Aqueous coating material
The aqueous coating material with a specific acrylic silicone resin emulsion and solvent combination addresses curability and weather resistance issues, ensuring crack resistance and longevity of coatings on buildings and structures.
Patent Information
- Application Number
- JP2023054927
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional water-based coating materials used for buildings and civil engineering structures face issues with room temperature curability, leading to potential cracks and insufficient weather resistance due to the interaction of acrylic silicone resin emulsions with pigments and pigment dispersants.
An aqueous coating material comprising an acrylic silicone resin emulsion with a residual silica content of 1 to 40% by weight and a glass transition temperature of 15°C or less, combined with a pigment, pigment dispersant, and specific ether or ester solvents, which enhances crack resistance and weather resistance.
The coating material exhibits excellent room temperature curability, crack resistance, and weather resistance, while reducing the amount of organic components derived from petroleum, contributing to carbonization and extending the lifespan of coated objects.
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel water-based coating material. [Background technology]
[0002] Conventionally, surface finishing with coating materials has been applied to buildings, civil engineering structures, etc. Such coating materials are required to exhibit excellent performance in terms of weather resistance, since they impart aesthetic appearance with various colors, gloss, etc., and also play a role in protecting the substrate from wind, rain, direct sunlight, etc. In recent years, in consideration of non-pollution and safety, water-based coating materials using resin emulsion as a binder have been increasingly used.
[0003] As one of the means for improving the weather resistance of water-based coating materials, it is known to use an acrylic silicone resin emulsion as a binder. For example, Patent Document 1 (JP Patent Publication 8-12930 A) describes a water-based coating material that contains a resin emulsion having a specific silicon content, acid value, and hydroxyl value, its crosslinking agent, and a pigment, etc.
[0004] Incidentally, water-based coating materials applied to buildings, civil engineering structures, and the like are required to have the ability to form and harden a film (room temperature curing ability) in a temperature range of about 5 to 40° C., since painting is performed outdoors. However, the above-mentioned patent documents do not sufficiently consider room temperature curing ability, and when painting is performed at room temperature, there is a risk that cracks will occur in the coating film or the weather resistance of the coating film will be insufficient. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-12930 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above-mentioned problems, and aims to provide an aqueous coating material which has excellent room temperature curing properties and exhibits excellent performance in terms of crack resistance, weather resistance, etc. [Means for solving the problem]
[0007] As a result of intensive research into achieving the above object, the inventors of the present invention came up with the idea of an aqueous coating material containing an acrylic silicone resin emulsion having a specific silica residual ratio and glass transition temperature, a pigment, a pigment dispersant, and a specific solvent, and completed the present invention.
[0008] That is, the present invention has the following features. 1. An aqueous coating material containing a resin emulsion, The present invention comprises an acrylic silicone resin emulsion (A) having a silica residual ratio of 1 to 40% by weight in the resin solid content and a glass transition temperature of 15°C or lower, a pigment (B), a pigment dispersant (C), and an ether or ester solvent (D), The ether or ester solvent (D) is An aqueous coating material comprising an ether or ester solvent (D1) having a water solubility of more than 1 g / 100 g H2O, and / or an ether or ester solvent (D2) having a water solubility of 1 g / 100 g H2O or less. Effect of the Invention
[0009] The aqueous coating material of the present invention has excellent room temperature curing properties and exhibits excellent performance in terms of crack resistance, weather resistance, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described.
[0011] The aqueous coating material of the present invention is an aqueous coating material that forms a colored coating film, and is characterized by comprising an acrylic silicone resin emulsion (A) having a silica residual ratio of 1 to 40% by weight in the resin solid content and a glass transition temperature of 15°C or lower, a pigment (B), a pigment dispersant (C), and an ether or ester solvent (D).
[0012] In general, resin emulsions can be cured at room temperature by setting the glass transition temperature (hereinafter also referred to as "Tg") below room temperature. Acrylic silicone resin emulsions can also be cured at room temperature by setting the glass transition temperature below room temperature. In such cases, it is not necessary to mix a solvent that can act as a film-forming assistant.
[0013] However, in water-based coating materials that use an acrylic silicone resin emulsion containing a large amount of silicone as a binder and further mix pigments and pigment dispersants, even if the glass transition temperature of the resin is set low, problems such as cracks in the coating film and insufficient weather resistance of the coating film are likely to occur. Such problems are thought to be caused by the pigment dispersant excessively promoting the reaction of the silicone component.
[0014] In the present invention, in addition to the above components, a specific solvent is an essential component in such an aqueous coating material. The aqueous coating material of the present invention having such a specific configuration can exhibit excellent performance in terms of crack resistance, weather resistance, etc. In addition, since the aqueous coating material of the present invention can exhibit stable performance while using a binder containing a high proportion of silicon components, it is possible to relatively reduce organic components derived from petroleum, which can also contribute to decarbonization. Furthermore, the aqueous coating material of the present invention can extend the life of the coated object due to its excellent weather resistance, and it is possible to reduce the number of maintenance times in total, and from this perspective, it can also contribute to decarbonization, etc.
