Insulating sheet, laminate, and semiconductor device

JP2024142984AInactive Publication Date: 2024-10-11SEKISUI CHEMICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023055417
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Benefits of technology

【0008】 本発明によれば、窒化ホウ素凝集粒子を含む無機充填材を高充填した絶縁性シートであって、柔軟性に優れ、熱負荷による絶縁性低下を抑制することが可能な絶縁性シートを提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142984000008
    Figure 2024142984000008
  • Figure 2024142984000009
    Figure 2024142984000009
  • Figure 2024142984000010
    Figure 2024142984000010
Patent Text Reader

Abstract

To provide an insulating sheet that is highly filled with an inorganic filler including agglomerated particles of boron nitride, has excellent flexibility, and is capable of suppressing deterioration of insulating properties due to thermal load.SOLUTION: An insulating sheet includes a thermosetting resin, a thermosetting agent, and an inorganic filler, the inorganic filler includes boron nitride agglomerated particles, the content of the inorganic filler is 65 volume% or more relative to 100 volume% of the insulating sheet, and the insulating sheet subjected to a heating and pressurizing treatment under a specific condition has a dielectric breakdown voltage of 4 kV or more after being subjected to a bending treatment using a no-load U-shaped stretch tester.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an insulating sheet, a laminate including a cured product of the insulating sheet, and a semiconductor device including the laminate. [Background technology]

[0002] Conventionally, power modules have been used in a wide range of fields, such as industrial equipment, household electrical appliances, and information terminals. Attempts have been made to use resin sheets as substrates in power modules, and power modules using resin sheets are expected to be deployed in, for example, high voltage applications. Resin sheets need to be insulating sheets having insulation properties, and are also required to have high thermal conductivity and excellent heat dissipation properties. From the viewpoint of improving the heat dissipation of resin sheets, a technology for highly filling boron nitride agglomerated particles is known.

[0003] Patent Document 1 describes an invention related to a composition for forming a thermally conductive material, which contains an epoxy resin, a specific phenol compound, and an inorganic nitride, and in its examples, describes an example of a composition containing 77 to 87 mass% of boron nitride agglomerated particles as the inorganic nitride. Patent Document 2 describes an invention related to a thermally conductive composition containing an epoxy resin, a cyanate resin, a thermally conductive filler, and a flexibility imparting agent, and in the examples, describes a thermally conductive sheet having a thickness of 400 μm, which contains 74.8 mass% of boron nitride agglomerated particles produced as the thermally conductive filler and has a thickness of 400 μm. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7136906 [Patent Document 2] Patent No. 7073716 Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, an insulating sheet in which a resin is highly filled with agglomerated particles of boron nitride can increase thermal conductivity to a certain degree. However, since boron nitride agglomerated particles have voids inside, the insulating sheet tends to be brittle, and there is room for improvement in flexibility. Also, it is generally known that boron nitride agglomerated particles do not mix well with resins. Therefore, insulating sheets containing boron nitride agglomerated particles tend to have poor physical properties such as insulation due to thermal loads caused by the reflow process during semiconductor device manufacturing and by turning on and off heat generated by chips after semiconductor device manufacturing. The compositions (or sheets) containing the boron nitride agglomerated particles of Patent Documents 1 and 2 described above have room for improvement in terms of satisfying all of the requirements of high thermal conductivity, good flexibility, and suppression of deterioration in insulation due to thermal load. Therefore, an object of the present invention is to provide an insulating sheet that is highly filled with an inorganic filler containing boron nitride agglomerated particles, which has excellent flexibility and is capable of suppressing a decrease in insulating properties due to thermal load. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by an insulating sheet that contains a certain amount or more of an inorganic filler that includes agglomerated particles of boron nitride, and that has a certain or higher dielectric breakdown voltage after being subjected to a heating and pressurizing treatment and a bending treatment under specific conditions, and have thus completed the present invention. That is, the present invention relates to the following [1] to

[14] .

[0007] [1] An insulating sheet comprising a thermosetting resin, a thermosetting agent, and an inorganic filler, the inorganic filler comprising boron nitride agglomerated particles, the content of the inorganic filler being 65% by volume or more relative to 100% by volume of the insulating sheet, the insulating sheet being heated and pressurized under the following conditions, and having a dielectric breakdown voltage of 4 kV or more after being bent using a no-load U-shaped stretch tester: (Conditions for heat and pressure treatment and bending treatment) Two insulating sheets are stacked and heated and pressurized in a heat press at 90°C, 20MPa, and 45 minutes. The insulating sheet after heat and pressure treatment is cut into a 50mm x 50mm square and bent into a U-shape using a no-load U-shaped stretch tester so that the distance between the ends of the insulating sheet is 15mm, then returned to its original shape, with this cycle being considered as one cycle, and a total of five bending cycles are performed. [2] The insulating sheet according to the above [1], wherein the content of the boron nitride agglomerated particles is 50 volume % or more based on 100 volume % of the insulating sheet. [3] The insulating sheet according to the above [1] or [2], wherein the content of boron nitride agglomerated particles, the primary particles of which have an average aspect ratio of less than 7, is 50 vol % or more based on 100 vol % of the insulating sheet. [4] The insulating sheet according to any one of the above [1] to [3], wherein the inorganic filler contains inorganic particles other than boron nitride agglomerated particles. [5] The insulating sheet according to any one of the above [1] to [4], wherein the thermosetting resin contains a liquid epoxy resin having a viscosity of 50,000 mPa s or less at 25°C, and the content of the liquid epoxy resin is 40 vol% or more in 100 vol% of the thermosetting resin. [6] The insulating sheet according to any one of the above [1] to [5], wherein the heat curing agent contains an imide oligomer. [7] The insulating sheet according to any one of the above [1] to [6], which has a thickness of 150 μm or less after the heating and pressurizing treatment. [8] The insulating sheet according to any one of the above [1] to [7], which has a thermal conductivity of 10 W / m·K or more. [9] The insulating sheet according to any one of the above [1] to [8], wherein the insulating sheet is vacuum-pressed under conditions of 195°C, 20 MPa, and 80 minutes, and when the insulating sheet is heated from 50°C to 300°C at a heating rate of 10°C / min in a dry nitrogen stream using a simultaneous differential thermal and thermogravimetric analyzer, the weight loss rate is 4% or less.

[10] A cured product of the insulating sheet according to any one of the above [1] to [9].

[11] A laminate comprising the cured product of the insulating sheet described in

[10] above, a metal base plate, and a metal plate, the cured product of the insulating sheet and the metal plate being disposed, in this order, on the metal base plate.

[12] The laminate according to the above

[11] , which is a circuit board.

[13] The laminate according to the above

[11] or

[12] , wherein the metal plate has a circuit pattern.

[14] A semiconductor device comprising the laminate according to any one of the above

[11] to

[13] and a semiconductor element provided on the metal plate. Effect of the Invention

[0008] According to the present invention, it is possible to provide an insulating sheet that is highly filled with an inorganic filler including boron nitride agglomerated particles, and that has excellent flexibility and is capable of suppressing a decrease in insulating properties due to thermal load. [Brief description of the drawings]

[0009] [Figure 1] FIG. 11 is a schematic cross-sectional view for explaining a bending process. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing a laminate according to one embodiment of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing a semiconductor device according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Insulating sheet] The insulating sheet of the present invention contains a thermosetting resin, a thermosetting agent, and an inorganic filler, the inorganic filler containing boron nitride agglomerated particles, the content of the inorganic filler being 65% by volume or more relative to 100% by volume of the insulating sheet, and the insulating sheet which has been subjected to a heating and pressurizing treatment under the following conditions has a dielectric breakdown voltage of 4 kV or more after being subjected to a bending treatment using a no-load U-shaped stretch tester. (Conditions for heat and pressure treatment and bending treatment) Two insulating sheets are stacked and heated and pressurized in a heat press at 90°C, 20MPa, and 45 minutes. The insulating sheet after heat and pressure treatment is cut into a 50mm x 50mm square and bent into a U-shape using a no-load U-shaped stretch tester so that the distance between the ends of the insulating sheet is 15mm, then returned to its original shape, with this cycle being considered as one cycle, and a total of five bending cycles are performed.

