Manufacturing method of welded structure, and welding device

By controlling current application sequence and duration, the method addresses burr formation in close welding points, achieving robust welding without burrs.

JP2024142707APending Publication Date: 2024-10-11TOYOTA JIDOSHA KK +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023054976
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Burr formation is exacerbated when the distance between welding points becomes shorter, as current shunts to already welded points, leading to molten metal ejection and hardening.

Method used

A method involving a specific sequence and duration of current application, including a main current followed by a larger current, and in some cases a break-in current, with controlled pressure, to manage current flow and suppress burr formation.

Benefits of technology

Effectively suppresses burr occurrence by managing current flow and growth direction, ensuring robust welding without burrs even at close welding point distances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142707000001_ABST
    Figure 2024142707000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a welded structure, and a welding device each enabling suppression of the occurrence of burr.SOLUTION: A manufacturing method of a welded structure is provided in which the welded structure is formed by laminating three pieces or more of metal plates W1 and at least one metal plate W3 of the three pieces of metal plates W1 is thinner than the other metal plates W1 to form a laminate W10 through spot welding. The manufacturing method includes: a step ST1 where a welding spot P1 of the laminate W 10 is pressurized and energized so that regular current flows on the welding spot P1 of the laminate W10; and a step ST2 where the welding spot P1 of the laminate W 10 is pressurized and energized so that heavy-current relative to the regular current flows on the welding spot P1 of the laminate W10. A period of time t1 where the regular current flows on the welding spot P1 of the laminate W10 is relatively longer than a period of time t2 where the heavy-current flows on the welding spot P1 of the laminate W10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a welded structure and a welding apparatus. [Background technology]

[0002] Patent Document 1 discloses a spot welding method for joining, using a pulse current, a laminate formed by stacking three or more metal plates, at least one of which has a thickness different from the other metal plates. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 7038193 Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have discovered the following problems. When the distance between a welded welding point and a welding point to be welded becomes short, burrs tend to occur easily. For example, when a current is passed through a welding point located between two already welded welding points while applying pressure, the current may be diverted to the already welded welding point, and burrs may occur at the welded welding point. Note that burrs are formed, for example, when molten metal generated directly under the welding point during current passing jumps out from the surface of the welding point and solidifies.

[0005] The present disclosure has been made in consideration of the above-mentioned problems, and provides a manufacturing method for a welded structure and a welding device that can suppress the occurrence of burrs. [Means for solving the problem]

[0006] A method for manufacturing a welded structure according to the present disclosure includes: A method for manufacturing a welded structure, which is formed by spot welding a laminate formed by stacking three or more metal plates, and at least one of the three or more metal plates is thinner than the other metal plates, a step of applying a current to the welding points of the laminate while applying pressure to the welding points of the laminate; and subsequently applying a current to the welding points of the laminate while applying pressure to the welding points of the laminate, thereby passing a large current, which is larger than the main current, through the welding points of the laminate. The period during which the current is passed through the welding point of the laminate is t 1 is the period t during which the large current is passed through the welding point of the laminate. 2 Longer compared to.

[0007] In the above-mentioned method for manufacturing a welded structure, the main current is passed through the welding point of the laminate during a period t 1 is the period t during which the large current is passed through the welding point of the laminate. 2 It is preferable that the value be 2.50 times or more.

[0008] In the above-described method for manufacturing a welded structure, the current value A2 of the large current may be 12 kA or more.

[0009] A method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure, which is formed by spot welding a laminate formed by stacking three or more metal plates, and at least one of the three or more metal plates is thinner than the other metal plates, and a step of applying pressure to the welding points of the laminate while passing a current through the welding points of the laminate; A step of applying pressure to the welding points of the laminate and passing a current through the welding points of the laminate, thereby passing a large current through the welding points of the laminate; and subsequently applying a current to the welding points of the laminate while applying pressure to the welding points of the laminate, thereby passing a main current, which is smaller than the large current, through the welding points of the laminate. The current value A13 of the running-in current is smaller than the current value A11 of the main current.

[0010] In the above-mentioned method for manufacturing a welded structure, the main current is passed through the welding point of the laminate during a period t 11 is the period t during which the large current is passed through the welding point of the laminate. 12 It is preferable that the value be 2.50 times or more.

[0011] In the above-mentioned method for manufacturing a welded structure, the main current is passed through the welding point of the laminate during a period t 11 is the period t during which the running-in current is passed through the welding point of the laminate. 13 It is said that the value is 3.00 times or less.