[0015] The aqueous coating material of the present invention uses an acrylic silicone resin emulsion (A) (hereinafter referred to as "component (A)") as a binder, the acrylic silicone resin emulsion having a silica residual ratio of 1 to 40% by weight in the resin solid content and a glass transition temperature of 15°C or lower.
[0016] As such an (A) component, a monomer component constituting the resin may contain an alkyl (meth)acrylate ester and an alkoxysilane compound. In the present invention, alkyl acrylate ester and alkyl methacrylate ester are collectively referred to as alkyl (meth)acrylate ester. In the present invention, "α to β" is synonymous with "α or more and β or less."
[0017] Examples of the (meth)acrylic acid alkyl ester include rigid (meth)acrylic acid alkyl esters having a homopolymer Tg of 50° C. or higher, such as methyl methacrylate (Tg: 105° C.), ethyl methacrylate (Tg: 65° C.), tert-butyl methacrylate (Tg: 107° C.), iso-butyl methacrylate (Tg: 53° C.), iso-propyl methacrylate (Tg: 81° C.), cyclohexyl methacrylate (Tg: 83° C.), isobornyl acrylate (Tg: 94° C.), isobornyl methacrylate (Tg: 155° C.), dicyclopentanyl acrylate (Tg: 120° C.), dicyclopentanyl methacrylate (Tg: 175° C.), and dicyclopentenyl acrylate (Tg: 120° C.); Methyl acrylate (Tg: 8°C), ethyl acrylate (Tg: -20°C), propyl acrylate (Tg: 3°C), propyl methacrylate (Tg: 35°C), iso-propyl acrylate (Tg: -3°C), n-butyl acrylate (Tg: -54°C), n-butyl methacrylate (Tg: 20°C), isobutyl acrylate (Tg: -26°C), tert-butyl acrylate (Tg: 43°C), isobutyl methacrylate (Tg: 48°C), isoamyl acrylate (Tg: -45°C), 2-ethylhexyl acrylate (Tg: -70°C), 2-ethylhexyl methacrylate (Tg: -10°C), octyl acrylate (Tg: -65°C), soft (meth)acrylic acid alkyl esters having homopolymer Tg of less than 50°C, such as iso-octyl methacrylate (Tg: -45°C), iso-octyl acrylate (Tg: -70°C), cyclohexyl acrylate (Tg: 15°C), lauryl acrylate (Tg: 10°C), lauryl methacrylate (Tg: -65°C), stearyl acrylate (Tg: 35°C), hexadecyl acrylate (Tg: 35°C), hexadecyl methacrylate (Tg: 15°C), hexyl acrylate (Tg: -57°C), hexyl methacrylate (Tg: -5°C), tetradecyl acrylate (Tg: 24°C), and tetradecyl methacrylate (Tg: -72°C); These can be used alone or in combination of two or more.
[0018] Examples of the alkoxysilane compound include polymerizable unsaturated double bond-containing silane coupling agents such as γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltriisopropoxysilane; Epoxy group-containing silane coupling agents such as γ-glycidoxymethacryloxypropyltrimethoxysilane, γ-glycidoxymethacryloxypropylmethyldimethoxysilane, γ-glycidoxymethacryloxypropyltriethoxysilane, γ-glycidoxymethacryloxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as N-2(aminoethyl)3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropylmethyldimethoxysilane, N-2(aminoethyl)3-aminopropyltriethoxysilane, N-2(aminoethyl)3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; mercapto group-containing silane coupling agents such as γ-mercaptopropyltrimethoxysilane; ureido group-containing silane coupling agents such as 3-ureidopropyltriethoxysilane; chloroalkyl group-containing silane coupling agents such as 3-chloropropyltrimethoxysilane; sulfide group-containing silane coupling agents such as bis(triethoxysilylpropyl)tetrasulfide; isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane; Silane coupling agents (i) such as
[0019] tetrafunctional alkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-t-butoxysilane, and tetraacetoxysilane; Methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltributoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrippropoxysilane, ethyltributoxysilane, propyltrimethoxysilane, propyltriethoxysilane, propyltrippropoxysilane, propyltributoxysilane, butyltrimethoxysilane, butyltriethoxysilane, butyltrippropoxysilane, butyltributoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, phenyltributoxysilane, methyltriacetoxysilane, phenyltriacetoxysilane, alkylalkoxysilanes such as dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldipropoxysilane, dimethyldibutoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diethyldipropoxysilane, diethyldibutoxysilane, dipropyldimethoxysilane, dipropyldiethoxysilane, dibutyldimethoxysilane, dibutyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, diphenyldibutoxysilane, dimethoxymethylphenylsilane, methylphenyldiethoxysilane, cyclohexylmethyldimethoxysilane, dimethyldiacetoxysilane, and diphenyldiacetoxysilane; or alkoxysilane-modified products obtained by modifying at least a portion of the alkoxyl groups of these tetrafunctional alkoxysilanes or alkylalkoxysilanes with a polyoxyalkylene group-containing compound, a fluorine-containing compound, or the like; These can be used alone or in combination of two or more.
