Method for manufacturing pellet, resin composition, pellet and molded article
By blending flat glass fibers with a sizing agent into polyamide resin and using a twin-screw extruder at specific conditions, the method addresses the need for high-strength polyamide resin pellets and molded articles, achieving enhanced mechanical properties and stability.
Patent Information
- Application Number
- JP2023055309
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
There is a need for polyamide resin pellets that can produce molded articles with higher mechanical strength, and a stable method to manufacture such pellets is required.
A method involving blending flat glass fibers with a sizing agent and/or surface treatment agent into polyamide resin, using a twin-screw kneading extruder at specific temperatures and conditions to create pellets with enhanced mechanical properties.
The method produces pellets and molded articles with excellent mechanical strength and stability, achieving improved adhesion and mechanical properties through the use of flat glass fibers and controlled processing conditions.
Smart Images

Figure 2024142910000001 
Figure 2024142910000002 
Figure 2024142910000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing pellets, a resin composition, pellets, and molded articles, and more particularly to a method for producing pellets containing a polyamide resin as a main component. [Background technology]
[0002] Polyamide resin, a representative engineering plastic, is easy to process and has excellent mechanical properties, electrical properties, heat resistance, and other physical and chemical properties, and is therefore widely used in vehicle parts, electrical and electronic equipment parts, and other precision equipment parts (Patent Document 1, etc.). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-143023 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, the applications of polyamide resins have expanded, and molded articles made from polyamide resins are required to have higher mechanical strength. Furthermore, it is required to stably provide pellets for producing such molded articles having high mechanical strength. The present invention aims to solve the above problems, and to provide a resin composition containing a polyamide resin, a method for producing pellets that can provide molded articles having excellent mechanical strength, a resin composition, and pellets and molded articles. Another object of the present invention is to provide a method for producing pellets that can stably provide pellets containing a polyamide resin. [Means for solving the problem]
[0005] In light of the above-mentioned problems, the present inventors have conducted research and found that the above-mentioned problems can be solved by blending flat glass fibers containing a specified sizing agent and / or surface treatment agent with a polyamide resin. Specifically, the above problems were solved by the following means. <1> The composition contains 150 to 230 parts by mass of flat glass fibers containing a bundling agent and / or a surface treatment agent per 100 parts by mass of polyamide resin, A method for producing pellets of a resin composition, comprising heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes to obtain a gas component containing xylylene diisocyanate, The method for producing pellets of the resin composition comprises using a twin-screw kneading extruder, and the temperature of the resin composition at the die discharge outlet of the twin-screw kneading extruder is 323 to 355°C. <2> The polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid. <1> A method for producing the pellets described in claim 1. <3> The difference between the temperature of the resin composition at the die outlet of the twin-screw kneading extruder and the melting point of the polyamide resin is 77° C. or more. <1> or <2> A method for producing the pellets described in claim 1. <4> The proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280°C for 10 minutes is 55 to 90 mass%. <1> ~ <3> 13. A method for producing pellets according to any one of the preceding claims. <5> The mass loss rate of the flat glass fiber when heated at 600° C. for 2 hours is 0.7 to 1.0% by mass. <1> ~ <4> 13. A method for producing pellets according to any one of the preceding claims. <6> The polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine. <1> ~ <5> 13. A method for producing pellets according to any one of the preceding claims. <7> The polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid; the difference between the temperature of the resin composition at the die outlet of the twin-screw kneading extruder and the melting point of the polyamide resin is 77° C. or more; The proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes is 55 to 90 mass %; The mass loss rate of the flat glass fiber when heated at 600° C. for 2 hours is 0.7 to 1.0% by mass, The polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine. <1> ~ <6> 13. A method for producing pellets according to any one of the preceding claims. <8> The composition contains 150 to 230 parts by mass of flat glass fibers containing a bundling agent and / or a surface treatment agent per 100 parts by mass of polyamide resin, A resin composition, wherein the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280°C for 10 minutes contains xylylene diisocyanate. <9> The polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid. <8> The resin composition according to claim 1. <10> The proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280°C for 10 minutes is 55 to 90 mass%. <8> or <9> The resin composition according to claim 1. <11> The mass loss rate of the flat glass fiber when heated at 600° C. for 2 hours is 0.7 to 1.0% by mass. <8> ~ <10> 10. The resin composition according to claim 9 . <12> The polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine. <8> ~ <11> 10. The resin composition according to claim 9 . <13> The polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid; The proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes is 55 to 90 mass %; The mass loss rate of the flat glass fiber when heated at 600° C. for 2 hours is 0.7 to 1.0% by mass, The polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine. <8> ~ <12> 10. The resin composition according to claim 9 . <14> <8> ~ <13> 2. A pellet of the resin composition according to claim 1. <15> <8> ~ <13> 2. A molded article formed from the resin composition according to claim 1. Effect of the Invention
[0006] According to the present invention, it is possible to provide a resin composition containing a polyamide resin, a method for producing pellets capable of providing a molded article having excellent mechanical strength, a resin composition, and pellets and molded articles. It has also become possible to produce pellets that can stably provide pellets containing polyamide resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified.
[0008] If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2023, unless otherwise stated.
