Polarizing plate
The polarizing plate with a specific adhesive layer configuration and optical laminate structure addresses rainbow unevenness and warpage issues, enhancing the performance of liquid crystal display devices.
Patent Information
- Application Number
- JP2023055361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polarizing plates fail to effectively suppress rainbow unevenness visible from oblique directions and deformation (warpage) of liquid crystal cells at high temperatures.
A polarizing plate design with a specific adhesive layer configuration, including a resin film and resin layer, where the resin film has a thickness of 60 μm or more and a retardation value within certain ranges, and the thickness ratio of the resin film to resin layer satisfies specific conditions, along with an optical laminate structure to enhance stability and reduce warpage.
The solution effectively suppresses rainbow unevenness and warpage of liquid crystal cells at high temperatures, improving visibility and durability of liquid crystal display devices.
Smart Images

Figure 2024142940000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing plate, and further to a polarizing plate with a pressure-sensitive adhesive layer and an optical laminate including the polarizing plate. [Background technology]
[0002] In recent years, there has been a demand for improved visibility of liquid crystal display devices. In order to improve the visibility of liquid crystal display devices, there is also a demand for suppressing unevenness in polarizing plates, which are one of the components constituting liquid crystal display devices.
[0003] In order to suppress unevenness in the polarizing plate, the type and combination of the polarizer protective film in the polarizing plate are being studied. For example, Patent Document 1 describes that when a biaxially stretched polyethylene terephthalate film having a thickness of 38 μm is used as one polarizer protective film, an acrylic-containing film having a cellulose ester resin composition is used as the other polarizer protective film, thereby suppressing unevenness in the polarization degree of the polarizing plate.
[0004] In addition, in liquid crystal display devices, the display quality is reduced due to deformation (warping) of the liquid crystal cell caused by the shrinkage of the polarizing plate in a high-temperature environment, and there is a need to suppress this. Therefore, research is being conducted on polarizing plates to suppress deformation of the liquid crystal cell. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-123402 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even the polarizing plate described in Patent Document 1 did not sufficiently suppress rainbow unevenness visible from an oblique direction of the polarizing plate, or suppress deformation (warping) of a liquid crystal cell to which the polarizing plate is attached at high temperatures.
[0007] The object of the present invention is to provide a polarizing plate that suppresses rainbow unevenness when viewed from an oblique direction of the polarizing plate and suppresses deformation (warping) of a liquid crystal cell to which the polarizing plate is bonded at high temperatures, as well as a polarizing plate with a pressure-sensitive adhesive layer that includes the polarizing plate, and an optical laminate that includes the polarizing plate with a pressure-sensitive adhesive layer. [Means for solving the problem]
[0008] The present invention includes the following inventions. [1] A polarizing plate with a pressure-sensitive adhesive layer, comprising a polarizing plate and a pressure-sensitive adhesive layer, The polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order. the pressure-sensitive adhesive layer is laminated on the resin layer side, the absolute value of retardation in the thickness direction of the resin layer is 100 nm or less, A polarizing plate with a pressure-sensitive adhesive layer, in which a thickness H1 of a resin film and a thickness H2 of a resin layer satisfy the following formula (i): H1 / H2>1.0 (i) [2] The polarizing plate with a pressure-sensitive adhesive layer according to [1], wherein the resin film has a thickness of 60 μm or more. [3] The resin film is a polyester-based resin film, The polarizing plate with a pressure-sensitive adhesive layer according to [1] or [2], wherein the polyester-based resin film satisfies the following [i] to [iv] with respect to a retardation value Re defined by formula (1). Re = (n x -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more. [4] The polarizing plate with a pressure-sensitive adhesive layer according to any one of [1] to [3], wherein the resin layer has a thickness of 60 μm or less. [5] The pressure-sensitive adhesive layer-attached polarizing plate according to any one of [1] to [4], wherein the resin layer is an acrylic resin film. [6] A polarizing plate with a pressure-sensitive adhesive layer, comprising a polarizing plate and a pressure-sensitive adhesive layer, the polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order; the pressure-sensitive adhesive layer is laminated on the resin layer side, A polarizing plate with an adhesive layer that satisfies the following formula (ii), where y is the thickness of the polarizing plate with an adhesive layer and z is the distance from the surface of the resin film opposite the polarizer to the center of the thickness of the polarizer. y / 2-z<10 (ii) [7] The resin film is a polyester-based resin film, The pressure-sensitive adhesive layer-attached polarizing plate according to [6], wherein the polyester-based resin film satisfies the following [i] to [iv] with respect to a retardation value Re defined by formula (1). Re = (nx -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more. [8] The absolute value of retardation in the thickness direction of the resin layer is 100 nm or less; The polarizing plate with a pressure-sensitive adhesive layer according to [6] or [7], wherein a thickness H1 of the resin film and a thickness H2 of the resin layer satisfy the following formula (i): H1 / H2>1.0 (i) [9] The polarizing plate with a pressure-sensitive adhesive layer according to any one of [6] to [8], wherein the resin layer has a thickness of 60 μm or less.
[10] The pressure-sensitive adhesive layer-attached polarizing plate according to any one of [6] to [9], wherein the resin layer is an acrylic resin film.
[11] An optical laminate comprising, in this order, a polarizing plate with a pressure-sensitive adhesive layer, the polarizing plate including a polarizing plate and a pressure-sensitive adhesive layer, and a substrate, the polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order; the pressure-sensitive adhesive layer is laminated on the resin layer side, An optical laminate which satisfies the following formula (iii), where y is the thickness of the polarizing plate with a pressure-sensitive adhesive layer, z is the distance from the surface of the resin film opposite the polarizer to the center of the thickness of the polarizer, and t is the thickness of the substrate. y / 2-(z+t)<-290 (iii)
[12] The resin film is a polyester-based resin film, The optical laminate according to
[11] , wherein the polyester-based resin film satisfies the following [i] to [iv] with respect to a retardation value Re defined by formula (1). Re = (n x -n y )×d (1) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more.
[13] The absolute value of retardation in the thickness direction of the resin layer is 100 nm or less, The optical laminate according to
[11] or
[12] , wherein a thickness H1 of the resin film and a thickness H2 of the resin layer satisfy the following formula (i): H1 / H2>1.0 (i)
[14] The optical laminate according to any one of
[11] to
[13] , which satisfies the following formula (ii), where y is the thickness of the polarizing plate with a pressure-sensitive adhesive layer, and z is the distance from the surface of the resin film opposite the polarizer to the center of the thickness of the polarizer: y / 2-z<10 (ii)
[15] The optical laminate according to any one of
[11] to
[14] , wherein the resin layer has a thickness of 60 μm or less.
[16] The optical laminate according to any one of
[11] to
[15] , wherein the resin layer is an acrylic resin film.
[17] A liquid crystal display device comprising the polarizing plate with the pressure-sensitive adhesive layer according to any one of [1] to
[10] .
[18] A liquid crystal display device comprising the optical laminate according to any one of
[11] to
[16] . Effect of the Invention
[0009] According to the present invention, it is possible to provide a polarizing plate that suppresses rainbow unevenness when viewed from an oblique direction of the polarizing plate and suppresses deformation (warping) of a liquid crystal cell to which the polarizing plate is bonded at high temperatures, as well as a polarizing plate with a pressure-sensitive adhesive layer that includes the polarizing plate and an optical laminate that includes the polarizing plate with a pressure-sensitive adhesive layer. [Brief description of the drawings]
[0010] [Figure 1] FIG. 11 is a schematic perspective view for explaining a phase difference value Re1 and a method for measuring the same. [Diagram 2] FIG. 13 is a schematic perspective view illustrating a phase difference value Re2 and a method for measuring the phase difference value Re2. [Diagram 3] FIG. 11 is a schematic perspective view illustrating a phase difference value Re3 and a method for measuring the phase difference value Re3. [Figure 4] FIG. 13 is a schematic perspective view illustrating a phase difference value Re4 and a method for measuring the same. [Diagram 5] 1 is a schematic cross-sectional view showing a polarizing plate with a pressure-sensitive adhesive layer of the present invention. [Figure 6] 1 is a schematic cross-sectional view showing a polarizing plate with a pressure-sensitive adhesive layer of the present invention. [Figure 7] FIG. 1 is a schematic cross-sectional view showing an optical laminate of the present invention. [Figure 8] FIG. 1 is a schematic cross-sectional view showing an optical laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Polarizing plate with adhesive layer> The present invention is a polarizing plate with an adhesive layer, which includes a polarizing plate and an adhesive layer, and the polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order, and the adhesive layer is laminated on the resin layer side. The polarizing plate with an adhesive layer can be applied to, for example, a liquid crystal display device. In the liquid crystal display device, the polarizing plate with an adhesive layer is disposed on the viewing side and / or the back side of a liquid crystal cell, which is an image display element.
[0012] <Resin film> The resin film functions as a protective film for the polarizer. The resin film is a film formed of a transparent resin, and examples of the transparent resin include a cellulose-based resin, a (meth)acrylic resin, a polyester resin, a polyolefin-based resin, a polycarbonate resin, a polyether ether ketone resin, and a polysulfone resin. The cellulose-based resin, the (meth)acrylic resin, and the polyester-based resin are preferable, and the polyester-based resin or the (meth)acrylic resin is more preferable. The resin film may contain additives (e.g., ultraviolet absorbers, infrared absorbers, organic dyes, pigments, inorganic dyes, antioxidants, antistatic agents, surfactants, lubricants, dispersants, heat stabilizers, etc.) within the scope of not impairing the function as a protective film for the polarizer. In terms of improving the weather resistance of the polarizing plate, the additive is preferably an ultraviolet absorber such as a salicylic acid ester compound, a benzophenone compound, a benzotriazole compound, a triazine compound, a cyanoacrylate compound, or a nickel complex salt.
[0013] In this specification, the term "(meth)acrylic resin" means either an acrylic resin or a methacrylic resin, and the "(meth)" in (meth)acrylic acid ester, (meth)acrylate, (meth)acryloyl, etc. has the same meaning.
[0014] Examples of the cellulose-based resin include cellulose acetate, propionate, butyrate, and mixed esters thereof. Among these, triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, and cellulose acetate butyrate are preferred.
[0015] The (meth)acrylic resin is preferably a polymer mainly composed of a (meth)acrylic acid ester. The (meth)acrylic resin may be a homopolymer of one type of (meth)acrylic ester, or may be a copolymer of a (meth)acrylic acid ester and another (meth)acrylic acid ester. Examples of the (meth)acrylic acid ester include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. Examples of polymerizable monomers that can be copolymerized with the (meth)acrylic acid ester include styrene-based monomers such as styrene and alkylstyrene; monofunctional monomers such as unsaturated nitriles such as acrylonitrile and methacrylonitrile; and polyfunctional monomers such as alkenyl esters of unsaturated carboxylic acids such as allyl (meth)acrylate and methallyl (meth)acrylate; dialkenyl esters of dibasic acids such as diallyl maleate; and unsaturated carboxylic acid diesters of glycols such as alkylene glycol di(meth)acrylate. The (meth)acrylic resin film may contain two or more kinds of (meth)acrylic resins.