[0011] <Breakdown voltage> The insulating sheet of the present invention has a breakdown voltage of 4 kV or more after heating and pressurizing treatment and bending treatment. If the breakdown voltage after heating and pressurizing treatment and bending treatment is less than 4 kV, the flexibility of the insulating sheet is poor, and the insulation is likely to decrease due to a thermal load such as reflow. This is thought to be because, if the flexibility of the insulating sheet is poor, the insulating sheet cracks during bending treatment, resulting in a decrease in the breakdown voltage. From the viewpoint of improving the flexibility of the insulating sheet and suppressing deterioration of insulating properties due to thermal load, the dielectric breakdown voltage after heating and pressurizing treatment and bending treatment is preferably 5 kV or more, more preferably 6 kV or more, and even more preferably 7 kV or more. The higher the breakdown voltage after the heating and pressurizing treatment and bending treatment, the better, but in practice it is 20 kV or less.

[0012] A sample for measuring the breakdown voltage is prepared as follows. First, two insulating sheets are laminated and heated and pressurized in a heat press at a temperature of 90°C, a pressure of 20 MPa, and a time of 45 minutes. In this case, two sets of laminated sheets are prepared, each having an insulating sheet formed on a release-treated PET (polyethylene terephthalate) film, and the two sets of laminated sheets are laminated so that the insulating sheets are in contact with each other, and then heated and pressurized in a heat press at a temperature of 90°C, a pressure of 20 MPa, and a time of 45 minutes.

[0013] Next, the insulating sheet that has been subjected to the above-mentioned heat and pressure treatment is cut into a piece having an area of ​​50 mm×50 mm square, and the release-treated PET film is peeled off. The insulating sheet cut as described above is subjected to a bending process using a no-load U-shaped stretch tester. Specifically, both ends of the insulating sheet are fixed to the jigs of the no-load U-shaped stretch tester. When fixed, the insulating sheet is flat as shown in the left diagram of FIG. 1. Then, one jig (not shown) is moved so as to approach the other, and the insulating sheet is folded into a U-shape as shown in the right diagram of FIG. 1. When folding into a U-shape, the insulating sheet is folded until the distance between the ends is 15 mm. After folding, one jig is moved away from the other jig, and the sheet is returned to the state shown in the left diagram of FIG. 1. This is regarded as one cycle, and a total of five cycles are performed. In the no-load U-shaped stretch tester, the stretch speed of the insulating sheet is 11 rpm. That is, the stretch speed is set to perform 11 cycles in 60 seconds. The insulation sheet that has been subjected to the heating and pressurizing treatment and bending treatment as described above is measured for its dielectric breakdown voltage. The method for measuring the dielectric breakdown voltage is as described in the Examples. The dielectric breakdown voltage can be adjusted by adjusting the type of boron nitride agglomerated particles (particle size, aspect ratio), the types of thermosetting resin and curing agent used, and the amounts of these blended.

[0014] <Weight reduction rate> From the viewpoint of improving heat resistance, the insulating sheet of the present invention preferably has a weight loss rate of 4% or less, and more preferably 2% or less, when heated from 50° C. to 300° C. The weight loss rate can be adjusted by the types and amounts of the thermosetting resin and thermosetting agent used. The weight loss rate is measured as follows using an insulating sheet sample after vacuum pressing under conditions of 195° C., 20 MPa, and 80 minutes. The weight loss rate is calculated from the sample weight before measurement and the sample weight after heating to 300°C when the insulating sheet after vacuum pressing is heated from 50°C to 300°C under conditions of a dry nitrogen gas flow and a heating rate of 10°C / min using a simultaneous thermogravimetry and differential thermal analyzer. Weight loss rate (%) = 100 × [(sample weight before measurement - sample weight when heated to 300 °C) / (sample weight before measurement)]

[0015] <Thermal conductivity> From the viewpoint of improving heat dissipation, the thermal conductivity of the insulating sheet of the present invention is preferably 10 W / (m·K) or more, more preferably 12 W / (m·K) or more, even more preferably 15 W / (m·K) or more, and preferably 50 W / (m·K) or less. The thermal conductivity of the insulating sheet can be adjusted mainly by the type and amount of the inorganic filler to be mixed.

[0016] <Inorganic filler> The insulating sheet of the present invention contains an inorganic filler including agglomerated particles of boron nitride. By containing the agglomerated particles of boron nitride, the thermal conductivity of the insulating sheet is increased, and heat dissipation properties are improved. From the viewpoint of increasing the thermal conductivity of the insulating sheet, the content of the boron nitride agglomerated particles is preferably 50% by volume or more, more preferably 60% by volume or more, and even more preferably 70% by volume or more, based on 100% by volume of the insulating sheet. From the viewpoint of maintaining good flexibility and mechanical strength of the sheet, the content of the boron nitride agglomerated particles is preferably 90% by volume or less, and more preferably 80% by volume or less, based on 100% by volume of the insulating sheet.

[0017] The average aspect ratio of the primary particles of the boron nitride agglomerated particles is preferably less than 7. By using boron nitride agglomerated particles having an average aspect ratio of less than 7, the flexibility of the insulating sheet is improved and a decrease in insulating properties due to thermal load can be suppressed. The average aspect ratio of the boron nitride agglomerated particles is preferably 6.0 or less, more preferably 5.5 or less. The lower limit of the average aspect ratio of the primary particles of the boron nitride agglomerated particles is not particularly limited, but the average aspect ratio is, for example, 1 or more, preferably 2 or more, and more preferably 4 or more. The content of boron nitride agglomerated particles having an average aspect ratio of primary particles of less than 7 is preferably 50 vol% or more, more preferably 60 vol% or more, even more preferably 70 vol% or more, and preferably 90 vol% or less, more preferably 80 vol% or less, based on 100 vol% of the insulating sheet.

[0018] The boron nitride agglomerated particles used in the present invention may be a mixture of boron nitride agglomerated particles having an average aspect ratio of primary particles less than 7 and boron nitride agglomerated particles having an average aspect ratio of primary particles of 7 or more, but it is preferable to use a larger amount of boron nitride agglomerated particles having an average aspect ratio of primary particles less than 7. In this case, when mixing the two, the proportion of boron nitride agglomerated particles having an average aspect ratio of primary particles less than 7 (blended amount of boron nitride agglomerated particles having an average aspect ratio of primary particles less than 7 / blended amount of all boron nitride agglomerated particles) is preferably 70 vol% or more, more preferably 80 vol% or more, and even more preferably 100 vol%.

[0019] The average aspect ratio of the boron nitride agglomerated particles is measured by a scanning electron microscope. For example, a cross section of a sheet made by mixing boron nitride agglomerated particles with a thermosetting resin or the like is smoothed by a cross section polisher (e.g., "IB-19500CP" manufactured by JEOL Ltd.), and the cross section of the processed sheet is observed by a field emission scanning electron microscope (e.g., "S-4800" manufactured by Hitachi High-Technologies Corporation). The average aspect ratio of the major axis / minor axis of 50 randomly selected primary particles of boron nitride can be calculated from the obtained electron microscope image.