[0020] The component (A) may contain a monomer (another monomer) other than the above-mentioned as a resin constituent component. Examples of such other monomers include: Carboxyl group-containing monomers such as acrylic acid (Tg: 106°C), methacrylic acid (Tg: 185°C), itaconic acid (Tg: 100°C), and maleic acid (Tg: 130°C); Aromatic monomers such as styrene (Tg: 100°C) and α-methylstyrene (Tg: 168°C); Carbonyl group-containing monomers such as acrolein (Tg: 60°C) and diacetone acrylamide (Tg: 65°C); Hydroxyl group-containing monomers such as 2-hydroxyethyl acrylate (Tg: -15°C), 2-hydroxyethyl methacrylate (Tg: 55°C), 2-hydroxybutyl acrylate (Tg: -7°C), 2-hydroxybutyl methacrylate (Tg: 26°C), and 4-hydroxybutyl acrylate (Tg: -80°C); Amino group-containing monomers such as N,N-dimethylaminoethyl acrylate (Tg: 18°C), N,N-dimethylaminoethyl methacrylate (Tg: 18°C), and N,N-diethylaminoethyl methacrylate (Tg: 20°C); Amide group-containing monomers such as acrylamide (Tg: 179°C) and N,N-dimethylaminopropylacrylamide (Tg: 134°C); Nitrile group-containing monomers such as acrylonitrile (Tg: 125°C); Epoxy group-containing monomers such as glycidyl methacrylate (Tg: 46°C); 2-Isopropenyl-2-oxazoline (Tg: 100°C) oxazoline group-containing monomer; UV absorbers containing ethylenically unsaturated double bonds, such as 2-[2'-hydroxy-5'-methacryloyloxyethylphenyl]-2H-benzotriazole (Tg: 100°C); Ethylenically unsaturated double bond-containing light stabilizers such as 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine (Tg: 130°C); Other examples include sulfonic acid-containing vinyl monomers, acid anhydrides, chlorine-containing monomers, fluorine-containing monomers, alkylene glycol monoallyl ethers, vinyl acetate, vinyl propionate, vinyl ethers, ethylene, propylene, isobutylene, etc. These can be used alone or in combination of two or more.
[0021] In the present invention, a monomer obtained from a biological resource, i.e., a biomass-based monomer, can be used as the monomer constituting component (A). By introducing such a biomass-based monomer, the biomass content of component (A) and thus the aqueous coating material can be increased, and the amount of petroleum-derived compounds used can be reduced. The use of such materials can also contribute to decarbonization. As the biomass-based monomer, for example, a monomer produced using alcohol, organic acid, hydrocarbon, etc. derived from a biological source can be used.
[0022] The component (A) can be produced by polymerizing a group of monomers including the above-mentioned resin constituents. Any known method may be used as the polymerization method, and in addition to normal emulsion polymerization, soap-free emulsion polymerization, feed emulsion polymerization, seed emulsion polymerization, multi-stage emulsion polymerization, etc. can also be used. In multi-stage emulsion polymerization, the component (A) can be produced by a two-stage or three-stage or more emulsion polymerization method, etc. When polymerizing the component (A), for example, an emulsifier, an initiator, a dispersant, a polymerization inhibitor, a polymerization retarder, a buffer, a chain transfer agent, a pH adjuster, etc. can be used.
[0023] As the emulsifier, various surfactants that can be used in emulsion polymerization can be used, and these may be reactive types (reactive surfactants) having polymerizable unsaturated double bonds. As the emulsifier, for example, anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc. can be used alone or in combination.
[0024] In the present invention, the (A) component has a silica residual ratio in the resin solid content of 1 to 40% by weight, preferably 5 to 35% by weight, and more preferably 10 to 30% by weight. By having the (A) component have a silica residual ratio within the above range, the component contains a large amount of silicon, and can exhibit excellent weather resistance while ensuring physical properties such as crack resistance. If the silica residual ratio is below the lower limit, it becomes difficult to obtain sufficient physical properties such as weather resistance, and if the silica residual ratio is above the upper limit, the crack resistance, etc. becomes insufficient, and weather resistance is also likely to be disadvantageous.
