanide, and benzothiazoles or their derivatives. In this method for producing a silver-plated product, the concentration of free cyanide in the silver plating solution is A (g / L), the concentration of the benzothiazole content of the benzothiazoles or their derivatives in the silver plating solution is B (g / L), the temperature of the silver plating solution is C (°C), and the current density of the electroplating is D (A / dm 2 ), then (BC / A) 2 / D is 10(℃ 2 dm 2 / A) or more. However, the silver-plated product obtained by the manufacturing method of Patent Document 1 has insufficient abrasion resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2022-159396 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present disclosure is to provide a metal material for contacts having excellent wear resistance, and a contact, a switch, and a connector using the same. [Means for solving the problem]

[0008] [1] A metal material for contacts comprising a conductive substrate and a silver-containing layer containing silver provided on at least a portion of a surface of the conductive substrate, wherein in a cross section of the metal material for contacts, the average KAM value of the silver-containing layer is 0.20° or more and 2.00° or less, and the elastic modulus in the thickness direction of a portion from the surface of the silver-containing layer to one-fifth of the thickness of the silver-containing layer is 1.0 GPa or more and less than 60.0 GPa. [2] The metal material for contacts according to the above [1], wherein the elastic force in the thickness direction of the inside of the silver-containing layer is greater than the elastic force in the thickness direction of the surface. [3] The metal material for contacts according to the above [1] or [2], wherein the elastic modulus X in the thickness direction of a portion from the surface of the silver-containing layer to one-tenth of the thickness of the silver-containing layer is 1.0 GPa or more and 10.0 GPa or less, the elastic modulus Y in the thickness direction of a portion from one-tenth of the silver-containing layer thickness on the surface side of the silver-containing layer to five-tenths of the silver-containing layer thickness is 50.0 GPa or more and less than 60.0 GPa, and the ratio of the elastic modulus Y to the elastic modulus X (elastic modulus Y / elastic modulus X) is 5.0 or more and 35.0 or less. [4] The metallic material for contacts according to any one of the above [1] to [3], wherein the average thickness of the silver-containing layer is 0.5 μm or more and 5.0 μm or less. [5] The metallic material for contacts according to any one of the above [1] to [4], wherein the silver-containing layer contains 99.0 mass % or more of silver. [6] The metal material for contacts according to any one of the above [1] to [5], further comprising one or more intermediate layers formed between the conductive substrate and the silver-containing layer and made of copper, a copper alloy, nickel or a nickel alloy. [7] The metal material for contacts according to the above [6], wherein the average thickness of the intermediate layer is 0.01 μm or more and 3.00 μm or less. [8] The metal material for contacts according to any one of the above [1] to [7], wherein the conductive base material is made of a copper-based material including pure copper and a copper alloy. [9] A contact made of the metal material for contacts according to any one of the above [1] to [8].

[10] A switch manufactured using the metal contact material according to any one of the above [1] to [8].

[11] A connector produced using the metal material for contacts according to any one of the above [1] to [8]. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a metal material for contacts having excellent wear resistance, as well as a contact, a switch, and a connector using the same. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a metallic material for contacts according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of the metallic material for contacts according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, a detailed description will be given based on an embodiment.

[0012] The present inventors have conducted extensive research into improving the wear resistance of metal materials for contacts and have discovered the following.

[0013] Even if the surface hardness of the silver plating layer in the silver-plated product obtained by the manufacturing method of Patent Document 1 is controlled, the wear resistance of the silver plating layer is insufficient because the hardness specified in Patent Document 1 is an index in the plastic deformation region. For the sliding wear phenomenon in the contact parts of terminals, etc., it is necessary to consider the phenomenon in the elastic deformation region, not the plastic deformation region. Furthermore, Patent Document 1 focuses on hardness, which is an index of the plastic deformation region, but does not consider the index of the elastic deformation region.

[0014] Therefore, the present inventors have clarified the effect of the sliding wear phenomenon at the contact portion of the terminal on the surface of the silver-containing layer, which is the surface layer of the metal material for contacts, by taking into account the elastic modulus, which is an index of the elastic deformation region. As a result, they have found that the wear resistance can be improved by controlling the average KAM value and the elastic modulus in the thickness direction of the silver-containing layer. The present disclosure has been completed based on such findings.

[0015] The metal material for contacts of the embodiment comprises a conductive substrate and a silver-containing layer containing silver provided on at least a portion of the surface of the conductive substrate, and in a cross-section of the metal material for contacts, the average KAM value of the silver-containing layer is 0.20° or more and 2.00° or less, and the elastic modulus in the thickness direction of the portion from the surface of the silver-containing layer to one-fifth the thickness of the silver-containing layer is 1.0 GPa or more and less than 60.0 GPa.