[0016] When the (meth)acrylic resin film contains two or more kinds of (meth)acrylic resins, it is preferable that the syndiotacticity (rr) of at least one of the (meth)acrylic resins is 50% or more. From the viewpoint of increasing the toughness of the film and increasing the heat resistance and adhesion to the polarizer of the film, the syndiotacticity (rr) of the triad is preferably 55% or more, more preferably 60% or more, even more preferably 65% or more, and even more preferably 70% or more. The syndiotacticity (rr) of the triad is usually 90% or less, and may be 85% or less.
[0017] The syndiotacticity (rr) of a triad is the proportion of two diads (diads) in a triad of three consecutive units that are both racemo (denoted as rr). The syndiotacticity (rr) of a triad (%) is calculated by the following formula: 1 The H-NMR spectrum is measured, and the area (X) of the region from 0.6 to 0.95 ppm and the area (Y) of the region from 0.6 to 1.35 ppm are measured from the spectrum when the internal standard TMS is set to 0 ppm, and the area is calculated as (X / Y)×100.
[0018] A (meth)acrylic resin having a triad syndiotacticity (rr) of 50% or more can be prepared, for example, according to the method described in WO 2016 / 080124.
[0019] When a (meth)acrylic resin having a syndiotacticity (rr) of 50% or more, expressed as a triad, is contained, the content of the (meth)acrylic resin having a syndiotacticity (rr) of 50% or more, expressed as a triad, relative to the entire (meth)acrylic resin, from the viewpoints of toughness of the film and adhesion to a polarizer, is preferably 1% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, even more preferably 10% by mass or more and 35% by mass or less, and still more preferably 15% by mass or more and 30% by mass or less.
[0020] As the (meth)acrylic resin, a (meth)acrylic resin having a ring structure can be used. Examples of the (meth)acrylic resin having a ring structure include a (meth)acrylic resin having a lactone ring structure, and a (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure. The (meth)acrylic resin having a ring structure is preferred because it has high heat resistance, high transparency, and high mechanical strength when biaxially stretched. Examples of (meth)acrylic resins having a ring structure such as a lactone ring structure include those described in JP-A Nos. 2000-230016, 2001-151814, 2002-120326, 2002-254544, and 2005-146084. Examples of (meth)acrylic resins having a glutaric anhydride structure or a glutarimide structure include those described in JP-A-6-256537, JP-A-6-11615, and JP-A-2009-203348.
[0021] The (meth)acrylic resin having a lactone ring structure is preferably represented by the following general formula: <1> The ring structure is represented by the following formula: [ka] (In the formula, R 1 , R 2 and R 3 each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. The organic residue may contain an oxygen atom.
[0022] General formula in the structure of (meth)acrylic resin having a lactone ring structure <1> The content of the lactone ring structure represented by the general formula in the structure of the (meth)acrylic resin having a lactone ring structure is preferably 5 to 90 mass %, more preferably 10 to 70 mass %, further preferably 10 to 60 mass %, and particularly preferably 10 to 50 mass %. <1> If the content of the lactone ring structure represented by the general formula in the structure of the (meth)acrylic resin having a lactone ring structure is less than 5 mass %, the heat resistance, solvent resistance, and surface hardness may be insufficient. <1> If the content of the lactone ring structure represented by the formula (I) is more than 90% by mass, the molding processability may be poor. The content of the lactone ring structure in the (meth)acrylic resin having the lactone ring structure can be determined by gas chromatography and dynamic TG measurement, for example, as described in JP-A-2006-171464.
[0023] The (meth)acrylic resin having a lactone ring structure is represented by the general formula: <1> The lactone ring structure may have a structure other than the lactone ring structure represented by the general formula: <1> The structure other than the lactone ring structure represented by the following general formula (I) is not particularly limited, but a method for producing a (meth)acrylic resin having a lactone ring structure includes the steps of: <2> A polymer structural unit (repeating structural unit) formed by polymerizing at least one monomer selected from the monomers represented by the following formula is preferred. [ka] (In the formula, R 4 represents a hydrogen atom or a methyl group, and X represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group, a -OAc group, a -CN group, or a -CO-R 5 represents an acetyl group; 5 represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms.
[0024] General formula in (meth)acrylic resin structure having lactone ring structure <1> The content ratio of structures other than the lactone ring structure represented by the formula (I) is preferably 10 to 95% by mass, more preferably 10 to 90% by mass, even more preferably 40 to 90% by mass, and particularly preferably 50 to 90% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a (meth)acrylic acid ester, and is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass in the case of a polymer structural unit (repeating structural unit) formed by polymerizing a hydroxyl group-containing monomer. In the case of a polymer structural unit (repeating structural unit) formed by polymerizing an unsaturated carboxylic acid, it is preferably 0 to 30% by mass, more preferably 0 to 20% by mass, even more preferably 0 to 15% by mass, and particularly preferably 0 to 10% by mass. <2> In the case of a polymer structural unit (repeating structural unit) formed by polymerizing a monomer represented by the following formula:
[0025] The (meth)acrylic resin having a lactone ring structure has a weight average molecular weight of preferably 1000 to 2000000, more preferably 5000 to 1000000, still more preferably 10000 to 500000, and particularly preferably 50000 to 500000. If the weight average molecular weight is outside the above range, it is not preferable from the viewpoint of molding processability.
[0026] Examples of thermoplastic resins to be mixed with the (meth)acrylic resin having a lactone ring structure include olefin polymers such as polyethylene, polypropylene, ethylene-propylene copolymer, and poly(4-methyl-1-pentene); halogen-containing polymers such as vinyl chloride and chlorinated vinyl resin; acrylic polymers such as polymethyl methacrylate; styrene polymers such as polystyrene, styrene-methyl methacrylate copolymer, styrene-acrylonitrile copolymer, and acrylonitrile-butadiene-styrene block copolymer; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamides such as nylon 6, nylon 66, and nylon 610; polyacetal; polycarbonate; polyphenylene oxide; polyphenylene sulfide; polyether ether ketone; polysulfone; polyethersulfone; polyoxybenzylene; polyamide imide; rubbery polymers such as ABS resins and ASA resins blended with polybutadiene rubber and acrylic rubber; and the like.
[0027] The (meth)acrylic resin having a glutaric anhydride structure or a glutarimide structure is preferably represented by the above general formula <2> and the following general formula: <3> The ring structure is represented by the following formula: [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; R 3 is hydrogen, an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or a substituent containing an aromatic ring having 5 to 15 carbon atoms.
[0028] The content of the glutarimide structure is preferably 20% by mass or more, more preferably 20% by mass to 95% by mass, further preferably 40% by mass to 90% by mass, and particularly preferably 50% by mass to 80% by mass, of the (meth)acrylic resin having a glutarimide structure.
[0029] When the content of the glutarimide unit is within the above range, the heat resistance and transparency of the obtained glutarimide-containing (meth)acrylic resin are not reduced, and the moldability and mechanical strength when processed into a film are not extremely reduced.
[0030] On the other hand, if the content of glutarimide units is less than the above range, the heat resistance of the resulting glutarimide resin tends to be insufficient and the transparency tends to be impaired, whereas if the content is more than the above range, the heat resistance and melt viscosity tend to be unnecessarily high, resulting in poor moldability, extremely low mechanical strength during film processing, and impaired transparency.
[0031] The weight-average molecular weight of the (meth)acrylic resin having the glutarimide structure is not particularly limited, but is preferably 10,000 to 500,000. If it is within the above range, the molding processability will not decrease, and the mechanical strength will not be insufficient when processed into a film. On the other hand, if the weight-average molecular weight is smaller than the above range, the mechanical strength when made into a film tends to be insufficient. Also, if it is larger than the above range, the viscosity during melt extrusion will be high, the molding processability will decrease, and the productivity of the molded product will tend to decrease.
[0032] In addition, the (meth)acrylic resin may be a mixture or copolymer of a (meth)acrylic acid ester and an imide compound, which is a thermoplastic resin. Examples of the imide compound include maleimide, and N-substituted maleimides such as N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, Ni-propylmaleimide, Nn-butylmaleimide, Ni-butylmaleimide, Ns-butylmaleimide, Nt-butylmaleimide, Nn-pentylmaleimide, Nn-hexylmaleimide, Nn-heptylmaleimide, Nn-octylmaleimide, N-laurylmaleimide, N-stearylmaleimide, N-cyclopropylmaleimide, N-cyclobutylmaleimide, N-cyclopentylmaleimide, N-cyclohexylmaleimide, N-cycloheptylmaleimide, and N-cyclooctylmaleimide. These maleimide compounds may be used alone or in combination of two or more.
[0033] The (meth)acrylic resin preferably contains acrylic rubber particles in terms of the impact resistance and film formability of the film. The amount of acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 5% by mass or more, more preferably 10% by mass or more, based on 100% by mass of the total amount of the (meth)acrylic resin and the acrylic rubber particles. The upper limit of the amount of the acrylic rubber particles is not critical, but if the amount of the acrylic rubber particles is too large, the surface hardness of the film decreases, and when the film is subjected to a surface treatment, the solvent resistance to the organic solvent in the surface treatment agent decreases. Therefore, the amount of the acrylic rubber particles that can be contained in the (meth)acrylic resin is preferably 80% by mass or less, more preferably 60% by mass or less.
[0034] The acrylic rubber particles are particles that contain an acrylic acid ester-based elastic polymer as an essential component, and may be a single-layer structure that is substantially made of this elastic polymer alone, or may be a multi-layer structure that has this elastic polymer as one layer.Specifically, as this elastic polymer, a crosslinked elastic copolymer obtained by polymerization of monomers consisting of 50-99.9 mass% alkyl acrylate, 0-49.9 mass% of at least one other vinyl monomer that can be copolymerized therewith, and 0.1-10 mass% of a copolymerizable crosslinkable monomer is preferably used.
[0035] Examples of the alkyl acrylate include methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate, and the number of carbon atoms in the alkyl group is usually about 1 to 8. Examples of other vinyl monomers copolymerizable with the alkyl acrylate include compounds having one polymerizable carbon-carbon double bond in the molecule, more specifically, methacrylic acid esters such as methyl methacrylate, aromatic vinyl compounds such as styrene, and vinyl cyanide compounds such as acrylonitrile. Examples of the copolymerizable crosslinkable monomer include crosslinkable compounds having at least two polymerizable carbon-carbon double bonds in the molecule, more specifically, (meth)acrylates of polyhydric alcohols such as ethylene glycol di(meth)acrylate and butanediol di(meth)acrylate, alkenyl esters of (meth)acrylic acid such as allyl (meth)acrylate and methallyl (meth)acrylate, and divinylbenzene.
[0036] In addition to the acrylic rubber particles, the (meth)acrylic resin may contain ordinary additives such as ultraviolet absorbers, organic dyes, pigments, inorganic dyes, antioxidants, antistatic agents, surfactants, etc. Among these, ultraviolet absorbers are preferably used to improve weather resistance. Examples of ultraviolet absorbers include 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(5-methyl-2-hydroxyphenyl)-2H-benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-2H-benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chloro-2H-benzotriazole, 2-(3,5-di-tert-amyl-2-hydroxyphenyl)-2H-benzotriazole, Benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-tert-octylphenyl)-2H-benzotriazole; 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-4'-chlorobenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; salicylic acid phenyl ester-based ultraviolet absorbers such as p-tert-butylphenyl salicylic acid ester and p-octylphenyl salicylic acid ester, and the like can be mentioned, and two or more of them may be used as necessary. When the (meth)acrylic resin contains an ultraviolet absorber, the amount thereof is usually 0.1% by mass or more, preferably 0.3% by mass or more, and preferably 2% by mass or less, based on 100% by mass of the total amount of the (meth)acrylic resin and the ultraviolet absorber.