[0025] The residual silica ratio is the weight ratio of silica (SiO2) that remains when a component with Si-O bonds is baked at 900°C. In general, alkoxysilanes react with water to undergo a hydrolysis reaction to become silanols, which then undergo condensation reactions between silanols or between silanols and alkoxy. When this reaction is carried to its ultimate state, it becomes silica (SiO2). These reactions are expressed by the general formula: RO(Si(OR)2O) n R+(n+1)H2O→nSiO2+(2n+2)ROH The silica remaining ratio is calculated based on this reaction formula and is the amount of silica remaining.
[0026] In the (A) component, the type and ratio of the alkoxysilane compound in the resin constituents can be set so as to satisfy the above-mentioned silica residual ratio. As for the alkoxysilane compound in the (A) component, for example, (1) an embodiment containing a silane coupling agent (i), (2) an embodiment containing an alkoxysilane (ii), and (3) an embodiment containing a silane coupling agent (i) and an alkoxysilane (ii), etc., can be mentioned. Among these, the above-mentioned (2) or (3) embodiment is preferable in terms of increasing the ratio of the silicon component, etc.
[0027] The glass transition temperature (Tg) of the component (A) is 15°C or less, preferably -50 to 10°C, more preferably -40 to 5°C, further preferably -35 to 0°C, and particularly preferably -30 to -5°C. The Tg of the component (A) within the above range is suitable in terms of crack resistance, weather resistance, stain resistance, and the like. If the Tg exceeds the above upper limit, it becomes difficult to obtain sufficient physical properties such as crack resistance. The glass transition temperature can be calculated by the Fox formula. However, in the calculation of the glass transition temperature of the present invention, alkoxysilane compounds are excluded.
[0028] In the (A) component, the type and ratio of monomers such as (meth)acrylic acid alkyl esters in the resin constituents can be set so as to satisfy the above glass transition temperature. As the (meth)acrylic acid alkyl esters, it is preferable to use the above-mentioned hard (meth)acrylic acid alkyl esters and soft (meth)acrylic acid alkyl esters. According to such an embodiment, it is easy to set the Tg of the resin within the above range, which is also advantageous in terms of weather resistance, strength, etc. of the coating film.
[0029] The average particle size of the component (A) is preferably 300 nm or less, more preferably 20 to 250 nm, and even more preferably 50 to 200 nm. The average particle size referred to here is a value measured by dynamic light scattering.
[0030] Pigment (B) (hereinafter also referred to as "component (B)") is a component that contributes to at least one of color development, hiding power, gloss, aesthetics, strength, etc. As component (B), for example, color pigment (B1) (hereinafter also referred to as "component (B1)"), extender pigment (B2) (hereinafter also referred to as "component (B2)"), etc. can be used.
[0031] Examples of the color pigment (B1) include titanium oxide, zinc oxide, carbon black, graphite, black iron oxide, iron-manganese composite oxide, iron-copper-manganese composite oxide, iron-chromium composite oxide, iron-chromium-cobalt composite oxide, copper-chromium composite oxide, copper-manganese-chromium composite oxide, copper-magnesium composite oxide, bismuth-manganese composite oxide, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum pigments, and pearl pigments. These can be used alone or in combination of two or more. The average particle size of the component (B1) is preferably 2 μm or less, more preferably 0.01 to 1 μm. The average particle size of the pigment (B) is a value measured by a laser diffraction particle size distribution measuring device.
[0032] The content of component (B1) is preferably 250 parts by weight or less, more preferably 5 to 200 parts by weight, and even more preferably 10 to 150 parts by weight, per 100 parts by weight of the solid content of component (A). If the content of component (B1) is within this range, it is suitable in terms of the color development, hiding power, aesthetics, etc. of the coating film, and is also advantageous in terms of the manifestation of the effects of the present invention.
[0033] Examples of the extender pigment (B2) include heavy calcium carbonate, light calcium carbonate, kaolin, clay, aluminum silicate, calcined clay, calcined kaolin, china clay, diatomaceous earth, hydrous silicic acid, silica gel, zeolite, sodium sulfate, allophane, talc, mica, barite powder, barium sulfate, precipitated barium sulfate, barium carbonate, magnesium carbonate, silica powder, aluminum hydroxide, porous calcium carbonate, siliceous shale, vermiculite, perlite, Oya stone powder, activated clay, activated carbon, and shirasu balloon. These can be used alone or in combination. The average particle size of the extender pigment is preferably 0.1 to 100 μm, more preferably 0.3 to 50 μm.
[0034] The content of component (B2) is preferably 400 parts by weight or less, more preferably 10 to 350 parts by weight, and even more preferably 20 to 300 parts by weight, per 100 parts by weight of the solid content of component (A). If the content of component (B2) is within this range, it is suitable in terms of the strength and aesthetics of the coating film, and is also advantageous in terms of the manifestation of the effects of the present invention.
[0035] The pigment dispersant (C) (hereinafter also referred to as "component (C)") is a component that contributes to stabilizing the dispersion of component (B) and achieving performance development.