[0016] 1 is a cross-sectional view showing an example of a metallic material for contacts according to an embodiment of the present invention, and FIG. 1 is a cross-sectional view showing an example of a metallic material for contacts according to an embodiment of the present invention. As shown in FIG.

[0017] The conductive substrate 10 constituting the metal material for contacts 1 is a rolled material made of metal, has electrical conductivity, and is obtained by rolling. Examples of the conductive substrate 10 include copper-based materials including pure copper and copper alloys, iron-based materials including pure iron and iron alloys, and aluminum-based materials including pure aluminum and aluminum alloys.

[0018] From the viewpoints of the rolling processability of the conductive substrate 10 and the high conductivity of the metal material for contacts 1, the conductive substrate 10 is preferably made of a copper-based material including pure copper and a copper alloy. Among them, pure copper, Cu-Zn-based, Cu-Sn-P-based, Cu-Ni-Si-based, Cu-Sn-Ni-based, Cu-Cr-Mg-based, or Cu-Ni-Si-Zn-Sn-Mg-based copper alloys are preferable.

[0019] The electrical conductivity of the conductive substrate 10 is preferably 20% IACS or more, and more preferably 30% IACS or more. When the electrical conductivity of the conductive substrate 10 is 20% IACS or more, the metallic material 1 for contacts has good electrical conductivity.

[0020] The electrical conductivity (IACS: International Annealed Copper Standard) of the conductive substrate 10 can be determined by measurement in a thermostatic chamber controlled at 20°C±1°C using a four-terminal method.

[0021] The shape of the conductive substrate 10 may be appropriately selected depending on the application of the metallic material for contacts 1, but is preferably a plate or strip shape.

[0022] The silver-containing layer 20 constituting the metal material for contacts 1 is provided on at least a part of the surface of the conductive substrate 10 and contains silver. From the viewpoint of maintaining a low contact resistance value of the metal material for contacts 1, the silver-containing layer 20 covering the surface of the conductive substrate 10 preferably contains 99.0 mass % or more of silver. Furthermore, from the viewpoint of providing the metal material for contacts 1 with excellent abrasion resistance, it is preferable that the silver-containing layer 20 is formed by plating, that is, the silver-containing layer 20 is a plating film.

[0023] 1, the average KAM value of the silver-containing layer 20 is 0.20° or more and 2.00° or less. The cross section of the metallic material for contacts 1 is a cross section parallel to the rolling direction of the conductive substrate 10.

[0024] When the average KAM value of the silver-containing layer 20 in the cross section of the metal material for contacts 1 is 0.20° or more, the amount of strain remaining in the silver-containing layer 20 can be maintained high, and the hardness of the silver-containing layer 20 can be increased, thereby improving the wear resistance of the metal material for contacts 1 (silver-containing layer 20). When the average KAM value of the silver-containing layer 20 is 2.00° or less, deterioration of bending workability due to excessive strain in the silver-containing layer 20 can be suppressed. From this viewpoint, the lower limit of the average KAM value of the silver-containing layer 20 in the cross section of the metal material for contacts 1 is 0.20° or more, preferably 0.50° or more, and the upper limit is 2.00° or less, preferably 1.00° or less.

[0025] The KAM (Kernel Average Misorientation) value at a measurement point i is the average value of the misorientation between the measurement point i and a measurement point j adjacent to the measurement point i, and is a value reflecting the amount of distortion in the silver-containing layer 20. The KAM value can be expressed by the following formula (1).

[0026]

number

[0027] α ij : Crystal orientation difference between measurement point i and measurement point j n: The number of measurement points j adjacent to measurement point i

[0028] The KAM value is calculated for all measurement points within the field of view, and the average value is used as the representative value for that field of view. It tends to be large in areas with large distortion and near grain boundaries.

[0029] The KAM value can be obtained from crystal orientation analysis data calculated using analysis software (OIM Analysis, manufactured by TSL Solutions) from crystal orientation data continuously measured using an EBSD detector (OIM5.0 HIKARI, manufactured by TSL Solutions) attached to a high-resolution scanning analytical electron microscope (JSM-7001FA, manufactured by JEOL Ltd.). The measurement object is the surface of the silver-containing layer 20 on the surface of the cross section of the contact metal material 1 parallel to the rolling direction of the conductive substrate 10, which is mirror-finished with a cross-section polisher (manufactured by JEOL Ltd.), and the measurement magnification is 30,000 times. Measurement is performed at measurement intervals of 50 nm or less, and measurement points with CI values ​​of 0.1 or less analyzed by the analysis software are excluded (noise removal), and the boundary where the orientation difference between adjacent pixels is 5.00° or more is regarded as a grain boundary, and the KAM value is obtained. This measurement is performed multiple times (multiple measurement areas of the same sample, different) and the average value is calculated to obtain the average KAM value.