[0012] In the above-described method for manufacturing a welded structure, the current value A13 of the running-in current may be equal to or less than 0.95 times the current value A11 of the main current.

[0013] In the above-mentioned method for manufacturing a welded structure, the laminate may have a weld point that has already been welded, and the weld point of the laminate may be located within 15 mm of the weld point that has already been welded.

[0014] A method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure, which is formed by spot welding a laminate formed by stacking three or more metal plates, and at least one of the three or more metal plates is thinner than the other metal plates, and determining a welding method for welding the welding points to be welded based on the positions of the welding points to be welded; In the step of determining a welding method, When the distance between the welding point to be welded and the already welded welding point exceeds a predetermined value, a current is applied while applying pressure to the welding point of the laminate, so that a large current is applied to the welding point of the laminate, and then a current is applied while applying pressure to the welding point of the laminate, so that a main current smaller than the large current is applied to the welding point of the laminate; When the distance between the welding point to be welded and the already welded welding point is equal to or less than a predetermined value, A current is passed through the welding point of the laminate while applying pressure to the welding point of the laminate, a main current is passed through the welding point of the laminate, and a current is passed through the welding point of the laminate while applying pressure to the welding point of the laminate to pass a large current larger than the main current through the welding point of the laminate. 1 is the period t during which the large current is passed through the welding point of the laminate. 2 The welding points to be welded are welded using a welding method that is longer than the welding method described above.

[0015] A method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure, which is formed by spot welding a laminate formed by stacking three or more metal plates, and at least one of the three or more metal plates is thinner than the other metal plates, and determining a welding method for welding the welding points to be welded based on the positions of the welding points to be welded; In the step of determining a welding method, If the distance between the welding point to be welded and the already welded welding point exceeds a predetermined value, A current is applied to the welding point of the laminate while applying pressure thereto, so that a large current is applied to the welding point of the laminate, and then a current is applied to the welding point of the laminate while applying pressure thereto, so that a main current smaller than the large current is applied to the welding point of the laminate; When the distance between the welding point to be welded and the already welded welding point is equal to or less than a predetermined value, The welding points to be welded are welded using a welding method in which a current is passed while pressure is applied to the welding points of the laminate, a running-in current is passed to the welding points of the laminate, a large current is passed to the welding points of the laminate while pressure is applied, and a main current which is smaller than the large current is passed to the welding points of the laminate while pressure is applied, and a current value A13 of the running-in current is smaller than a current value A11 of the main current.

[0016] The welding apparatus according to the present disclosure is a welding apparatus for spot welding a laminate formed by stacking three or more metal plates, in which at least one of the three or more metal plates is thinner than the other metal plates, an electrode for applying pressure to the welding points of the laminate; a current generating circuit that applies a current to the welding point of the laminate pressed by the electrode; By controlling the current generating circuit, A first control that maintains the current at this current; and a second control for maintaining the current at a large current larger than the main current after maintaining the current at the main current; The period during which the current is passed through the welding point of the laminate is t 1 is the period t during which the large current is passed through the welding point of the laminate. 2 Longer compared to.

[0017] The welding apparatus according to the present disclosure is a welding apparatus for spot welding a laminate formed by stacking three or more metal plates, in which at least one of the three or more metal plates is thinner than the other metal plates, an electrode for applying pressure to the welding points of the laminate; a current generating circuit that applies a current to the welding point of the laminate pressed by the electrode; By controlling the current generating circuit, A first control that maintains the current at a running-in current; a second control for maintaining the current at a running-in current and then maintaining the current at a high current; and a third control of maintaining the current at a main current smaller than the large current after maintaining the current at a large current, The running-in current is smaller than the main current. Effect of the Invention

[0018] According to the present disclosure, the occurrence of burrs can be suppressed. [Brief description of the drawings]