[0036] As the component (C), one or more commercially available or known products can be used. For example, those having a resin skeleton of a styrene-maleic acid copolymer resin, a polyurethane resin, a polyester resin, an acrylic resin, etc. can be used.
[0037] In the present invention, a pigment dispersant having an acid group and / or a basic group is suitable as component (C). Such a pigment dispersant can improve the dispersion stability of component (B). Moreover, in the present invention, even when such a pigment dispersant is used, excellent performance can be exhibited in terms of crack resistance, weather resistance, etc.
[0038] Examples of the acid group include a carboxy group, a sulfonic acid group, and a phosphoric acid group. Examples of the basic group include a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt group. The component (C) may have one or more of these acid groups or basic groups. Suitable examples of the component (C) include polycarboxylic acid type dispersants such as polyacrylic acid, polymethacrylic acid, and styrene-maleic acid copolymer resins; sulfonic acid type dispersants such as lignin sulfonic acid and naphthalene sulfonic acid; and polymer dispersants having an acid value and / or an amine value.
[0039] The content of the component (C) is preferably 0.01 to 20 parts by weight, and more preferably 0.1 to 10 parts by weight, calculated as solid content, per 100 parts by weight of the solid content of the component (A).
[0040] In addition to the above components, the aqueous coating material of the present invention contains an ether or ester solvent (D) (hereinafter also referred to as "component (D)"). Of the components (D), the ether solvent is a solvent having an ether bond in the molecule, and the ester solvent is a solvent having an ester bond in the molecule. By containing such a component (D), the aqueous coating material of the present invention can exhibit excellent performance in terms of crack resistance, weather resistance, etc. In the present invention, it is particularly desirable to use an ether or ester solvent (D1) (hereinafter also referred to as "component (D1)") having a solubility in water of more than 1 g / 100 gH2O in combination with an ether or ester solvent (D2) (hereinafter also referred to as "component (D2)") having a solubility in water of 1 g / 100 gH2O or less. This is more suitable in terms of the manifestation of the effects of the present invention, and when the aqueous coating material is of a glossy type, it is also possible to increase the gloss, etc. In addition, the solubility in water in the present invention refers to the maximum mass (g) that can be dissolved in 100 g of water. The measurement temperature is 20°C.
[0041] As the component (D1), an ether solvent or an ester solvent having a solubility in water within the above range can be used. Specific examples of the compound include: Ethylene glycol monomethyl ether (solubility in water is infinite, boiling point is 125°C), Ethylene glycol monoethyl ether (solubility in water is infinite, boiling point is 135°C), Ethylene glycol monopropyl ether (solubility in water is infinite, boiling point is 150°C), Ethylene glycol monoisopropyl ether (solubility in water is infinite, boiling point is 143°C), Ethylene glycol monobutyl ether (solubility in water is infinite, boiling point is 171°C), Ethylene glycol monoisobutyl ether (solubility in water is infinite, boiling point is 161°C), Ethylene glycol mono-tertiary butyl ether (solubility in water is infinite, boiling point is 153°C), Ethylene glycol monomethyl ether acetate (solubility in water is infinite, boiling point is 145°C), Ethylene glycol monoethyl ether acetate (solubility in water is infinite, boiling point is 156°C), Ethylene glycol dimethyl ether (solubility in water is infinite, boiling point is 85°C), Diethylene glycol monomethyl ether (solubility in water is infinite, boiling point is 194°C), Diethylene glycol monoethyl ether (solubility in water is infinite, boiling point is 202°C), Diethylene glycol monobutyl ether (solubility in water is infinite, boiling point is 230°C), Diethylene glycol monoisobutyl ether (solubility in water is infinite, boiling point is 220°C), Diethylene glycol monoethyl ether acetate (solubility in water is infinite, boiling point is 217°C), Diethylene glycol dimethyl ether (solubility in water is infinite, boiling point is 162°C), Diethylene glycol diethyl ether (solubility in water is infinite, boiling point is 189°C), Triethylene glycol monomethyl ether (solubility in water is infinite, boiling point is 249°C), Triethylene glycol monobutyl ether (solubility in water is infinite, boiling point is 271°C), Triethylene glycol monoethyl ether (solubility in water is infinite, boiling point is 255°C), Propylene glycol monomethyl ether (solubility in water is infinite, boiling point is 120°C), Propylene glycol monoethyl ether (solubility in water is infinite, boiling point is 133°C), Propylene glycol monopropyl ether (solubility in water is infinite, boiling point is 150℃), Dipropylene glycol monomethyl ether (solubility in water is infinite, boiling point is 