[0030] The present inventors have also found that when the elastic modulus in the thickness direction of the portion from the surface of the silver-containing layer 20 to one-fifth of the thickness of the silver-containing layer (hereinafter, the elastic modulus in the thickness direction is also simply referred to as the elastic modulus) is within the following range, it is effective in improving the wear resistance of the metal material for contacts 1. When the silver-containing layer 20 provided on the surface of the metal material for contacts 1 has a predetermined elastic modulus, the silver-containing layer 20 can maintain high slidability while maintaining a contact area necessary to maintain low resistance at the sliding contact portion, thereby suppressing wear.

[0031] Specifically, the elastic modulus in the thickness direction of the portion from the surface of the silver-containing layer 20 to one-fifth of the thickness of the silver-containing layer 20 is 1.0 GPa or more and less than 60.0 GPa. On the surface side of the silver-containing layer 20, i.e., on the surface side of the metal material for contacts 1, if the elastic modulus of the portion from the surface of the silver-containing layer 20 to one-fifth of the thickness of the silver-containing layer 20 is 1.0 GPa or more, the amount of strain in the silver-containing layer 20 can be kept high, and the hardness of the silver-containing layer 20 can be increased, thereby improving the wear resistance of the metal material for contacts 1. In addition, if the elastic modulus of the portion from the surface of the silver-containing layer 20 to one-fifth of the thickness of the silver-containing layer 20 is less than 60.0 GPa, the deterioration of bending workability due to the excessive amount of strain in the silver-containing layer 20 can be suppressed. From this viewpoint, the lower limit of the elastic modulus in the thickness direction of the portion from the surface of the silver-containing layer 20 to one-fifth of the thickness of the silver-containing layer is 1.0 GPa or more, preferably 3.0 GPa or more, and the upper limit is less than 60.0 GPa, preferably 10.0 GPa or less, and more preferably 7.0 GPa or less.

[0032] In addition, the elastic force in the thickness direction inside the silver-containing layer 20 is preferably greater than the elastic force in the thickness direction on the surface. When the elastic force inside the silver-containing layer 20 is greater than the elastic force on the surface of the silver-containing layer 20, the excellent wear resistance of the metal material for contacts 1 can be maintained even when the thickness of the silver-containing layer 20 is reduced due to wear of the silver-containing layer 20 caused by sliding of the silver-containing layer 20.

[0033] In particular, it is preferable that the elastic modulus X in the thickness direction of the portion from the surface of the silver-containing layer 20 to one-tenth of the silver-containing layer thickness is 1.0 GPa or more and 10.0 GPa or less, the elastic modulus Y in the thickness direction of the portion from one-tenth of the silver-containing layer thickness on the surface side of the silver-containing layer 20 to five-tenths of the silver-containing layer thickness is 50.0 GPa or more and less than 60.0 GPa, and the ratio of the elastic modulus Y to the elastic modulus X (elastic modulus Y / elastic modulus X) is 5.0 or more and 35.0 or less.

[0034] When the elastic modulus X of the portion on the surface side of the silver-containing layer 20 from the surface of the silver-containing layer 20 to one-tenth of the thickness of the silver-containing layer 20 is 1.0 GPa or more, and the elastic modulus Y of the portion on the surface side of the silver-containing layer 20 from one-tenth of the thickness of the silver-containing layer 20 to five-tenths of the thickness of the silver-containing layer 20 is 50.0 GPa or more, and the ratio (elastic modulus Y / elastic modulus X) is 5.0 or more, the amount of strain in the silver-containing layer 20 can be maintained high, and the hardness of the silver-containing layer 20 can be increased, thereby improving the wear resistance of the metal material for contacts 1. In addition, since the elastic modulus of the silver-containing layer 20 is higher inside the silver-containing layer 20, particularly inside the conductive substrate 10 side, than the elastic modulus of the surface of the silver-containing layer 20, the excellent wear resistance of the metal material for contacts 1 can be further maintained even when the thickness of the silver-containing layer 20 is reduced due to wear of the silver-containing layer 20 caused by sliding of the silver-containing layer 20.