[0009] The resin composition of this embodiment is characterized in that it contains 150 to 230 parts by mass of flat glass fibers containing a bundling agent and / or a surface treatment agent (hereinafter sometimes referred to as "surface treatment agent, etc.") per 100 parts by mass of polyamide resin, and the gas component obtained by heating the bundling agent and / or surface treatment agent of the flat glass fibers at 280°C for 10 minutes contains xylylene diisocyanate. By adopting such a configuration, a resin composition capable of providing a molded product having excellent mechanical strength can be obtained. That is, by limiting the type of sizing agent and using flat glass, the mechanical strength of the molded product obtained from the resin composition can be increased. In addition, by adjusting the temperature of the resin during extrusion and the content of the flat glass, it is possible to provide pellets of the resin composition that can be produced stably and have excellent mechanical properties.
[0010] <Polyamide resin> The resin composition of the present embodiment contains a polyamide resin. The polyamide resin used in the present embodiment is not particularly limited, and any known polyamide resin can be used. The polyamide resin may be an aliphatic polyamide resin or a semi-aromatic polyamide resin. Examples of aliphatic polyamide resins include polyamide 4, polyamide 46, polyamide 6, polyamide 66, polyamide 666, polyamide 610, polyamide 11, polyamide 12, and the like. The polyamide resin used in the present embodiment is preferably a semi-aromatic polyamide resin. Here, the semi-aromatic polyamide resin is composed of a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 30 to 70 mol% of the total structural units of the diamine-derived structural unit and the dicarboxylic acid-derived structural unit are structural units containing an aromatic ring, and it is preferable that 40 to 60 mol% of the total structural units of the diamine-derived structural unit and the dicarboxylic acid-derived structural unit are structural units containing an aromatic ring. By using such a semi-aromatic polyamide resin, the mechanical strength of the obtained resin molded product can be increased. Examples of semi-aromatic polyamide resins include terephthalic acid-based polyamide resins (polyamide 6T, polyamide 9T) and xylylenediamine-based polyamide resins described later.
[0011] The polyamide resin used in this embodiment contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and is preferably a polyamide resin in which 70 mol% or more of the diamine-derived structural unit is derived from xylylenediamine (hereinafter, sometimes referred to as a "xylylenediamine-based polyamide resin"). By using a xylylenediamine-based polyamide resin, compatibility with xylylenediisocyanate is excellent, and the mechanical strength of the obtained molded product tends to be further improved. The diamine-derived constituent units of the xylylenediamine-based polyamide resin are preferably derived from xylylenediamine (preferably paraxylylenediamine and / or metaxylylenediamine, more preferably metaxylylenediamine) at 75 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, still more preferably 95 mol% or more, and particularly preferably 99 mol% or more. The dicarboxylic acid-derived constituent units of the xylylenediamine-based polyamide resin are preferably derived from α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms at 70 mol% or more, more preferably 75 mol% or more, even more preferably 80 mol% or more, still more preferably 90 mol% or more, still more preferably 95 mol% or more, and particularly preferably 99 mol% or more. Paraxylylenediamine and metaxylylenediamine may be used in combination. When these are used in combination, the molar ratio of metaxylylenediamine and paraxylylenediamine in the xylylenediamine is preferably 10 to 100 / 90 to 0, more preferably 30 to 100 / 70 to 0, even more preferably 50 to 100 / 50 to 0, even more preferably 80 to 100 / 20 to 0, and even more preferably 90 to 100 / 10 to 0, when the total of metaxylylenediamine and paraxylylenediamine is 100 moles.
[0012] Diamines other than metaxylylenediamine and paraxylylenediamine that can be used as the raw diamine component of the xylylenediamine-based polyamide resin include aliphatic diamines such as tetramethylenediamine, pentamethylenediamine, 2-methylpentanediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine, 1,3-bis( Examples of the diamines include alicyclic diamines such as bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminomethyl)decalin, and bis(aminomethyl)tricyclodecane; and diamines having an aromatic ring such as bis(4-aminophenyl)ether, paraphenylenediamine, and bis(aminomethyl)naphthalene. These can be used alone or in combination of two or more.
[0013] In the xylylenediamine-based polyamide resin, 70 mol % or more of the constitutional units derived from dicarboxylic acid are preferably derived from α,ω-linear aliphatic dicarboxylic acid having 4 to 20 carbon atoms. Examples of α,ω-linear aliphatic dicarboxylic acids having 4 to 20 carbon atoms that are suitable for use as the raw dicarboxylic acid component of the xylylenediamine-based polyamide resin include aliphatic dicarboxylic acids such as succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, adipic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid. One or a mixture of two or more of these can be used. Among these, adipic acid or sebacic acid are more preferred, and adipic acid is even more preferred, since the melting point of the polyamide resin falls within a range suitable for molding. A preferred embodiment of the xylylenediamine-based polyamide resin in this embodiment is one in which 50 mol % or more (preferably 70 mol % or more, more preferably 90 mol % or more) of the constitutional units derived from dicarboxylic acid are derived from adipic acid.
[0014] Examples of dicarboxylic acid components other than the above-mentioned α,ω-linear aliphatic dicarboxylic acids having 4 to 20 carbon atoms include phthalic acid compounds such as isophthalic acid, terephthalic acid, and orthophthalic acid, and isomers of naphthalenedicarboxylic acids such as 1,2-naphthalenedicarboxylic acid, 1,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid. These can be used alone or in combination of two or more kinds.
