Electro gas arc-welding method

The electrogas arc welding method improves workability by using a water-cooled sliding copper dowel and ceramic backing bar with a convex surface, addressing the challenges of attaching copper stoppers in varying joint shapes, thereby enhancing the welding process efficiency.

JP2024142855AActive Publication Date: 2024-10-11NIPPON STEEL WELDING & ENGINEERING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023055217
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

The existing electrogas arc welding method for butt joints of steel plates faces challenges in workability due to the use of copper stoppers that are heavy and difficult to attach, requiring matching shapes, limiting reuse when joint shapes differ.

Method used

The method employs a water-cooled sliding copper dowel and a ceramic backing bar with a convex curved surface to facilitate easy attachment and repeated use, allowing for improved workability by using a lighter material that can be easily fitted to varying groove shapes.

Benefits of technology

This approach enhances the workability of welders by enabling easy attachment of the backing bar to different groove shapes, improving the efficiency and ease of the welding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142855000001_ABST
    Figure 2024142855000001_ABST
Patent Text Reader

Abstract

To provide an electro gas arc-welding method by which improvement in workability of a welding operator is achieved.SOLUTION: An electro gas arc-welding method has: a first weld zone formation process in which a water-cooled slidable copper strap 4 is installed on a first surface f1 so as to cover at least a part of a first groove part 21 of a pair of steel plates 1, a backing rod stock 3 made of ceramics having a width L6 larger than a root gap L5 is installed by bringing a convex surface thereof into contact with a second groove part 22 so as to cover an opening bottom 220, a welding wire 6 is supplied between the water-cooled slidable copper strap 4 and the backing rod stock 3, and a first weld zone is formed; and a second weld zone formation process in which the backing rod stock 3 is removed from the second groove part 22, the water-cooled slidable copper strap 4 is removed from the first surface f1 and is installed on a second surface f2 so as to cover at least a part of the second groove part 22, the welding wire 6 is supplied between the water-cooled slidable copper strap 4 and the first well zone, and a second weld zone is formed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrogas arc welding method for welding a pair of steel plates, one pass at a time, from both surfaces of the butt joint. [Background technology]

[0002] Electrogas arc welding is a highly efficient automatic welding method that is widely used for welding large structures in the shipbuilding, energy and construction industries.

[0003] Patent Document 1 discloses a welding method for butt joints of a pair of steel plates, in which a convex copper pad is placed on one surface and a copper pad that can be tightly inserted into the groove is placed on the other surface, the center portion of the plate thickness is welded, and then the grooves on both surfaces are welded. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 55-54289 Summary of the Invention [Problem to be solved by the invention]

[0005] According to the welding method disclosed in Patent Document 1, a copper backing pad is used that has a shape that allows it to be inserted closely into the groove on one side when welding the groove on the other side. Here, the copper pad is heavier than a non-metallic pad, and cannot be easily attached to the groove as a backing pad. In addition, since the shapes of the butt joint and the copper backing pad must be matched to enable it to be inserted closely, the copper backing pad cannot be used repeatedly when the shapes of the butt joints are different. For this reason, the welding method disclosed in Patent Document 1 has a problem in that it cannot improve the workability of the welding operator.

[0006] SUMMARY OF THE PRESENT DISCLOSURE OF THE PRESENT DISCLOSURE The present invention has been devised in view of the above-mentioned problems, and has as its object to provide an electrogas arc welding method which improves the workability of the welding operator. [Means for solving the problem]

[0007] The electrogas arc welding method according to the first aspect of the present invention is an electrogas arc welding method for welding a butt joint consisting of two opposing grooves whose width gradually decreases from both surfaces of a pair of steel plates in a depth direction and which are continuous through an opening bottom, the method comprising the steps of: installing a water-cooled sliding copper backing bar which slides in the welding direction on a first surface of the pair of steel plates so as to cover at least a part of a first groove provided on the first surface of the pair of steel plates; and welding a ceramic backing bar having a width larger than the root spacing of the pair of steel plates on a second surface opposite to the first surface and continuous with the first groove. the water-cooled sliding copper pad is placed on the second surface of the second groove so as to cover at least a portion of the second groove, and a welding wire is supplied between the water-cooled sliding copper pad and the backing bar to form a first welded portion; and after the first welded portion forming step, the backing bar is removed from the second groove, the water-cooled sliding copper pad is removed from the first surface and placed on the second surface of the second groove so as to cover at least a portion of the second groove, and a welding wire is supplied between the water-cooled sliding copper pad and the first welded portion to form a second welded portion.