[0020] The average particle size of the boron nitride agglomerated particles is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and preferably 150 μm or less, more preferably 80 μm or less, even more preferably 70 μm or less. When the average particle size of the boron nitride agglomerated particles is equal to or larger than the lower limit, the thermal conductivity of the insulating sheet is easily increased.When the average particle size of the boron nitride agglomerated particles is equal to or smaller than the upper limit, the flexibility of the insulating sheet is increased, and the breakdown voltage after bending treatment is easily increased. The average particle size of the boron nitride agglomerated particles refers to the particle size (d50) of the boron nitride agglomerated particles when the cumulative volume is 50% as measured using a laser diffraction particle size distribution measuring device.

[0021] Generally, whether or not a boron nitride agglomerated particle is an agglomerated particle can be determined by, for example, observing the cross section by a scanning electron microscope (SEM). The boron nitride agglomerated particle may maintain the shape of the agglomerated particle by undergoing various processes such as press molding, or may be deformed, collapsed, or crushed. However, even if the boron nitride agglomerated particle is deformed, collapsed, or crushed by undergoing a process such as press molding after being mixed with a thermosetting resin, it is not generally oriented and exists in a certain degree of aggregation, so that, for example, by observing the above-mentioned cross section, it is suggested that the particle is a boron nitride agglomerated particle, and therefore it can be determined whether or not the particle is an agglomerated particle.

[0022] The method for producing the boron nitride aggregated particles is not particularly limited, and they can be produced by a known method. For example, they can be obtained by aggregating (granulating) the primary particles prepared in advance, and specifically, the spray drying method and the fluidized bed granulation method can be mentioned. The spray drying method (also called spray drying) can be classified into a two-fluid nozzle method, a disk method (also called rotary method), and an ultrasonic nozzle method, etc., depending on the spray method, and any of these methods can be applied. The method for producing agglomerated particles of boron nitride does not necessarily require a granulation step. For example, agglomerated particles may be formed by natural aggregation of primary particles of boron nitride as crystals of boron nitride crystallized by a known method grow. Examples of boron nitride agglomerated particles include "HP-40" manufactured by JFE Mineral Co., Ltd. and "UHP-G1H" manufactured by Resonac Corporation.

[0023] The inorganic filler may contain inorganic particles other than the boron nitride agglomerated particles. Examples of inorganic particles other than the boron nitride agglomerated particles include alumina, aluminum nitride, magnesium oxide, diamond, silicon carbide, boron nitride other than the boron nitride agglomerated particles, etc. Among these, the inorganic particles other than the boron nitride agglomerated particles are preferably alumina or aluminum nitride. The inorganic particles other than the boron nitride agglomerated particles have an average particle size of, for example, 0.1 μm to 200 μm, preferably 5 μm to 50 μm. The average particle size refers to the particle size (d50) of the inorganic particles when the cumulative volume is 50% as measured using a laser diffraction particle size distribution analyzer.

[0024] In the insulating sheet of the present invention, the content of the inorganic filler is 65% by volume or more in 100% by volume of the insulating sheet. Here, the content of the inorganic filler is the total amount of the boron nitride agglomerated particles and inorganic particles other than the boron nitride agglomerated particles. Note that the inorganic filler does not necessarily need to contain inorganic particles other than the boron nitride agglomerated particles. If the content of the inorganic filler is less than 65% by volume, the thermal conductivity of the insulating sheet is low and good heat dissipation cannot be obtained. From the viewpoint of improving the thermal conductivity, the content of the inorganic filler is preferably 70% by volume or more, and from the viewpoint of maintaining good flexibility and mechanical strength of the sheet, it is preferably 90% by volume or less, more preferably 80% by volume or less.

[0025] <Thermosetting resin> The insulating sheet of the present invention contains a thermosetting resin. The thermosetting resin is not particularly limited, but examples thereof include amino resins such as urea resins and melamine resins, phenolic resins, thermosetting urethane resins, epoxy resins, thermosetting polyimide resins, aminoalkyd resins, and benzoxazine resins. The thermosetting resins used in the insulating sheet may be used alone or in combination of two or more. Among the above, epoxy resins are preferred as the thermosetting resin.

[0026] Examples of epoxy resins include compounds containing two or more epoxy groups in the molecule. Examples of epoxy resins include styrene skeleton-containing epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, biphenol type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, fluorene type epoxy resins, phenol aralkyl type epoxy resins, naphthol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, anthracene type epoxy resins, epoxy resins having an adamantane skeleton, epoxy resins having a tricyclodecane skeleton, epoxy resins having a triazine nucleus in the skeleton, and glycidylamine type epoxy resins. The epoxy resin may also be a phenoxy resin. The phenoxy resin is, for example, a resin obtained by reacting epihalohydrin with a divalent phenol compound, or a resin obtained by reacting a divalent epoxy compound with a divalent phenol compound. Examples of the phenoxy resin include those having a bisphenol A type skeleton, a bisphenol F type skeleton, a bisphenol A / F mixed skeleton, a naphthalene skeleton, a fluorene skeleton, a biphenyl skeleton, anthracene skeleton, a pyrene skeleton, a xanthene skeleton, a bisphenol TMC skeleton, an adamantane skeleton, or a dicyclopentadiene skeleton. Among the epoxy resins, bisphenol A type epoxy resins or bisphenol F type epoxy resins are preferred from the viewpoint of improving the flexibility of the insulating sheet.

[0027] From the viewpoint of improving the flexibility and insulating properties of the insulating sheet, the epoxy resin is preferably a liquid epoxy resin, where liquid epoxy resin means an epoxy resin that is liquid at 25°C. From the viewpoint of improving the flexibility and insulating properties of the insulating sheet, it is preferable that the thermosetting resin contains a liquid epoxy resin having a viscosity at 25° C. of 50,000 m·Pa or less. The viscosity of the liquid epoxy resin is preferably 1000 mPa·s or more and 50000 mPa·s or less, more preferably 1500 mPa·s or more and 20000 mPa·s or less, and even more preferably 2000 mPa·s or more and 10000 mPa·s or less. The above viscosity is measured using a Brookfield viscometer at 25° C. and 10 rpm.

[0028] From the viewpoint of improving the flexibility and insulating properties of the insulating sheet, the content of the liquid epoxy resin having a viscosity of 50,000 mPa s or less at 25°C is preferably 40 vol% or more, more preferably 60 vol% or more, even more preferably 80 vol% or more, and even more preferably 100 vol% in 100 vol% of the thermosetting resin.

[0029] The content of the thermosetting resin is preferably 5 vol% or more, more preferably 10 vol% or more, and preferably 30 vol% or less, more preferably 20 vol% or less, based on 100 vol% of the insulating sheet. When the content of the thermosetting resin is equal to or greater than these lower limits, the flexibility of the insulating sheet is easily improved, and when the content of the thermosetting resin is equal to or less than these upper limits, a certain amount or more of inorganic filler can be blended, making it easier to increase the thermal conductivity.