[0035] Furthermore, when the elastic modulus X is 10.0 GPa or less, the elastic modulus Y is less than 60.0 GPa, and the ratio (elastic modulus Y / elastic modulus X) is 35.0 or less, deterioration of bending workability due to an excessive amount of strain in the silver-containing layer 20 can be suppressed.

[0036] From this viewpoint, the lower limit of the elastic modulus X in the thickness direction of the portion from the surface of the silver-containing layer 20 to 1 / 10 of the silver-containing layer thickness is preferably 1.0 GPa or more, more preferably 3.0 GPa or more, and the upper limit is preferably 10.0 GPa or less, more preferably 7.0 GPa or less. From the same viewpoint, the lower limit of the elastic modulus Y in the thickness direction of the portion from 1 / 10 of the silver-containing layer thickness to 5 / 10 of the silver-containing layer thickness on the surface side of the silver-containing layer 20 is preferably 50.0 GPa or more, more preferably 53.0 GPa or more, and the upper limit is preferably less than 60.0 GPa, more preferably less than 57.0 GPa. From the same viewpoint, the lower limit of the ratio (elastic modulus Y / elastic modulus X) is preferably 5.0 or more, more preferably 7.0 or more, and the upper limit is preferably 35.0 or less, more preferably 25.0 or less.

[0037] Elastic modulus E in the thickness direction of the silver-containing layer 20 ITcan be calculated from the following formulas (2) and (3) using an ultra-microindentation hardness tester (Elionix, ENT-2100) in accordance with the test method of ISO14577-1 2002-10-01 Part 1. Specifically, for the modulus of elasticity in the thickness direction of the portion from the surface of the silver-containing layer 20 to one-fifth of the thickness of the silver-containing layer, the modulus of elasticity (indentation modulus) (GPa) at an indentation depth equivalent to one-fifth of the thickness of the silver-containing layer 20 from the surface of the silver-containing layer 20 was measured by the tester. For the modulus of elasticity in the thickness direction of the portion from the surface of the silver-containing layer 20 to one-tenth of the thickness of the silver-containing layer 20, the modulus of elasticity at an indentation depth equivalent to one-tenth of the thickness of the silver-containing layer 20 from the surface of the silver-containing layer 20 was measured by the tester. Regarding the elastic modulus in the thickness direction of the portion on the surface side of the silver-containing layer 20 from 1 / 10 of the thickness of the silver-containing layer to 5 / 10 of the thickness of the silver-containing layer, the elastic modulus at an indentation depth corresponding to 1 / 10 of the thickness of the silver-containing layer 20 to 5 / 10 of the thickness of the silver-containing layer 20 on the surface side of the silver-containing layer 20 was measured by a testing machine. The elastic force of the surface of the silver-containing layer 20 and the elastic force inside the silver-containing layer 20 were also measured by the testing machine.

[0038]

number

[0039]

number

[0040] ν s : Poisson's ratio of the test piece ν i : Poisson's ratio of the indenter E r : Converted elastic modulus due to indentation contact E i : Elastic modulus of indenter C: Contact Compliance A p :Projected contact area

[0041] The silver-containing layer 20 may also contain one or more elements (hereinafter also referred to as the second element) selected from the group consisting of Zn, Cu, Ni, Se, Sb, and Co. The coexistence of the second element in the silver-containing layer 20 can improve wear resistance. In particular, from the viewpoint of efficient wear resistance improvement by the addition of the second element, the silver-containing layer 20 preferably contains one or more elements selected from the group consisting of Zn, Cu, Ni, Se, Sb, and Co in a total amount of 0.1 at% or more. From the viewpoint of improving the electrical connectivity of the contact metal material 1 and reducing material costs, the silver-containing layer 20 preferably contains one or more elements selected from the group consisting of Zn, Cu, Ni, Se, Sb, and Co in a total amount of less than 15.0 at%.

[0042] The lower limit of the average thickness of the silver-containing layer 20 is preferably 0.5 μm or more, more preferably 2.0 μm or more, and even more preferably 3.0 μm or more. The upper limit of the average thickness of the silver-containing layer 20 is preferably 5.0 μm or less. When the lower limit of the average thickness of the silver-containing layer 20 is 0.5 μm or more, the excellent wear resistance of the contact metal material 1 can be maintained for a long period of time. When the upper limit of the average thickness of the silver-containing layer 20 is 5.0 μm or less, the material cost can be suppressed.

