Method of continuous casting of steel
The continuous casting method with optimized light reduction rolls and electromagnetic braking addresses the challenges of center segregation and porosity in thicker slabs by enhancing rolling efficiency and uniformity, thereby improving slab quality.
Patent Information
- Application Number
- JP2023054876
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The continuous casting of thicker steel slabs faces challenges in reducing center segregation and porosity without increasing equipment size or rigidity, as conventional methods either lead to bulging or insufficient rolling, potentially worsening these defects.
A continuous casting method using a continuous casting machine with pairs of light reduction rolls, where at least one roll has a larger diameter at the center, and a rolling process is performed at specific speeds and ranges to optimize rolling without increasing equipment size or rigidity, combined with an electromagnetic brake to apply a magnetic field for uniform shell thickness.
This method effectively suppresses internal cracking, reduces center segregation, and minimizes porosity in steel slabs by optimizing rolling forces and shell uniformity, ensuring high-quality slab production.
Smart Images

Figure 2024142642000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for continuous casting of steel. [Background technology]
[0002] In the continuous casting of steel, the slab solidifies and shrinks, causing defects such as center segregation and porosity in the slab. The slab obtained by continuous casting is rolled to become a product. In recent years, products have become thicker and stronger, and as a result, there are increasing demands for the internal quality of the slab. For this reason, it is necessary to further reduce center segregation and porosity in the center of the slab in its thickness direction. In order to improve the internal quality caused by these defects, the slab is usually soft-reduced in the thickness direction in a continuous casting machine. For soft reduction, multiple reduction rolls arranged in the casting direction of the slab are usually used.
[0003] For example, Patent Document 1 discloses a technique for arranging a convex roll, the roll diameter of which at the width direction center is larger than the roll diameter at both ends, at the upstream portion of the soft reduction zone in order to prevent center segregation and deterioration of porosity even when the crater end shape at both ends of the slab shifts upstream. In the continuous casting method described in Patent Document 1, the temperature distribution in the width direction is measured before the slab reaches the soft reduction zone. Patent Document 1 also describes that when the temperature at the width direction center of the slab is a predetermined temperature lower than the temperatures at both ends, a convex roll is used to perform soft reduction centered on the width direction center of the slab.
[0004] Patent Document 2 discloses a technique for bulging a slab in order to reduce the rolling load during soft reduction. In the continuous casting method described in Patent Document 2, the slab is intentionally bulged by gradually increasing the distance between the support rolls in the thickness direction, and then the slab is reduced by a plurality of guide rolls.
[0005] Patent Document 3 discloses a technique in which one or both of two or more consecutive reduction roll pairs are convex rolls in order to improve center porosity (center segregation) of a slab. In the continuous casting method described in Patent Document 3, a slab is reduced using a reduction roll pair including a convex roll when the central solid fraction of the slab is in the range of 0.7 or more. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-66302 A [Patent Document 2] International Publication No. 2019 / 167855 [Patent Document 3] JP 2016-78083 A Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, the thickness of the slab has been increased in response to the demand for thicker products, and the reduction force of the reduction roll required to sufficiently reduce the center segregation and porosity of the slab has been increasing. In order to increase the reduction force, in addition to increasing the size of equipment such as hydraulic devices, it is necessary to increase the rigidity of the reduction roll and the rigidity of the segment frame so that they can withstand the increased reduction force. In order to increase the rigidity of the reduction roll, for example, it is possible to increase the diameter of the reduction roll. However, if the diameter of the reduction roll is increased, the distance between adjacent reduction rolls in the casting direction inevitably increases. Then, bulging is likely to occur in the slab between the adjacent reduction rolls, and conversely, there is a possibility that the center segregation will increase. In addition, in order to increase the rigidity of the reduction roll, it is also possible to divide the reduction roll into multiple parts in the width direction and provide bearings between each reduction roll. However, in this case, the slab is not reduced at the bearing parts between the reduction rolls, so that the center segregation and porosity may worsen.