[0019] [Figure 1] 4 is a flowchart showing a method for manufacturing a welded structure according to the first embodiment. [Diagram 2] 1 is a schematic diagram showing a step of a manufacturing method for a welded structure according to the first embodiment. [Diagram 3] 4 is a graph showing a change in current in the manufacturing method of a welded structure according to the first embodiment. [Figure 4] FIG. 4 is a schematic diagram showing a positional relationship between a welding point that has already been welded and a welding point that is to be welded. [Diagram 5] 10 is a flowchart showing a method for manufacturing a welded structure according to a second embodiment. [Figure 6] 10 is a graph showing a change in current in a manufacturing method for a welded structure according to the second embodiment. [Figure 7] 1 is a flowchart illustrating a method for manufacturing a welded structure according to a technique related to the present disclosure. [Figure 8] 1 is a schematic diagram showing one step of a method for manufacturing a welded structure according to a technique related to the present disclosure. [Figure 9] 1 is a graph showing a current curve in a manufacturing method for a welded structure according to a technique related to the present disclosure. [Figure 10] 1 is a photograph showing burrs generated at a welded joint after welding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] <Related technologies> Prior to describing specific embodiments to which the present disclosure is applied, a method for manufacturing a welded structure according to a technique related to the present disclosure will be described with reference to Figs. 7 to 9. Fig. 7 is a flowchart showing a method for manufacturing a welded structure according to a technique related to the present disclosure. Fig. 8 is a schematic diagram showing one step of the method for manufacturing the welded structure shown in Fig. 7. Fig. 9 is a graph showing a current curve in the method for manufacturing the welded structure shown in Fig. 7.

[0021] As shown in Fig. 7 and Fig. 8, a current is applied while pressure is applied to the welding point P91 of the laminate W910, and a large current is passed through the welding point P91 of the laminate W910 (step ST91). Specifically, the laminate W910 is formed by stacking three or more metal plates, and at least one of the three or more metal plates is thinner than the other metal plates. An example of the laminate W910 shown in Fig. 8 is formed by stacking metal plates W91, W92, and W93 in this order. A large current is passed while electrodes E91 and E92 are pressed against the welding point P91. The large current is applied for a period of t 91 During this time, the large current is passed through a welding point P91 of the laminate W910. The current value of the large current is larger than the current value of the main current passed in step ST92. A current curve CA9 shown in Fig. 9 shows the change in current value in this manufacturing method. The current value of the large current is current value A91.

[0022] Next, current is applied while pressure is applied to the welding point P91 of the laminate W910, and the main current is applied to the welding point P91 of the laminate W910 (step ST92). The current value of the main current is current value A92 shown in FIG. 9, which is smaller than current value A91. Specifically, the current is reduced from current value A91 to current value A92, and current is applied while pressure is applied to the welding point P91. 92 During the period t 92 is the period t 91 Longer compared to.

[0023] In the manufacturing method of the welded structure according to the technique related to the present disclosure, burrs are often generated. As shown in Fig. 8, in step ST91, a large current may flow from the welding point P91 to the already welded welding points WP91 and WP92 in the planar direction of the laminate W910 (here, the X-axis direction). When the current flows separately to the already welded welding points WP91 and WP92, burrs are often generated at the welding point P91. In addition, when the distance between the welding point P91 and the already welded welding points WP91 and WP92 is short, the current is likely to flow separately to the already welded welding points WP91 and WP92, and burrs are likely to be generated at the welding point P91.

[0024] The present inventors have focused on the effect that electric current has on the generation of burrs, and have thoroughly investigated various factors such as the magnitude, duration and order of electric current, leading to the invention.

[0025] Hereinafter, specific embodiments to which the present invention is applied will be described in detail with reference to the drawings. However, the present invention is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.

[0026] <Embodiment 1> A first embodiment will be described with reference to Figs. 1 to 4. Fig. 1 is a flowchart showing a method for manufacturing a welded structure according to the first embodiment. Fig. 2 is a schematic diagram showing one step of a method for manufacturing the welded structure shown in Fig. 1. Fig. 3 is a graph showing a change in current in the method for manufacturing the welded structure shown in Fig. 1. Fig. 4 is a schematic diagram showing the positional relationship between a weld point that has already been welded and a weld point that is to be welded.

[0027] Naturally, the right-handed XYZ coordinate system shown in Figure 2 and other drawings is for the convenience of explaining the positional relationship of the components. Usually, the positive direction of the Z axis is vertically upward, and the XY plane is a horizontal plane, which is common among the drawings.