[0030] <Thermal hardener> The insulating sheet of the present invention contains a thermosetting agent. The thermosetting agent is not particularly limited as long as it is a curing agent that can cure the thermosetting resin. It is preferable that the above-mentioned thermosetting resin is cured by the thermosetting agent and binds the inorganic filler. Examples of the heat curing agent include a phenol compound (phenol heat curing agent), an amine compound (amine heat curing agent), an imidazole compound, an acid anhydride, a cyanate ester compound, a carbodiimide compound, an imide oligomer, etc. The heat curing agent may be used alone or in combination of two or more kinds. Among the above, the thermosetting agent preferably contains an imide oligomer from the viewpoint of improving the heat resistance of the insulating sheet.

[0031] Examples of the phenol compound include novolak type phenol, biphenol type phenol, naphthalene type phenol, dicyclopentadiene type phenol, aralkyl type phenol, and dicyclopentadiene type phenol. Examples of the amine compound include dicyandiamide, diaminodiphenylmethane, and diaminodiphenylsulfone.

[0032] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylate. Examples of the compound include melitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.

[0033] Examples of acid anhydrides include styrene / maleic anhydride copolymer, benzophenone tetracarboxylic anhydride, pyromellitic anhydride, trimellitic anhydride, 4,4'-oxydiphthalic anhydride, phenylethynylphthalic anhydride, glycerol bis(anhydrotrimellitate) monoacetate, ethylene glycol bis(anhydrotrimellitate), methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and trialkyltetrahydrophthalic anhydride.

[0034] Examples of the cyanate ester compound include novolac type cyanate resins and bisphenol type cyanate resins. Examples of the bisphenol type cyanate resins include bisphenol A type cyanate resins, bisphenol E type cyanate resins, and tetramethylbisphenol F type cyanate resins.

[0035] The carbodiimide compound includes a resin having one or more carbodiimide groups (-N=C=N-) in the molecule.

[0036] The imide oligomer is a compound having an imide skeleton in the main chain, and preferably has an aromatic ring in the skeleton. By having an aromatic ring in the skeleton, the insulating sheet is less likely to undergo thermal decomposition, and heat resistance is easily improved. In addition, from the viewpoint of improving heat resistance, it is preferable that the imide oligomer does not have a linear saturated hydrocarbon chain having 16 or more carbon atoms in the skeleton.

[0037] The imide oligomer has reactive functional groups at both ends or one end of the molecule that can react with the thermosetting resin, and the reactive functional groups are preferably acid anhydride groups, amino groups, or hydroxyl groups. The amino groups are not particularly limited and may be any of primary amino groups, secondary amino groups, and tertiary amino groups. The hydroxyl groups may be phenolic hydroxyl groups or hydroxyl groups other than phenolic hydroxyl groups. By using an imide oligomer having such reactive functional groups, the heat resistance of the insulating sheet is easily improved. The reactive functional groups of the imide oligomer are more preferably acid anhydride groups or phenolic hydroxyl groups from the viewpoint of heat resistance.

[0038] The molecular weight of the imide oligomer is preferably 500 to 10,000. When the molecular weight is within this range, the heat resistance of the insulating sheet is likely to be improved. The molecular weight of the imide oligomer is more preferably 700 to 7,000, and further preferably 900 to 5,000. The molecular weight of the imide oligomer is preferably 500 or more, more preferably 700 or more, and further preferably 900 or more, and is preferably 10,000 or less, more preferably 7,000 or less, and further preferably 5,000 or less. The molecular weight is a number average molecular weight measured by gel permeation chromatography (GPC) and calculated as polystyrene. Examples of columns used for measuring the number average molecular weight calculated as polystyrene by GPC include JAIGEL-2H-A (manufactured by Japan Analytical Industry Co., Ltd.). Specifically, the measurement can be performed using tetrahydrofuran as a solvent at room temperature and at a flow rate of 1 mL / min. The solvent is not particularly limited as long as it dissolves the sample to be measured, and the flow rate can be selected according to the column and device.

[0039] The imide oligomer may, for example, have a segment derived from an acid dianhydride represented by the following formula (1) and a segment derived from a polyamine compound. In this case, it is preferable that the segment derived from the acid dianhydride represented by the formula (1) is present at the end of the main chain, and more preferably at both ends of the main chain. In addition, the polyamine compound may, for example, be an aromatic diamine compound, an aliphatic diamine compound, or an aliphatic triamine compound.

[0040] [ka] In formula (1), A is an acid dianhydride residue and is a tetravalent group represented by the following formula (3-1) or (3-2).

[0041] [ka] In formula (3-1) and formula (3-2), * is a bonding position, and in formula (3-1), Z is a bond, an oxygen atom, a carbonyl group, a sulfur atom, a sulfonyl group, a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position. The hydrogen atoms of the aromatic ring in formula (3-1) and formula (3-2) may be substituted.

[0042] The polyamine compound includes an aromatic polyamine compound and an aliphatic polyamine compound, and among them, an aromatic polyamine compound is preferable. By using an imide oligomer having a segment derived from an aromatic polyamine compound, it becomes easier to obtain an insulating sheet having excellent heat resistance.

[0043] Examples of the aromatic polyamine compound include aromatic diamine compounds and aromatic triamine compounds, and the aromatic diamine compound represented by the following formula (2) is preferred. [ka] In formula (2), B is an aromatic diamine residue and is a divalent group represented by the following formula (4-1) or (4-2): 1 ~R 4 are each independently a hydrogen atom or a monovalent hydrocarbon group.

[0044] [ka] In formula (4-1) and formula (4-2), * is a bonding position, and in formula (4-1), Y is a bond, an oxygen atom, a carbonyl group, a sulfur atom, a sulfonyl group, a linear or branched divalent hydrocarbon group which may have an oxygen atom at the bonding position, or a divalent group having an aromatic ring which may have an oxygen atom at the bonding position. In formula (4-1) and formula (4-2), some or all of the hydrogen atoms of the phenylene group may be substituted with a hydroxyl group or a monovalent hydrocarbon group.

[0045] Examples of the aliphatic polyamine compound include an aliphatic diamine compound, an aliphatic triamine compound, etc. Examples of commercially available aliphatic diamine compounds and aliphatic triamine compounds include Versamine 551 and Versamine 552 manufactured by BASF, and Priamine 1071, Priamine 1073, Priamine 1074, and Priamine 1075 manufactured by Croda.

[0046] Specifically, the imide oligomer is preferably an imide oligomer represented by the following formula (5-1), (5-2), (5-3), (5-4), or (5-5). [ka]

[0047] In the formulas (5-1) to (5-5), A is an acid dianhydride residue and may be the same as in the above formula (1). In the formulas (5-1) to (5-5), A may be the same or different. In the formulas (5-1) to (5-5), B is an aliphatic diamine residue or an aromatic diamine residue, or an aliphatic triamine residue or an aromatic triamine residue, and in the formulas (5-3) and (5-4), B may be the same or different. When B is an aliphatic diamine residue or an aliphatic triamine residue, the carbon number is, for example, 4 to 60, and when B is an aromatic diamine residue or an aromatic triamine residue, the carbon number is, for example, 6 to 60. When B is an aromatic diamine residue, it may be as described in the formula (2). In formula (5-2), X is a hydrogen atom, a halogen atom, or an optionally substituted monovalent hydrocarbon group, and in formula (5-4), W is a hydrogen atom, a halogen atom, or an optionally substituted monovalent hydrocarbon group. In formulas (5-3) and (5-4), n is the number of repeating units.

[0048] Examples of a method for producing an imide oligomer having an acid anhydride group as a reactive functional group include a method of reacting an acid dianhydride represented by the above formula (1) with a polyamine compound such as the above aromatic diamine compound, aliphatic diamine compound, or aliphatic triamine compound.