190°C), Tripropylene glycol monomethyl ether (solubility in water is infinite, boiling point is 242°C), Butylene glycol monomethyl ether (solubility in water is infinite, boiling point is 161°C), Dipropylene glycol dimethyl ether (solubility in water 53g / 100gH2O, boiling point 175℃), Ethylene glycol monoethyl ether acetate (solubility in water 23g / 100gH2O, boiling point 156℃), Ethylene glycol diethyl ether (solubility in water 20g / 100gH2O, boiling point 121℃), Dipropylene glycol monomethyl ether acetate (solubility in water 19g / 100gH2O, boiling point 209℃), Dipropylene glycol monopropyl ether (solubility in water 19g / 100gH2O, boiling point 212℃), Propylene glycol monomethyl ether acetate (solubility in water 16g / 100gH2O, boiling point 146℃), Propylene glycol diacetate (solubility in water 8g / 100gH2O, boiling point 161℃), Diethylene glycol monobutyl ether acetate (solubility in water 6.5g / 100gH2O, boiling point 247℃), Propylene glycol monobutyl ether (solubility in water 6g / 100gH2O, boiling point 170℃), Dipropylene glycol monobutyl ether (solubility in water 5g / 100gH2O, boiling point 229℃), Diethylene glycol monophenyl ether (solubility in water 3.4g / 100gH2O, boiling point 283℃), Tripropylene glycol monobutyl ether (solubility in water 3g / 100gH2O, boiling point 274℃), Ethylene glycol monophenyl ether (solubility in water 2.7g / 100gH2O, boiling point 245℃), Ethylene glycol monophenyl ether (solubility in water 2.6g / 100gH2O, boiling point 245℃), Diethylene glycol monohexyl ether (solubility in water 1.7g / 100gH2O, boiling point 258℃), Ethylene glycol monobutyl ether acetate (solubility in water 1.1g / 100gH2O, boiling point 188℃), These can be used alone or in combination of two or more.
[0042] The solubility of the component (D1) in water is more than 1 g / 100 gH2O, preferably 2 g / 100 gH2O or more, more preferably 5 g / 100 gH2O or more, even more preferably 10 g / 100 gH2O or more, and particularly preferably ∞. The boiling point of the component (D1) is preferably 150°C or more, more preferably 200°C or more, and even more preferably 220°C or more. The component (D1) that satisfies such physical property values is suitable in terms of manifesting the effects of the present invention.
[0043] As the component (D2), an ether solvent or an ester solvent having a solubility in water within the above range can be used. Specific examples of the compound include: Propylene glycol phenyl ether (solubility in water 1g / 100gH2O, boiling point 243℃), Ethylene glycol monohexyl ether (solubility in water 0.99g / 100gH2O, boiling point 208℃), Diethylene glycol dibutyl ether (solubility in water 0.3g / 100gH2O, boiling point 255℃), Diethylene glycol mono 2-ethylhexyl ether (solubility in water 0.3g / 100gH2O, boiling point 272℃), Ethylene glycol mono 2-ethylhexyl ether (solubility in water 0.2g / 100gH2O, boiling point 229℃), Ethylene glycol dibutyl ether (solubility in water 0.2g / 100gH2O, boiling point 203℃), 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (solubility in water 0.09g / 100gH2O, boiling point 255℃), 2,2,4-trimethyl-1,3-pentanediol diisobutyrate (solubility in water 0.04g / 100gH2O, boiling point 282℃) These can be used alone or in combination of two or more.
[0044] The solubility of component (D2) in water is less than 1 g / 100 g H2O, preferably 0.5 g / 100 g H2O or less, more preferably 0.1 g / 100 g H2O or less. The boiling point of component (D2) is preferably 200° C. or more, more preferably 220° C. or more, and even more preferably 250° C. or more. Component (D2) that satisfies such physical property values is suitable in terms of manifesting the effects of the present invention.
[0045] The content of the (D1) component is preferably 0.5 to 30 parts by weight, more preferably 1 to 20 parts by weight, based on 100 parts by weight of the solid content of the (A) component. The content of the (D2) component is preferably 1 to 40 parts by weight, more preferably 2 to 30 parts by weight, based on 100 parts by weight of the solid content of the (A) component. If the contents of the (D1) and (D2) components are within these ranges, the composition can exhibit even more excellent performance in room temperature curing properties, cracking resistance, weather resistance, and the like.
[0046] In the present invention, when both the (D1) component and the (D2) component are used, the weight ratio of the (D) component to the (D2) component ((D1):(D2)) is preferably 10:90 to 80:20, more preferably 15:85 to 60:40, and further preferably 20:80 to 45:55. In the present invention, by using both components in such a ratio, the above-mentioned effects can be sufficiently enhanced.
[0047] In addition to the above-mentioned components, various additives can be mixed into the aqueous coating material of the present invention. Examples of such additives include viscosity regulators, leveling agents, coupling agents, wetting agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, antifoaming agents, adsorbents, deodorizers, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, crosslinking agents, solvents, and water. These can be used alone or in combination as needed.