[0028] In the manufacturing method of the welded structure according to the first embodiment, a welding device E10 shown in FIG. 2 can be used. The welding device E10 includes electrodes E1 and E2, a current generating circuit E3, and a control unit E4. The electrodes E1 and E2 are movably held by a movable arm (not shown) or the like. The electrodes E1 and E2 press the welding point P1 of the laminate W10 by clamping it with the movable arm or the like. The current generating circuit E3 is electrically connected to a power source (not shown) and generates a current from the power source. The current generating circuit E3 passes a current through the welding point P1 of the laminate W10 pressed by the electrodes E1 and E2. The control unit E4 may control the operation of the electrodes E1 and E2 via the movable arm or the like. The control unit E4 includes a current control unit E41. The current control unit E41 controls the current generating circuit E3 and can change the magnitude of the current passed by the current generating circuit E3 over time.

[0029] As shown in FIG. 2, a current is applied to the welding point P1 of the laminate W10 while applying pressure to the welding point P1 of the laminate W10, and the main current is passed through the welding point P1 of the laminate W10 (step ST1). Specifically, the laminate W10 is formed by stacking three or more metal plates. In addition, in the laminate W10, at least one metal plate among the three or more metal plates is thinner than the other metal plates. In other words, the laminate W10 is a plate assembly with a high plate thickness ratio. An example of the laminate W10 shown in FIG. 2 is formed by stacking metal plates W1, W2, and W3 in this order. The metal plate W3 is thinner than the metal plate W1 and the metal plate W2. The metal plates W1, W2, and W3 may be, for example, different types of steel plates. The main current is passed while the electrodes E1 and E2 are pressed against the welding point P1. As shown in FIG. 2 and FIG. 3, the main current is passed at a current value A1 for a period t 1 Current is passed through the welding point P1 of the laminate W10 in this state. The electrodes E1 and E2 may be electrically connected to a power source (not shown). The power source may pass a current through the laminate W10 via the electrodes E1 and E2 as appropriate. The diameters of the electrodes E1 and E2 and the pressure with which the electrodes E1 and E2 press the welding point P1 may be selected as appropriate based on widely used standards.

[0030] In addition, this current is 1A large current is applied to the welding point P1 of the laminate W10 for a period of t 2 During the period t 1 is the period t 2 If it is longer than the

[0031] 4, a distance L1 between the welding point P1 and the already welded welding point WP1, and a distance L2 between the welding point P1 and the already welded welding point WP2 may be determined appropriately. The distances L1 and L2 are not particularly limited and can be selected from a wide range of values, for example, 15 mm and 30 mm.

[0032] In step ST1, as shown in FIG. 2, when the main current is applied to the welding point P1 of the laminate W10, the main current passes through the welding point P1 and flows in the thickness direction (here, Z direction) of the laminate W10. A current path is secured so that the current flows from the electrode E1 through the welding point P1 and the laminate W10 to the electrode E2. A nugget N1 is formed inside the laminate W10 from the welding point P1 of the laminate W10. Specifically, the nugget N1 is formed on the metal plate W1 and the metal plate W2. The nugget N1 grows mainly in the planar direction (here, XY direction) of the laminate W10. In addition, in many cases, in step ST1, the nugget N1 grows inside the metal plate W1 and the metal plate W2, but does not reach the inside of the metal plate W3.

[0033] Next, continuing from step ST1, a current is applied while pressure is applied to the welding point P1 of the laminate W10, and a large current is applied to the welding point P1 of the laminate W10 (step ST2). Specifically, the current is increased from a current value A1 to a current value A2, and a current is applied while pressure is applied to the welding point P1. As shown in FIG. 2 and FIG. 3, the large current is applied at the current value A2 for a period t 2 At this time, the welding wire is caused to flow to the welding point P1 of the laminate W10. This causes the nugget N1 to grow and reach the inside of the metal plate W3. As a result, the nugget N1 grows to a sufficient size inside the metal plates W1, W2, and W3.

[0034] A current curve CA1 shown in FIG. 3 shows the change in current value in this manufacturing method. As shown in FIG. 3, the current value A1 of the main current is smaller than the current value A2 of the large current. The current ratio A2 / A1 of the current value A2 to the current value A1 may be, for example, 1.4 or more, specifically, 1.4 or more and 1.7 or less. The current value A2 may be, for example, 11 kA or more, specifically, 12 kA or more. Even if the thickness of the metal plate W3 is small, welding may be performed with good welding quality.

[0035] Also, in period t 1 is the period t 2 If the period is longer than t, burrs are less likely to occur. 1 is the period t 2 It is preferable that the period is 1.00 times or more. 2 It is even better if the period is 2.50 times or more. 1 is the period t 2 It is preferable that the period is 2.8 times or more and 5.0 times or less. 2 It is preferable that the period t 1 Range and period t 2 By specifying the range of the thickness of the burr, the occurrence of burrs can be further suppressed.