[0037] As a method for obtaining a (meth)acrylic resin film, various generally known methods such as a method using a feed block and a method using a multi-manifold die can be used. Among them, a method of laminating via a feed block, performing multi-layer melt extrusion from a T-die, and contacting at least one side of the obtained laminated film-like material with a roll or belt to form a film is preferable in that a film with good surface properties can be obtained. In particular, from the viewpoint of improving the surface smoothness and surface gloss of the (meth)acrylic resin film, a method of contacting both sides of the laminated film-like material obtained by the above-mentioned multi-layer melt extrusion with a roll or belt surface to form a film is preferable. In the roll or belt used in this case, the roll surface or belt surface that comes into contact with the (meth)acrylic resin is preferably a mirror surface in order to impart smoothness to the (meth)acrylic resin film surface. The obtained film can be stretched to improve the film strength.
[0038] A film formed from a (meth)acrylic resin is unlikely to have a retardation in an unstretched state, but a retardation occurs when stretched, so that a retardation-reducing agent can be added to the (meth)acrylic resin to prevent the retardation from occurring even when stretched. Examples of the retardation-reducing agent include styrene-acrylonitrile copolymers. The retardation value can be controlled by the stretching ratio and the amount of the retardation-reducing agent added.
[0039] The thickness of the (meth)acrylic resin film is usually 1 μm or more and 80 μm or less, preferably 3 μm or more and 65 μm or less, more preferably 5 μm or more and 55 μm or less, even more preferably 7 μm or more and 45 μm or less, and particularly preferably 20 μm or more and 45 μm or less.
[0040] The glass transition temperature of the (meth)acrylic resin film is 100°C or higher, preferably 110°C or higher, more preferably 115°C or higher, and even more preferably 120°C or higher. The glass transition temperature is usually 170°C or lower. When the glass transition temperature of the (meth)acrylic resin film is 110°C or higher, the change in the molecular orientation of the (meth)acrylic resin in the (meth)acrylic resin film in a high-temperature environment is suppressed, and the change in the retardation value Re and the retardation value Rth in the thickness direction is suppressed, and light leakage in a high-temperature environment tends to be more effectively suppressed. The retardation value Re and the retardation value Rth in the thickness direction of the (meth)acrylic resin film are retardation values at a wavelength of 587 nm.
[0041] When the absolute value of the thickness direction retardation value Rth of the (meth)acrylic resin film is 15 nm or less, the (meth)acrylic resin film may serve both as an optical compensation film and a polarizer protective film in an IPS liquid crystal display device. The absolute value of the retardation value Rth in the thickness direction of the (meth)acrylic resin film is preferably 11 nm or less, more preferably 8 nm or less, and even more preferably 5 nm or less.
[0042] The polyester resin is not particularly limited, and is a polymer obtained by condensation polymerization of a dibasic acid and a dihydric alcohol, and examples thereof include polyethylene terephthalate and polyethylene naphthalate. In addition, it may contain other copolymer components. From the viewpoint of controlling the retardation of the polyester resin film, the polyester resin is preferably a polyethylene terephthalate resin. The polyester resin film can be produced according to a general polyester film production method, for example, by the method described in JP-A-2021-103319, JP-A-2021-99521, etc.
[0043] The polyester resin film preferably has a retardation Re defined by the following formula (1) that satisfies the following [i] to [iv]. Re = (nx-ny) × d (1) [In the formula, nx represents the refractive index in the slow axis direction in the film plane, ny represents the refractive index in the fast axis direction in the film plane (the direction perpendicular to the slow axis direction in the film plane), and d represents the thickness of the film.] [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is measured to be 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the phase difference value Re4 measured is 7000 nm or more.
[0044] The slow axis direction in the film plane is the direction in which the refractive index is maximum in the plane. In addition, in this specification, the retardation value Re is the retardation value at a wavelength of 587 nm.
[0045] 1 is a schematic perspective view illustrating a retardation value Re1 and a method for measuring the retardation value Re1. The retardation value Re1 is a retardation value measured in a first arrangement in which a polyester resin film 100 is arranged so that the angle between the surface of the polyester resin film 100 and a measurement direction 210 is 90°. The measurement direction is a direction from a light source 201 of the retardation measurement device to an observation device 202 that detects and observes light transmitted through the polyester resin film, and is the so-called optical path of the retardation measurement device.
[0046] 2 is a schematic perspective view illustrating the retardation value Re2 and a method for measuring the retardation value Re2. The retardation value Re2 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° about its fast axis 400 as a central axis 300, that is, a polyester resin film 110 in the second arrangement. The angle between the surface of the polyester resin film 110 in the second arrangement and the measurement direction 210 is 60°.
[0047] 3 is a schematic perspective view illustrating the retardation value Re3 and its measurement method. The retardation value Re3 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° around a central axis 310 that is at an angle of 45° to the fast axis 400 in the polyester resin film plane, that is, a polyester resin film 120 in the third arrangement. The angle between the plane of the polyester resin film 120 in the third arrangement and the measurement direction 210 is 60°.
[0048] 4 is a schematic perspective view illustrating the retardation value Re4 and its measurement method. The retardation value Re4 is a retardation value measured for a polyester resin film tilted by rotating the polyester resin film 100 in the first arrangement by 30° about its slow axis 500 as the central axis 320, that is, a polyester resin film 130 in the fourth arrangement. The angle between the surface of the polyester resin film 130 in the fourth arrangement and the measurement direction 210 is 60°.
[0049] From the viewpoint of suppressing rainbow unevenness and handling as an optical film, the retardation value Re1 of the polyester resin film is preferably 6000 nm or more, preferably 7000 nm or more, more preferably 7500 nm or more, and even more preferably 8000 nm or more. The retardation value Re1 of the polyester resin film is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and even more preferably 9000 nm or less.
[0050] When the upper limit of the retardation value Re1 exceeds 30,000 nm, the thickness of the polyester film is considerably increased in order to satisfy the retardation value, and the handleability as an optical film tends to be significantly reduced. When the retardation value Re1 of the polyester resin film is 6,000 nm or more, rainbow unevenness (rainbow-like color spots) when viewed from an oblique direction is more likely to be reduced.
[0051] In addition, the phase difference value Re2 of the polyester resin film is preferably 5000 nm or more. The phase difference value Re2 is more preferably 5500 nm or more, more preferably 6000 nm or more, even more preferably 6500 nm or more, and particularly preferably 7000 nm or more. In addition, the phase difference value Re2 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and particularly preferably 9000 nm or less. By having the phase difference value Re2 of the polyester resin film be 5000 nm or more, it is easy to reduce rainbow unevenness when viewed from an oblique direction.
[0052] The retardation value Re3 of the polyester resin film is preferably 6000 nm or more. The retardation value Re3 is more preferably 7000 nm or more, even more preferably 7500 nm or more, and particularly preferably 8000 nm or more. The retardation value Re3 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, even more preferably 10000 nm or less, and particularly preferably 9000 nm or less. When the retardation value Re3 of the polyester resin film is 6000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.
[0053] The retardation value Re4 of the polyester resin film is preferably 7000 nm or more. The retardation value Re4 is more preferably 8000 nm or more, even more preferably 8500 nm or more, and particularly preferably 9000 nm or more. The retardation value Re4 is usually 30000 nm or less, preferably 20000 nm or less, more preferably 15000 nm or less, and even more preferably 10000 nm or less. When the retardation value Re4 of the polyester resin film is 7000 nm or more, rainbow unevenness when viewed from an oblique direction is easily reduced.
[0054] Re1 to Re4 can be measured using a phase difference measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.).
[0055] By using a polyester resin film in which Re1 to Re4 are each within the above range, rainbow unevenness visible from an oblique direction of the polarizing plate can be suppressed.
[0056] The retardation values of Re1 to Re4 can be controlled within a specific range by appropriately setting the stretching ratio, stretching temperature, and film thickness. For example, a high retardation value can be easily obtained by increasing the stretching ratio, decreasing the stretching temperature, and increasing the film thickness. The retardation values of Re1 to Re4 can be set by selecting the film formation conditions and thickness from the above conditions, taking into account the physical properties required for processing.
[0057] The ratio Re1 / Rth of the retardation value Re1 to the retardation value Rth in the thickness direction of the polyester resin film is usually 0.4 or more, preferably 0.5 or more, more preferably 0.6 or more, even more preferably 0.7 or more, and particularly preferably 0.9 or more. If the ratio (Re1 / Rth) is large, rainbow unevenness due to the observation angle tends to be less likely to occur. Since the ratio Re1 / Rth is 2.0 in a completely uniaxial (uniaxially symmetric) film, the ratio Re1 / Rth is preferably 2.0 or less, and more preferably 1.5 or less.
[0058] The thickness direction retardation value Rth is expressed by the following formula (2): The thickness direction retardation value Rth is the thickness direction retardation value at a wavelength of 587 nm. Rth = (n x +n y ) / 2-n z 〕×d (2) [where n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and n z represents the refractive index in the film thickness direction (direction perpendicular to the film surface), and d represents the film thickness.
[0059] The angle between the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer is, for example, -20° to +20°, preferably -15° to +15°, more preferably -10° to +10°, even more preferably -5° to +5°, still more preferably -3° to +3°, particularly preferably -2° to +2°, and particularly preferably -1° to +1°. In a preferred embodiment, the fast axis or slow axis of the polyester resin film and the transmission axis of the polarizer are substantially parallel. Here, being substantially parallel means that the transmission axis of the polarizer and the fast axis or slow axis of the polyester resin film are parallel to an extent that allows for a misalignment that inevitably occurs when the polarizer and the polyester resin film are bonded together. The smaller the angle between the fast axis or slow axis of the polyester-based resin film and the transmission axis of the polarizer, the smaller the change in polarization state caused by linearly polarized light passing through the polyester-based resin film, and therefore the more likely it is that the occurrence of rainbow unevenness can be suppressed.
[0060] In order to suppress deterioration of the optically functional dye such as iodine contained in the polarizer, the resin film preferably has a light transmittance of 40% or less at a wavelength of 380 nm. The light transmittance of 380 nm is more preferably 35% or less, even more preferably 30% or less, and particularly preferably 20% or less. If the light transmittance is 40% or less, deterioration of the optically functional dye due to ultraviolet rays can be suppressed.
[0061] The resin film may have one or more surface treatment layers, if necessary, on the side opposite to the surface in contact with the polarizing film. Examples of the surface treatment layers include a hard coat layer, an antiglare layer, an antireflection layer, a low antireflection layer, and an antistatic layer. In terms of suppressing rainbow unevenness, it is preferable to provide at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer on the surface of the polyester resin film.
[0062] The surface reflectance of the antireflection layer is preferably 5.7% or less. If the surface reflectance of the antireflection layer exceeds 5.7%, rainbow unevenness tends to be easily visible. The surface reflectance of the antireflection layer is more preferably 5.3% or less, even more preferably 5.0% or less, and particularly preferably 4.5% or less. The lower limit of the surface reflectance of the antireflection layer is not particularly limited, but is, for example, 2.0% or more. The surface reflectance can be measured by any method. For example, a polyester resin film is attached to a black acrylic plate via an adhesive on the opposite side of the resin film from the antireflection layer side, and the light reflectance at a wavelength of 550 nm can be measured from the surface on the antireflection layer side using a spectrophotometer (CM-2600d, manufactured by Konica Minolta Japan, Inc.).