[0008] The electrogas arc welding method according to a second aspect of the present invention is characterized in that, in the first aspect of the present invention, the backing bar is circular in cross section. Effect of the Invention

[0009] According to the first and second inventions, the method includes a first weld forming step of placing a water-cooled sliding copper abutment on the first surface so as to cover at least a part of the first groove, placing a ceramic backing bar having a width larger than the root distance between the pair of steel plates in the second groove with the convex curved surface in contact with the opening bottom, and then supplying a welding wire between the water-cooled sliding copper abutment and the backing bar to form the first weld. That is, a ceramic backing bar that is lighter than a copper backing bar is used. Therefore, the backing bar can be easily attached to the second groove. Also, since the backing bar is placed in the second groove with the convex curved surface in contact with the backing bar, the backing bar can be easily attached. This improves the workability of the welding operator.

[0010] In particular, according to the second aspect of the present invention, the backing bar is circular in cross section. Therefore, the backing bar can be more easily attached to the second groove so as to cover the opening bottom regardless of the shape of the groove. This can further improve the workability of the welding operator. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic side view showing an example of materials to be welded and a welding machine when welding one surface in an electrogas arc welding method according to the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the AA cross section of FIG. [Diagram 3] FIG. 3 is a schematic side view showing an example of materials to be welded and a welding machine when welding the other surface in the electrogas arc welding method of the present embodiment. [Figure 4] FIG. 4 is a schematic cross-sectional view showing an example of the cross section BB of FIG. [Diagram 5] FIG. 5 is a schematic diagram showing a modified example of a water-cooled sliding copper backing used in the electrogas arc welding method of the present embodiment, where FIG. 5(a) is a front view, FIG. 5(b) is a side view, and FIG. 5(c) is a plan view. [Figure 6]6A to 6C are schematic cross-sectional views showing the cross section of FIG. 5A, where FIG. 6A is the CC cross section, FIG. 6B is the DD cross section, and FIG. 6C is the EE cross section. [Figure 7] FIG. 7 is a schematic cross-sectional view showing a modification of the cross section AA of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an example of an electrogas arc welding method according to an embodiment of the present invention will be described in detail with reference to the drawings. In each drawing, a first direction X is indicated, a direction perpendicular to the first direction X is indicated as a second direction Y, and a direction perpendicular to each of the first direction X and the second direction Y is indicated as a third direction Z. The configurations in each drawing are shown diagrammatically for the purpose of explanation, and for example, the size of each component and the size comparison between the components may differ from those in the drawing.

[0013] (Electrogas arc welding method) An example of an electrogas arc welding method in this embodiment will be described with reference to Figs. 1 to 4. The electrogas arc welding method in this embodiment is a welding method in which, as shown in Fig. 1, a groove 2 consisting of two opposing grooves 21, 22 whose width gradually decreases from both surfaces f1, f2 of a pair of steel plates 1 toward the depth direction and which are continuous through opening bottoms 210, 220 is welded as a butt joint, with both sides being welded in two layers, one pass at a time. Here, both surfaces f1, f2 refer to the first surface f1 shown in Fig. 1 and the second surface f2 opposite to the first surface f1. In addition, when the pair of steel plates 1 are arranged along a plane direction including the first direction X and the second direction Y, the depth direction refers to the direction from both surfaces f1, f2 of the pair of steel plates 1 toward the center along the third direction Z.

[0014] In the electrogas arc welding method, a groove 2 of a pair of steel plates 1 is welded by a welding equipment. Here, the welding equipment includes a backing bar 3, a water-cooled sliding copper backing 4, a welding torch 5, and a welding wire 6.

[0015] <Pair of steel plates 1> The pair of steel plates 1 are arranged, for example, along a planar direction including a first direction X and a second direction Y, spaced apart from each other to provide a predetermined root distance. The pair of steel plates 1 are provided with a groove portion 2. The pair of steel plates 1 are welded together with the groove portion 2 as a butt joint.

[0016] The pair of steel plates 1 has a dimension, for example, of a width L1 along the third direction Z of 80 mm to 100 mm.