[0008] In the technology described in Patent Document 1, reduction is performed with a convex roll upstream of the soft reduction zone, and reduction is performed with a flat roll downstream of the convex roll. In general, the temperature of the slab is lower downstream in the casting direction than the upstream side, so the reduction force of the reduction roll required increases. Therefore, even if the slab is reduced with a flat roll downstream, the widthwise center of the slab cannot be reduced sufficiently, and central segregation and porosity may worsen. In addition, a dent is transferred to the widthwise center of the slab by the convex roll. Since the flat roll cannot reduce this dent, central segregation and porosity may worsen depending on the conditions. Furthermore, Patent Document 1 does not specify the specific central solid fraction or soft reduction amount at which soft reduction should be started.
[0009] The technology of Patent Document 2 intentionally bulges the slab before soft reduction. However, depending on the steel type of the slab and the amount of bulging, internal cracks may occur, which may adversely affect product quality. The technology of Patent Document 3 reduces the slab using a pair of reduction rolls when the center solid fraction of the slab is in the range of 0.7 or more, but it may not be possible to fully improve center segregation that occurs before this range.
[0010] An object of the present disclosure is to provide a method for continuous casting of steel that can suppress internal cracks in a cast slab while reducing center segregation and porosity. [Means for solving the problem]
[0011] The continuous casting method according to the present disclosure is a method for continuously casting steel using a continuous casting machine. The continuous casting machine includes a plurality of pairs of soft reduction rolls arranged in the casting direction of a slab. At least one of the pairs of soft reduction rolls has a diameter at a widthwise center portion larger than the diameter at both ends. At least one of the pairs of soft reduction rolls satisfies the following formula (1), where the width at the widthwise center portion is Wr (mm), the width of the slab is Ws (mm), and the thickness of the slab is D (mm). The continuous casting method includes a reduction step. In the reduction step, the slab is soft reduced in the thickness direction at a reduction speed of 0.5 mm / min or more and 1.3 mm / min or less using the plurality of pairs of soft reduction rolls from when the central solid fraction of the slab reaches 0.3 until the central solid fraction reaches 1.0. Ws-1.15×D≦Wr≦Ws-1.15×D+250 (1) Effect of the Invention
[0012] According to the method for continuous casting steel according to the present disclosure, it is possible to suppress internal cracks in a slab while reducing center segregation and porosity. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram of a continuous casting machine used in a continuous casting method according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the continuous casting machine taken along a plane perpendicular to the casting direction. [Diagram 3] FIG. 3 is a flow diagram showing the method for continuous casting steel according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] A continuous casting method according to an embodiment is a method for continuously casting steel using a continuous casting machine. The continuous casting machine includes a plurality of pairs of soft reduction rolls arranged in the casting direction of a slab. At least one of the pairs of soft reduction rolls has a diameter at the widthwise center that is larger than the diameter at both ends. At least one of the pairs of soft reduction rolls satisfies the following formula (1), where the width at the widthwise center is Wr (mm), the width of the slab is Ws (mm), and the thickness of the slab is D (mm). The continuous casting method includes a reduction step. In the reduction step, the slab is soft reduced in the thickness direction at a reduction speed of 0.5 mm / min or more and 1.3 mm / min or less using the plurality of pairs of soft reduction rolls from when the central solid fraction of the slab reaches 0.3 until the central solid fraction reaches 1.0 (first configuration). Ws-1.15×D≦Wr≦Ws-1.15×D+250 (1)
[0015] In the continuous casting method of the first configuration, in the reduction step, a plurality of pairs of soft reduction rolls are used to softly reduce the slab in the thickness direction. At least one of the pairs of soft reduction rolls is a convex roll having a diameter at the widthwise center greater than the diameter at both ends. The convex roll has a shape that satisfies the above formula (1) in relation to the slab. In short, the width of the part (widthwise center) of the convex roll that has a diameter greater than the diameter at both ends is appropriately set. In the soft reduction using this convex roll, the range in which the slab is reduced in the width direction is optimized, and both ends of the slab, which have a relatively low temperature, are not reduced significantly. Therefore, the reduction force required for reducing the slab is suppressed, and center segregation and porosity can be reduced without increasing the size of the equipment or the rigidity of the soft reduction roll.