[0063] The anti-reflection layer may be a single layer or a multi-layer. Examples of the anti-reflection layer include an anti-glare hard coat layer having a fine uneven surface to prevent reflection of external light. The anti-glare hard coat layer may be formed by dispersing a filler inside the hard coat layer to form an uneven surface, or may be formed by embossing the hard coat layer to form an uneven surface. For example, when forming an anti-glare hard coat layer using an ultraviolet curing resin, a resin composition obtained by dispersing a filler in an ultraviolet curing resin may be applied to a resin film and irradiated with ultraviolet light, or an ultraviolet curing resin may be applied to a resin film and the coating film may be adhered to the uneven surface of a mold and irradiated with ultraviolet light.
[0064] As a material for forming the antiglare hard coat layer, an ultraviolet curable resin, a thermosetting resin, an electron beam curable resin, etc. can be used, but from the viewpoints of productivity, hardness, etc., an ultraviolet curable resin is preferably used.
[0065] The surface reflectance of the low antireflection layer is preferably 4.0% or less. The surface reflectance of the low antireflection layer is more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.5% or less, and particularly preferably 1.0% or less. The lower limit of the surface reflectance of the low antireflection layer is not particularly limited, but may be, for example, 0.01%.
[0066] The low-reflection anti-layer may be a single layer or a multilayer. When the low-reflection anti-layer is a single layer, the anti-reflection effect can be obtained by forming the low-refractive index layer, which is made of a material having a lower refractive index than the resin film, to have a thickness of 1 / 4 the wavelength of the light or an odd multiple of that. When the anti-reflection layer is a multilayer, the anti-reflection effect can be obtained by alternately forming two or more low-refractive index layers and high-refractive index layers and laminating them while appropriately controlling the thickness of each layer. If necessary, a hard coat layer can be laminated between the low-reflection anti-layer and the resin film.
[0067] The low reflection anti-layer may be a known one, and is preferably a layer formed by coating an organic thin film having a lower refractive index than the resin film or the hard coat layer laminated on the resin film.
[0068] The thickness of at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is usually 0.01 to 20 μm, preferably 0.03 to 1 μm, and more preferably 0.05 to 0.15 μm.
[0069] The surface reflectance of the resin film is preferably 5.7% or less, more preferably 5.3% or less, even more preferably 4.0% or less, even more preferably 3.0% or less, particularly preferably 2.0% or less, and most preferably 1.5% or less. The lower limit of the surface reflectance of the resin film is affected by the type of resin in the resin film, but when the resin film is a polyester resin film, it is 0.01% or more. When the surface reflectance of the resin film is 5.7% or less, rainbow unevenness in the polarizing plate tends to be more effectively suppressed, and among these, it is preferable that the resin film is a polyester-based resin film. In addition, when at least one layer selected from the group consisting of an antireflection layer and a low reflection layer is laminated as described above, the surface reflectance of the entire laminate of at least one layer selected from the group consisting of an antireflection layer and a low reflection layer may be 5.7% or less. By lowering the surface reflectance, the interface reflectance between the substrate film and air can be lowered, and it is presumed that rainbow unevenness is suppressed.
[0070] When at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided on only one side of the resin film, it is preferable that the at least one layer selected from the group consisting of an antireflection layer and a low antireflection layer is provided on the side of the resin film opposite the polarizer.
[0071] In order to improve the adhesion to the polarizer, the resin film may have an easy-adhesion layer on the polarizer side surface. From the viewpoint of suppressing interference caused by reflected light, it is preferable to adjust the refractive index of the easy-adhesion layer so that it is close to the geometric mean of the refractive index of the antireflection layer or low antireflection layer and the refractive index of the resin film. The refractive index of the easy-adhesion layer can be adjusted by a known method, and can be easily adjusted by, for example, adding titanium, germanium, or other metal species to the binder resin.
[0072] The coating liquid constituting the easy-adhesion layer is preferably an aqueous coating liquid containing at least one of water-soluble or water-dispersible copolymer polyester resin, acrylic resin, and polyurethane resin. Examples of these coating liquids include water-soluble or water-dispersible copolymer polyester resin solutions, acrylic resin solutions, and polyurethane resin solutions disclosed in Japanese Patent No. 3567927, Japanese Patent No. 3589232, Japanese Patent No. 3589233, Japanese Patent No. 3900191, and Japanese Patent No. 4150982, etc.
[0073] When a polyester resin is used as the easy-adhesion layer, it is preferable to use a water-soluble or water-dispersible resin in terms of compatibility with the polyvinyl alcohol resin. In order to make the polyester resin water-soluble or water-dispersible, it is preferable to copolymerize a compound containing a hydrophilic group such as a sulfonate group or a carboxylate group. Among them, a dicarboxylic acid component having a sulfonate group is suitable from the viewpoint of imparting hydrophilicity while maintaining the acid value of the polyester resin low and controlling the reactivity with the crosslinking agent. Examples of the dicarboxylic acid component having a sulfonate group include sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfonaphthaleneisophthalic acid-2,7-dicarboxylic acid, and 5-(4-sulfophenoxy)isophthalic acid or an alkali metal salt thereof, and among them, 5-sulfoisophthalic acid is preferable. The dicarboxylic acid component having a sulfonate group is preferably 1 to 15 mol %, more preferably 1.5 to 12 mol %, and even more preferably 2 to 10 mol % of the dicarboxylic acid component of the polyester resin. When the amount of the dicarboxylic acid component having a sulfonate group is equal to or more than the lower limit, it is suitable for making the polyester resin water-soluble or water-dispersible, whereas when the amount of the dicarboxylic acid component having a sulfonate group is equal to or less than the upper limit, it is suitable for improving adhesion to the polyester film substrate.
[0074] The easy-adhesion layer can be obtained by applying the coating liquid to one or both sides of a polyester resin film, drying the film at 100 to 150° C., and then stretching the film in the lateral direction. The final coating amount of the easy-adhesion layer is 0.05 to 0.20 g / m 2 The coating amount is preferably 0.05 g / m 2 If the coating amount is less than 0.20 g / m, the adhesion to the polarizer may be insufficient. 2 When the easy-adhesion layer is provided on both sides of the polyester-based resin film, the coating amount of the easy-adhesion layer on both sides may be the same or different, and each can be independently set within the above range.
[0075] It is preferable to add particles to the easy-adhesion layer to give it easy slipperiness. The average particle size of the particles is preferably 2 μm or less. If the average particle size of the particles exceeds 2 μm, the particles are likely to fall off from the easy-adhesion layer. Examples of particles to be contained in the easy-adhesion layer include inorganic particles such as titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconia, tungsten oxide, lithium fluoride, and calcium fluoride, and organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles. These may be added to the easy-adhesion layer alone, or two or more types may be added in combination.
[0076] The coating liquid can be applied by any known method, such as reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, wire bar coating, and pipe doctor coating, which can be used alone or in combination.
[0077] The thickness of the resin film is not particularly limited, but is usually 15 μm to 200 μm, preferably 20 μm to 100 μm, more preferably 25 μm to 95 μm, further preferably 60 μm to 90 μm, and particularly preferably 75 μm to 85 μm. If the thickness of the resin film is less than 15 μm, the anisotropy of the mechanical properties of the film becomes significant, making it more susceptible to tears, breaks, etc., and the practicality of the film tends to decrease. On the other hand, if the thickness of the resin film exceeds 200 μm, the thickness as a polarizing plate becomes too thick. When the surface treatment layer is provided as described above, the total thickness including the surface treatment layer may be within the above range.
[0078] <Adhesive layer> The adhesive layer is a layer formed from an adhesive composition. The adhesive composition is not particularly limited as long as it is a known adhesive composition, and may be an aqueous adhesive composition or a curable adhesive composition that is cured by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays.
[0079] Examples of the aqueous adhesive composition include those in which a polyvinyl alcohol resin or a urethane resin is dissolved in water as the main component, and those in which a polyvinyl alcohol resin or a urethane resin is dispersed in water as the main component. The aqueous adhesive composition may further contain a curing component or a crosslinking agent such as a polyaldehyde, a melamine compound, a zirconia compound, a zinc compound, a glyoxal compound, or a water-soluble epoxy resin. Examples of the aqueous adhesive composition include the adhesive composition described in JP 2010-191389 A, the adhesive composition described in JP 2011-107686 A, the composition described in JP 2020-172088 A, and the composition described in JP 2005-208456 A.
[0080] The curable adhesive composition is preferably an active energy ray curable adhesive composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray curable adhesive composition include a cationic polymerization type adhesive composition that contains a cationic polymerizable compound as a curable compound, a radical polymerization type adhesive composition that contains a radical polymerizable compound as a curable compound, and a hybrid type adhesive composition that contains both a cationic polymerizable compound and a radical polymerizable compound as a curable compound.
[0081] The cationically polymerizable compound is a compound or oligomer that undergoes a cationic polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays, or when heated. Specific examples of the cationically polymerizable compound include epoxy compounds, oxetane compounds, and vinyl compounds. Examples of epoxy compounds include alicyclic epoxy compounds such as 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule); aromatic epoxy compounds such as diglycidyl ether of bisphenol A (compounds having an aromatic ring and an epoxy group in the molecule); and aliphatic epoxy compounds such as 2-ethylhexyl glycidyl ether and 1,4-butanediol diglycidyl ether (compounds having at least one oxirane ring bonded to an aliphatic carbon atom in the molecule). Examples of the oxetane compound include compounds having one or more oxetane rings in the molecule, such as 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane.
[0082] The cationic polymerization adhesive composition preferably contains a cationic polymerization initiator. The cationic polymerization initiator may be a thermal cationic polymerization initiator or a photo-induced cationic polymerization initiator. Examples of the cationic polymerization initiator include aromatic diazonium salts such as benzenediazonium hexafluoroantimonate; aromatic iodonium salts such as diphenyliodonium tetrakis(pentafluorophenyl)borate; aromatic sulfonium salts such as triphenylsulfonium hexafluorophosphate; and iron-arene complexes such as xylene-cyclopentadienyl iron(II) hexafluoroantimonate. The content of the cationic polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the cationic polymerizable compound. Two or more kinds of cationic polymerization initiators may be included.
[0083] Examples of cationic polymerization adhesive compositions include the cationic polymerizable compositions described in JP 2016-126345 A and JP 2021-113969 A.
[0084] The radical polymerizable compound is a compound or oligomer that undergoes a radical polymerization reaction and hardens when exposed to active energy rays such as ultraviolet light, visible light, electron beams, and X-rays or when heated, and specifically includes a compound having an ethylenically unsaturated bond. Examples of the compound having an ethylenically unsaturated bond include a (meth)acrylic compound having one or more (meth)acryloyl groups in the molecule, and a vinyl compound having one or more vinyl groups in the molecule.