[0017] <Bevel part 2> The groove portion 2 is composed of, for example, a first groove portion 21 provided on the first surface f1 and a second groove portion 22 provided on the second surface f2 opposite to the first surface f1. The first groove portion 21 faces the second groove portion 22. Each of the groove portions 21, 22 has an open bottom portion 210, 220 that opens at the bottom. The open bottom portion 210 of the first groove portion 21 is continuous with the open bottom portion 220 of the second groove portion 22. That is, the first groove portion 21 is continuous with the second groove portion 22 through each open bottom portion 210, 220. The groove portion 2 may be provided with a root face 23 that connects each open bottom portion 210, 220.

[0018] As for the dimensions of the groove portion 2, for example, when L1 is 100 mm, the depth L2 of the first groove portion 21 along the third direction Z is about 49 mm, the depth L3 of the second groove portion 22 along the third direction Z is about 49 mm, the width L4 of the root face 23 along the third direction Z is about 2 mm, and the width L5 of the root interval along the second direction Y is about 8 mm. In addition, as for the groove angle, for example, the groove angle of the first groove portion 21 is about 20°, and the groove angle of the second groove portion 22 is about 20° similar to the first groove portion 21. The groove angle of the second groove portion 22 may be different from the groove angle of the first groove portion 21.

[0019] Next, the backing bar 3, the water-cooled sliding copper backing 4, and the welding torch 5 used as the welding equipment will be described.

[0020] <Backing bar 3> The backing bar 3 is a backing bar used in the electrogas arc welding method. The backing bar 3 is rod-shaped with a convex curved surface on one side. When welding the first groove 21, the backing bar 3 is placed with the convex curved surface abutting against the second groove 22 so as to cover the opening bottom 220. In this case, the backing bar 3 can be easily attached to a groove having a different shape from the groove 2. This can improve the workability of the welding operator.

[0021] The backing bar 3 may be, for example, circular in cross section. In this case, the backing bar 3 can be more easily attached to the second groove portion 22 so as to cover the opening bottom portion 220 regardless of the shape of the groove portion 2. This can further improve the workability of the welding operator.

[0022] The width L6 of the backing bar 3 is larger than the width L5 of the root gap, and is, for example, 9 to 12 mm. By using this backing bar 3, it is possible to abut against the second groove portion 22 so as to cover the opening bottom 220 of the second groove portion 22.

[0023] The length of the backing bar 3 is, for example, 30 to 40 mm. For example, as shown in Fig. 2, a plurality of backing bars 3 may be attached continuously along the welding direction F1.

[0024] The backing bar 3 is made of ceramics. The composition of the backing bar 3 is not particularly limited, but may be, for example, cordierite, whose main components are alumina, silicon dioxide, and magnesium oxide. Cordierite has a lower thermal expansion coefficient than general alumina, and is excellent in thermal shock resistance and mechanical strength, and is also lighter than metals.

[0025] <Water-cooled sliding copper pad 4> The water-cooled sliding copper pad 4 is a pad made of copper used in an electrogas arc welding method. As shown in Fig. 1, for example, the water-cooled sliding copper pad 4 is installed on both surfaces f1 and f2 so as to cover at least a part of the groove portion 2. The water-cooled sliding copper pad 4 is mounted on a welding carriage (not shown), for example, and slides along both surfaces f1 and f2 as the welding of the groove portion 2 progresses.

[0026] The water-cooled sliding copper contact 4 includes a contact block 41 and a shielding gas hood 42. The surfaces of the contact block 41 that are placed on both surfaces f1 and f2 have installation surfaces 41a and 41b, and a concavely curved groove 43 provided between the installation surfaces 41a and 41b. When the water-cooled sliding copper contact 4 is placed on both surfaces f1 and f2, the installation surfaces 41a and 41b come into contact with both surfaces f1 and f2, and the groove 43 of the contact block 41 covers at least a part of the groove portion 2.

[0027] For example, a cold water pipe 411 is inserted inside the contact block 41. When cold water flows inside the cold water pipe 411, the vicinity of the groove 43 of the contact block 41 is cooled.

[0028] The shielding gas hood 42 has, for example, a gas pipe 421 inserted therein. The shielding gas hood 42 blows a shielding gas such as carbon dioxide gas toward the groove portion 2, thereby isolating the region of the groove portion 2 covered with the water-cooled sliding copper backing 4 from the atmosphere.