[0043] Fig. 2 is a cross-sectional view showing another example of the metal material for contacts according to the embodiment. The metal material for contacts 2 shown in Fig. 2 has basically the same structure as the metal material for contacts 1 shown in Fig. 1, except that an intermediate layer 30 is added.

[0044] 2, the metal material for contacts 2 further includes one or more intermediate layers 30 provided between the conductive substrate 10 and the silver-containing layer 20. The intermediate layer 30 is made of copper, a copper alloy, nickel, or a nickel alloy. Here, an example is shown in which the metal material for contacts 2 includes one intermediate layer 30, but the number of intermediate layers 30 may be multiple.

[0045] When the intermediate layer 30 is provided between the surface of the conductive substrate 10 and the silver-containing layer 20, the thermal diffusion of the elements constituting the conductive substrate 10 to the silver-containing layer 20 can be suppressed, and the adhesion between the conductive substrate 10 and the silver-containing layer 20 can be improved. From this viewpoint, the copper alloy is preferably a Cu-Sn-based or Cu-Co-based alloy. The nickel alloy is preferably a Ni-P-based alloy.

[0046] The lower limit of the average thickness of the intermediate layer 30 is preferably 0.01 μm or more, more preferably 0.10 μm or more, and even more preferably 0.30 μm or more. The upper limit of the average thickness of the intermediate layer 30 is preferably 3.00 μm or less, more preferably 2.00 μm or less, and even more preferably 1.00 μm or less. When the lower limit of the average thickness of the intermediate layer 30 is 0.01 μm or more, the above-mentioned thermal diffusion suppression and adhesion can be further improved. When the upper limit of the average thickness of the intermediate layer 30 is 3.00 μm or less, bending workability can be improved. When the metal material for contacts is used in a terminal, bending workability of R / t≧1 (bending radius ratio: R / t) is required.

[0047] The contact metal materials 1 and 2 may further include a copper layer (not shown) directly below the silver-containing layer 20, which is the surface layer. The copper layer (not shown) is made of pure copper or a copper alloy. The thickness of the copper layer (not shown) is significantly smaller than the thickness of the conductive substrate 10. When the contact metal materials 1 and 2 further include a copper layer (not shown) directly below the silver-containing layer 20, the adhesion and bending workability can be further improved.

[0048] As described above, the metal contact materials 1 and 2 have excellent wear resistance, and therefore the metal contact materials 1 and 2 can be suitably used for contacts, switches, and connectors. Such contacts are contacts made using the metal contact materials 1 and 2, the switches are switches made using the metal contact materials 1 and 2, and the connectors are connectors made using the metal contact materials 1 and 2.

[0049] Next, the manufacturing method of the contact metal materials 1 and 2 will be described.

[0050] First, a silver-containing layer is formed on at least a part of the surface of a conductive base material by a plating method under the following conditions. In this manner, a metal material 1 for contacts can be produced.

[0051] Moreover, an intermediate layer is formed on at least a part of the surface of the conductive base material by a plating method or the like. Then, a silver-containing layer is formed on the surface of the intermediate layer by a plating method under the following conditions. In this manner, the contact metal material 2 can be produced.

[0052] The plating conditions for the silver-containing layer were: current density 15A / dm 2 More than 30A / dm 2 Hereinafter, the bath temperature (liquid temperature) is set to 30°C or higher and 40°C or lower. In this way, by setting the current density at a high temperature, the nucleation rate of plating can be increased, and the number of crystal grains constituting the silver-containing layer, which is the plating film, increases, so that the amount of strain in the grain boundaries increases more than usual. Therefore, the average KAM value and the elastic modulus of the silver-containing layer can be controlled within the above ranges.

[0053] According to the embodiment described above, by controlling the average KAM value in the silver-containing layer and controlling the elastic modulus, a metal material for contacts having excellent wear resistance can be obtained.

[0054] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. EXAMPLES

[0055] Next, examples and comparative examples will be described, but the present disclosure is not limited to these examples.

[0056] Example 1 The conductive substrate (pure copper) was electrolytically degreased and then acid-washed. An aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0057] 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 30°C and 15 A / dm 2 A silver-containing layer was formed on the surface of the conductive substrate by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0058] (Examples 2 to 3) A metal material for contacts was produced in the same manner as in Example 1, except that the bath temperature and current density were changed to the values ​​shown in Table 1.

[0059] Example 4 A metal material for contacts was produced in the same manner as in Example 1, except that an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 10 g / L of zinc chloride was used as the electrolytic plating solution for forming the silver-containing layer, and the bath temperature and current density were changed to the values ​​shown in Table 1.