[0085] Examples of the (meth)acrylic compound include (meth)acrylate monomers having at least one (meth)acryloyloxy group in the molecule, (meth)acrylamide monomers, and (meth)acryl group-containing compounds obtained by reacting two or more functional group-containing compounds and having at least two (meth)acryloyl groups in the molecule, such as (meth)acrylic oligomers.
[0086] The radical polymerization adhesive composition preferably contains a radical polymerization initiator. The radical polymerization initiator may be a thermal radical polymerization initiator or a photoradical polymerization initiator. Examples of the radical polymerization initiator include acetophenone-based initiators such as acetophenone and 3-methylacetophenone; benzophenone-based initiators such as benzophenone, 4-chlorobenzophenone, and 4,4'-diaminobenzophenone; benzoin ether-based initiators such as benzoin propyl ether and benzoin ethyl ether; thioxanthone-based initiators such as 4-isopropylthioxanthone; xanthone, fluorenone, and the like. The content of the radical polymerization initiator is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the radical polymerizable compound. Two or more types of radical polymerization initiators may be included.
[0087] Examples of radical polymerization adhesive compositions include the radical polymerizable compositions described in JP 2016-126345 A, JP 2016-153474 A, and WO 2017 / 183335 A.
[0088] The active energy ray-curable adhesive composition may contain additives such as an ion trapping agent, an antioxidant, a chain transfer agent, a tackifier, a thermoplastic resin, a filler, a flow adjuster, a plasticizer, an antifoaming agent, an antistatic agent, a leveling agent, and a solvent, as necessary.
[0089] When the adhesive layer is formed from a water-based adhesive, the thickness of the adhesive layer may be, for example, 5 μm or less, preferably 1 μm or less, and more preferably 0.5 μm or less, and may be 0.01 μm or more, and preferably 0.05 μm or more. When the adhesive layer is formed from a curable adhesive composition (preferably an active energy ray-curable adhesive composition), the thickness of the adhesive layer may be, for example, 10 μm or less, preferably 5 μm or less, and more preferably 3 μm or less, and may be 0.1 μm or more, preferably 0.5 μm or more, and more preferably 1 μm or more.
[0090] The adhesive layer can be formed by applying an adhesive composition to at least one of the bonding surfaces selected from the bonding surface of the resin film and the bonding surface of the polarizer, laminating the two with the coating layer of the adhesive composition therebetween, pressing them together from above and below using a laminating roll or the like, and then drying the adhesive layer, curing it by irradiating it with active energy rays, or curing it by heating. To form a coating layer of the adhesive composition, various coating methods can be used, such as a die coater, a comma coater, a gravure coater, a wire bar coater, or a doctor blade coater. Alternatively, the adhesive composition may be allowed to flow while continuously supplying the polarizer and the resin film so that the bonding surfaces of both are inside.
[0091] Before forming the coating layer of the adhesive layer, at least one of the bonding surfaces selected from the bonding surface of the polarizer and the bonding surface of the resin film may be subjected to an adhesion-facilitating treatment such as a saponification treatment, a corona treatment, a plasma treatment, a primer treatment, or an anchor coating treatment.
[0092] The light irradiation intensity when irradiating with active energy rays is determined depending on the composition of the active energy ray-curable adhesive composition and is not particularly limited, but is preferably 10 mW / cm 2 More than 1,000mW / cm 2 The irradiation intensity is preferably an intensity in a wavelength region effective for activating a photocationic polymerization initiator or a photoradical polymerization initiator. Irradiation is performed once or multiple times with such a light irradiation intensity, and the integrated light amount is 10 mJ / cm or less. 2 More preferably, it is 100 mJ / cm or more. 2 More than 1,000mJ / cm 2 It is more preferable to set it as follows:
[0093] The light source used to polymerize and cure the active energy ray-curable adhesive composition is not particularly limited, but examples include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, xenon lamps, halogen lamps, chemical lamps, black light lamps, microwave excited mercury lamps, and metal halide lamps.
[0094] <Polarizer> A polarizer is a film that has the function of selectively transmitting linearly polarized light in one direction from natural light. Examples of polarizers include iodine-based polarizers in which iodine as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, dye-based polarizers in which a dichroic dye as a dichroic pigment is adsorbed and oriented on a polyvinyl alcohol-based resin film, and coated polarizers in which a dichroic dye in a lyotropic liquid crystal state is coated, oriented, and fixed. These polarizers are called absorption-type polarizers because they selectively transmit linearly polarized light in one direction from natural light and absorb linearly polarized light in the other direction.
[0095] The polarizer is not limited to an absorptive polarizer, and may be a reflective polarizer that selectively transmits linearly polarized light in one direction from natural light and reflects linearly polarized light in the other direction, or a scattering polarizer that scatters linearly polarized light in the other direction. However, an absorptive polarizer is preferred because it provides excellent visibility when the polarizing plate is applied to a liquid crystal display device or the like. Among these, the polarizer is more preferably a polyvinyl alcohol-based polarizer made of a polyvinyl alcohol-based resin, even more preferably a polyvinyl alcohol-based polarizer in which a dichroic pigment such as iodine or a dichroic dye is adsorbed and oriented in a polyvinyl alcohol-based resin film, and particularly preferably a polyvinyl alcohol-based polarizer in which iodine is adsorbed and oriented in a polyvinyl alcohol-based resin film.
[0096] Polyvinyl alcohol resins can be obtained by saponifying polyvinyl acetate resins. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, as well as copolymers of vinyl acetate and monomers copolymerizable with vinyl acetate. Examples of monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.
[0097] The saponification degree of the polyvinyl alcohol resin is usually 85 mol% to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, for example, polyvinyl formal or polyvinyl acetal modified with an aldehyde. The polymerization degree of the polyvinyl alcohol resin is usually 1,000 to 10,000, preferably 1,500 to 5,000.
[0098] A film of a polyvinyl alcohol-based resin is usually used as the raw film of a polarizing film. The polyvinyl alcohol-based resin can be formed into a film by a known method. The thickness of the raw film is usually 1 to 150 μm, and considering the ease of stretching, the thickness is preferably 10 μm or more.
[0099] The polarizing film is produced, for example, by subjecting a raw film to a uniaxial stretching process, a process of dyeing the film with a dichroic dye to adsorb the dichroic dye, a process of treating the film with an aqueous boric acid solution, and a process of washing the film with water, and finally drying. The film thickness of the polarizing film can be 30 μm or less, and is preferably 25 μm or less (for example, 20 μm or less, further 15 μm or less, further 10 μm or less, and further 8 μm or less). The thickness of the polarizer 30 is usually 2 μm or more. Reducing the thickness of the polarizer is advantageous for reducing the thickness of the polarizing plate, and further the liquid crystal panel and liquid crystal display device to which it is applied.
[0100] <Resin layer> The resin layer may be a resin film or a layer of a cured product of a curable composition. When the resin layer is a resin film, it may be a resin film formed from a transparent resin. Specifically, it may be the same as the above-mentioned resin film, preferably a cellulose-based resin film, an acrylic-based resin film, or a polyester-based resin film, and more preferably an acrylic-based resin film. As the acrylic-based resin film, for example, the acrylic-based resin film described in the above-mentioned resin film may be mentioned.
[0101] When the resin layer is a cured product layer of a curable composition, it is formed from a curable composition that is cured by heating or irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays. The curable composition is preferably an active energy ray curable composition that contains a curable (polymerizable) compound as a main component and is cured by irradiation with active energy rays. Examples of the active energy ray curable composition include a cationic polymerization type composition containing a cationic polymerizable compound as a curable compound, a radical polymerization type composition containing a radical polymerizable compound as a curable compound, and a hybrid type composition containing both a cationic polymerizable compound and a radical polymerizable compound as a curable compound. Specifically, the same as the above-mentioned cationic polymerization type adhesive composition and radical polymerization type adhesive composition can be mentioned.
[0102] When the resin layer is a resin film, the thickness of the resin layer is usually 1 μm or more and 80 μm or less, preferably 3 μm or more and 60 μm or less, more preferably 5 μm or more and 55 μm or less, even more preferably 7 μm or more and 45 μm or less, and particularly preferably 20 μm or more and 45 μm or less. When the resin layer is a cured layer of a curable composition, the thickness of the resin layer is usually 0.5 μm or more and 15 μm or less, preferably 1 μm or more and 10 μm or less, more preferably 1 μm or more and 7 μm or less, and particularly preferably 1 μm or more and 5 μm or less.
[0103] The resin layer in the present invention has an absolute value of retardation value (Rth) in the thickness direction of the resin layer of 100 nm or less. The absolute value of retardation in the thickness direction of the resin layer is preferably 80 nm or less, more preferably 50 nm or less, even more preferably 30 nm or less, particularly preferably 15 nm or less, and even more preferably 10 nm or less. The absolute value of retardation in the thickness direction of the resin layer may be 0 or more. When the absolute value of retardation in the thickness direction of the resin layer is 100 nm or less, there is a tendency that light leakage through the polarizing plate in a liquid crystal display device having an IPS (In-Plane Switching) type driving method is easily suppressed.
[0104] The resin layer may be a single layer or may have a multi-layer structure of two or more layers. When the resin layer has a multi-layer structure of two or more layers, the absolute value of retardation in the thickness direction of the entire resin layer may be 100 nm or less.
[0105] When the resin layer is a resin film, the polarizer and the resin layer are laminated via an adhesive layer A. Examples of the adhesive layer A include the same adhesive layers as those described above. The thickness of the adhesive layer A may be, for example, 15 μm or less, preferably 10 μm or less, and more preferably 5 μm or less, and may be 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more. The adhesive layer and adhesive layer A are preferably formed from the same type of adhesive composition. The adhesive layer and adhesive layer A are preferably formed from a cationic polymerization type adhesive composition. The adhesive layer and adhesive layer A may have the same thickness or different thicknesses, but are preferably the same thickness. Note that "the same thickness" includes an error of about 0.3 μm. The adhesive layer A is not included in the resin layer.
[0106] In the present invention, the thickness H1 of the resin film and the thickness H2 of the resin layer are expressed by the following formula (i): H1 / H2>1.0 (i) When the thickness H1 of the resin film and the thickness H2 of the resin layer satisfy the above relationship, warping in a high-temperature environment tends to be suppressed. The ratio (H1 / H2) of the thickness H1 of the resin film to the thickness H2 of the resin layer is preferably 1.2 or more, more preferably 1.5 or more, and even more preferably 2.0 or more, and is usually 200 or less, preferably 100 or less, more preferably 80 or less, even more preferably 50 or less, even more preferably 10 or less, and particularly preferably 6 or less.
[0107] <Adhesive layer> The adhesive layer is laminated on the resin layer of the polarizing plate. The polarizing plate with the adhesive layer can be attached to a liquid crystal cell via the adhesive layer. That is, from the viewpoint of visibility, in a liquid crystal panel and a liquid crystal display device, it is preferable that the polarizing plate of the present invention is arranged so that the resin film side faces the liquid crystal cell side.
[0108] Examples of the pressure-sensitive adhesive composition forming the pressure-sensitive adhesive layer include pressure-sensitive adhesive compositions containing, as a base polymer, a (meth)acrylic resin, a silicone resin, a polyester resin, a polyurethane resin, a polyether resin, etc. Among these, from the viewpoints of transparency, adhesive strength, reliability, heat resistance, reworkability, etc., a (meth)acrylic pressure-sensitive adhesive composition containing a (meth)acrylic resin is preferred.