[0015] In addition, the xylylenediamine-based polyamide resin is mainly composed of diamine-derived structural units and dicarboxylic acid-derived structural units, but does not completely exclude other structural units, and may contain lactams such as ε-caprolactam and laurolactam, and aliphatic aminocarboxylic acid-derived structural units such as aminocaproic acid and aminoundecanoic acid. Here, the main component means that the total number of diamine-derived structural units and dicarboxylic acid-derived structural units is the largest among all structural units among the structural units constituting the xylylenediamine-based polyamide resin. In this embodiment, the total of diamine-derived structural units and dicarboxylic acid-derived structural units in the xylylenediamine-based polyamide resin preferably accounts for 90% by mass or more of all structural units, more preferably accounts for 95% by mass or more, even more preferably accounts for 97% by mass or more, and even more preferably accounts for 99% by mass or more.
[0016] The relative viscosity of the polyamide resin is preferably 2.0 or more, more preferably 2.1 or more. The upper limit of the relative viscosity is not particularly set, but may be, for example, 2.5 or less, or even 2.3 or less. When the resin composition of the present embodiment contains two or more types of polyamide resins, the relative viscosity refers to the relative viscosity of a mixture of the polyamide resins. The relative viscosity is determined by the following method. Weigh out 0.2 g of polyamide resin and dissolve it in 20 mL of 96% by weight sulfuric acid at 25°C with stirring. After complete dissolution, immediately transfer 5 mL of the solution to a Cannon-Fenske viscometer and leave it in a thermostatic bath at 25°C for 10 minutes, then measure the drop time (t) of the solution. Also measure the drop time (t0) of 96% by weight sulfuric acid itself under the same conditions. Calculate the relative viscosity from t and t0 using the following formula. Relative viscosity=t / t0
[0017] The melting point of the polyamide resin is preferably 150 to 350° C., more preferably 180 to 330° C., even more preferably 200 to 330° C., and still more preferably 200 to 320° C. When the resin composition of the present embodiment contains two or more types of polyamide resins, the melting point is the melting point of the polyamide resin contained in the largest amount.
[0018] In this specification, the melting point (Tm) is a value measured by differential scanning calorimetry (DSC) in accordance with ISO11357. A differential scanning calorimeter is used, and the resin is placed in the measurement pan of the differential scanning calorimeter, heated to a temperature above the melting point at a heating rate of 10°C / min under a nitrogen atmosphere, and then rapidly cooled before measurement. The measurement conditions are a heating rate of 10°C / min, held at 280°C for 5 minutes, and then cooled down to 100°C at a cooling rate of -5°C / min to determine the melting point (Tm). As the differential scanning calorimeter, a "DSC-60" manufactured by SHIMADZU CORPORATION is used.
[0019] The lower limit of the number average molecular weight (Mn) of the polyamide resin is preferably 6,000 or more, more preferably 8,000 or more, and even more preferably 10,000 or more, and is preferably 35,000 or less, more preferably 30,000 or less, even more preferably 25,000 or less, and even more preferably 20,000 or less. In such a range, the heat resistance, elastic modulus, dimensional stability, and moldability are improved. When the resin composition of the present embodiment contains two or more polyamide resins, the number average molecular weight is the number average molecular weight of the mixture.
[0020] The number average molecular weight (Mn) of polyamide resin is measured by gel permeation chromatography (GPC) using a standard polymethyl methacrylate (PMMA) equivalent value. Two columns packed with styrene polymers are used as the packing material, and hexafluoroisopropanol (HFIP) with a sodium trifluoroacetate concentration of 2 mmol / L is used as the solvent. The resin concentration is 0.02 mass%, the column temperature is 40°C, the flow rate is 0.3 mL / min, and the measurement is performed using a refractive index detector (RI). In addition, the calibration curve is measured by dissolving six levels of PMMA in HFIP.
[0021] The content of the polyamide resin in the resin composition of the present embodiment is preferably 20% by mass or more, more preferably 25% by mass or more, and may be 28% by mass or more in the resin composition. By making it equal to or more than the lower limit, the content of the flat glass fiber tends to be suppressed to a certain extent, and the flowability balance tends to be easily adjusted. In addition, the content of the polyamide resin in the resin composition of the present embodiment is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 42% by mass or less in the resin composition. By making it equal to or less than the upper limit, the compounding ratio of the flat glass fiber increases, and high physical properties in terms of rigidity and strength tend to be easily obtained. In particular, when the polyamide resin contained in the resin composition of the present embodiment is taken as 100 parts by mass, the proportion of the xylylenediamine-based polyamide resin therein is preferably 80 to 100 parts by mass. The resin composition of the present embodiment may contain only one type of polyamide resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range. In addition, in the resin composition of this embodiment, the total of the polyamide resin and the flat glass fibers preferably accounts for 90 mass% or more of the resin composition, more preferably 95 mass% or more, and preferably 100 mass% or less.
[0022] <Glass fiber> The resin composition of the present embodiment is characterized in that it contains flat glass fibers containing a bundling agent and / or a surface treatment agent, and the gas component obtained by heating the bundling agent and / or the surface treatment agent of the flat glass fibers at 280°C for 10 minutes contains xylylene diisocyanate. By using such a surface treatment agent, the adhesion between the polyamide resin and the flat glass fibers can be improved. In addition, by using flat glass, the adhesion area of the surface treatment agent, etc. increases, and the adhesion with the polyamide resin is improved. When the adhesion between the polyamide resin and the flat glass fibers is improved, the mechanical strength of the obtained molded product is improved. In addition, since the adhesion strength is high, even if a break point occurs, the break can be suppressed because there are many points of adhesion.
[0023] As the glass fiber, a fiber obtained by melt spinning a glass such as E glass, C glass, A glass, S glass, D glass, R glass, and alkali-resistant glass that is generally supplied is used, but any glass fiber that can be used is not particularly limited. In the present embodiment, it is preferable to include E glass.