[0016] In addition, in the continuous casting method of the first configuration, intentional bulging of the slab is not performed. Furthermore, since there is no need to increase the rigidity of the soft reduction rolls, there is no need to increase the diameter of the soft reduction rolls. Therefore, bulging is less likely to occur between the pair of soft reduction rolls. As a result, the continuous casting method of the first configuration suppresses internal cracking of the slab.
[0017] The continuous casting method according to the first aspect preferably has the following configuration: The continuous casting machine includes a mold including an electromagnetic brake. The continuous casting method further includes an application step, in which a magnetic field having a magnetic flux density of 1000 Gauss or more is applied to the molten steel in the mold by the electromagnetic brake (second aspect).
[0018] In the continuous casting method according to the second aspect, in the applying step, a magnetic field having a magnetic flux density of 1000 Gauss or more is applied to the molten steel in the mold by an electromagnetic brake. This makes the thickness of the solidified shell of the slab uniform in the width direction. By lightly reducing the slab in the thickness direction in the reducing step, it is possible to reduce center segregation and porosity.
[0019] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the same description will not be repeated.
[0020] [Continuous casting machine] FIG. 1 is a schematic diagram of a continuous casting machine 1 used in the continuous casting method according to the present embodiment. The continuous casting machine 1 produces a cast piece 10. In the example of the present embodiment, the cast piece 10 is a slab. In this specification, a slab means a cast piece having a width-to-thickness ratio of 3 or more. The continuous casting machine 1 includes a tundish 2, a mold 4, a plurality of support rolls 5, and a plurality of soft reduction roll pairs 6. In the example of the present embodiment, the continuous casting machine 1 is a vertical bending type. In short, the continuous casting machine 1 includes a vertical band, a curved portion, and a horizontal band. However, the continuous casting machine 1 may be, for example, a vertical type consisting of only a vertical band, or a curved type consisting of a curved portion and a horizontal band.
[0021] Molten steel M is supplied to the tundish 2 from a ladle (not shown). The molten steel M in the tundish 2 is supplied to the mold 4 through the submerged nozzle 3. The molten steel M in the mold 4 is cooled by the mold 4. The mold 4 includes an electromagnetic brake 4a. The electromagnetic brake 4a is, for example, an electromagnet. For example, the electromagnetic brakes 4a are disposed on both outer sides of the mold 4 in the thickness direction of the slab 10.
[0022] A plurality of secondary cooling nozzles (not shown) and a plurality of support rolls 5 are arranged downstream in the casting direction of the mold 4. The molten steel M is cooled in the mold 4, and then further cooled by secondary cooling water being sprayed from the secondary cooling nozzle. This forms a solidified shell S. The slab 10 in the process of solidifying here includes the solidified shell S (solid fraction 1.0) and unsolidified molten steel M (solid fraction less than 1.0). The slab 10 in the process of solidifying and including the unsolidified molten steel M is guided downstream in the casting direction by the plurality of support rolls 5. In the process, the unsolidified molten steel M gradually decreases, and a completely solidified slab 10 is formed. The secondary cooling nozzles are arranged, for example, alternately with the plurality of support rolls 5 in the casting direction.
[0023] A slab 10 containing unsolidified molten steel M is guided downstream in the casting direction by a plurality of support rolls 5. In the process, the unsolidified molten steel M gradually decreases, and the slab 10 becomes a completely solidified slab. In this type of continuous casting, the slab 10 is fed in the casting direction by pinch rolls (not shown). In other words, the casting speed of the slab 10 is controlled by the pinch rolls.
[0024] A plurality of soft reduction roll pairs 6 are arranged downstream in the casting direction of the plurality of support rolls 5. Each of the soft reduction roll pairs 6 includes two soft reduction rolls 61, 62, and softly reduces the slab 10. A series of the soft reduction roll pairs 6 constitute a soft reduction zone 7. The plurality of soft reduction roll pairs 6 are arranged at approximately equal intervals between an entrance 7i and an exit 7o of the soft reduction zone 7. Here, in the soft reduction zone 7, the position of the entrance 7i coincides with the position of the soft reduction roll pair 6 arranged at the most upstream position in the casting direction, and the position of the exit 7o coincides with the position of the soft reduction roll pair 6 arranged at the most downstream position in the casting direction.