[0109] The thickness of the pressure-sensitive adhesive layer is determined depending on the adhesive strength etc., and is, for example, from 1 μm to 50 μm, preferably from 2 μm to 40 μm, and more preferably from 3 μm to 30 μm.
[0110] The polarizing plate with a pressure-sensitive adhesive layer of the present invention can be prepared by forming a pressure-sensitive adhesive layer on the resin layer side of the polarizing plate. Examples of methods for forming a pressure-sensitive adhesive layer on a polarizing plate include a method of applying a pressure-sensitive adhesive composition onto a suitable substrate, drying the substrate to form a pressure-sensitive adhesive sheet, laminating a polarizing plate onto the pressure-sensitive adhesive layer surface of the formed pressure-sensitive adhesive sheet, and then peeling off the substrate; and a method of applying a pressure-sensitive adhesive composition onto a polarizing plate.
[0111] The substrate is preferably a plastic film, and specifically, a release film that has been subjected to a release treatment can be mentioned. Examples of the release film include a film made of a resin such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polyarylate, etc., and one side of the film is subjected to a release treatment such as silicone treatment. A release film may be attached to the surface of the adhesive layer in order to temporarily protect the surface of the adhesive layer of the adhesive sheet.
[0112] An example of the layer structure of the pressure-sensitive adhesive layer-attached polarizing plate of the present invention is shown in Fig. 5. The pressure-sensitive adhesive layer-attached polarizing plate 1 shown in Fig. 5 includes, in this order, a resin film 10, an adhesive layer 15, a polarizer 30, a resin layer 25, and a pressure-sensitive adhesive layer 20. In the pressure-sensitive adhesive layer-attached polarizing plate 1, the resin layer 25 can be a cured layer of a curable composition. 5, in the polarizing plate with a pressure-sensitive adhesive layer of the present invention, the resin film 10 and the adhesive layer 15 are preferably in direct contact with each other. Also, the pressure-sensitive adhesive layer 20 and the resin layer 25 are preferably in direct contact with each other. The polarizer 30 and the adhesive layer 15 are preferably in direct contact with each other. The polarizer 30 and the resin layer 25 are preferably in direct contact with each other.
[0113] Another example of the layer structure of the polarizing plate with a pressure-sensitive adhesive layer of the present invention is shown in Fig. 6. The polarizing plate with a pressure-sensitive adhesive layer 2 shown in Fig. 6 includes a resin film 10, an adhesive layer 15, a polarizer 30, an adhesive layer A 35, a resin layer 40, and a pressure-sensitive adhesive layer 20. In the polarizing plate with a pressure-sensitive adhesive layer 2, the resin layer 40 can be a resin film. As shown in Fig. 6, in the polarizing plate of the present invention, the resin film 10 and the adhesive layer 15 are preferably in direct contact with each other. Also, the pressure-sensitive adhesive layer 20 and the resin layer 40 are preferably in direct contact with each other. The polarizer 30 and the adhesive layer 15 are preferably in direct contact with each other. The resin layer 40 and the adhesive layer A35 are preferably in direct contact with each other. The polarizer 30 and the adhesive layer A35 are preferably in direct contact with each other.
[0114] In the polarizing plate with a pressure-sensitive adhesive layer of the present invention, when the overall film thickness of the polarizing plate with a pressure-sensitive adhesive layer is y (the length of y shown in Figure 5) and the distance from the surface of the resin film opposite the polarizer to the center of the film thickness of the polarizer is z (the length of z shown in Figure 5), it is preferable that the following formula (ii) is satisfied. y / 2-z<10 (ii) When y and z satisfy the relationship of formula (ii), the polarizing plate tends to suppress deformation (warping) of the liquid crystal cell to which the polarizing plate is attached in a heat-resistant environment. The reason why warping is suppressed by formula (ii) is not clear, but it is thought that warping due to shrinkage of the polarizer in a heat-resistant environment can be suppressed by positioning the polarizer close to the liquid crystal cell surface in the overall film thickness of the polarizing plate.
[0115] The value of the left side of formula (ii) is preferably 5 or less, more preferably 0 or less, further preferably -5 or less, and particularly preferably -10 or less. Also, it is usually -50 or more, and preferably -30 or more.
[0116] <Optical laminate> Another embodiment of the present invention includes an optical laminate in which the pressure-sensitive adhesive layer of the above-mentioned pressure-sensitive adhesive layer-attached polarizing plate and a substrate are laminated. Here, the substrate may be a glass substrate of a liquid crystal cell, etc. Also, a transparent electrode may be provided on the surface of the glass substrate of the liquid crystal cell. The thickness of the substrate is usually 300 μm or more and 1000 μm or less, preferably 300 μm or more and 800 μm or less, and more preferably 300 μm or more and 700 μm or less.
[0117] It is preferable that the optical laminate of the present invention satisfies the following formula (iii), when the thickness of the entire pressure-sensitive adhesive layer-attached polarizing plate is y (the length indicated by y in Figure 7), the distance from the surface of the resin film opposite the polarizer to the center of the polarizer is z (the length indicated by z in Figure 7), and the thickness of the substrate is t (the length indicated by t in Figure 7). y / 2-(z+t)<-290 (iii) When the above relational expression is satisfied, the polarizing plate tends to suppress deformation (warping) of the liquid crystal cell to which the polarizing plate is attached in a heat-resistant environment. Although the reason why the warping is suppressed by the expression (iii) is not clear, it is considered that the warping caused by the shrinkage of the polarizer in a heat-resistant environment can be suppressed by the position of the polarizer in the entire film thickness of the polarizing plate being close to the liquid crystal cell surface and the increase in substrate rigidity due to the increase in the thickness of the substrate.
[0118] The value of the left side of formula (iii) is preferably −300 or less, usually −1050 or more, and preferably −1000 or more.
[0119] 7 and 8 are schematic cross-sectional views showing an example of the layer structure of the optical laminate of the present invention. 7 has a layer configuration in which a resin film 10, an adhesive layer 15, a polarizer 30, a resin layer 25, a pressure-sensitive adhesive layer 20, and a substrate 60 are laminated in this order. The resin layer 25 can be a cured layer of a curable composition. 8 has a layer configuration in which a resin film 10, an adhesive layer 15, a polarizer 30, an adhesive layer A 35, a resin layer 40, a pressure-sensitive adhesive layer 20, and a substrate 60 are laminated in this order. The resin layer 40 can be a resin film. 7, in the optical laminate of the present invention, the resin film 10 and the adhesive layer 15 are preferably in direct contact with each other. Also, the resin layer 25 and the pressure-sensitive adhesive layer 20 are preferably in direct contact with each other. The polarizer 30 and the adhesive layer 15 are preferably in direct contact with each other. The polarizer 30 and the resin layer 25 are preferably in direct contact with each other. When the resin layer is a resin film as shown in FIG. 8, the polarizer 30 and the adhesive A 35 are preferably in direct contact with each other.
[0120] On the opposite side of the substrate of the optical laminate shown in FIG. 7 or FIG. 8, the polarizing plate with a pressure-sensitive adhesive layer of the present invention may be disposed, or another polarizing plate with a pressure-sensitive adhesive layer may be disposed.
[0121] The polarizing plate and optical laminate with a pressure-sensitive adhesive layer of the present invention can be suitably used in liquid crystal displays, such as various mobile devices such as tablet terminals, personal computers including notebooks, desktops, and PDAs (Personal Digital Assistants), televisions, and in-vehicle displays. EXAMPLES
[0122] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0123] (Production Example 1: Production of Polarizer) A long polyvinyl alcohol film (average polymerization degree: about 2400, saponification degree: 99.9 mol% or more, thickness: 60 μm) was continuously conveyed and immersed in a swelling bath of pure water at 20 ° C. for a residence time of 31 seconds (swelling step). Thereafter, the film pulled out of the swelling bath was immersed in a dyeing bath at 30 ° C. containing iodine with potassium iodide / water at 2 / 100 (mass ratio) for a residence time of 122 seconds (dyeing step). Next, the film pulled out of the dyeing bath was immersed in a crosslinking bath at 56 ° C. with potassium iodide / boric acid / water at 12 / 4.1 / 100 (mass ratio) for a residence time of 70 seconds, and then in a crosslinking bath at 40 ° C. with potassium iodide / boric acid / water at 9 / 2.9 / 100 (mass ratio) for a residence time of 13 seconds (crosslinking step). In the dyeing and crosslinking steps, the film was uniaxially stretched longitudinally by inter-roll stretching in the bath. The total stretch ratio based on the original film was 5.5 times. Next, the film was pulled out of the crosslinking bath and immersed in a washing bath of pure water at 5°C for a residence time of 3 seconds (washing step), and then introduced into a drying oven at 80°C for a residence time of 190 seconds and dried (drying step) to obtain a polarizer. The polarizer obtained by the above process had a thickness of 24 μm.
[0124] (Production Example 2: Production of Polyethylene Terephthalate Resin (1)) While the esterification reactor was heated to 200°C, 86.4 parts of terephthalic acid and 64.6 parts of ethylene glycol were charged into the esterification reactor to obtain a mixture. While stirring the mixture, 0.017 parts of antimony trioxide, 0.064 parts of magnesium acetate tetrahydrate, and 0.16 parts of triethylamine were added as catalysts to the mixture. The gauge pressure in the esterification reactor was set to 0.34 MPa, and a pressurized esterification reaction was carried out under conditions of 240°C. The esterification reactor was then returned to normal pressure, and 0.014 parts of phosphoric acid were added. The temperature was then raised to 260°C over 15 minutes, and 0.012 parts of trimethyl phosphate were added to obtain a mixture. After 15 minutes, the mixture was dispersed using a high-pressure disperser, and after another 15 minutes, the esterification reaction product was transferred to a polycondensation reactor and subjected to a polycondensation reaction under reduced pressure at 280°C. After the polycondensation reaction was completed, the mixture was filtered using a Naslon filter with a 95% cutoff diameter of 5 μm, extruded from a nozzle in the form of a strand, cooled and solidified using cooling water that had been previously filtered (pore diameter: 1 μm or less), and cut into pellets to obtain polyethylene terephthalate resin (hereinafter referred to as PET (1)).
[0125] (Production Example 3: Production of polyethylene terephthalate resin (2)) 10 parts of the dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) and 90 parts of the PET (1) obtained in Production Example 2 were mixed and kneaded using an extruder to obtain a polyethylene terephthalate resin (2) containing an ultraviolet absorber (hereinafter referred to as PET (2)).
[0126] (Production Example 4: Preparation of Coating Solution for Forming Adhesive Layer) A water-dispersible sulfonate metal salt group-containing copolymer polyester resin was prepared by carrying out an ester exchange reaction and a polycondensation reaction in a conventional manner between a dicarboxylic acid component consisting of 46 mol % terephthalic acid, 46 mol % isophthalic acid, and 8 mol % sodium 5-sulfonatoisophthalate, and a glycol component consisting of 50 mol % ethylene glycol and 50 mol % neopentyl glycol. Next, 51.4 parts of water, 38 parts of isopropyl alcohol, 5 parts of n-butyl cellosolve, and 0.06 parts of nonionic surfactant were mixed to obtain a mixture. The mixture obtained was heated to 77°C and stirred, while adding 5 parts of the above-mentioned water-dispersible sulfonate metal salt group-containing copolymer polyester resin, and continued to stir until no resin lumps remained, to obtain a resin water dispersion. The obtained resin water dispersion was cooled to 25°C to obtain a uniform water-dispersible copolymer polyester resin solution with a solid content concentration of 5.0% by mass. 3 parts of aggregated silica particles were dispersed in 50 parts of water to obtain an aqueous dispersion of aggregated silica particles. 0.54 parts of the aqueous dispersion of aggregated silica particles was added to 99.46 parts of the water-dispersible copolymerized polyester resin liquid, and 20 parts of water was further added while stirring to obtain a coating liquid for forming an easy-adhesion layer.