[0036] As a result, the nugget N1 solidifies and the metal plates W1, W2, and W3 of the laminate W10 are welded together. That is, a welded structure can be manufactured in which the metal plates W1, W2, and W3 of the laminate W10 are welded together. In the manufacturing method for a welded structure according to the first embodiment described above, the main current and the large current hardly flow separately from the welding point P1 to the welded welding points WP1 and WP2 in the planar direction of the laminate W10, but flow from the welding point P1 in the thickness direction of the laminate W10. Therefore, the generation of burrs at the welding point P1 can be suppressed.

[0037] Also, the distance L1 and the distance L2 shown in FIG. 4 may be short. Even in such a case, in the manufacturing method of the welded structure according to the first embodiment, the main current and the large current are unlikely to flow from the welding point P1 to the welded welding points WP1 and WP2 in the planar direction of the laminate W10, and are likely to flow from the welding point P1 in the thickness direction of the laminate W10. As a result, the nugget N1 grows inside the metal plates W1, W2, and W3, and the metal plates W1, W2, and W3 are welded with good welding quality. Therefore, burrs are hardly generated at the welding point P1. That is, even when the distance L1 and the distance L2 shown in FIG. 4 are short, the manufacturing method of the welded structure according to the first embodiment is suitable.

[0038] <Embodiment 2> A second embodiment will be described with reference to Fig. 2, Fig. 5, and Fig. 6. Fig. 5 is a flowchart showing a method for manufacturing a welded structure according to the second embodiment. Fig. 6 is a graph showing a change in current in the method for manufacturing the welded structure shown in Fig. 5.

[0039] In the method for manufacturing a welded structure according to the second embodiment, like the method for manufacturing a welded structure according to the first embodiment described above, the welding device E10 shown in FIG. 2 can be used.

[0040] As shown in Fig. 2, a current is applied while pressure is applied to the welding point P1 of the laminate W10, and a break-in current is passed through the welding point P1 of the laminate W10 (step ST11). Specifically, the break-in current is passed while the electrodes E1 and E2 are pressed against the welding point P1. As shown in Figs. 2 and 6, the break-in current is applied at a current value A13 for a period t 13 The wire is caused to flow through the welding point P1 of the laminate W10 in the above manner. The diameters of the electrodes E1 and E2 and the pressure with which the electrodes E1 and E2 press the welding point P1 may be appropriately selected based on widely used standards.

[0041] In step ST11, when a break-in current is applied to the weld point P1 of the laminate W10, the break-in current flows from the weld point P1 in the thickness direction (here, the Z direction) of the laminate W10. This increases the temperature of the laminate W10, and reduces the electrical resistivity of the laminate W10. A current path is secured so that the current flows from the electrode E1 through the weld point P1 and the laminate W10 to the electrode E2. Furthermore, nuggets N1 are hardly generated in the laminate W10.

[0042] Next, current is applied while pressure is applied to the welding point P1 of the laminate W10, and a large current is applied to the welding point P1 of the laminate W10 (step ST12). Specifically, the current is increased from current value A13 to current value A12, and current is applied while pressure is applied to the welding point P1. As shown in FIG. 2 and FIG. 6, the large current is applied at current value A12 for a period t 12 The welding wire is caused to flow to a welding point P1 of the laminate W10 at the welding point P1. This causes a nugget N1 to form in the laminate W10 and grow in the thickness direction (here, the Z-axis direction) of the laminate W10. As a result, the nugget N1 grows inside the metal plate W1, the metal plate W2, and the metal plate W3.

[0043] Finally, the welding point P1 of the laminate W10 is pressed while being energized, and the main current is passed through the welding point P1 of the laminate W10 (step ST13). Specifically, the current is reduced from current value A12 to current value A11, and the welding point P1 is pressed while being energized. As shown in FIG. 2 and FIG. 6, the main current is passed at current value A11 for a period t 11 The welding wire is caused to flow to a welding point P1 of the laminate W10 at the welding position P1. This causes the nugget N1 to grow in the planar direction of the laminate W10 (here, the XY direction). As a result, the nugget N1 grows to a sufficient size inside the metal plate W1, the metal plate W2, and the metal plate W3.