[0025] The soft reduction zone 7 is divided into a plurality of segments, and each segment is provided with a reduction device (not shown) and a plurality of soft reduction roll pairs 6. In each segment, the reduction device reduces the slab 10, for example, by hydraulic pressure. The reduction amount of the soft reduction roll pairs 6 is controlled for each segment (reduction device). However, the upper limit of the force with which the reduction device can reduce the slab 10 is determined for each device. When the reaction force from the slab 10 is equal to or greater than the upper limit of the reduction force of the reduction device, the actual reduction speed is smaller than the set reduction speed. This is because, when the reaction force from the slab 10 reaches the upper limit of the reduction force of the reduction device, the reduction of the slab 10 does not proceed at that point, and the reduction gradient when the slab 10 is actually reduced is less than the set reduction gradient. Here, the set reduction speed means the product of the casting speed (m / min) set in the continuous casting machine 1 and the set reduction gradient (mm / m). The actual reduction rate means the reduction rate (mm / min) when the slab 10 is actually reduced using the reduction device of the continuous casting machine 1 .
[0026] Fig. 2 is a cross-sectional view of the continuous casting machine 1 cut along a plane perpendicular to the casting direction. Fig. 2 shows a slab 10 being reduced by a pair of soft reduction rolls 6. Referring to Fig. 2, the soft reduction roll 61 is disposed at a distance from the light reduction roll 62 in the up-down direction. The up-down direction corresponds to the thickness direction of the slab 10. The light reduction roll 61 is disposed above the slab 10, and the light reduction roll 62 is disposed below the slab 10.
[0027] At least one of the light reduction rolls of the light reduction roll pair 6 (light reduction rolls 61, 62) is a convex roll. In the example of this embodiment, the light reduction roll 61 is a convex roll, and the light reduction roll 62 is a flat roll. However, the configuration of the light reduction roll pair 6 is not limited to this. The light reduction roll 61 may be a flat roll, and the light reduction roll 62 may be a convex roll. Furthermore, both the light reduction rolls 61, 62 may be convex rolls. When both the light reduction rolls 61, 62 are convex rolls, the effect of reducing center segregation and porosity is significantly exhibited.
[0028] The soft reduction roll 61 includes a large diameter portion 611 located at the center in the width direction, two small diameter portions 612, 612 located at both ends in the width direction, and two tapered portions 613, 613 connecting the large diameter portion 611 and the small diameter portions 612, 612. The soft reduction roll 61 is typically arranged so that the center of the large diameter portion 611 in the width direction coincides with the center of the slab 10 in the width direction. The diameter of the large diameter portion 611 is larger than the diameter of the small diameter portions 612, 612. When the slab 10 is reduced using the pair of soft reduction rolls 6, the large diameter portion 611 comes into contact with the slab 10, and the small diameter portions 612, 612 and the tapered portions 613, 613 do not come into contact with the slab 10. Each of the small diameter portions 612, 612 is rotatably supported by bearings 614, 614 arranged on the outer side in the width direction.
[0029] The soft reduction roll 61 satisfies the above formula (1) when the width of the large diameter portion 611 is Wr (mm), the width of the slab 10 is Ws (mm), and the thickness of the slab 10 is D (mm). In short, the width Wr of the large diameter portion 611 is (Ws-1.15×D) or more and (Ws-1.15×D+250) or less. If the width Wr of the large diameter portion 611 is smaller than (Ws-1.15×D), the reduction near both ends of the slab 10 during soft reduction is insufficient, and the center segregation and porosity cannot be reduced in that portion. If the width Wr of the large diameter portion 611 is larger than (Ws-1.15×D+250), the both ends of the slab 10, which have a relatively low temperature, are reduced more widely by the soft reduction roll 61. Therefore, the reaction force received from the slab 10 becomes large, and there is a risk of exceeding the upper limit of the reduction force of the reduction device. As described above, when the reaction force from the slab 10 exceeds the upper limit of the rolling force, the actual rolling speed becomes smaller than the set rolling speed. Therefore, in this case, the rolling amount by the soft reduction roll pair 6 is insufficient for the solidification shrinkage of the slab 10, and center segregation and porosity cannot be reduced. For the above reasons, the width Wr of the large diameter portion 611 of the soft reduction roll 61 used in the continuous casting method according to this embodiment satisfies the above formula (1).