[0048] The aqueous coating material of the present invention can be produced by uniformly mixing the above-mentioned components (A) to (D) and, if necessary, various additives, by a conventional method.
[0049] The aqueous coating material of the present invention can be preferably applied to surface finishing of the coated surface of buildings, civil engineering structures, etc. Examples of the substrate constituting the coated surface include concrete, mortar, porcelain tile, fiber-mixed cement board, cement calcium silicate board, slag cement perlite board, cement board, ALC board, siding board, gypsum board, plywood, extrusion molding board, steel plate, plastic plate, etc. The surface of these substrates may be subjected to some surface treatment (e.g., treatment with putty, sealer, surfacer, filler, etc.), or may be one on which a coating film has already been formed (e.g., one with an old coating film).
[0050] When applying the coating material of the present invention, various application tools can be used, such as a spray, roller, brush, etc. Among these, as the roller, for example, a fibrous roller with short, medium or long hair (wool roller, etc.) can be used.
[0051] When applying, it is possible to dilute the coating material with water. The amount of water to be mixed may be appropriately determined taking into consideration the type of coating equipment, the condition of the surface to be coated, the temperature during application, etc., but is preferably 0 to 20% by weight based on the total weight of the aqueous coating material.
[0052] The amount of the aqueous coating material of the present invention applied is preferably 0.05 to 1 kg / m 2 , more preferably 0.1 to 0.8 kg / m 2 , and more preferably 0.15 to 0.6 kg / m 2 By applying the water-based coating material in such an amount, a coating film having excellent appearance and weather resistance can be formed.
[0053] The aqueous coating material of the present invention can be used as a room temperature curing aqueous coating material. Therefore, the application of the aqueous coating material of the present invention or drying after application can be carried out in an environment of room temperature (preferably 5 to 40°C). However, heating is also possible if necessary. The drying time is preferably about 0.5 to 4 hours at room temperature. The number of coats can be one or two or more (preferably one or two). When the number of coats is two or more, it is desirable that the total amount of coats is within the above range. EXAMPLES
[0054] The following examples will be given to clarify the features of the present invention, but the present invention is not limited to these examples.
[0055] (Production of water-based coating materials) The following raw materials were used to produce the aqueous coating materials in the examples. Resin 1: Acrylic silicone resin emulsion (emulsion polymer consisting mainly of methyl methacrylate, cyclohexyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, silane coupling agent, and alkoxysilanes; glass transition temperature 4°C; residual silica ratio in resin solids 5% by weight; solids 40% by weight) Resin 2: Acrylic silicone resin emulsion (cyclohexyl methacrylate-2-ethylhexyl acrylate-silane coupling agent-alkoxysilanes as main components of emulsion polymer, glass transition temperature -12°C, silica residual ratio in resin solid content 15% by weight, solid content 40% by weight) Resin 3: Acrylic silicone resin emulsion (cyclohexyl methacrylate-2-ethylhexyl acrylate-silane coupling agent-alkoxysilanes as main components of emulsion polymer, glass transition temperature -12°C, silica remaining ratio in resin solid content 20% by weight, solid content 40% by weight) Color pigment 1: Titanium oxide (average particle size 0.3 μm) Pigment dispersant 1: Polycarboxylic acid type dispersant (aqueous solution of polycarboxylic acid ammonium salt, solid content 30% by weight) Solvent 1: Ether solvent (diethylene glycol monobutyl ether (solubility in water is infinite, boiling point is 230°C) Solvent 2: Ether solvent (tripropylene glycol monomethyl ether (solubility in water is infinite, boiling point is 242°C) Solvent 3: Ester solvent (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, solubility in water 0.09g / 100gH2O, boiling point 255℃) Solvent 4: Ester solvent (2,2,4-trimethyl-1,3-pentanediol diisobutyrate, solubility in water 0.04g / 100gH2O, boiling point 282℃) Thickener 1: Cellulose-based thickener Thickener 2: Polyurethane-based associative thickener Defoamer 1: Mineral oil-based defoamer Defoamer 2: Silicone-based defoamer
[0056] ○Aqueous coating material 1 A color pigment dispersion was prepared by mixing and stirring 27 parts by weight of water, 0.4 parts by weight of thickener 1, 0.1 parts by weight of defoamer 1, 2.5 parts by weight of pigment dispersant 1, and 70 parts by weight of color pigment 1. Next, 100 parts by weight of this color pigment dispersion liquid was mixed and stirred with 250 parts by weight of resin 1 (100 parts by weight in terms of solid content), 4 parts by weight of solvent 1, 11 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2 to produce aqueous coating material 1.