[0024] The glass fiber used in this embodiment contains a sizing agent and / or a surface treatment agent (such as a surface treatment agent). The surface treatment agent is usually present on the surface of the glass fiber. The surface treatment agent is heated at 280°C for 10 minutes, and the gas component obtained contains xylylene diisocyanate (preferably metaxylylene diisocyanate). This configuration tends to improve adhesion to xylylene diamine polyamide resin. In the flat glass fiber used in this embodiment, when the glass fiber is heated at 280°C for 10 minutes and the gas generated is analyzed by TD GC / MS, the proportion of xylylene diisocyanate gas in 100% by mass of gas is preferably 1% by mass or more, more preferably 3% by mass or more, and preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, and even more preferably 6% by mass or less. The gas components of the flat glass fiber used in the present embodiment are preferably substantially free of isophorone diisocyanate. Substantially free means that the gas is contained in an amount of 1% by mass or less, preferably 0.5% by mass or less, and may be less than 0.1% by mass, based on 100% by mass of the gas.
[0025] In this embodiment, it is preferable that the gas component obtained by heating the surface treatment agent etc. at 280° C. for 10 minutes further contains dimethylalkylamine gas.
[0026] The proportion of dimethylalkylamine gas in the flat glass fiber used in this embodiment is, when the surface treatment agent of the flat glass fiber is heated at 280°C for 10 minutes and the gas generated is analyzed by TD GC / MS, preferably 55 mass% or more, more preferably 60 mass% or more, and even more preferably 65 mass% or more, out of 100 mass% of gas, and is usually 90 mass% or less, preferably 85 mass% or less, and even more preferably 80 mass% or less. In this embodiment, the generated gas may contain only one type of dimethylalkylamine gas, or may contain two or more types. When two or more types of dimethylalkylamine gas are contained, it is preferable that the total amount is within the above range.
[0027] The surface treatment agent or the like used in the present embodiment preferably contains a urethane-based sizing agent. The urethane-based sizing agent is usually obtained from an isocyanate and an alcohol. The urethane-based sizing agent used in the present embodiment preferably contains xylylene diisocyanate as an isocyanate component.
[0028] In this embodiment, in the 100% by mass of the gas, the total amount of xylylene diisocyanate and dimethylalkylamine is preferably 60% by mass or more, more preferably 65% by mass or more, and even more preferably 69% by mass or more, and is preferably 90% by mass or less, and more preferably 88% by mass or less.
[0029] The flat glass fiber used in this embodiment has a mass reduction rate of preferably 0.7% by mass or more, more preferably 0.75% by mass or more, even more preferably 0.80% by mass or more, even more preferably 0.85% by mass or more, and even more preferably 0.90% by mass or more when heated at 600°C for 2 hours. By setting the mass reduction rate to the lower limit or more, the adhesion between the glass fiber and the polyamide resin tends to be further improved. In addition, the mass reduction rate of the flat glass fiber used in this embodiment when heated at 600°C for 2 hours is preferably 1.0% by mass or less, more preferably 0.95% by mass or less. By setting the mass reduction rate to the upper limit or less, the defibrability of the glass fiber tends to be further improved. The mass reduction rate is measured according to the description in the Examples section below.
[0030] The cross section of the glass fiber used in this embodiment is flat. Flat means that the cross section of the glass fiber is noncircular, and includes elliptical and oval shapes. Here, the flat glass used in this embodiment preferably has an aspect ratio of 1.1 or more, more preferably 2.0 or more, and even more preferably 3.0 or more, and preferably 10.0 or less, more preferably 8.0 or less, and even more preferably 6.0 or less. By setting the aspect ratio to the lower limit or more, the surface area of the glass fiber cross section increases, improving the adhesion between the glass fiber and the polyamide resin, and further effectively improving the warping and molding shrinkage of the molded product. In addition, by setting the aspect ratio to the upper limit or less, crushing of the glass fiber due to the load applied to the polyamide resin during mixing and kneading with the polyamide resin or molding of the resin composition can be effectively suppressed. Here, the flattening is defined as follows. Flattening ratio = Long diameter of glass fiber cross section (d1) / Short diameter of glass fiber cross section (d2) In other words, the (d1) / (d2) ratio indicates the degree of flatness of the cross section of the glass fiber. The flatness can be determined by observing the cross section of the glass fiber under a microscope and measuring the actual dimensions of the long diameter (d1) and short diameter (d2) of the cross section of the glass fiber. An electron microscope is used for the measurement, and the average value is taken from the values of 100 pieces randomly taken. The cross-sectional area of the glass fiber is also measured in the same manner.
[0031] Examples of the flat shape of the glass fiber include a cocoon shape with a constricted central portion in the longitudinal direction as shown in (A) of FIG. 1 of JP-A-62-268612, an oval shape with a portion that is approximately parallel to the center of gravity of the cross section as shown in (B), and an ellipse shape as shown in (C). When the flat shape is a cocoon shape, the major axis (d1) in this embodiment corresponds to a in FIG. 1 (A) of JP-A-62-268612, and the minor axis (d2) corresponds to b. When the flat shape is an oval shape, the major axis (d1) corresponds to a in FIG. 1 (B) of Patent Document 2, and the minor axis (d2) corresponds to b. When the flat shape is an ellipse shape, the major axis (d1) corresponds to a in FIG. 1 (C) of Patent Document 2, and the minor axis (d2) corresponds to b.