[0029] <Welding torch 5> A welding torch 5 supplies a welding wire 6 to a region of the groove 2 that is covered with the water-cooled sliding copper backing 4. The welding torch 5 is mounted on, for example, a welding carriage (not shown), and slides along both surfaces f1, f2 as the welding of the groove 2 progresses.

[0030] <Welding wire 6> The welding wire 6 is supplied to a region of the groove 2 that is covered with the water-cooled sliding copper pad 4, and melts while generating an arc in the groove 2 to form molten metal. The molten metal that fills the groove 2 is cooled by the water-cooled sliding copper pad 4 and solidifies to form a weld bead.

[0031] The material of the welding wire 6 may be, for example, a flux-cored wire for electrogas arc welding described in "JIS Z 3319:1999 / AMENDMENT 1:2007" or a known solid wire for electrogas arc welding.

[0032] Next, the procedure of the electrogas arc welding method will be described. The electrogas arc welding method has a first welded portion forming step and a second welded portion forming step. In the electrogas arc welding method, the second welded portion forming step is carried out after the first welded portion forming step. Note that, although a method in which an operator carries out various steps will be described in this embodiment, at least some of the steps may be carried out via a control device externally connected to various welding machines.

[0033] <First weld formation process> In the first weld forming step, as shown in FIG. 2, the worker places the water-cooled sliding copper pad 4 on the first surface f1 so as to cover at least a part of the first groove 21, and places the backing bar 3 on the second groove 22 with the convex curved surface in contact with the opening bottom 220. Thereafter, the worker slides the water-cooled sliding copper pad 4 in the welding direction F1, blows shielding gas into the first space Q1 between the water-cooled sliding copper pad 4 and the backing bar 3, and supplies the welding wire 6 to form the first weld 81, which is a weld bead. In detail, the welding wire 6 supplied by the heat of an arc (not shown) generated between the welding wire 6 and the molten pool 71 melts, and is cooled by the water-cooled sliding copper pad 4 to form the first weld 81. The backing bar 3 is supported by a metal plate 31 (made of steel), for example, so that it can be detachably attached near the opening bottom 220 of the second groove 22. The metal plate 31 is supported by, for example, one or more steel restraint plates 33 temporarily welded to the second surfaces f2 of the pair of steel plates 1. An operator may, for example, drive a steel wedge 32 between the metal plate 31 and the restraint plate 33 to make the backing bar 3 more firmly supported by the metal plate 31. Note that since the temporarily welded portion can be easily destroyed by applying an impact to the restraint plate 33, an operator can easily remove the restraint plate 33 from the second surfaces f2 by, for example, hitting the restraint plate 33 with a hammer or the like after forming the first weld portion 81.

[0034] In this case, the backing bar 3, which is lighter than a copper backing metal, can be easily attached to the second groove portion 22. This improves the workability of the welding operator. In addition, since the backing bar 3 is made of ceramics having a higher melting point than the welding wire 6, it is partially melted by the molten pool 71. After that, a part of the melted backing bar 3 becomes part of the molten slag 91 generated on the molten pool 71 formed in the groove.

[0035] Molten slag 91 is generated on the molten pool 71. The molten slag 91 is appropriately discharged from between the first welded portion 81 to be formed and the groove 43 of the water-cooled sliding copper contact 4 (molten slag 910). The discharged molten slag 910 improves the appearance of the first welded portion 81 in the groove 43 while covering the surface of the first welded portion 81. In addition, since the melting point of the molten slag 910 is lower than the melting point of the first welded portion 81, the molten slag 910 solidifies in the middle of the groove 43 as it moves in the welding direction F1, becoming solidified slag 911. The solidified slag 911 is removed from the surface of the first welded portion 81 after the first welded portion 81 is formed.

[0036] <Second weld formation process> After the first welded portion forming step, in a second welded portion forming step, the worker removes the backing bar 3 from the second groove portion 22, as shown in Fig. 3, for example. In addition, the worker removes the water-cooled sliding copper pad 4 from the first surface f1 and installs it on the second surface f1 so as to cover at least a part of the second groove portion 22.

[0037] 4, the worker slides the water-cooled sliding copper pad 4 in the welding direction F1 while supplying the welding wire 6 into the second space Q2 between the water-cooled sliding copper pad 4 and the first welded portion 81 to form a weld bead, that is, a second welded portion 82. In more detail, the welding wire 6 is melted while an arc is generated between the welding wire 6 and the molten pool 72, and a molten metal is formed.