[0060] Example 5 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of copper chloride dihydrate was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0061] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 20 A / dm. Then, 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0062] Example 6 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0063] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 20 A / dm. Then, 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0064] Example 7 The conductive substrate (pure copper) was electrolytically degreased and then acid-washed. In addition, an aqueous solution containing 180 g / L of copper sulfate and 80 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming the intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared as an electrolytic plating solution for forming the silver-containing layer.

[0065] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 40°C and 5 A / dm 2An intermediate layer made of pure copper was formed on the surface of the conductive substrate by passing a current at a current density of 25 A / dm. Then, 3 L of an electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0066] Example 8 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride hexahydrate, 30 g / L of boric acid, and 16 g / L of phosphorous acid was prepared as an electrolytic plating solution for forming an intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0067] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 10 A / dm 2 An intermediate layer made of a nickel alloy was formed on the surface of the conductive substrate by passing a current at a current density of 25 A / dm. Then, 3 L of an electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath having an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0068] Example 9 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming the intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of nickel chloride was prepared as an electrolytic plating solution for forming the silver-containing layer.

[0069] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 20 A / dm. Then, 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0070] Example 10 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 10 g / L of cobalt chloride was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0071] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 20 A / dm. Then, 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution.2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0072] Example 11 A conductive substrate made of a copper alloy (Furukawa Electric, EFTEC-550T, 80% IACS) was used as the conductive substrate, and the bath temperature and current density were changed to the values ​​shown in Table 1. The same procedure as in Example 1 was used to produce a metal material for contacts.

[0073] Example 12 A conductive substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was electrolytically degreased and then acid washed. An aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. An aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 2.2 mg / L of potassium selenocyanate was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0074] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 25 A / dm. Then, 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0075] (Example 13) A conductive substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was electrolytically degreased and then acid washed. An aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. An aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0076] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 25 A / dm. Then, 3 L of electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0077] (Comparative Examples 1 to 4) A metal material for contacts was produced in the same manner as in Example 1, except that the bath temperature and current density were changed to the values ​​shown in Table 1.

[0078] Comparative Example 5 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming the intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 2.2 mg / L of potassium selenocyanate was prepared as an electrolytic plating solution for forming the silver-containing layer.

[0079] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 10 A / dm. Then, 3 L of an electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0080] Comparative Example 6 The conductive substrate (pure copper) was electrolytically degreased and then acid washed. In addition, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. In addition, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0081] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 10 A / dm. Then, 3 L of an electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0082] Comparative Example 7 A conductive substrate made of a copper alloy (Furukawa Electric, EFTEC-550T, 80% IACS) was used as the conductive substrate, and the bath temperature and current density were changed to the values ​​shown in Table 1. In the same manner as in Example 1, except that, a metal material for contacts having a silver-containing layer was produced.

[0083] Comparative Example 8 A conductive substrate (Furukawa Electric, EFTEC-550T, 80% IACS) was electrolytically degreased and then acid washed. An aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming an intermediate layer. An aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 2.2 mg / L of potassium selenocyanate was prepared as an electrolytic plating solution for forming a silver-containing layer.

[0084] 3 L of electrolytic plating solution for forming the intermediate layer was placed in a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate was immersed in the electrolytic plating solution. After that, the bath temperature was 55°C and 15 A / dm 2 An intermediate layer made of pure nickel was formed on the surface of the conductive substrate by passing a current at a current density of 40 A / dm. Then, 3 L of an electrolytic plating solution for forming a silver-containing layer was placed in a cylindrical plating electrolytic bath with an inner diameter of 120 mm, and the conductive substrate with the intermediate layer was immersed in the electrolytic plating solution. 2 A silver-containing layer was formed on the surface of the intermediate layer by passing a current at a current density of 1000 μm to 1000 μm. Thus, a metal material for contacts was produced.

[0085] [Measurement and Evaluation] The metallic materials for contacts obtained in the above examples and comparative examples were subjected to the following measurements and evaluations. The results are shown in Tables 1 and 2.

[0086] [1] Average thickness of each layer The average thickness of the silver-containing layer and the intermediate layer was measured using a fluorescent X-ray thickness gauge (STF9400, Hitachi High-Tech Science Corp.) Measurements were taken at five different locations on the same sample, and the average value was calculated to obtain the average thickness of each layer.