[0032] The cross-sectional diameter (equivalent circle diameter) of the flat glass used in this embodiment is preferably 10 μm or more, more preferably 12 μm or more, and is preferably 20 μm or less, more preferably 18 μm or less. The equivalent circle diameter means the diameter of a circle having the same area as the cross-sectional area of the flat glass.
[0033] The flat glass fiber used in the present embodiment has a number average fiber length of preferably 100 μm or more, more preferably 150 μm or more, and even more preferably 200 μm or more. The upper limit is preferably 7 mm or less, more preferably 6 mm or less, and even more preferably 5 mm or less. In this embodiment, the flat glass fibers are preferably chopped strands.
[0034] The content of the flat glass fiber in the resin composition of the present embodiment is 150 parts by mass or more relative to 100 parts by mass of the polyamide resin, and may be 160 parts by mass or more, 170 parts by mass or more, 180 parts by mass or more, 190 parts by mass or more, or 200 parts by mass or more depending on the application. By making it equal to or more than the above lower limit, the mechanical strength can be improved. In addition, the content of the glass fiber in the resin composition of the present embodiment is 230 parts by mass or less, preferably 225 parts by mass or less, and more preferably 220 parts by mass or less relative to 100 parts by mass of the polyamide resin. On the other hand, by making the amount of the flat glass fiber equal to or less than the above upper limit, the appearance of the obtained molded product tends to be further improved. The content of the flat glass fibers in the resin composition of the present embodiment is preferably 55 to 70 mass % relative to 100 mass % of the resin composition. The resin composition of the present embodiment may contain only one type of flat glass fiber, or may contain two or more types. When two or more types are contained, the total amount is preferably within the above range.
[0035] The resin composition of this embodiment may or may not contain a reinforcing filler other than the flat glass fiber containing a predetermined surface treatment agent. It is preferable that the resin composition of this embodiment does not substantially contain a reinforcing filler other than the flat glass fiber containing a predetermined surface treatment agent. "Substantially free" means that the content of the reinforcing filler other than the flat glass fiber containing a predetermined surface treatment agent is 10% by mass or less of the content of the flat glass fiber containing a predetermined surface treatment agent contained in the resin composition, preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less.
[0036] <Nucleating agent> The resin composition of the present embodiment may contain a nucleating agent. By containing the nucleating agent, the appearance of the obtained molded article can be improved. The nucleating agent is preferably talc. The talc used may be surface-treated with at least one compound selected from polyorganohydrogensiloxanes and organopolysiloxanes. In this case, the amount of the siloxane compound attached to the talc is preferably 0.1 to 5 parts by mass of the talc.
[0037] When the resin composition of this embodiment contains a nucleating agent, the content thereof is preferably 0.1 parts by mass or more, and preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1.2 parts by mass or less, per 100 parts by mass of the resin composition. The resin composition of the present embodiment may contain only one type of nucleating agent, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0038] <Release agent> The resin composition of the present embodiment preferably contains a release agent. The release agent is mainly used to improve the productivity during molding of the resin composition. Examples of the release agent include aliphatic carboxylic acid amides, aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15000, polysiloxane silicone oils, and higher fatty acid metal salts, and higher fatty acid metal salts are preferred. The higher fatty acid constituting the higher fatty acid metal salt is preferably a fatty acid having 8 or more carbon atoms, more preferably a fatty acid having 8 to 40 carbon atoms. The fatty acid is preferably a monocarboxylic acid. Examples of the higher fatty acid include saturated fatty acids such as octylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, behenic acid, montanic acid, and sebacic acid, and unsaturated fatty acids such as erucic acid, oleic acid, and ricinoleic acid, and preferably montanic acid, 12-hydroxystearic acid, and behenic acid, and more preferably montanic acid. The higher fatty acid metal salt that can be used in this embodiment is preferably the metal salt of the above higher fatty acid. Examples of the metal element that forms the metal salt include Group 1 elements (alkali metals) such as sodium and potassium; Group 2 elements (alkaline earth metals) such as calcium, magnesium, and barium; and Group 3 elements such as zinc and aluminum, and preferably calcium salt, magnesium salt, zinc salt, and aluminum salt, and more preferably calcium salt. Examples of the metal salts of higher fatty acids include calcium 12-hydroxystearate, zinc 12-hydroxystearate, magnesium 12-hydroxystearate, aluminum 12-hydroxystearate, calcium behenate, zinc behenate, magnesium behenate, calcium montanate, zinc montanate, magnesium montanate, and aluminum montanate, with calcium montanate being preferred.
[0039] For details of the release agent, in addition to the above, the descriptions in paragraphs 0037 to 0042 of JP 2016-196563 A, the descriptions in paragraphs 0067 to 0070 of JP 2021-161125 A, and the descriptions in paragraphs 0048 to 0058 of JP 2016-078318 A can be referred to, the contents of which are incorporated herein by reference.
[0040] The content of the mold release agent is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and the upper limit is preferably 1 part by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the resin composition. By setting the content within such a range, the mold releasability can be improved when performing mold molding such as injection molding, and mold contamination can be effectively suppressed. The release agent may be used alone or in combination of two or more. When two or more types are used, the total amount is preferably within the above range.
[0041] <Coloring agent> The resin composition of the present embodiment may contain a colorant, in particular, a black colorant. The type of black colorant is not particularly limited, but examples include pigments such as carbon black and titanium black, nigrosine and aniline black, with carbon black being preferred.
[0042] The carbon black used in the present embodiment may be any conventionally known carbon black. Examples include furnace black, channel black, ketjen black, and acetylene black. Among them, carbon black with DBP absorption of 30 to 300 g / 100 cm3 has excellent hiding power. 3 The use of carbon black, particularly furnace black, is preferred because it allows a stable color tone to be expressed.