[0049] A specific example of the method for reacting the acid dianhydride represented by the above formula (1) with a polyamine compound is shown below. First, a polyamine compound is dissolved in a solvent (e.g., N-methylpyrrolidone, dimethylformamide, dimethylacetamide, etc.) in which the amic acid oligomer obtained by the reaction is soluble, and the acid dianhydride represented by the above formula (1) is added to the obtained solution and reacted to obtain an amic acid oligomer solution. Next, the solvent is removed from the obtained amic acid oligomer solution by heating or reducing pressure, or the amic acid oligomer is recovered by reprecipitation by putting it into a poor solvent such as water, methanol, or hexane, and further heated at about 200°C or higher for 1 hour or more to proceed with the imidization reaction. By adjusting the molar ratio of the acid dianhydride represented by the above formula (1) to the polyamine and the imidization conditions, an imide oligomer having a desired number average molecular weight and an acid anhydride group as a reactive functional group at both ends can be obtained.

[0050] The imide oligomer may have a segment derived from an acid dianhydride represented by the above formula (1) and a segment derived from a phenolic hydroxyl group-containing monoamine represented by the following formula (5). Furthermore, the imide oligomer may have a segment derived from the acid dianhydride represented by the above formula (1), a segment derived from the above polyamine compound, and a segment derived from a phenolic hydroxyl group-containing monoamine represented by the following formula (5). In this case, it is preferable that the main chain has a segment derived from a phenolic hydroxyl group-containing monoamine represented by the following formula (5) at an end thereof, and more preferably at both ends thereof.

[0051] [ka] In formula (5), Ar is an optionally substituted divalent aromatic group, and R 5 and R 6 are each independently a hydrogen atom or a monovalent hydrocarbon group.

[0052] Examples of a method for producing an imide oligomer having a hydroxyl group as a reactive functional group include the following method. That is, examples of the method include a method of reacting the acid dianhydride represented by the above formula (1) with the phenolic hydroxyl group-containing monoamine represented by the above formula (5), and a method of reacting the acid dianhydride represented by the above formula (1) with the above polyamine compound, and then further reacting with the phenolic hydroxyl group-containing monoamine represented by the above formula (5).

[0053] A specific example of the method for reacting the acid dianhydride represented by the above formula (1) with the phenolic hydroxyl group-containing monoamine represented by the above formula (5) is shown below. First, the phenolic hydroxyl group-containing monoamine represented by the above formula (5) is dissolved in a solvent (e.g., N-methylpyrrolidone, dimethylformamide, dimethylacetamide, etc.) in which the amic acid oligomer obtained by the reaction is soluble, and the acid dianhydride represented by the above formula (1) is added to the obtained solution and reacted to obtain an amic acid oligomer solution. Next, the solvent is removed from the obtained amic acid oligomer solution by heating or reducing pressure, or the amic acid oligomer is recovered by reprecipitation by putting it into a poor solvent such as water, methanol, or hexane, and further heated at about 200°C or higher for 1 hour or more to proceed with the imidization reaction. By adjusting the molar ratio of the acid dianhydride represented by the above formula (1) and the phenolic hydroxyl group-containing monoamine represented by the above formula (5) and the imidization conditions, an imide oligomer having a desired number average molecular weight and phenolic hydroxyl groups as reactive functional groups at both ends can be obtained.

[0054] A specific example of the method of reacting the acid dianhydride represented by the above formula (1) with a polyamine compound and then reacting it with a phenolic hydroxyl group-containing monoamine represented by the above formula (5) is shown below. First, a polyamine compound is dissolved in a solvent (e.g., N-methylpyrrolidone, dimethylformamide, dimethylacetamide, etc.) in which the amic acid oligomer obtained by the reaction is soluble, and the acid dianhydride represented by the above formula (1) is added to the obtained solution and reacted to obtain a solution of an amic acid oligomer (A) having acid anhydride groups at both ends. Next, the solvent is removed from the obtained solution of amic acid oligomer (A) by heating or reducing pressure, or the amic acid oligomer (A) is recovered by reprecipitation by pouring into a poor solvent such as water, methanol, or hexane, and the amic acid oligomer (A) is further heated at about 200°C or higher for 1 hour or more to proceed with the imidization reaction. The imide oligomer thus obtained, which has an acid anhydride group as a reactive functional group at both ends, is dissolved again in a solvent (e.g., N-methylpyrrolidone, dimethylformamide, dimethylacetamide, etc.), and the phenolic hydroxyl group-containing monoamine represented by the above formula (5) is added and reacted to obtain a solution of amic acid oligomer (B). The solvent is removed from the obtained solution of amic acid oligomer (B) by heating or reducing pressure, or the amic acid oligomer (B) is recovered by reprecipitation by putting it into a poor solvent such as water, methanol, or hexane, and the amic acid oligomer (B) is then recovered, and the imidization reaction is allowed to proceed by heating at about 200°C or higher for 1 hour or more. By adjusting the molar ratio of the acid dianhydride represented by the above formula (1), the polyamine compound, and the phenolic hydroxyl group-containing monoamine represented by the above formula (5), and the imidization conditions, an imide oligomer having a desired number average molecular weight and having a hydroxyl group as a reactive functional group at both ends can be obtained.

[0055] The method for producing an imide oligomer having an amine group as a reactive functional group is not particularly limited, but may be, for example, a method in which an imide oligomer having an acid anhydride group at the end is obtained by the above-mentioned method, and the imide oligomer is reacted with a polyamine compound (e.g., an aromatic diamine compound, etc.). Another method may be a method in which, when producing an imide oligomer by the above-mentioned method, the acid anhydride and the polyamine compound are adjusted to an appropriate molar ratio.

[0056] The content of the curing agent in the insulating sheet is not particularly limited, but is preferably 1 vol% or more, more preferably 5 vol% or more, even more preferably 10 vol% or more, even more preferably 15 vol% or more, and is preferably 30 vol% or less, more preferably 25 vol% or less, based on 100 vol% of the insulating sheet.

[0057] <Curing accelerator> The insulating sheet may further include a curing accelerator. The use of the curing accelerator increases the curing speed, allows the thermosetting resin to be cured quickly, and allows the crosslinked structure in the insulating sheet to be uniform. In addition, the number of unreacted functional groups is reduced, resulting in a high crosslink density. The curing accelerator is not particularly limited, and conventionally known curing accelerators can be used. Specific examples include anionic curing accelerators such as imidazole compounds, cationic curing accelerators such as amine compounds, curing accelerators other than anionic and cationic curing accelerators such as phosphorus compounds and organometallic compounds, and radical curing accelerators such as peroxides. The curing accelerator may be used alone or in combination of two or more kinds.

[0058] <Other> In addition to the above-mentioned components, the insulating sheet according to the present invention may contain other additives such as a coupling agent such as a silane coupling agent, a dispersant, a flame retardant, an antioxidant, a tackifier, a plasticizer, a thixotropy imparting agent, and a colorant.

[0059] <Thickness> The thickness of the insulating sheet of the present invention is not particularly limited, but is preferably 150 μm or less. If the thickness is 150 μm or less, the thermal resistance value of the insulating sheet can be reduced, and the heat dissipation property is improved. The thickness of the insulating sheet is preferably 150 μm or less, more preferably 130 μm or less, and preferably 80 μm or more, more preferably 100 μm or more. Similarly, the thickness of the insulating sheet after the heating and pressurizing treatment as described above is preferably 150 μm or less, more preferably 130 μm or less, and preferably 80 μm or more, more preferably 100 μm or more.