[0087] [2] Average KAM value of silver-containing layer The KAM value of the silver-containing layer was obtained from crystal orientation analysis data calculated using analysis software (TSL Solutions, OIM Analysis) from crystal orientation data continuously measured using an EBSD detector (TSL Solutions, OIM5.0 HIKARI) attached to a high-resolution scanning analytical electron microscope (JEOL Ltd., JSM-7001FA).

[0088] Using a cross-section polisher (manufactured by JEOL Ltd.), the silver-containing layer surface on the mirror-finished cross section of the metal material for contacts parallel to the rolling direction of the conductive substrate was obtained as the measurement target. The measurement magnification was 30,000 times. Measurements were performed at intervals of 50 nm or less, and measurement points with CI values ​​of 0.1 or less analyzed by the analysis software were excluded. Boundaries with orientation differences of 5.00° or more between adjacent pixels were considered to be grain boundaries, and the KAM value was obtained. This measurement was performed five times (at five different measurement areas on the same sample), and the average value was calculated to obtain the average KAM value of the silver-containing layer.

[0089] [3] Elastic modulus in the thickness direction of the silver-containing layer Elastic modulus E of the silver-containing layer in the thickness direction ITwas calculated from the above formulas (2) and (3) using an ultra-microindentation hardness tester (Elionix, ENT-2100) in accordance with the test method of ISO14577-1 2002-10-01 Part 1. Specifically, the elastic modulus in the thickness direction of the portion from the surface of the silver-containing layer to one-fifth of the silver-containing layer thickness was measured by the tester at an indentation depth equivalent to one-fifth of the silver-containing layer thickness from the surface of the silver-containing layer. The elastic modulus in the thickness direction of the portion from the surface of the silver-containing layer to one-tenth of the silver-containing layer thickness was measured by the tester at an indentation depth equivalent to one-tenth of the silver-containing layer thickness from the surface of the silver-containing layer. The elastic modulus in the thickness direction of the portion from one-tenth of the silver-containing layer thickness to one-fifth of the silver-containing layer thickness on the surface side of the silver-containing layer was measured by the tester at an indentation depth equivalent to one-tenth of the silver-containing layer thickness on the surface side of the silver-containing layer. The elasticity of the surface of the silver-containing layer and the elasticity of the inside of the silver-containing layer were also measured using a tester. Regarding the relationship between the elasticity of the inside and the elasticity of the surface of the silver-containing layer, the larger elasticity is listed in the table.

[0090] [4] Abrasion resistance The surface of the silver-containing layer of the contact metal material was subjected to 50 reciprocating strokes using a friction and wear tester Tribogear (surface property measuring device TYPE: 14FW, manufactured by Shinto Scientific Co., Ltd.) with a contact load of 4N, a sliding distance of 50mm, and a sliding speed of 100mm / min. A laser roughness meter was used to measure the ratio of the depth from the reference surface (the surface that was not subjected to reciprocating strokes) to the thickness of the silver-containing layer. The wear resistance was ranked as follows.

[0091] ◎: The ratio of the depth from the reference plane to the thickness of the silver-containing layer is less than 1 / 10 ○: The ratio of the depth from the reference plane to the thickness of the silver-containing layer is 1 / 10 or more and less than 1 / 5. ×: The ratio of the depth from the reference plane to the thickness of the silver-containing layer is 1 / 5 or more.

[0092] [5] Contact resistance The contact resistance of the surface of the silver-containing layer of the metal contact material was measured 10 times using an electric contact simulator (manufactured by Yamazaki Seiki Kenkyusho Co., Ltd.) at a current value of 20 mA and a load of 1 N, and the average of the measured values ​​was taken as the contact resistance of the metal contact material. The contact resistance was ranked as follows:

[0093] ◎: Contact resistance is less than 0.5mΩ ○: Contact resistance is 0.5 mΩ or more and less than 1.0 mΩ ×: Contact resistance is 1.0mΩ or more

[0094] [6] Electrical conductivity The electrical conductivity γ (%) of the metal materials for contacts was measured using a tester in accordance with the test method of JIS H 0505. The electrical conductivity was calculated using the following formula (4) (gravimetric method). The electrical conductivity was ranked as follows:

[0095] ◎: Conductivity is 50% or more ○: Conductivity is 20% or more and less than 50% ×: Conductivity is less than 20%

[0096]

number

[0097] R t : Electrical resistance of the test piece at t℃ (Ω) m: total mass of the test piece (g) l 1 : Length between electrical resistance measurements (m) l 2 : Total length of test piece (m) t: Temperature at the time of measurement (℃) α 20 : Constant mass temperature coefficient at 20℃ C is a constant and can be calculated using the following formula: C = A x s (A: 0.017241, s: specific gravity)

[0098] [7] Bending workability In accordance with the test method of the Japan Copper and Brass Association technical standard JCBA-T307:2007, five test pieces (n=5) of 10 mm wide x 30 mm long were taken from the metal material for contacts so that the longitudinal direction of the test piece was parallel to the rolling direction. A bending test was performed on each test piece at a bending angle of 90 degrees and R / t=1 to determine the presence or absence of cracks.