[0044] A current curve CA2 shown in FIG. 6 shows the change in current value in this manufacturing method. As shown in FIG. 6, the current value A13 of the running-in current is smaller than the current value A11 of the main current. The current value A11 of the main current is smaller than the current value A12 of the large current. The current ratio A13 / A11 of the current value A13 to the current value A11 may be, for example, 0.95 or less, and more specifically, may be 0.65 or more and 0.95 or less. In this way, by specifying the range of the current ratio A13 / A11, it is possible to suppress the occurrence of burrs.

[0045] Also, in period t 11 is the period t 12 It is better to set the period t 12 It is even better if the period is between 2.86 and 5.00 times the period t 11 is the period t 13 It is preferable that the period t 13 It is even better if the period is 2.00 to 2.90 times the period t 11 , period t 12 , and period t 13 By specifying the range, the occurrence of burrs can be suppressed.

[0046] As a result, the nugget N1 solidifies and the metal plates W1, W2, and W3 of the laminate W10 are welded together. That is, a welded structure can be manufactured in which the metal plates W1, W2, and W3 of the laminate W10 are welded together. In the manufacturing method for a welded structure according to the second embodiment described above, the main current and the large current hardly flow separately from the welding point P1 to the welded welding points WP1 and WP2 in the planar direction of the laminate W10, but flow from the welding point P1 in the thickness direction of the laminate W10. Therefore, the generation of burrs at the welding point P1 can be suppressed. EXAMPLES

[0047] Next, examples of the manufacturing methods for the welded structures according to the first and second embodiments will be described.

[0048] In Examples 1 to 5, a welded structure was manufactured by welding a laminate under the conditions shown in Table 1 below, using an example of the manufacturing method of a welded structure according to the first embodiment. The laminate is formed by laminating a mild steel plate, a hot stamping steel plate made of a hot stamping material, and an ultra-high tensile steel plate. The detailed manufacturing conditions are: thickness of the mild steel plate: 0.65 mm, thickness of the hot stamping steel plate: 1.8 mm, thickness of the ultra-high tensile steel plate: 1.6 mm, total sheet thickness of the laminate: 4.50 mm, sheet thickness ratio of the laminate: 6.23, diameter of the electrode: 6 mm, pressure of the electrode pressing the laminate: 3820 kN, distance between the welding point and the already welded welding point: 15 mm. Note that in Comparative Example 1, as shown in Table 1, the period t of the high current was 0.65 mm, 2 The manufacturing conditions are the same as those in Example 1, except for the above.

[0049] In Examples 6 to 12, a welded structure was manufactured by welding a laminate under the conditions shown in Table 2 below, using an example of the manufacturing method for a welded structure according to the second embodiment. The laminate had the same configuration as the laminate used in Examples 1 to 5. The detailed manufacturing conditions were the same as those of Examples 1 to 5. In Comparative Examples 2 to 5, the manufacturing conditions were the same as those of Examples 6 to 12, except for the current and period shown in Table 2. For example, in Comparative Example 2, step ST11 was omitted.

[0050] The weld quality of the welded structures according to the examples and the comparative examples was evaluated. Specifically, the weld quality was evaluated as good (OK) when no burrs were generated at the welded points of the welded structures according to the examples and the comparative examples, and was evaluated as poor (NG) when burrs were generated. One specific example of burrs, B1, is shown in FIG. 10. The evaluation results are shown in Tables 1 and 2.

[0051] [Table 1]

[0052] In Examples 1 to 5, the evaluation was OK, and no burrs were generated. On the other hand, in Comparative Example 1, the evaluation was NG, and burrs were generated. One of the reasons for this is the period ratio t 1 / t 2is 0.91, which is smaller than those in Examples 1 to 5.

[0053] [Table 2]

[0054] In Example 6, the evaluation was OK, and no burrs were generated. On the other hand, in Comparative Example 2, the evaluation was NG, and burrs were generated. One reason for this is that, while step ST11 was performed in Example 6, step ST11 was omitted in Comparative Example 2.

[0055] In Examples 6 to 10, the evaluation was OK, and no burrs were generated. On the other hand, in Comparative Example 3, the evaluation was NG, and burrs were generated. One of the reasons for this is the period ratio t 11 / t 12 is 2.86 to 5.00, which is larger than that of Comparative Example 3.

[0056] In Example 11, the evaluation was OK, and no burrs were generated. On the other hand, in Comparative Example 4, the evaluation was NG, and burrs were generated. One of the reasons for this is that the current ratio A13 / A11 in Example 11 was 0.95, which is smaller than that in Comparative Example 4.