[0127] (Production Example 5: Production of Protective Film 1) PET (3) was prepared by mixing 90 parts of PET (1) produced in Production Example 2 and 10 parts of PET (2) produced in Production Example 3, and was dried under reduced pressure at 135 ° C for 6 hours, and then fed to extruder 2 (for intermediate layer B layer). PET (1) was also dried and fed to extruder 1 (for outer layer A layer and outer layer C layer), respectively. PET (1) fed to extruder 1 and PET (3) fed to extruder 2 were each melted at 285 ° C. These two types of polymers were each filtered with a stainless steel sintered filter medium (nominal filtration accuracy 10 μm particles 95% cut) and laminated in a two-type three-layer merging block, extruded from a die in the form of a sheet, and then wrapped around a casting drum with a surface temperature of 30 ° C. using an electrostatic casting method, cooled and solidified, and an unstretched PET film was produced. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of A layer, B layer, and C layer was 10:80:10.
[0128] Next, both sides of the obtained unstretched PET film were coated with 0.08 g / m2 of PET using the reverse roll method. 2 After the coating liquid for forming the easy-adhesion layer was applied so as to become The unstretched PET film on which this coating layer was formed was stretched 4.0 times in the width direction in a hot air zone at a temperature of 125°C in a tenter stretching machine while holding the ends of the film with clips. Next, while maintaining the width stretched in the width direction, it was treated at a temperature of 225°C for 10 seconds, and further subjected to a relaxation treatment of 3.0% in the width direction to obtain a uniaxially stretched PET film on which an easy-adhesion layer with a film thickness of about 80 μm was formed. This was named protective film 1.
[0129] (Production Example 6: Production of Protective Film 2) A mixture of 90 parts of a (meth)acrylic resin having a lactone ring structure and 10 parts of an acrylonitrile-styrene (AS) resin (lactone ring content: 28.5%) was extruded and stretched 2.0 times in length and 2.4 times in width to obtain a 40 μm thick acrylic resin film, which was designated as protective film 2.
[0130] (Production Example 7: Production of Protective Film 3) A mixture of 70 parts of a copolymer of methyl methacrylate / methyl acrylate = 96 / 4 (mass ratio) and 30 parts of acrylic rubber particles, an acrylic multilayer polymer with a three-layer structure (1st layer: copolymer of methyl methacrylate and allyl methacrylate (mass ratio 99.8 / 0.2) / 2nd layer: copolymer of butyl acrylate, styrene and allyl methacrylate (mass ratio 79 / 19 / 2) / 3rd layer: copolymer of methyl acrylate and ethyl acrylate (mass ratio 96 / 4)) was melt extruded to produce an acrylic resin film with a thickness of 20 μm. This was used as protective film 3.
[0131] (Production Example 8: Production of Protective Film 4) A mixture of 70 parts of a copolymer of methyl methacrylate / methyl acrylate = 96 / 4 (mass ratio) and 30 parts of acrylic rubber particles, an acrylic multilayer polymer with a three-layer structure (1st layer: copolymer of methyl methacrylate and allyl methacrylate (mass ratio 99.8 / 0.2) / 2nd layer: copolymer of butyl acrylate, styrene and allyl methacrylate (mass ratio 79 / 19 / 2) / 3rd layer: copolymer of methyl acrylate and ethyl acrylate (mass ratio 96 / 4)) was melt extruded to produce an acrylic resin film with a thickness of 50 μm. This was used as protective film 4.
[0132] (Production Example 9: Production of Protective Film 5) A mixture of 70 parts of a copolymer of methyl methacrylate / methyl acrylate = 96 / 4 (mass ratio) and 30 parts of acrylic rubber particles, an acrylic multilayer polymer having a three-layer structure (1st layer: copolymer of methyl methacrylate and allyl methacrylate (mass ratio 99.8 / 0.2) / 2nd layer: copolymer of butyl acrylate, styrene and allyl methacrylate (mass ratio 79 / 19 / 2) / 3rd layer: copolymer of methyl acrylate and ethyl acrylate (mass ratio 96 / 4)) was melt extruded to produce an acrylic resin film with a thickness of 60 μm. This was used as protective film 5.
[0133] (Production Example 10: Production of Protective Film 6) A mixture of 70 parts of a copolymer of methyl methacrylate / methyl acrylate = 96 / 4 (mass ratio) and 30 parts of acrylic rubber particles, an acrylic multilayer polymer with a three-layer structure (1st layer: copolymer of methyl methacrylate and allyl methacrylate (mass ratio 99.8 / 0.2) / 2nd layer: copolymer of butyl acrylate, styrene and allyl methacrylate (mass ratio 79 / 19 / 2) / 3rd layer: copolymer of methyl acrylate and ethyl acrylate (mass ratio 96 / 4)) was melt extruded to produce an acrylic resin film with a thickness of 80 μm. This was used as protective film 6.
[0134] <Example 1> One side of protective film 1 (polyester resin film) obtained in Production Example 5 and protective film 3 ((meth)acrylic resin film with a thickness of 20 μm) obtained in Production Example 7 were each subjected to a corona treatment, and an epoxy-based ultraviolet-curable adhesive was applied to the corona-treated surface by using an adhesive applicator. The polarizer obtained in Production Example 1 was then superimposed on the coated layer surface, and a lamination roll was used to press and laminate the layers together to obtain a polarizing plate precursor. At this time, the protective film 1 (polyester resin film) was laminated so that the stretching direction (width direction) and the absorption axis direction (stretching direction of the polarizer) were perpendicular to each other. A belt conveyor-equipped ultraviolet irradiation device (the lamp was a metal halide lamp manufactured by Eye Graphics) was used to irradiate the polarizing plate precursor with an integrated light dose of 200 mJ / cm from the protective film 3 side. 2 The adhesive was cured by irradiating ultraviolet light so that the thickness of the adhesive layer was 3 μm. From the above, a polarizing plate having protective film 1 (polyester resin film) / adhesive layer / polarizer / adhesive layer / protective film 3 ((meth)acrylic resin film) was obtained.
[0135] Next, a release film-attached adhesive layer having a (meth)acrylic adhesive layer (thickness 20 μm) on the release-treated surface of a release film was prepared. The release film-attached adhesive layer was laminated on the (meth)acrylic resin film side of the polarizing plate after the surface of the (meth)acrylic resin film was corona-treated to obtain a polarizing plate with an adhesive layer. The polarizing plate with an adhesive layer has a structure of polyester resin film (resin film) / adhesive layer / polarizer / adhesive layer / (meth)acrylic resin film (resin layer) / adhesive layer / release film.
[0136] The adhesive release film of the polarizing plate with the adhesive layer was peeled off, and the adhesive layer was attached to a non-alkali glass substrate (thickness 0.3 mm, Corning "Eagle XG", 160 mm x 103 mm) to obtain a glass-attached polarizing plate laminate. The size of the adhesive-attached polarizing plate attached to the glass was 150 mm x 90 mm, and the long side direction was set to be the absorption axis of the polarizing plate.
[0137] <Example 2> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 40 μm thick (meth)acrylic resin film (protective film 2 obtained in Production Example 6) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3).
[0138] <Example 3> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 50 μm thick (meth)acrylic resin film (protective film 4 obtained in Production Example 8) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3).
[0139] <Example 4> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 60 μm thick (meth)acrylic resin film (protective film 5 obtained in Production Example 9) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3).
[0140] <Example 5> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 20 μm thick cellulose-based resin film (manufactured by Konica Minolta) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3).
[0141] <Example 6> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 40 μm thick cellulose-based resin film (manufactured by Konica Minolta) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3).
[0142] <Example 7> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that the 60 μm-thick (meth)acrylic resin film used in Example 4 (protective film 5 obtained in Manufacturing Example 9) was used as the resin film.
[0143] <Example 8> A polarizing plate and a polarizing plate with an adhesive layer were obtained in the same manner as in Example 1, except that a 60 μm thick (meth)acrylic resin film (protective film 5 obtained in Production Example 9) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3). Furthermore, a glass-laminated polarizing plate laminate was obtained in the same manner as in Example 1, except that a Corning "Eagle XG" glass substrate having a thickness of 0.7 mm was used as the alkali-free glass substrate.
[0144] <Comparative Example 1> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that the 60 μm-thick (meth)acrylic resin film (protective film 5) used in Example 4 was used as the resin film, and an 80 μm-thick (meth)acrylic resin film (protective film 6 obtained in Production Example 10) was used as the resin layer instead of the 20 μm-thick (meth)acrylic resin film (protective film 3).
[0145] <Comparative Example 2> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 80 μm thick (meth)acrylic resin film (protective film 6 obtained in Production Example 10) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3).
[0146] <Comparative Example 3> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-attached polarizing plate laminate were obtained in the same manner as in Example 1, except that a biaxially stretched polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Corporation) with a thickness of 38 μm was used as the resin film, and a (meth)acrylic resin film (protective film 6 obtained in Production Example 10) with a thickness of 80 μm was used as the resin layer. Note that, as in Example 1, this polarizing plate was attached so that the stretching direction (width direction) of the biaxially stretched polyester resin film and the absorption axis direction (stretching direction of the polarizer) were perpendicular to each other. The stretching direction (width direction) of the biaxially stretched polyethylene terephthalate protective film refers to the width direction when the film is unwound from the film roll.
[0147] <Comparative Example 4> A polarizing plate, a polarizing plate with an adhesive layer, and a glass-laminated polarizing plate laminate were obtained in the same manner as in Example 1, except that a 38 μm-thick biaxially oriented polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Corporation) was used instead of the 20 μm-thick (meth)acrylic resin film (protective film 3).
[0148] <Comparative Example 5> A polarizing plate and a polarizing plate with an adhesive layer were obtained in the same manner as in Example 1, except that a 80 μm thick (meth)acrylic resin film (protective film 6 obtained in Production Example 10) was used as the resin layer instead of the 20 μm thick (meth)acrylic resin film (protective film 3). Furthermore, a glass-attached polarizing plate laminate was obtained in the same manner as in Example 1, except that a Corning "Eagle XG" glass substrate having a thickness of 0.2 mm was used as the alkali-free glass substrate.
[0149] (Measurement of Retardation Value of Polyester Resin Film) The retardation values Re1 to Re4 of the polyester resin films used in the examples and comparative examples were measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-HB-RESPC, manufactured by Oji Scientific Instruments Co., Ltd.). The results are shown in Table 1. Re1: A retardation value measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the surface of the polyester-based resin film and the measurement direction is 90°. Re2: Retardation value measured in a second arrangement in which the polyester-based resin film in the first arrangement is rotated 30° about its fast axis as the central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. Re3: A phase difference value measured in a third arrangement in which the polyester-based resin film in the first arrangement is rotated 30° around an axis that forms an angle of 45° with respect to the fast axis in the plane of the polyester-based resin film as the central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. Re4: Retardation value measured in a fourth arrangement in which the polyester-based resin film in the first arrangement is rotated 30° about its slow axis as the central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°.