[0057] ○Aqueous coating material 2 Aqueous coating material 2 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 4 parts by weight of solvent 1, 11 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0058] ○Aqueous coating material 3 Aqueous coating material 3 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 8 parts by weight of solvent 1, 11 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0059] ○Aqueous coating material 4 Aqueous coating material 4 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 8 parts by weight of solvent 1, 19 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0060] ○Aqueous coating material 5 100 parts by weight of the same color pigment dispersion as in Example 1 was mixed and stirred with 250 parts by weight of resin 3 (100 parts by weight in terms of solid content), 8 parts by weight of solvent 1, 11 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2 to produce an aqueous coating material 5.
[0061] ○Aqueous coating material 6 Aqueous coating material 6 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 8 parts by weight of solvent 2, 11 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0062] ○Aqueous coating material 7 Aqueous coating material 7 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 8 parts by weight of solvent 2, 11 parts by weight of solvent 4, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0063] ○Aqueous coating material 8 Aqueous coating material 8 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion liquid as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 19 parts by weight of solvent 3, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0064] ○Aqueous coating material 9 Aqueous coating material 9 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight of resin 2 (100 parts by weight in terms of solid content), 19 parts by weight of solvent 1, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0065] ○Aqueous coating material 10 Aqueous coating material 10 was produced by mixing and stirring 100 parts by weight of the same color pigment dispersion as in Example 1, 250 parts by weight (100 parts by weight in terms of solid content) of resin 2, 2 parts by weight of thickener 2, and 0.2 parts by weight of defoamer 2.
[0066] ○Aqueous coating material 11 An aqueous coating material 11 was produced by mixing and stirring 250 parts by weight of resin 2 (100 parts by weight calculated as solid content), 2 parts by weight of thickener 2, and 0.2 parts by weight of antifoaming agent 2.
[0067] (Test Method) Each water-based coating material was tested in the following manner.
[0068] Test 1 Each water-based coating material was applied to one side of a glass plate using a film applicator with a gap of 150 μm, and the coated surface was placed horizontally in an incubator at 0°C and dried for 2 hours, after which the appearance of the coating was observed. The evaluation criteria were "A" for no cracks, "B" for slight cracks, and "C" for obvious cracks.
[0069] Test 2 Each water-based coating material was applied to one side of a glass plate using a film applicator with a gap of 150μm, and the coated surface was placed horizontally and dried for 48 hours under standard conditions (air temperature 23℃, relative humidity 50%), after which the 20 degree specular gloss (measurement angle 20 degrees) was measured. The evaluation criteria were as follows: 20 degree specular gloss of 43 or more was given an "A", over 40 and up to 43 was given a "B", and 40 or less was given a "C".
[0070] Test 3 Each water-based coating material was applied to one side of a glass plate using a film applicator with a gap of 150μm, and the coated surface was placed horizontally and dried for 48 hours under standard conditions (air temperature 23℃, relative humidity 50%), after which the 60 degree specular gloss (measurement angle 60 degrees) was measured. The evaluation criteria were as follows: 60 degree specular gloss of 78 or more was given an "A", 75 to 78 or less was given a "B", and 75 or less was given a "C".
[0071] Test 4 Each water-based coating material was sprayed onto a slate board that had previously been coated with an epoxy resin emulsion sealer, with an application rate of 0.3 kg / m. 2 The coating was applied and dried under standard conditions for 14 days. The obtained test specimens were exposed to an accelerated weathering tester (xenon weather meter) for 1400 hours, and the degree of chalking was evaluated using the method of JIS K5600-8-6. The evaluation criteria were as follows: "A" for no chalking, "B" for chalking grade 1 to 2, and "C" for chalking grade 3 or higher.
[0072] (Test Results) The test results are shown in Table 1. Examples 1 to 9 (aqueous coating materials 1 to 9) achieved good results in all tests and were excellent in crack resistance, gloss, and weather resistance. Comparative Example 1 (aqueous coating material 10) achieved insufficient results in tests 1 to 3, so test 4 was not performed. Comparative Example 2 (aqueous coating material 11) did not contain pigments, etc., and was outside the scope of the present invention, so tests 2 to 4 were not performed.
[0073] [Table 1]
Claims
[Claim 1] An aqueous coating material comprising a resin emulsion, The present invention comprises an acrylic silicone resin emulsion (A) having a silica residual ratio of 1 to 40% by weight in the resin solid content and a glass transition temperature of 15°C or lower, a pigment (B), a pigment dispersant (C), and an ether or ester solvent (D), The ether or ester solvent (D) is Solubility in water is 1g / 100gH 2 Ether or ester solvents (D1) with a solubility in water of 1 g / 100 gH or more, and / or 2 1. An aqueous coating material comprising an ether or ester solvent (D2) of 0 or less.
Citation Information
Patent Citations
Water-based crosslinking coating composition comprising silicon-containing polymer latex
JP1996012930A
Cited By
Water-based coating material, coating film forming method, and topcoat material set
JP7753595B1
Aqueous coating material, method for forming coating film, and top coating set
WO2025143019A1