[0038] Molten slag 92 is generated on the molten pool 72. The molten slag 92 is appropriately discharged from between the second welded portion 82 to be formed and the groove 43 of the water-cooled sliding copper abutment 4 (molten slag 920). The molten slag 920 improves the appearance of the second welded portion 82 in the groove 43 while covering the surface of the second welded portion 82. In addition, since the melting point of the molten slag 920 is lower than the melting point of the second welded portion 82, the molten slag 920 solidifies in the middle of the groove 43 as it moves in the welding direction F1, becoming solidified slag 921. The solidified slag 921 is removed from the surface of the second welded portion 82 after the second welded portion 82 is formed.

[0039] The electrogas arc welding method is completed by carrying out the above-mentioned steps. The welding direction in the first weld forming step may be different from the welding direction in the second weld forming step. In addition, when the first weld forming step is carried out with the first groove portion 21 facing upward and the second groove portion 22 facing downward, the pair of steel plates 1 may be rotated so that the second groove portion 22 faces upward, and then the second weld forming step may be carried out.

[0040] In addition, in the present embodiment, a one-electrode welding method using one welding torch 5 and one welding wire 6 has been described, but a so-called two or more electrode welding method using two or more welding torches 5 and two or more welding wires 6 may also be applied. In this case, as the welding wire 6, two or more flux-cored wires for electrogas arc welding may be used, two or more solid wires for electrogas arc welding may be used, or a combination of these may be used.

[0041] (Modification of electrogas arc welding method) A modified example of the electrogas arc welding method in this embodiment will be described with reference to Fig. 5 to Fig. 7. The electrogas arc welding method of this modified example uses a water-cooled sliding copper backing 4 having a shape shown in Fig. 5.

[0042] 5(a) shows the surface of the water-cooled sliding copper pad 4 facing both surfaces f1 and f2 of the pair of steel plates 1, FIG. 5(b) shows the right side surface of the water-cooled sliding copper pad 4 shown in FIG. 5(a), and FIG. 5(c) shows the upper surface of the water-cooled sliding copper pad 4 shown in FIG. 5(a). The groove 43 of the water-cooled sliding copper pad 4 is composed of a first groove 431 parallel to both surfaces f1 and f2 for forming the welded portion 8, and a second groove 432 for discharging the molten slags 910 and 920. One end of the second groove 432 is continuous with one end of the first groove 431.

[0043] 6(a) to 6(c) show a cross section of the contact block 41 which is the base of the water-cooled sliding copper contact 4. In detail, Fig. 6(a) shows a CC cross section of the water-cooled sliding copper contact 4 shown in Fig. 5(a), Fig. 6(b) shows a DD cross section of the water-cooled sliding copper contact 4 shown in Fig. 5(a), and Fig. 6(c) shows an EE cross section of the water-cooled sliding copper contact 4 shown in Fig. 5(a).

[0044] The width W2 and depth D2 of the second groove 432 in the DD cross section are larger than the width W1 and depth D1 of the first groove 431 in the CC cross section. Moreover, the width W3 and depth D3 of the second groove 432 in the EE cross section are larger than the width W2 and depth D2 of the second groove 432 in the DD cross section. That is, the groove width of the second groove 432 is continuously larger and deeper from one end portion connected to the first groove 431 toward the other end portion. Specifically, the groove width of the second groove 432 is continuously larger, inclined by θ1 with respect to the groove width of the first groove 431, for example, in the plan view shown in FIG. 5(a). Moreover, the groove width of the second groove 432 is continuously deeper, inclined by θ2 with respect to the groove width of the first groove 431, for example, in the side view shown in FIG. 5(b).

[0045] By using this water-cooled sliding copper abutment 4, as shown in Fig. 7, the molten slag 91 on the molten pool 71 is discharged more smoothly from between the first welded portion 81 to be formed and the groove 43 of the water-cooled sliding copper abutment 4 (molten slag 910a). In this case, it is easy to maintain an appropriate amount of molten slag 91 on the molten pool 71, and slag splashing is reduced, making it possible to perform welding for a long time. The discharged molten slag 910a solidifies in the middle of the groove 43 as it moves in the welding direction F1, becoming solidified slag 911a.