[0057] In Example 12, the evaluation was OK, and no burrs were generated. On the other hand, in Comparative Example 5, the evaluation was NG, and burrs were generated. One of the reasons for this is the period ratio t 11 / t 13 is 2.50, which is smaller than that of Comparative Example 5.

[0058] The present invention is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present invention. In addition, the present invention can be implemented by appropriately combining the above-described embodiment and examples thereof.

[0059] For example, the manufacturing method of the welded structure according to the first and second embodiments described above may further include a step of determining a welding method for welding the weld points P1 to be welded based on the positions of the weld points P1 to be welded.

[0060] In the step of determining this welding method, if the distances L1, L2 between the to-be-welded welding point P1 and the already-welded welding points WP1, P2 exceed a predetermined value, a current is passed through the welding point P1 of the laminate W10 while pressure is applied to the welding point P1 of the laminate W10, and a main current smaller than the large current is passed through the welding point P1 of the laminate W10 while pressure is applied to the welding point P1 of the laminate W10.

[0061] On the other hand, when the distances L1, L2 are equal to or less than the predetermined values, the steps ST1 and ST2 of the manufacturing method for a welded structure according to the first embodiment described above may be performed to weld the to-be-welded welding point P1.

[0062] In addition, when the distances L1 and L2 are equal to or less than a predetermined value, the steps ST11, ST12, and ST13 of the method for manufacturing a welded structure according to the second embodiment described above may be performed to weld the welding point P1 to be welded.

[0063] The control unit E4 of the welding device E10 may include a recording unit and a welding method determination unit. The recording unit records the distances L1 and L2 in advance. The welding method determination unit determines a welding method for welding the to-be-welded welding point P1 based on the distances L1 and L2.

[0064] As described above, the manufacturing method of the welded structure according to the first and second embodiments may further include a step of determining a welding method for welding the weld point P1 to be welded based on the position of the weld point P1 to be welded. In such a case, the weld point P1 to be welded can be welded using a welding method according to the distances L1 and L2. Specifically, welding is performed on the weld break point where there is little risk of burrs being generated using the manufacturing method of the welded structure according to the technology related to the present disclosure. On the other hand, welding can be performed on the weld point where there is a risk of burrs being generated using the manufacturing method of the welded structure according to the first and second embodiments. [Explanation of symbols]

[0065] W10 laminate W1, W2, W3 metal plate P1 Welding point WP1, WP2 Welded joints E10 Welding equipment E1, E2 electrode E3 Current generation circuit E4 Control section E41 Current control section ST1, ST2, ST21, ST22, ST23 process N1 Nugget L1, L2 distance

Claims

1. A method for manufacturing a welded structure, the method being formed by spot welding a laminate formed by stacking three or more metal plates, at least one of which is thinner than the other metal plates, the method comprising the steps of: a step of applying a current to the welding points of the laminate while applying pressure to the welding points of the laminate; and subsequently applying a current to the welding points of the laminate while applying pressure to the welding points of the laminate, thereby passing a large current, which is larger than the main current, through the welding points of the laminate. The period during which the main current is passed through the welding point of the laminate is t 1 is the period t during which the large current is passed through the welding point of the laminate. 2 Longer than A method for manufacturing a welded structure.

2. The period during which the main current is passed through the welding point of the laminate is t 1 is the period t during which the large current is passed through the welding point of the laminate. 2 is 2.50 times or more, The method for manufacturing the welded structure according to claim 1 .

3. The current value A2 of the large current is 12 kA or more. The method for manufacturing a welded structure according to claim 1 or 2.

4. A method for manufacturing a welded structure, the method being formed by spot welding a laminate formed by stacking three or more metal plates, at least one of which is thinner than the other metal plates, the method comprising the steps of: a step of applying pressure to the welding points of the laminate while passing a current through the welding points of the laminate; A step of applying pressure to the welding points of the laminate and passing a current through the welding points of the laminate, thereby passing a large current through the welding points of the laminate; and subsequently applying a current to the welding points of the laminate while applying pressure to the welding points of the laminate, thereby passing a main current, which is smaller than the large current, through the welding points of the laminate. The current value A13 of the running-in current is smaller than the current value A11 of the main current. A method for manufacturing a welded structure.