[0030] The shape of the light reduction roll 61 (convex roll) is not particularly limited as long as the width Wr of the large diameter portion 611 satisfies the above formula (1). For example, the large diameter portion 611 and the small diameter portions 612, 612 may be directly connected to each other without the tapered portions 613, 613. Alternatively, the large diameter portion 611 may be divided into a plurality of portions in the width direction, and a bearing may be provided between each of the large diameter portions 611.
[0031] In the light reduction roll 61 (convex roll), the difference between the diameter of the large diameter portion 611 and the diameter of the small diameter portion 612, 612 is preferably 5 mm or more and 30 mm or less. If the difference between the diameter of the large diameter portion 611 and the diameter of the small diameter portion 612, 612 is 5 mm or more, the effect of reducing center segregation and porosity is sufficiently exhibited even when the light reduction roll 61 is at the end of its life. In addition, if the difference between the diameter of the large diameter portion 611 and the diameter of the small diameter portion 612, 612 is 30 mm or less, the diameter of the small diameter portion 612, 612 is prevented from becoming extremely small, and the risk of breakage of the light reduction roll 61 can be reduced. The ratio of the diameter of the large diameter portion 611 to the diameter of the small diameter portion 612, 612 is preferably 1.017 or more and 1.150 or less.
[0032] The soft reduction roll 62 includes a main body 621 having a constant diameter in the width direction. When the slab 10 is reduced using the soft reduction roll pair 6, the main body 621 comes into contact with the slab 10. The main body 621 is rotatably supported by bearings 622, 622 arranged on the outer side in the width direction.
[0033] [Continuous casting method] Fig. 3 is a flow diagram showing the method for continuous casting of steel according to this embodiment. As shown in Fig. 3, the method for continuous casting of steel according to this embodiment includes an application step (#5) and a reduction step (#10). A slab 10 obtained by this continuous casting method becomes a material for products such as steel plate. Each step shown in Fig. 3 will be specifically described below.
[0034] [Marking process (#5)] In the application step (#5), a magnetic field is applied to the molten steel M in the mold 4 by the electromagnetic brake 4a. As a result, the molten steel M discharged from the discharge hole of the submerged entry nozzle 3 in the mold 4 receives a braking force in the direction opposite to the flow direction due to the action of the magnetic field. This weakens the flow of the molten steel M discharged from the discharge hole toward the width direction end of the solidified shell S. In addition, the electromagnetic brake 4a can promote the floating of inclusions, etc. in the molten steel M, and also plays a role in separating the inclusions, etc. from the molten steel M.
[0035] The magnitude of the magnetic flux density of the magnetic field applied in the application step (#5) is preferably 1000 Gauss or more. If the magnetic flux density is 1000 Gauss or more, a sufficient braking force acts on the molten steel M. In other words, if a magnetic field of less than 1000 Gauss is applied to the molten steel M, the braking force acting on the molten steel M is insufficient. In this case, the temperature in the vicinity of the width direction end of the slab 10 becomes high, and the completion of solidification is likely to be delayed, so that the internal quality of the slab 10 deteriorates. By applying a magnetic field of 1000 Gauss or more in the application step (#5), the thickness of the solidified shell S of the slab 10 becomes uniform in the width direction. By lightly reducing the thickness of this slab 10 in the reduction step (#10) described later, it is possible to reduce center segregation and porosity.
[0036] The magnitude of the magnetic flux density of the magnetic field is not particularly limited as long as it is 1000 Gauss or more. However, the magnetic flux density is preferably 3000 Gauss or less. If a magnetic field of more than 3000 Gauss is applied to the molten steel M, the temperature of the molten steel M in the vicinity of the submerged nozzle 3 increases, and the initial solidification of the molten steel M in the mold 4 becomes non-uniform. If the initial solidification of the molten steel M becomes non-uniform, there is a risk of vertical cracks occurring on the surface of the slab 10 when continuously casting steel that is prone to surface cracks (e.g., hypoperitectic steel).