[0060] [Insulating sheet manufacturing method] The method for producing the insulating sheet of the present invention is not particularly limited, but may be a method in which a composition for insulating sheets containing the above-mentioned thermosetting resin, thermosetting agent, and inorganic filler containing boron nitride agglomerated particles is applied onto a substrate such as a release PET film, and then dried. The insulating sheet composition may contain, as necessary, an inorganic filler other than the boron nitride agglomerated particles, a curing accelerator, and other additives. The drying conditions after application of the insulating sheet composition are, for example, a drying temperature of 60 to 100°C, and preferably 70 to 90°C.

[0061] [Cured insulating sheet] The insulating sheet of the present invention can be cured by heating at a temperature equal to or higher than the curing temperature of the thermosetting resin to form a cured product of the insulating sheet. The curing is preferably performed by heating under pressure. The cured product of the insulating sheet can constitute a part of the laminate shown below.

[0062] [Laminate] As shown in FIG. 2, the laminate of the present invention comprises, in addition to the cured product 10 of the insulating sheet of the present invention, a metal base plate 11 and a metal plate 12, and is a laminate 13 comprising the cured product 10 of the insulating sheet and the metal plate 12 on the metal base plate 11, in this order.

[0063] The laminate of the present invention may be produced by press molding. Specifically, the laminate may be produced by stacking a metal base plate, an insulating sheet, and a metal plate in this order and press molding the laminate. The insulating sheet is fully cured by the press molding, and the cured insulating sheet can adhere to the metal base plate and the metal plate with a certain level of adhesive strength or more. The press molding may be carried out at a temperature of, for example, 150° C. or higher and 250° C. or lower, preferably 180° C. or higher and 210° C. or lower, and at a pressure of, for example, 8 MPa or higher and 25 MPa or lower. The pressing time is not particularly limited, but is, for example, from 10 minutes to 240 minutes, and preferably from 30 minutes to 200 minutes. The pressing may be performed under normal pressure, or may be performed by vacuum pressing. The laminate of the metal base plate, the insulating sheet, and the metal plate is preferably pressed under a reduced pressure environment, specifically, for example, under an environment of 10 kPa or less, preferably 3 kPa or less, more preferably 1.5 kPa or less.

[0064] Since the metal base plate 11 and the metal plate 12 each function as a thermal conductor, it is preferable that they have a thermal conductivity of 10 W / m·K or more. Materials used for these include metals such as aluminum, copper, gold, and silver, as well as graphite sheets. From the viewpoint of more effectively increasing thermal conductivity, aluminum, copper, or gold is preferable, and aluminum or copper is more preferable. The thickness of the metal base plate 11 is preferably 0.1 to 5 mm, and the thickness of the metal plate 12 is preferably 10 to 2000 μm, and more preferably 10 to 900 μm. The metal plate may be a plate such as a copper plate or a foil such as a copper foil.

[0065] The laminate 13 is preferably used as a circuit board. When used as a circuit board, the metal plate 12 in the laminate 13 may have a circuit pattern. The circuit pattern may be appropriately patterned according to the elements to be mounted on the circuit board. The circuit pattern is not particularly limited, but may be formed by etching or the like. In the circuit board, the metal base plate 11 is used as a heat sink or the like.

[0066] [Semiconductor Devices] The present invention also provides a semiconductor device having the laminate. Specifically, as shown in Fig. 3, the semiconductor device 15 includes a laminate 13 having a cured insulating sheet 10, a metal base plate 11, and a metal plate 12, and a semiconductor element 14 provided on the metal plate 12 of the laminate 13. The metal plate 12 may be patterned by etching or the like to have a circuit pattern.

[0067] Although two semiconductor elements 14 are shown in FIG. 3, the number of semiconductor elements 14 is not limited and may be any number as long as it is one or more. In addition to the semiconductor elements 14, other electronic components such as transistors (not shown) may be mounted on the metal plate 12. Each semiconductor element 14 is connected to the metal plate 12 via a connection conductive part 16 formed on the metal plate 12. The connection conductive part 16 is preferably formed of solder. Furthermore, a sealing resin 19 is provided on the surface of the laminate 13 on the metal plate 12 side. At least the semiconductor elements 14 are sealed with the sealing resin 19, and if necessary, the metal plate 12 may also be sealed with the sealing resin 19 together with the semiconductor elements 14. Although the semiconductor elements 14 are not particularly limited, it is preferable that at least one of them is a power element (i.e., a power semiconductor element), and thus the semiconductor device 15 is preferably a power module. The power module is used, for example, in an inverter or the like. Furthermore, the power module is used in industrial equipment such as elevators and uninterruptible power supplies (UPS), but its use is not particularly limited.

[0068] Leads 20 are connected to the metal plate 12. The leads 20 extend, for example, from the sealing resin 19 to the outside and connect the metal plate 12 to an external device or the like. Wires 17 may also be connected to the semiconductor element 14. The wires 17 may connect the semiconductor element 14 to another semiconductor element 14, the metal plate 12, the leads 20, or the like, as shown in FIG. The semiconductor element 14 generates heat when power is supplied via the leads 20 or the like to operate, and the heat generated by the semiconductor element 14 is transmitted to the metal base plate 11 via the cured insulating sheet 10 and dissipated from the metal base plate 11. The metal base plate 11 may be connected to a heat sink consisting of heat dissipation fins or the like as necessary.

[0069] The semiconductor device 15 may be manufactured through a reflow process in the manufacturing process. Specifically, in the manufacturing method of the semiconductor device 15, first, the laminate 13 is prepared, and the connection conductive portion 16 is formed on the metal plate 12 of the laminate 13 by solder printing or the like, and the semiconductor element 14 is mounted on the connection conductive portion 16. Thereafter, the laminate 13 on which the semiconductor element 14 is mounted is passed through the inside of a reflow furnace and heated in the reflow furnace, and the semiconductor element 14 is connected to the metal plate 12 by the connection conductive portion 16. The temperature in the reflow furnace is not particularly limited, but is, for example, about 200 to 300°C. In the manufacturing method of the semiconductor device 15, after the reflow process, the sealing resin 19 may be laminated on the laminate 13 to seal the semiconductor element 14. In addition, before sealing with the sealing resin 19, the wires 17, the leads 20, and the like may be attached as appropriate. Although the above describes an embodiment in which the semiconductor element 14 is connected to the metal plate 12 by a reflow process, the present invention is not limited to such an embodiment. For example, the laminate 13 (i.e., a circuit board) may be connected to another board (not shown) by a reflow process.

[0070] In addition, when manufacturing a laminate including a cured insulating sheet, a metal base plate, and a metal plate, the insulating sheet is placed between the metal base plate and the metal plate, and heated and pressurized by press molding to bond the metal base plate and the metal plate via the cured insulating sheet, thereby manufacturing the laminate. The insulating sheet is preferably cured by heating during press molding, but may be partially or completely cured before press molding. EXAMPLES

[0071] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0072] The components used in the examples and comparative examples are as follows. <Thermosetting resin> Epoxy resin 1 Bisphenol A type epoxy resin "YD-127" manufactured by Nippon Steel Chemical & Material Co., Ltd., liquid, viscosity (25°C) 10000mPa·s Epoxy resin 2 Bisphenol F type epoxy resin "EPICLON-830" manufactured by DIC, liquid (25°C) 4000mPa·s Epoxy resin 3: Phenol novolac type epoxy resin, DIC "EPICLON-N-730A", viscous liquid (25°C) 42000mPa s Epoxy resin 4 Biphenyl type epoxy resin "YH4000H" manufactured by Mitsubishi Chemical Corporation, solid (25°C)

[0073] <Heat curing agents, curing accelerators> Curing agent 1: Imide oligomer (IMO-1), synthesized as described below. ·Curing accelerator-1··Imidazole compound Shikoku Kasei Corporation "2P4MHZ-PW" · Hardener 2 · Cyanate ester compound "NCN" manufactured by Mitsubishi Gas Chemical Company, Inc.