[0099] ○: No cracks in the five test pieces ×: One or more test pieces have cracks

[0100] [8] Heat resistance The metal contact material was heated at 150°C for 1000 hours in an air atmosphere. After heating, the contact resistance of the silver-containing layer side surface of the metal contact material was measured 10 times using an electric contact simulator (manufactured by Yamazaki Seiki Kenkyusho Co., Ltd.) at a current value of 20 mA and a load of 1 N, and the average of the measured values ​​was taken as the contact resistance of the metal contact material. Heat resistance was ranked as follows.

[0101] ◎: Contact resistance after heating is less than 1.0mΩ ○: Contact resistance after heating is 1.0 mΩ or more and less than 5.0 mΩ ×: Contact resistance after heating is 5.0mΩ or more

[0102] [Table 1]

[0103] [Table 2]

[0104] As shown in Tables 1 and 2, in the examples, the average KAM value of the silver-containing layer and the modulus of elasticity in the thickness direction of the portion from the surface of the silver-containing layer to one-fifth of the silver-containing layer thickness were within the specified range, so the wear resistance of the metal material for contacts was excellent. On the other hand, in the comparative examples, at least one of the average KAM value of the silver-containing layer and the modulus of elasticity in the thickness direction of the portion from the surface of the silver-containing layer to one-fifth of the silver-containing layer thickness was outside the specified range, so the wear resistance of the metal material for contacts was poor. [Explanation of symbols]

[0105] 1, 2 Metal materials for contacts 10 Conductive base material 20 Silver-containing layer 30 Middle Class

Claims

1. A conductive substrate; a silver-containing layer that contains silver and is provided on at least a portion of the surface of the conductive substrate; A metal material for contacts comprising: In a cross section of the contact metal material, the average KAM value of the silver-containing layer is 0.20° or more and 2.00° or less, A metal material for contacts, wherein the elastic modulus in the thickness direction of a portion from the surface of the silver-containing layer to one-fifth of the thickness of the silver-containing layer is 1.0 GPa or more and less than 60.0 GPa.

2. 2. The metal material for contacts according to claim 1, wherein the elastic force in the thickness direction of the inside of said silver-containing layer is greater than the elastic force in the thickness direction of the surface of said silver-containing layer.

3. the elastic modulus X in the thickness direction of a portion from the surface of the silver-containing layer to one-tenth of the thickness of the silver-containing layer is 1.0 GPa or more and 10.0 GPa or less; the elastic modulus Y in the thickness direction of a portion of the surface side of the silver-containing layer from 1 / 10 of the thickness of the silver-containing layer to 5 / 10 of the thickness of the silver-containing layer is 50.0 GPa or more and less than 60.0 GPa; 2. The metallic material for contacts according to claim 1, wherein a ratio of said elastic modulus Y to said elastic modulus X (elastic modulus Y / elastic modulus X) is 5.0 or more and 35.0 or less.

4. 2. The metal material for contacts according to claim 1, wherein the average thickness of said silver-containing layer is 0.5 μm or more and 5.0 μm or less.

5. 2. The metal material for contacts according to claim 1, wherein the silver-containing layer contains 99.0 mass % or more of silver.

6. 2. The contact metal material of claim 1, further comprising one or more intermediate layers disposed between the conductive substrate and the silver-containing layer, the intermediate layers being made of copper, a copper alloy, nickel, or a nickel alloy.

7. 7. The metal material for contacts according to claim 6, wherein the average thickness of said intermediate layer is 0.01 [mu]m or more and 3.00 [mu]m or less.

8. The metal material for contacts according to claim 1 , wherein the conductive substrate is made of a copper-based material including pure copper and copper alloys.

9. A contact made of the metal material for contacts according to any one of claims 1 to 8.

10. A switch manufactured using the metal contact material according to any one of claims 1 to 8.

11. A connector produced by using the metal material for contacts according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Silver plating material and method for producing the same

    JP2020012202A

  • Silver-plated material and its manufacturing method

    JP2022159396A

Cited By

  • Electric contact material and electric / electronic component

    WO2026211110A1