[0037] [Reduction process (#10)] In the reduction step (#10), the slab 10 is soft reduced in the thickness direction using a plurality of soft reduction roll pairs 6 in the soft reduction zone 7. The soft reduction is performed from when the central solid fraction of the slab 10 reaches 0.3 until it reaches 1.0. That is, the central solid fraction of the slab 10 is 0.3 at the entrance 7i of the soft reduction zone 7, and is 1.0 at the exit 7o of the soft reduction zone 7. If the soft reduction is started after the central solid fraction of the slab 10 reaches 0.3, the central segregation and porosity cannot be sufficiently reduced. Similarly, if the soft reduction is terminated before the central solid fraction of the slab 10 reaches 1.0, the central segregation and porosity cannot be sufficiently reduced. In addition, even if the soft reduction is performed on the region where the central solid fraction of the slab 10 is 1.0, i.e., the region where the thickness center of the slab 10 is completely solidified, it has almost no effect on reducing the central segregation and porosity, so there is no need to soft reduce this region.
[0038] Soft reduction of the region of the slab 10 where the central solid fraction is less than 0.3 does not have any effect on reducing the central segregation and porosity formed at the final stage of solidification, so it is not necessarily required to soft reduce this region. However, soft reduction may be performed on the region of the slab 10 where the central solid fraction is less than 0.3.
[0039] In the reduction step (#10), if the actual reduction rate in the soft reduction zone 7 is less than 0.5 mm / min, the reduction amount is insufficient relative to the solidification shrinkage of the slab 10, making it impossible to reduce center segregation and porosity. On the other hand, if the reduction rate is more than 1.3 mm / min, the reduction amount becomes too large relative to the solidification shrinkage of the slab 10, causing the molten steel M to flow back from downstream to upstream in the casting direction, and the resulting flow of concentrated molten steel worsens center segregation. For this reason, the actual reduction rate of the slab 10 in the reduction step (#10) is 0.5 mm / min or more and 1.3 mm / min or less.
[0040] In the continuous casting method of this embodiment, a plurality of soft reduction roll pairs 6 are used in the reduction step (#10). In this case, compared to the case where the slab 10 is reduced using only one soft reduction roll pair 6, the slab 10 can be given a tapered gradient, and therefore the slab 10 can be gradually narrowed down due to solidification shrinkage.
[0041] [effect] In the continuous casting method of this embodiment, in the reduction step (#10), the slab 10 is soft reduced in the thickness direction using a plurality of soft reduction roll pairs 6. In the example of this embodiment, the soft reduction roll 61 of the soft reduction roll pair 6 is a convex roll in which the diameter of the center in the width direction is larger than the diameter of both ends. The soft reduction roll 61 has a shape that satisfies the above formula (1) in relation to the slab 10. In short, the width of the large diameter portion 611 of the soft reduction roll 61 is appropriately set. In the soft reduction using this soft reduction roll 61 (convex roll), the range in which the slab 10 is reduced in the width direction is optimized, and both ends of the slab 10, which have a relatively low temperature, are not reduced much. Therefore, the reduction force required for reducing the slab 10 is suppressed, and center segregation and porosity can be reduced without increasing the size of the equipment or the rigidity of the soft reduction roll.
[0042] Moreover, in the continuous casting method of this embodiment, intentional bulging of the slab 10 is not performed. Furthermore, since there is no need to increase the rigidity of the soft reduction rolls 61, 62, there is no need to increase the diameter of the soft reduction rolls 61, 62. Therefore, bulging is less likely to occur between the pair of soft reduction rolls 6. As described above, the continuous casting method of this embodiment suppresses internal cracking of the slab 10. EXAMPLES
[0043] In order to confirm the effect of the continuous casting method according to the embodiment, the following tests were carried out and the results were evaluated. Specifically, the Mn segregation degree and porosity volume of the cast piece obtained by the continuous casting were evaluated. The Mn segregation degree and porosity volume will be described later.
[0044] In this test, a slab was produced using the continuous casting machine shown in Figure 1. The mold was a copper water-cooled mold. The length of the mold was 800 mm. The cross section of the mold was rectangular. The soft reduction zone was provided 16 m from the meniscus (the molten metal surface in the mold). The slab was soft reduced in the thickness direction at a set reduction rate of 0.8 mm / min using a pair of soft reduction rolls from when the central solid fraction of the slab reached 0.3 until it reached 1.0. No soft reduction was performed in the region after the central solid fraction of the slab reached 1.0.