[0074] <Synthesis of hardener 1 (IMO-1)> 104 parts by weight of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (Tokyo Chemical Industry Co., Ltd.) was dissolved in 300 parts by weight of N-methylpyrrolidone (Fujifilm Wako Pure Chemical Industries, Ltd., "NMP"). A solution of 28 parts by weight of dimer diamine Priamine 1074 (Croda) diluted with 100 parts by weight of N-methylpyrrolidone was added to the obtained solution, and the mixture was stirred at 25°C for 2 hours to react, thereby obtaining an amic acid oligomer solution. After removing N-methylpyrrolidone from the obtained amic acid oligomer solution under reduced pressure, the mixture was heated at 300°C for 2 hours to obtain an imide oligomer composition B (imidization rate 93%). The obtained imide oligomer composition B was subjected to 1H-NMR, GPC, and FT-IR analysis. As a result, it was confirmed that the imide oligomer composition B contained an imide oligomer having a structure represented by the above formula (5-1) or (5-3) (A is a 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride residue, and B is a dimer diamine residue). In addition, the number average molecular weight of the imide oligomer composition B was 2200.

[0075] <Dispersant> Dispersant 1: BYK-9076 manufactured by BYK-Chemie

[0076] <Inorganic filler> ·Boron nitride filler 1·Boron nitride agglomerated particles, JFE Mineral Co., Ltd. "HP-40 MF100", average particle size 40 μm, average aspect ratio of primary particles 5.7 · Boron nitride filler 2 · Boron nitride agglomerated particles, Resonac Corporation "UHP-G1H", average particle size 40 μm, average aspect ratio of primary particles 5.1 Boron nitride filler 3 Boron nitride agglomerated particles, Momentive's "PTX-60", average particle size 60 μm, average primary particle aspect ratio 12.9 Alumina filler 4: "AA-18" manufactured by Sumitomo Chemical Co., Ltd., average particle size 18 μm ·Aluminum nitride filler 5·Tokuyama Corporation "HF-20a", average particle size 20μm

[0077] [Examples 1 to 13, Comparative Examples 1 to 2] An insulating sheet having the composition shown in Table 1 was prepared as follows. The inorganic filler and dispersant shown in Table 1 were mixed in a blending cup, an appropriate amount of cyclohexanone was added, and the mixture was stirred for 3 minutes at 2000 rpm with a planetary stirrer. After that, each component was added to the blending cup in order according to the contents of Table 1, and the mixture was stirred for 3 minutes at 2000 rpm with a planetary stirrer to prepare a coating liquid (composition for insulating sheet). The obtained insulating sheet composition was applied to a release PET sheet (thickness 50 μm) using a 350 mm wide doctor blade to an arbitrary thickness. The coated sheet was cut to a size of 300 mm x 500 mm, placed on a metal rack, and dried in an oven at 80°C for 20 minutes to obtain an insulating sheet A formed on a release PET sheet. The oven used was a "DKM600" manufactured by Yamato Scientific Co., Ltd.

[0078] (heat and pressure treatment) Two sheets of insulating sheet A obtained in the drying process were laminated together with the insulating layers overlapping, with the release PET sheet from coating still attached, and then heated and pressurized (90°C, 45 min, 20 MPa) in a heat press to obtain semi-cured insulating sheet B. The heat press used was a "Hot Cold Press for PCB Molding" manufactured by Kitagawa Seiki Co., Ltd.

[0079] (Bending process using a no-load U-shaped stretch tester) After the heat and pressure treatment, the insulating sheet B was cut into a 50 x 50 mm square, and the PET film on both sides was peeled off. The ends of the sheet were then set in a sheet-shaped body no-load U-shape stretch tester, and bending treatment was performed under the following conditions. In the bending treatment, the insulating sheet was set so that it was in a flat state as the initial state, and then folded from the flat state into a U-shape until the distance between the ends of the insulating sheet was 15 mm, and then returned to the original flat state. This operation constituted one cycle. A total of five cycles were performed, and the stretching speed was 11 rpm. The unloaded U-shaped stretch test machine used was "DLDM111LHA" manufactured by Yuasa System Devices Co., Ltd.

[0080] (Breakdown voltage after bending) Using the insulating sheet after bending treatment as a sample, a voltage resistance tester ("MODEL 7473" manufactured by ETECH Electronics) was used to apply 200 V between the sample in Fluorinert, hold for 5 seconds, and then apply an AC voltage using a step-boosting method in which the voltage was increased by 200 V each time and held for 5 seconds in the same manner. The voltage at which a current of 10 mA flowed through the sample was taken as the dielectric breakdown voltage.

[0081] (Check for cracks after bending: flexibility evaluation) The insulating sheet after bending was observed with an optical microscope, and the presence or absence of cracks after bending was evaluated with the following criteria: "A" if there were no cracks or chips, "B" if cracks or chips occurred in only a certain area, and "C" if cracks or chips occurred over the entire surface of the film.

[0082] [Evaluation of substrate properties] (Preparation of substrates (laminates) for evaluating various physical properties) Two insulating sheets A after the drying treatment were laminated so that the insulating sheets A overlapped each other with the release PET sheets still attached, and then the release PET sheets on both sides were peeled off to obtain insulating sheet C. Next, a 0.5 mm thick copper plate was laminated on the first side of insulating sheet C, and a 2.0 mm thick copper plate was laminated on the second side, and a laminate was produced by vacuum pressing under conditions of a temperature of 195°C, a pressure of 20 MPa, and a time of 80 minutes. The laminate was a copper plate, a cured product of insulating sheet C, and a copper plate laminated in this order.

[0083] (Thermal Conductivity) Teflon (registered trademark) sheets were laminated on both sides of insulating sheet A from which the release PET sheet had been peeled off, and the sheet was vacuum pressed at a temperature of 195°C and a pressure of 20 MPa to produce measuring sheet 1. In addition, measuring sheets 2 and 3 were produced by vacuum pressing three sheets of insulating sheet A stacked together and five sheets of insulating sheet A stacked together under the same conditions as above. The thermal resistance values ​​of the measurement sheets 1 to 3 were measured, and the thermal conductivity was measured in a steady state method from the slope represented by the thermal resistance value versus the sheet thickness using the following formula (measured in accordance with ASTM D5470). The measurement device used was a "T3Ster-DynTIM" manufactured by Mentor Graphics. Formula: Thermal conductivity = [1 / (slope x measurement area)] x 10 -2 The unit of the thermal conductivity is (W / m K), the unit of the slope (thermal resistance value / sheet thickness) is (K / (W μm)), and the unit of the measurement area is (cm 2 ). The sheet thickness when calculating the slope is the thickness (μm) when pressed at 3400 kPa, the thermal resistance value is the thermal resistance value (K / W) when pressed at 3400 kPa, and the slope is the slope of a linear function calculated by the least squares method. The measurement area is the area of ​​the part that transfers heat (cm 2 ). The thermal conductivity was evaluated as follows. A:15W / (m·K) or more B: 12W / (m K) or more and less than 15W / (m K) C: 10W / (m K) or more and less than 12W / (m K) D: 8W / (m K) or more and less than 10W / (m K) E: Less than 8W / (m K)