[0046] If the second groove 432 has a width that is parallel to the first groove 431 and a depth that increases continuously, depending on the width L1 of the pair of steel sheets 1, the amount of molten slag 91 on the molten pool 71 may increase, and the molten slag 91 may not be sufficiently discharged, resulting in slag splashing. Also, if the inclination angle θ2 is set too large in order to improve the dischargeability of the molten slag 91, the molten metal may flow out of the molten pool 71, causing the welding to be interrupted.

[0047] For this reason, in the water-cooled sliding copper backing 4 of the present invention, it is preferable that the second groove 432 is inclined by θ1 = 5 to 30° in the width direction relative to the first groove 431 to continuously increase in size, and is inclined by θ2 = 2 to 10° in the depth direction to continuously increase in size. In this case, the molten metal is not discharged from the molten pool 71, and only the molten slag 91 on the molten pool 71 is smoothly discharged, and no slag splashing occurs. This allows welding for a long time, and further improves the workability of the welding operator.

[0048] According to this embodiment, the water-cooled sliding copper abutment 4 is installed on the first surface f1 so as to cover at least a part of the first groove portion 21, and a ceramic backing bar 3 having a width L6 larger than the root distance L5 of the pair of steel plates 1 is installed on the second groove portion 22 with a convex curved surface in contact with the opening bottom portion 220, and then a welding wire 6 is supplied between the water-cooled sliding copper abutment 4 and the backing bar 3 to form a first welded portion 81. That is, a ceramic backing bar 3 that is lighter than a copper backing bar is used. Therefore, the backing bar 3 can be easily attached to the second groove portion 22. In addition, since the backing bar 3 is installed with a convex curved surface in contact with the second groove portion 22, it can be easily attached to a groove portion having a shape different from that of the groove portion 2. This can improve the workability of the welding operator.

[0049] According to the present embodiment, the backing bar 3 is circular in cross section. Therefore, the backing bar 3 can be more easily attached to the second groove 22 so as to cover the opening bottom 220 regardless of the shape of the groove 2. This can further improve the workability of the welding operator.

[0050] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0051] 1 pair of steel plates 1a, 1b steel plate 2 Bevel section 21 1st groove section 210 (First groove) opening bottom 22 2nd groove section 220 (Second groove) opening bottom 23 Root Face 3 Backing bar 31 Metal plate 32 Wedge 33 Restraint plate 4 Water-cooled sliding copper pad 41 Gold Block 41a, 41b Installation surface 411 Cold water pipe 42 Shielded Gas Hood 421 Gas Pipe 43 Groove 431 First Groove 432 Second Groove 5. Welding torch 6 Welding Wire 7, 71, 72 Molten pool 8 Welding 81 First Welding Section 82 Second Welding Section 9, 91, 92 Molten slag f1 1st surface f2 2nd surface F1 Welding direction Q1 1st space Q2 2nd space

Claims

1. An electrogas arc welding method for welding a pair of steel plates to a butt joint having two opposing grooves whose widths gradually decrease from both surfaces in a depth direction and continue through an opening bottom, comprising: a first weld formation process in which a water-cooled sliding copper backing metal that slides in a welding direction is placed on a first surface of a pair of steel plates so as to cover at least a part of a first groove provided on the first surface, a ceramic backing bar having a width larger than the root spacing of the pair of steel plates is placed on a second surface opposite to the first surface, the second groove being continuous with the first groove, with its convex curved surface in contact with the second groove so as to cover an opening bottom, and a welding wire is supplied between the water-cooled sliding copper backing metal and the backing bar to form a first weld; a second weld forming step of removing the backing bar from the second groove after the first weld forming step, removing the water-cooled sliding copper pad from the first surface and placing it on the second surface so as to cover at least a portion of the second groove, and then supplying a welding wire between the water-cooled sliding copper pad and the first weld to form a second weld; Having Electrogas arc welding method comprising:

2. The backing bar is circular in cross section.

2. The electrogas arc welding method according to claim 1 .

Citation Information

Patent Citations

  • Multilayer builddup electrogas welding method

    JP1980054289A

  • JP1981156478U

  • Backing strip device for butt joint welding

    JP1996281485A

  • Backing for welding

    JP1999156590A

  • Wire for electroslag weldment, flux for electroslag weldment, and weld joint

    JP2018043288A