[0045] In the soft reduction zone, only the upper soft reduction roll was a convex roll. The diameter of the large diameter part of the convex roll was 15 mm larger than the diameter of the small diameter part. The specific water amount of the cooling water sprayed from the nozzle for secondary cooling was 0.7 to 1.5 L / kg-steel depending on the thickness of the slab and the casting speed.
[0046] The main chemical composition of the slab used in this test was C: 0.15%, Si: 0.19%, Mn: 0.90%, P: 0.011%, and S: 0.003%.
[0047] The central temperature and solid fraction of the slab were calculated by two-dimensional solidification analysis in the thickness and width directions of the slab. However, the actual reduction speed during soft reduction may vary depending on the capacity of the reduction device and the reaction force from the slab. Therefore, the position of the reduction device in the thickness direction of the slab was recorded, and the actual reduction speed was calculated based on this. The upper limit of the reduction force of the reduction device was set to 600 tons, taking into account the rigidity of the segments and rolls.
[0048] The degree of Mn segregation in the slab was investigated by the following procedure. The cast slab was cut at the center in the width direction, and a sample was taken from the center in the thickness direction of the cut surface, including an area of 40 mm in the casting direction and 40 mm in the thickness direction. A surface analysis of the Mn concentration was performed on this sample using an EPMA (Electron Probe Micro Analyzer). The Mn concentration was integrated over a 2 mm width along the casting direction, centered on the position with the highest Mn concentration, and the average value was taken as the maximum Mn concentration (Cmax). The value (Cmax / C0) obtained by dividing the maximum Mn concentration (Cmax) by the Mn concentration (C0) in the bulk composition of the slab was taken as the degree of Mn segregation. The Mn concentration (C0) in the bulk composition was determined by chemical analysis of an analysis sample taken from the slab.
[0049] The porosity volume of the slab was investigated using the following procedure. Samples were taken from the center of the slab in the thickness direction, measuring 50 mm in the casting direction, 100 mm in the width direction, and 7 mm in the thickness direction. Samples were taken from 16 locations along the width direction of the slab. The density ρ of each sample was measured using the method for measuring density and specific gravity of solids specified in JIS Z 8807. Samples were also taken from the 1 / 4 thickness portion of the slab in the same manner as above, and the density ρ was measured using the same method as for density ρ. 0 The porosity volume per unit weight, V (cm), was then calculated using the following formula (2): 3 The maximum porosity volume V among the porosity volumes V measured for each sample was taken as the porosity volume V of the slab.
[0050]
number
[0051] The test conditions and test results of this embodiment are shown in Table 1. In Table 1, the test conditions include the thickness of the slab produced by continuous casting, the width of the slab, the width of the large diameter part of the soft reduction roll, the magnetic flux density of the magnetic field of the electromagnetic brake, the actual reduction speed, and the central solid fraction at the entrance of the soft reduction zone. The magnetic flux density is the magnetic flux density of the magnetic field applied to the molten steel in the mold by the electromagnetic brake. In Table 1, the slab produced under the test conditions that satisfy the following condition 1 is represented as an invention example, and the slab produced under the test conditions that do not satisfy condition 1 is represented as a comparative example. In Comparative Examples 1 to 4 shown in Table 1, the test conditions that do not satisfy condition 1 are marked with a "*". In addition, among the invention examples 1 to 7 and Comparative Examples 1 to 4 shown in Table 1, the surface temperatures that do not satisfy the following condition 2 are marked with a "#". Condition 1: The width of the large diameter part of the soft reduction roll (convex roll) satisfies the above formula (1), and the actual reduction speed is 0.5 mm / min or more and 1.3 mm / min or less, and the central solid fraction of the slab at the entrance of the soft reduction zone is 0.3 or less. Condition 2: The magnetic flux density is 1000 Gauss or more.