[0043] The content of the colorant (preferably, a black colorant) in the resin composition of the present embodiment is preferably 0.1 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, relative to 100 parts by mass of the resin composition. By making the content equal to or less than the upper limit, higher mechanical properties tend to be obtained. The resin composition of the present embodiment may contain only one type of colorant, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0044] <Other additives> The resin composition of the present embodiment may contain additives other than those described above (other additives). Examples of other additives include impact resistance improvers, alkalis, titanium oxide, hydrolysis resistance improvers, matting agents, plasticizers, dispersants, antistatic agents, coloring inhibitors, gelling inhibitors, colorants, antioxidants, heat stabilizers, light stabilizers, flame retardants, etc. For details of these, refer to the descriptions in paragraphs 0130 to 0155 of Japanese Patent No. 4894982, the contents of which are incorporated herein by reference. In addition, the resin composition of this embodiment can be blended with the additives described in paragraphs 0047 to 0103 of WO 2021 / 241471 without departing from the spirit of the present invention, the contents of which are incorporated herein by reference. The other additives are preferably contained in a total amount of 20.0 parts by mass or less, more preferably 10.0 parts by mass or less, even more preferably 5.0 parts by mass or less, and even more preferably 1.0 part by mass or less, relative to 100 parts by mass of the resin composition. Only one type of other additive may be used, or two or more types may be used in combination.
[0045] <Method of producing resin composition> In this embodiment, the method for producing the resin composition is not particularly specified, and a wide variety of known methods for producing thermoplastic resin compositions can be used. Specifically, the resin composition can be produced by premixing each component using various mixers such as a tumbler or a Henschel mixer, and then melt-kneading the components using a Banbury mixer, a roll, a Brabender, a single-screw extruder, a twin-screw extruder, a kneader, or the like. In this embodiment, it is preferable to use a twin-screw extruder for melt-kneading.
[0046] Also, for example, the resin composition can be produced by not mixing the components in advance, or by mixing only some of the components in advance, feeding the mixture to an extruder using a feeder, and melt-kneading the mixture. Furthermore, for example, some of the components may be mixed in advance, fed to an extruder, and melt-kneaded to obtain a masterbatch composition, which may then be mixed again with the remaining components and melt-kneaded to produce pellets.
[0047] More preferably, the method for producing pellets of the present embodiment is a method for producing pellets of a resin composition, which comprises 150 to 230 parts by mass of flat glass fiber containing a sizing agent and / or a surface treatment agent relative to 100 parts by mass of polyamide resin, and the gas component obtained by heating the sizing agent and / or surface treatment agent of the flat glass fiber at 280 ° C. for 10 minutes contains xylylene diisocyanate, and is characterized in that a twin-screw kneading extruder is used during the production of pellets of the resin composition, and the temperature of the resin composition at the die outlet of the twin-screw kneading extruder is 323 to 355 ° C. In this way, by using a predetermined amount of flat glass fiber containing a specific surface treatment agent, etc., and setting the temperature of the resin composition at the die outlet during extrusion high, it is possible to provide a molded product having stable and excellent mechanical properties. In the method for producing pellets of this embodiment, the polyamide resin, the flat glass fiber, and the resin composition are synonymous with the polyamide resin, the flat glass fiber, and the resin composition described above, and the preferred ranges are also the same.
[0048] In the present embodiment, the temperature of the resin composition at the die discharge port can be achieved by adjusting, for example, the cylinder temperature and rotation speed of the extruder. In this embodiment, the temperature of the resin composition at the die outlet is preferably 323°C or higher, more preferably 325°C or higher, even more preferably 327°C or higher, even more preferably 330°C or higher, even more preferably 335°C or higher, and may be 340°C or higher. By setting it to the lower limit or higher, the reaction between the coupling agent in the glass fiber and the polyamide resin tends to be more effectively promoted. In addition, the temperature of the resin composition at the die outlet is preferably 355°C or lower, more preferably 354°C or lower, even more preferably 353°C or lower, and even more preferably 352°C or lower. By setting it to the upper limit or lower, the decomposition of the polyamide resin tends to be more effectively suppressed. In this embodiment, the difference between the temperature of the resin composition at the die outlet of the twin-screw kneading extruder and the melting point of the polyamide resin is preferably 77°C or more. By setting the difference between the temperature of the resin composition at the die outlet of the extruder (resin temperature) and the melting point of the polyamide to a lower limit or more, the melt viscosity of the polyamide resin tends to be lower. The melting point difference is preferably 77°C or more, more preferably 79°C or more, even more preferably 80°C or more, even more preferably 85°C or more, even more preferably 93°C or more, even more preferably 95°C or more, and even more preferably 100°C or more. The upper limit of the difference between the resin temperature at the die outlet of the extruder and the melting point of the polyamide is preferably 140°C or less, more preferably 120°C or less, and even more preferably 108°C or less. By setting it to the upper limit or less, the decomposition of the polyamide resin tends to be more effectively suppressed.
[0049] <Molded products> The molded article of the present embodiment is formed from the resin composition or pellets of the present embodiment. The method for producing the molded article of the present embodiment is not particularly limited. As an example, an injection molded article molded by injection molding is exemplified. For example, the molded product of this embodiment may be produced by melt-kneading the components and then directly molding the components using various molding methods, or by melt-kneading the components and pelletizing them, and then melting them again and molding them using various molding methods.