[0084] (Breakdown voltage, initial and after heat treatment at 300℃) In the obtained laminate, a copper plate having a thickness of 0.5 mm was etched to form a pattern into a circle having a diameter of 2 cm, and the patterned copper foil was cut into a 4 cm square at the center to obtain a laminate sample. Using a voltage resistance tester ("MODEL7473" manufactured by ETECH Electronics), 200 V was applied between the laminate samples in Fluorinert, and after holding for 5 seconds, an AC voltage was applied using a step-up method in which the voltage was increased by 200 V each time and held for 5 seconds in the same manner. The voltage at which a current of 10 mA flowed through the laminate sample was taken as the initial breakdown voltage A1 (breakdown voltage before reflow). The insulation properties were evaluated according to the following criteria based on the measured initial dielectric breakdown voltage A1. Note that the insulation properties are better when the alphabetical order is lower. A: 60kV / mm or more B: 50kV / mm or more and less than 60kV / mm C: 40kV / mm or more and less than 50kV / mm D: 30kV / mm or more and less than 40kV / mm E: Less than 30kV / mm

[0085] A 4 cm square laminate sample was obtained in the same manner as in the initial insulation evaluation. The obtained laminate sample was placed on the hot plate surface with the copper plate side having a thickness of 2 mm, and the hot plate temperature was adjusted so that the surface temperature of the cured insulating sheet of the laminate sample was 300°C. In this state, the laminate sample was heat-treated for 5 minutes. The insulation breakdown voltage of the laminate sample after the heat treatment was measured in the same manner as in the evaluation of the initial insulation breakdown voltage. The insulation after the 300°C treatment was evaluated based on the above evaluation criteria using the measured insulation breakdown voltage A2 (insulation breakdown voltage after reflow) after the 300°C heat treatment. The breakdown voltage reduction rate was calculated from the initial breakdown voltage (A1) and the breakdown voltage after 300°C treatment (A2), and was evaluated according to the following criteria. Note that the lower the alphabetical order, the better the breakdown voltage reduction rate. Breakdown voltage reduction rate (%) = [(A1-A2) / A1] x 100 A: 15% or less B: More than 15% and less than 20% C: More than 20% and less than 25% D: More than 25% and less than 30% E: Over 30%

[0086] (Heat resistance) The cured product of insulating sheet C was taken out from the laminate produced as described above, and used as a sample to measure the weight loss rate when the temperature was raised from 50°C to 300°C at a heating rate of 10°C / min under a dry nitrogen stream using a simultaneous differential thermal analyzer (apparatus name "TG / DTA7300", manufactured by Hitachi High-Tech Science Corporation), and evaluated according to the following evaluation criteria. The cured product of insulating sheet C used as the sample corresponds to an insulating sheet obtained by vacuum pressing the insulating sheet at a temperature of 195°C, a pressure of 20 MPa, and for 80 minutes. Weight loss rate (%) = 100 × [(sample weight before measurement - sample weight when heated to 300 °C) / (sample weight before measurement)] A: 2.0% or less B: More than 2.0% but less than 4.0% C: More than 4.0%

[0087] [Table 1]

[0088] The results of each example show that insulating sheets containing 65% by volume or more of inorganic filler including boron nitride agglomerated particles and having a breakdown voltage of 4 kV or more after specific heating and pressurizing treatment and bending treatment had a high thermal conductivity of 10 W / m K or more and good flexibility as evidenced by the absence of cracks after bending tests. Furthermore, the insulating sheets of each example showed a low rate of decrease in breakdown voltage before and after reflow, suppressing the decrease in insulation due to heat load. In contrast, the insulating sheets in each of the comparative examples contained 65 vol. % or more of inorganic filler including agglomerated particles of boron nitride and had thermal conductivity of 10 W / m K or more. However, after specific heating and pressurizing treatment and bending treatment, the insulation voltage was less than 4 kV, indicating that the flexibility was poor, or the rate of decrease in the insulation voltage before and after reflow was large, indicating that the insulation properties were easily deteriorated by thermal load. [Explanation of symbols]

[0089] 10. Hardened insulating sheet 11 Metal base plate 12 metal plate 13 Laminate 14 Semiconductor elements 15 Semiconductor Devices 16 Conductive connection 17 Wire 19 Sealing resin 20 Lead

Claims

1. An insulating sheet comprising a thermosetting resin, a thermosetting agent, and an inorganic filler, the inorganic filler comprises agglomerated particles of boron nitride; The content of the inorganic filler is 65% by volume or more in 100% by volume of the insulating sheet, An insulating sheet, which has a dielectric breakdown voltage of 4 kV or more after being subjected to a bending treatment using a no-load U-shaped stretch tester after being subjected to a heating and pressurizing treatment under the following conditions: (Conditions of heat and pressure treatment and bending treatment) Two insulating sheets are stacked and subjected to a heat and pressure treatment in a hot press under conditions of a temperature of 90° C., a pressure of 20 MPa, and a time of 45 minutes. The insulating sheet after the heat and pressure treatment is cut into a 50 mm×50 mm square and subjected to a bending treatment for a total of 5 cycles, with one cycle being a U-fold so that the distance between the ends of the insulating sheet is 15 mm and a return cycle being performed in a no-load U-shaped stretch tester.

2. 2 . The insulating sheet according to claim 1 , wherein a content of the boron nitride agglomerated particles is 50% by volume or more based on 100% by volume of the insulating sheet.

3. 3. The insulating sheet according to claim 1, wherein a content of boron nitride agglomerated particles having an average aspect ratio of primary particles of less than 7 is 50% by volume or more based on 100% by volume of the insulating sheet.

4. The insulating sheet according to claim 1 , wherein the inorganic filler contains inorganic particles other than agglomerated particles of boron nitride.

5. The thermosetting resin contains a liquid epoxy resin having a viscosity of 50,000 mPa·s or less at 25°C, 3. The insulating sheet according to claim 1, wherein a content of the liquid epoxy resin is 40% by volume or more relative to 100% by volume of the thermosetting resin.

6. The insulating sheet according to claim 1 , wherein the heat curing agent comprises an imide oligomer.

7. 3. The insulating sheet according to claim 1, wherein the insulating sheet has a thickness of 150 μm or less after the heating and pressurizing treatment.

8. 3. The insulating sheet according to claim 1, having a thermal conductivity of 10 W / m·K or more.

9. 3. The insulating sheet according to claim 1 or 2, wherein the insulating sheet has a weight loss rate of 4% or less when the insulating sheet is vacuum-pressed under conditions of 195°C, 20 MPa, and 80 minutes and then heated from 50°C to 300°C at a heating rate of 10°C / min in a dry nitrogen stream using a simultaneous differential thermal and thermogravimetric analyzer.

10. A cured product of the insulating sheet according to claim 1 or 2.

11. A laminate comprising the cured product of the insulating sheet according to claim 10, a metal base plate, and a metal plate, the cured product of the insulating sheet and the metal plate being disposed in this order on the metal base plate.

12. The laminate according to claim 11 , which is a circuit board.

13. The laminate according to claim 11 , wherein the metal plate has a circuit pattern.

14. A semiconductor device comprising the laminate according to claim 11 and a semiconductor element provided on the metal plate.

Citation Information

Patent Citations

  • Thermally conductive resin composition, thermally conductive sheet and semiconductor device

    JP7073716B2

  • Composition for forming thermally conductive material, thermally conductive material, thermally conductive sheet, device with thermally conductive layer, film

    JP7136906B2