[0052] [Table 1]
[0053] It is known that if the Mn segregation ratio of the obtained slab is 1.4 or less, toughness can be ensured in the product (steel plate) after rolling the slab. Therefore, in Table 1, the test results are shown as "Excellent" if the Mn segregation ratio is 1.4 or less, and "Fail" if it is not. In addition, if the porosity volume is 4.0 cm3 or less, 3 / g or less, defects are known to be rendered harmless in the product (steel plate) after rolling the slab. 3 If it was less than / g, it was marked as "excellent", otherwise it was marked as "unacceptable".
[0054] As shown in Table 1, all of Examples 1 to 6 satisfied Condition 1 and Condition 2. Therefore, in Examples 1 to 6, slab cast pieces with good Mn segregation and porosity volume were obtained. In other words, center segregation and porosity were reduced.
[0055] Although Example 7 satisfied condition 1, the magnetic flux density was less than 1000 Gauss and did not satisfy condition 2. In Example 7, the Mn segregation degree and porosity volume were somewhat higher than those of Example 1, which had the same test conditions except for the magnetic flux density, but were below the thresholds, and a good cast slab was obtained. In other words, in Example 7, the center segregation and porosity could be reduced.
[0056] In Comparative Example 1, the width of the large diameter portion did not satisfy the above formula (1). Therefore, Comparative Example 1 did not satisfy Condition 1. In this case, the Mn segregation degree was greater than the threshold value, and the evaluation was "unacceptable."
[0057] In Comparative Example 2, the width of the large diameter portion did not satisfy the above formula (1), and the actual rolling reduction rate was less than 0.5 mm / min. Therefore, Comparative Example 2 did not satisfy Condition 1. In this case, both the Mn segregation degree and the porosity volume were larger than the threshold value, and the evaluation was "fail."
[0058] In Comparative Example 3, similarly to Comparative Example 2, the width of the large diameter portion did not satisfy the above formula (1), and the actual rolling reduction rate was less than 0.5 mm / min. Therefore, Comparative Example 3 did not satisfy Condition 1. Furthermore, in Comparative Example 3, a magnetic field was not applied to the molten steel in the mold. Therefore, Comparative Example 3 did not satisfy Condition 2 either. In this case, both the Mn segregation degree and the porosity volume were deteriorated compared to the results of Comparative Example 2, and the evaluation was "unacceptable."
[0059] In Comparative Example 4, the central solid fraction of the slab at the entrance of the soft reduction zone was greater than 0.3, which did not satisfy Condition 1. In this case, in Comparative Example 4, the Mn segregation degree was greater than the threshold value, and the evaluation was "unacceptable."
[0060] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure. [Explanation of symbols]
[0061] 1: Continuous casting machine 4: Mold 4a: Electromagnetic brake 6: Light reduction roll pair 61, 62: Light reduction roll 10: Casting
Claims
1. A method for continuously casting steel using a continuous casting machine having a plurality of pairs of soft reduction rolls arranged in a casting direction of a slab, comprising the steps of: At least one of the soft reduction rolls in the pair of soft reduction rolls has a diameter at a widthwise center portion larger than the diameters at both ends, and satisfies the following formula (1), where the width of the widthwise center portion is Wr (mm), the width of the slab is Ws (mm), and the thickness of the slab is D (mm): The continuous casting method includes: The continuous casting method includes a reduction step of softly reducing the slab in a thickness direction at a reduction speed of 0.5 mm / min or more and 1.3 mm / min or less using the plurality of pairs of soft reduction rolls from when the central solid fraction of the slab reaches 0.3 until when the central solid fraction of the slab reaches 1.
0. Ws-1.15×D≦Wr≦Ws-1.15×D+250 (1)
2. The continuous casting method according to claim 1, The continuous casting machine includes a mold including an electromagnetic brake; The continuous casting method further includes an application step of applying a magnetic field having a magnetic flux density of 1000 Gauss or more to the molten steel in the mold by the electromagnetic brake.
Citation Information
Patent Citations
Method for reducing center segregation of continuous cast slab
JP2001138021A
Method for producing continuously cast slab
JP2010082638A
Continuous casting method for steel
JP2010274299A
Continuous casting method and continuous casting apparatus of steel
JP2012066302A
Method for manufacturing continuously cast slab
JP2012218047A