[0050] The method for molding a molded article from the resin composition or pellets is not particularly limited, and any conventionally known molding method can be used, such as injection molding, injection compression molding, extrusion molding, profile extrusion, transfer molding, hollow molding, gas-assisted hollow molding, blow molding, extrusion blow molding, IMC (in-mold coating molding), rotational molding, multi-layer molding, two-color molding, insert molding, sandwich molding, foam molding, and pressure molding.
[0051] The shape of the molded product of the present embodiment is not particularly limited and can be appropriately selected depending on the application and purpose of the molded product. Examples of the shape include plate-like, plate-like, rod-like, sheet-like, film-like, cylindrical, annular, circular, elliptical, gear-like, polygonal, irregularly shaped, hollow, frame-like, box-like, and panel-like shapes.
[0052] The application field of the molded product of this embodiment is not particularly limited, and it is widely used in automobile and other transportation machinery parts, general machine parts, precision machine parts, electronic and electrical equipment parts, office automation equipment parts, building materials and housing related parts, medical devices, leisure sports goods, play equipment, medical products, daily necessities such as food packaging films, defense and aerospace products, etc. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0054] 1.Raw materials The following raw materials were used: <Polyamide> MXD6: Mitsubishi Gas Chemical Company, #6000, polyamide resin synthesized from metaxylylenediamine and adipic acid, melting point 243°C, relative viscosity (RV) = 2.1 PA66: U4800, Invista, polyamide 66, melting point 265°C, RV=2.7 PA6: UBE, product number 1011FB, RV=2.2
[0055] <Nucleating agent> Talc: Micron White MW5000S, manufactured by Hayashi Kasei Co., Ltd., average particle size 5 μm
[0056] <Release agent> CS8CP: Calcium montanate, manufactured by Nitto Kasei Kogyo Co., Ltd.
[0057] <Coloring agent> #45: Mitsubishi Carbon Black #45, manufactured by Mitsubishi Chemical Corporation, carbon black
[0058] <Glass fiber> The glass fibers shown in Table 1 below were used. [Table 1]
[0059] In the above Table 1, GF means glass fiber. GF-A and GF-B were produced by changing the isophorone diisocyanate in the glass fiber surface-treated with the urethane-based sizing agent used in CSG 3PA-810S to m-xylylene diisocyanate, and adjusting the contents of m-xylylene diisocyanate and dimethylalkylamine to the gas component amounts shown in Table 1 above.
[0060] <<Analysis of gas evolved from heating glass fiber>> For each glass fiber, a 5 g sample was heat-treated at 600° C. for 2 hours, and the mass reduction rate (unit mass %) was confirmed. In addition, 1 g of each glass fiber was heated at 280°C for 10 minutes, and the gas generated was analyzed by TD GC / MS. The proportions (mass %) of isophorone diisocyanate, m-xylylene diisocyanate and dimethylalkylamine were measured when the total amount of generated gas was taken as 100 mass %.
[0061] 2. Examples 1 to 9 and Comparative Examples 1 to 14 <Compound> As shown in Tables 2 to 5, each component was weighed (each component is expressed in parts by mass), and the components other than the glass fiber were blended in a tumbler, fed into the base of a twin-screw kneading extruder (Shibaura Machine Co., Ltd., TEM26SS) and melted. The glass fiber was then side-fed to produce polyamide resin pellets. The barrel temperature settings of the twin-screw kneading extruder are shown in Tables 2 to 5.
[0062] <Extruder die outlet resin temperature> The temperature of the resin composition at the die outlet of the extruder was measured by the following method. Specifically, a portable thermometer (DP-350, manufactured by Rika Kogyo Co., Ltd.) was used, and the resin discharged from the die outlet was brought into contact with the sensor until the displayed temperature stabilized, and the displayed temperature when it stabilized was taken as the temperature of the resin composition at the die outlet of the extruder (extruder die outlet resin temperature, unit: °C).
[0063] <Bending properties> The pellets obtained by the above manufacturing method were dried at 120°C for 4 hours, and then injection molded into ISO multipurpose test pieces (4 mm thick) using an injection molding machine (Nissei Plastic Industrial Co., Ltd., "NEX140III") under conditions of a cylinder temperature of 290°C, a mold temperature of 130°C, and a molding cycle of 50 seconds. The flexural modulus (unit: GPa) and flexural strength (unit: MPa) were measured at a temperature of 23°C in accordance with ISO178.
[0064] <Tensile strength> The pellets obtained by the above manufacturing method were dried at 120°C for 4 hours, and then injection molded into ISO tensile test specimens type A1 (4 mm thick) using an injection molding machine (manufactured by Nissei Plastic Industrial Co., Ltd., "NEX140III") under conditions of a cylinder temperature of 290°C, a mold temperature of 130°C, and a molding cycle of 50 seconds. The tensile strength (unit: MPa) of the obtained ISO tensile test piece (4 mm thick) was measured in accordance with ISO527-1 and 2 at a gauge length of 50 mm in an environment of a temperature of 23° C. and a humidity of 50%.
[0065] <Sum of tensile strength and bending strength> The sum of the tensile strength and flexural strength (MPa) was calculated.