5. The period during which the main current is passed through the welding point of the laminate is t 11 is the period t during which the large current is passed through the welding point of the laminate. 12 is 2.50 times or more, The method for manufacturing a welded structure according to claim 4.

6. The period during which the main current is passed through the welding point of the laminate is t 11 is the period t during which the running-in current is passed through the welding point of the laminate. 13 is 3.00 times or less, The method for manufacturing a welded structure according to claim 4 or 5.

7. The current value A13 of the running-in current is 0.95 times or less than the current value A11 of the main current. The method for manufacturing a welded structure according to claim 4 or 5.

8. The laminate has already welded weld points, The welding point of the laminate is within 15 mm of the already welded welding point. The method for manufacturing a welded structure according to claim 1 or 4.

9. A method for manufacturing a welded structure, the method being formed by spot welding a laminate formed by stacking three or more metal plates, at least one of which is thinner than the other metal plates, the method comprising the steps of: determining a welding method for welding the welding points to be welded based on the positions of the welding points to be welded; In the step of determining a welding method, When the distance between the welding point to be welded and the already welded welding point exceeds a predetermined value, a current is applied while applying pressure to the welding point of the laminate, so that a large current is applied to the welding point of the laminate, and then a current is applied while applying pressure to the welding point of the laminate, so that a main current smaller than the large current is applied to the welding point of the laminate; When the distance between the welding point to be welded and the already welded welding point is equal to or less than a predetermined value, A current is passed through the welding point of the laminate while applying pressure to the welding point of the laminate, and a large current larger than the main current is passed through the welding point of the laminate while applying pressure to the welding point of the laminate. The main current is passed through the welding point of the laminate during a period t. 1 is the period t during which the large current is passed through the welding point of the laminate. 2 The welding points to be welded are welded using a welding method that is longer than the welding method described above. A method for manufacturing a welded structure.

10. A method for manufacturing a welded structure, the method being formed by spot welding a laminate formed by stacking three or more metal plates, at least one of which is thinner than the other metal plates, the method comprising the steps of: determining a welding method for welding the welding points to be welded based on the positions of the welding points to be welded; In the step of determining a welding method, If the distance between the welding point to be welded and the already welded welding point exceeds a predetermined value, A current is applied to the welding point of the laminate while applying pressure thereto, so that a large current is applied to the welding point of the laminate, and then a current is applied to the welding point of the laminate while applying pressure thereto, so that a main current smaller than the large current is applied to the welding point of the laminate; When the distance between the welding point to be welded and the already welded welding point is equal to or less than a predetermined value, the welding points to be welded are welded using a welding method in which a current is passed while pressure is applied to the welding points of the laminate, a large current is passed through the welding points of the laminate, and a main current smaller than the large current is passed through the welding points of the laminate while pressure is applied to the welding points of the laminate, and a current value A13 of the running-in current is smaller than a current value A11 of the main current. A method for manufacturing a welded structure.

11. A welding apparatus for spot welding a laminate formed by stacking three or more metal plates, in which at least one of the three or more metal plates is thinner than the other metal plates, comprising: an electrode for applying pressure to the welding points of the laminate; a current generating circuit that applies a current to the welding point of the laminate pressed by the electrode; By controlling the current generating circuit, A first control that maintains the current at this current; and a second control for maintaining the current at a large current larger than the main current after maintaining the current at the main current, The period during which the main current is passed through the welding point of the laminate is t 1 is the period t during which the large current is passed through the welding point of the laminate. 2 Longer than Welding equipment.

12. A welding apparatus for spot welding a laminate formed by stacking three or more metal plates, in which at least one of the three or more metal plates is thinner than the other metal plates, comprising: an electrode for applying pressure to the welding points of the laminate; a current generating circuit that applies a current to the welding point of the laminate pressed by the electrode; By controlling the current generating circuit, A first control that maintains the current at a running-in current; a second control for maintaining the current at a running-in current and then at a high current; a current control unit that performs a third control of maintaining the current at a main current that is smaller than the large current after maintaining the current at a large current, The running-in current is smaller than the main current. Welding equipment.

Citation Information

Patent Citations

  • Resistance spot welding method of high-strength steel sheet

    JP2010172946A

  • Manufacturing method for spot welded joint

    JP2020049541A

  • Method of manufacturing spot-welding joint, spot-welding device and program

    JP2021154363A

  • Resistance spot welding method

    JP2022085358A

  • Method for manufacturing resistance spot welded joints

    JP6593572B1