[0150] (Measurement of Retardation Value of (Meth)Acrylic Resin Film) The retardation values Re1 to Re4 of the (meth)acrylic resin films used in the examples and comparative examples were measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-WPR, manufactured by Oji Scientific Instruments Co., Ltd.). The results are shown in Table 1. Re1: A retardation value measured in a first arrangement in which the (meth)acrylic resin film is arranged so that the angle between the surface of the (meth)acrylic resin film and the measurement direction is 90°. Re2: Retardation value measured in a second arrangement in which the (meth)acrylic resin film in the first arrangement is rotated 30° about its fast axis as the central axis, so that the angle between the plane of the (meth)acrylic resin film and the measurement direction is 60°. Re3: A phase difference value measured in a third arrangement in which the (meth)acrylic resin film in the first arrangement is rotated 30° around an axis that forms an angle of 45° with respect to the fast axis in the plane of the (meth)acrylic resin film as the central axis, thereby arranging the (meth)acrylic resin film so that the angle between the plane of the (meth)acrylic resin film and the measurement direction becomes 60°. Re4: A phase difference value measured in a fourth arrangement in which the (meth)acrylic resin film in the first arrangement is rotated 30° about its slow axis as the central axis, so that the angle between the plane of the (meth)acrylic resin film and the measurement direction is 60°.
[0151] (Measurement of Retardation Value in the Thickness Direction of Acrylic Resin Film, Cellulosic Resin Film, and Polyester Resin Film) The resin layers ((meth)acrylic resin film, cellulose resin film, and polyester resin film) used in the examples and comparative examples were measured at a wavelength of 587 nm using a retardation measuring device (KOBRA-WPR, manufactured by Oji Scientific Instruments Co., Ltd.) with an angle of 50° between the surface of the resin layer and the measurement direction, and the absolute value of the retardation value (Rth) in the thickness direction, |Rth|, was calculated. The results are shown in Table 1.
[0152] <Warpage evaluation> The glass-attached polarizing plate laminates obtained in Examples 1 to 8 and Comparative Examples 1 to 5 were left to stand for 48 hours in an environment at a temperature of 80° C., and then taken out, and the warpage state was observed and evaluated according to the following criteria. The results are shown in Table 1. ◎: Very small warpage ○: Small warpage △: Warping: Medium ×: Large warpage
[0153] <Light leakage evaluation> The polarizing plate with the adhesive layer obtained in Example 1 was cut to a size of 150 mm x 90 mm. Either the long side or the short side of the cut polarizing plate with the adhesive layer was parallel to the absorption axis. After peeling off the release film from the cut polarizing plate with the adhesive layer (the long side direction is parallel to the absorption axis), the adhesive layer was attached to one side of an alkali glass substrate (thickness 1.1 mm, manufactured by Nippon Sheet Glass Co., Ltd.). Furthermore, the polarizing plate with the adhesive layer obtained in Example 1, which was cut in the same manner as above (the short side direction is parallel to the absorption axis), was attached to a surface of the glass substrate other than the polarizing plate attachment surface so that the transmission axes of the two polarizing plates were perpendicular to each other, to obtain a glass-attached polarizing plate laminate A. The glass-attached polarizing plate laminate A has a structure of resin film / adhesive layer / polarizer / adhesive layer / resin layer / adhesive layer / glass substrate / adhesive layer / resin layer / adhesive layer / polarizer / adhesive layer / resin film.
[0154] The glass-bonded polarizing plate laminate A was placed on a backlight source, and the light leakage in the center of the sample was visually observed and evaluated in a dark place according to the following criteria. The results are shown in Table 1. ○: Small light leakage ×: Large light leakage
[0155] For Examples 2 to 8 and Comparative Examples 1 to 5, the glass-laminated polarizing plate laminate A obtained in Example 1 was replaced with the glass-laminated polarizing plate laminate A obtained in Examples 2 to 8 and Comparative Examples 1 to 5, respectively, and evaluations were carried out in the same manner. The results are shown in Table 1.
[0156] (Measurement of rainbow unevenness) After peeling off the release film from the polarizing plate with the adhesive layer obtained in Example 1, the adhesive layer side was attached to a non-alkali glass substrate (thickness 0.7 mm, Corning "Eagle XG") to obtain a glass-attached polarizing plate laminate B. The above-mentioned glass-bonded polarizing plate laminate B was placed in a backlight light source so that the glass substrate side was the light source, and the polarizing plate was visually observed in a dark place from the polyester resin film side of the polarizing plate in an oblique direction to check the visibility of rainbow unevenness and evaluate it according to the following criteria. Moreover, rainbow unevenness was similarly evaluated for the pressure-sensitive adhesive layer-attached polarizing plates obtained in Examples 2 to 8 and Comparative Examples 1 to 5. The results are shown in Table 1. ○: Weak rainbow unevenness ×: Strong rainbow unevenness
[0157] [Table 1] [Explanation of symbols]
[0158] 1,2 Polarizing plate with adhesive layer, 3,4 Optical laminate, 10 Resin film, 15 Adhesive layer, 20 Adhesive layer, 25,40 Resin layer, 30 Polarizer, 35 Adhesive layer A, 60 Substrate, 100 Polyester-based resin film (first arrangement), 110 Polyester-based resin film (second arrangement), 120 Polyester-based resin film (third arrangement), 130 Polyester-based resin film (fourth arrangement), 201 Light source, 202 Observation device, 210 Measurement direction, 300, 310, 320 Central axis, 400 Fast axis of polyester-based resin film in first arrangement, 500 Slow axis of polyester-based resin film in first arrangement.
Claims
1. A polarizing plate with a pressure-sensitive adhesive layer, comprising a polarizing plate and a pressure-sensitive adhesive layer, The polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order. the pressure-sensitive adhesive layer is laminated on the resin layer side, the absolute value of retardation in the thickness direction of the resin layer is 100 nm or less, A polarizing plate with a pressure-sensitive adhesive layer, in which a thickness H1 of a resin film and a thickness H2 of a resin layer satisfy the following formula (i): H1 / H2>1.0 (i)
2. 2. The polarizing plate with a pressure-sensitive adhesive layer according to claim 1, wherein the resin film has a thickness of 60 [mu]m or more.
3. The resin film is a polyester-based resin film, The pressure-sensitive adhesive layer-attached polarizing plate according to claim 1, wherein the polyester-based resin film satisfies the following [i] to [iv] with respect to a retardation value Re defined by formula (1): Re = (n x -n y ) × d (1) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as a central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated by 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the retardation value Re4 is 7000 nm or more.
4. 2. The polarizing plate with a pressure-sensitive adhesive layer according to claim 1, wherein the resin layer has a thickness of 60 [mu]m or less.
5. The pressure-sensitive adhesive layer-attached polarizing plate according to claim 4 , wherein the resin layer is an acrylic resin film.
6. A polarizing plate with a pressure-sensitive adhesive layer, comprising a polarizing plate and a pressure-sensitive adhesive layer, the polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order; the pressure-sensitive adhesive layer is laminated on the resin layer side, A polarizing plate with a pressure-sensitive adhesive layer that satisfies the following formula (ii), where y is the thickness of the polarizing plate with a pressure-sensitive adhesive layer and z is the distance from the surface of the resin film opposite the polarizer to the center of the thickness of the polarizer. y / 2-z<10 (ii)
7. The resin film is a polyester-based resin film, The pressure-sensitive adhesive layer-attached polarizing plate according to claim 6, wherein the polyester-based resin film satisfies the following [i] to [iv] with respect to a retardation value Re defined by formula (1): Re = (n x -n y ) × d (1) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as a central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated by 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the retardation value Re4 is 7000 nm or more.
8. the absolute value of retardation in the thickness direction of the resin layer is 100 nm or less, The polarizing plate with a pressure-sensitive adhesive layer according to claim 6 or 7, wherein a thickness H1 of the resin film and a thickness H2 of the resin layer satisfy the following formula (i): H1 / H2>1.0 (i)
9. The polarizing plate with a pressure-sensitive adhesive layer according to claim 6 , wherein the resin layer has a thickness of 60 μm or less.
10. The pressure-sensitive adhesive layer-attached polarizing plate according to claim 9 , wherein the resin layer is an acrylic resin film.
11. An optical laminate including, in this order, a polarizing plate with a pressure-sensitive adhesive layer, the polarizing plate including a polarizing plate and a pressure-sensitive adhesive layer, and a substrate, the polarizing plate includes a resin film, an adhesive layer, a polarizer, and a resin layer in this order; the pressure-sensitive adhesive layer is laminated on the resin layer side, An optical laminate which satisfies the following formula (iii), wherein y is the thickness of the polarizing plate with a pressure-sensitive adhesive layer, z is the distance from the surface of the resin film opposite the polarizer to the center of the thickness of the polarizer, and t is the thickness of the substrate. y / 2-(z+t)<-290 (iii)
12. The resin film is a polyester-based resin film, The optical laminate according to claim 11, wherein the polyester resin film satisfies the following [i] to [iv] with respect to the retardation value Re defined by the formula (1). Re = (n x -n y ) × d (1) [In the formula, n x represents the refractive index in the slow axis direction in the film plane, and n y represents the refractive index in the fast axis direction in the film plane, and d represents the thickness of the film. [i] The retardation value Re1 measured in a first arrangement in which the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 90° is 6000 nm or more. [ii] The polyester-based resin film in the first arrangement is rotated 30° about its fast axis as a central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this second arrangement, the phase difference value Re2 is 5000 nm or more. [iii] The polyester-based resin film in the first arrangement is rotated by 30° around an axis that is at an angle of 45° to the fast axis in the plane of the polyester-based resin film as a central axis, so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this third arrangement, the phase difference value Re3 measured is 6000 nm or more. [iv] The polyester-based resin film in the first arrangement is rotated by 30° about its slow axis as the central axis, and the polyester-based resin film is arranged so that the angle between the plane of the polyester-based resin film and the measurement direction is 60°. In this fourth arrangement, the retardation value Re4 is 7000 nm or more.
13. the absolute value of retardation in the thickness direction of the resin layer is 100 nm or less, The optical laminate according to claim 11 or 12, wherein a thickness H1 of the resin film and a thickness H2 of the resin layer satisfy the following formula (i). H1 / H2>1.0 (i)
14. 13. The optical laminate according to claim 11 or 12, wherein the following formula (ii) is satisfied, where y is the thickness of the polarizing plate with the pressure-sensitive adhesive layer, and z is the distance from the surface of the resin film opposite the polarizer to the center of the thickness of the polarizer. y / 2-z<10 (ii)
15. 12. The optical laminate according to claim 11, wherein the resin layer has a thickness of 60 μm or less.
16. The optical laminate according to claim 15, wherein the resin layer is an acrylic resin film.
17. A liquid crystal display comprising the pressure-sensitive adhesive layer-attached polarizing plate according to claim 1 .
18. A liquid crystal display device comprising the optical laminate according to claim 11.
Citation Information
Patent Citations
Sheet polarizer and liquid crystal display device using the same
JP2011123402A