[0066] <Relative viscosity (RV) of polyamide resin> 0.2 g of the polyamide resin (a mixture when two or more polyamide resins are included) used in the resin composition described in each Example and Comparative Example was precisely weighed and dissolved in 20 mL of 96% by mass sulfuric acid at 25°C with stirring. After complete dissolution, 5 mL of the solution was immediately taken in a Cannon-Fenske viscometer, and the solution was left in a thermostatic bath at 25°C for 10 minutes, after which the drop time (t) of the solution was measured. The drop time (t0) of 96% by mass sulfuric acid itself was also measured under the same conditions. The relative viscosity was calculated from t and t0 using the following formula. Relative viscosity=t / t0
[0067] <Difference between extruder die outlet resin temperature and polyamide melting point> The difference between the temperature of the resin composition at the die discharge port of the extruder and the melting point of the polyamide resin was calculated.
[0068] <Mechanical property evaluation> The mechanical properties were evaluated comprehensively as follows. A: The sum of tensile strength and bending strength is 750 MPa or more. B: The sum of tensile strength and bending strength is 700 MPa or more and less than 750 MPa C: The sum of tensile strength and bending strength is 650 MPa or more and less than 700 MPa D: The sum of tensile strength and bending strength is less than 650 MPa
[0069] <Extrusion evaluation> The extrusion properties were evaluated comprehensively as follows. The evaluation was carried out by five experts and judged by majority vote. A: There was no strand breakage and extrusion was good. B: Strand breakage rarely occurs, but extrusion is good. C: Strand breakage was frequent and extrudability was poor. D: Extrusion itself became impossible due to resin decomposition and foaming.
[0070] [Table 2]
[0071] [Table 3]
[0072] [Table 4]
[0073] [Table 5]
[0074] As is clear from the above results, the molded articles obtained from the resin composition of the present embodiment had excellent mechanical strength (Examples 1 to 9). Furthermore, by setting the temperature of the resin composition at the die outlet of the twin-screw kneading extruder within a predetermined range and adjusting the content of the flat glass fiber, it was possible to provide pellets of the resin composition that had excellent extrudability, that is, excellent production stability. In particular, by using a xylylenediamine-based polyamide resin as the polyamide resin, molded articles having better mechanical strength were obtained (Examples 1 to 8). In contrast, when a specific sizing agent or the like was not used, the mechanical strength of the obtained molded product was significantly inferior (Comparative Examples 3 to 8). Furthermore, when glass fibers having a circular cross section were used, the mechanical strength of the resulting molded products was significantly inferior, regardless of whether a specific sizing agent or the like was used (Comparative Examples 9 to 14).
Claims
1. The composition contains 150 to 230 parts by mass of flat glass fibers containing a bundling agent and / or a surface treatment agent per 100 parts by mass of polyamide resin, A method for producing pellets of a resin composition, comprising heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes to obtain a gas component containing xylylene diisocyanate, The method for producing pellets of the resin composition comprises using a twin-screw kneading extruder, and the temperature of the resin composition at the die discharge port of the twin-screw kneading extruder is 323 to 355°C.
2. The method for producing pellets according to claim 1, wherein the polyamide resin has a relative viscosity in 96% by mass sulfuric acid of 2.0 to 2.
5.
3. The method for producing pellets according to claim 1 or 2, wherein a difference between a temperature of the resin composition at a die discharge port of the twin-screw kneading extruder and a melting point of the polyamide resin is 77° C. or more.
4. The method for producing pellets according to claim 1 or 2, wherein the proportion of dimethylalkylamine gas in the gas component obtained by heating the sizing agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes is 55 to 90 mass %.
5. The method for producing pellets according to claim 1 or 2, wherein the mass reduction rate of the flat glass fiber when heated at 600° C. for 2 hours is 0.7 to 1.0 mass %.
6. 3. The method for producing pellets according to claim 1, wherein the polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine.
7. The polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid; the difference between the temperature of the resin composition at the die outlet of the twin-screw kneading extruder and the melting point of the polyamide resin is 77° C. or more; The proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes is 55 to 90 mass %; The mass loss rate when the flat glass fiber is heated at 600° C. for 2 hours is 0.7 to 1.0% by mass, 2. The method for producing pellets according to claim 1, wherein the polyamide resin contains constitutional units derived from a diamine and constitutional units derived from a dicarboxylic acid, and 70 mol % or more of the constitutional units derived from the diamine are derived from xylylenediamine.
8. The composition contains 150 to 230 parts by mass of flat glass fibers containing a bundling agent and / or a surface treatment agent per 100 parts by mass of polyamide resin, A resin composition, wherein the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280°C for 10 minutes contains xylylene diisocyanate.
9. The resin composition according to claim 8, wherein the polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid.
10. The resin composition according to claim 8 or 9, wherein the proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280 ° C. for 10 minutes is 55 to 90 mass %.
11. The resin composition according to claim 8 or 9, wherein the mass reduction rate when the flat glass fiber is heated at 600° C. for 2 hours is 0.7 to 1.0 mass%.
12. The resin composition according to claim 8 or 9, wherein the polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine.
13. The polyamide resin has a relative viscosity of 2.0 to 2.5 in 96% by mass sulfuric acid; The proportion of dimethylalkylamine gas in the gas component obtained by heating the bundling agent and / or surface treatment agent for the flat glass fibers at 280° C. for 10 minutes is 55 to 90 mass %; The mass loss rate when the flat glass fiber is heated at 600° C. for 2 hours is 0.7 to 1.0% by mass, The resin composition according to claim 8, wherein the polyamide resin contains a diamine-derived structural unit and a dicarboxylic acid-derived structural unit, and 70 mol % or more of the diamine-derived structural unit is derived from xylylenediamine.
14. A pellet of the resin composition according to claim 8, 9 or 13.
15. A molded article formed from the resin composition according to claim 8, 9 or 13.