By reacting phenol resin with epihalohydrin to create a specific epoxy resin structure and combining it with a curing agent, the epoxy resin composition achieves enhanced heat resistance and mechanical strength in carbon fiber reinforced composites, addressing the low thermal stability of biomass-derived epoxy resins.
Patent Information
- Application Number
- JP2023055547
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing epoxy resins derived from biomass exhibit low heat resistance, limiting their application in carbon fiber reinforced composite materials (CFRP) due to insufficient thermal stability.
A phenol resin is reacted with epihalohydrin to produce an epoxy resin with specific molecular structures and molar ratios, combined with a curing agent to form a curable resin composition, which is then cured to create a carbon fiber reinforced composite material with enhanced heat resistance.
The resulting composite material exhibits excellent heat resistance, mechanical strength, and improved thermal stability, suitable for applications requiring high thermal endurance.
Smart Images

Figure 2024143063000016 
Figure 2024143063000017 
Figure 2024143063000018
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin having a specific structure, a curable resin composition, and a carbon fiber reinforced composite material obtained by curing the same. [Background technology]
[0002] By curing epoxy resins with various curing agents, they become cured products with excellent mechanical properties, water resistance, chemical resistance, heat resistance, and electrical properties, and are used in a wide range of fields such as adhesives, paints, laminates, molding materials, and casting materials. Carbon fiber reinforced composite materials (CFRP), which are made by impregnating and curing reinforcement fibers with epoxy resin and a curing agent as a matrix resin, can be given properties such as light weight and high strength, and in recent years they have been widely used in aircraft structural members, wind turbine blades, automobile exterior panels, and computer applications such as IC trays and laptop computer housings, and demand for them is increasing. In particular, they are used as matrix resins for aircraft applications, taking advantage of the light weight and high strength properties of the molded products.
[0003] In particular, fiber-reinforced plastic molded products made with reinforcing fibers have attracted attention for their lightweight yet excellent mechanical strength characteristics, and their use is expanding in a variety of structural applications, including housings and various components for automobiles, aircraft, ships, etc. In particular, as carbon fiber composite materials (CFRP) are increasingly being used in the aircraft and automotive fields, the amount of epoxy resin used as their matrix resin is steadily increasing.
[0004] Traditionally, many of the raw materials used for epoxy resins and hardeners have been derived from petroleum. However, in recent years, concerns have arisen about the depletion of petroleum resources, and methods of recycling many materials, such as using renewable resources such as plants or decomposing the hardened materials, are being investigated. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-211254 A Summary of the Invention [Problem to be solved by the invention]
[0006] Patent Document 1 describes an epoxy resin that uses raw materials derived from biomass. However, the epoxy resin described in Patent Document 1 has low heat resistance, and therefore there is a problem in using it as a CFRP material.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide an epoxy resin having excellent heat resistance, a curable resin composition containing the epoxy resin, and a carbon fiber reinforced composite material obtained by curing the composition or the cured composition, as well as a phenolic resin that is a precursor of the epoxy resin. [Means for solving the problem]
[0008] That is, the present invention is as shown in the following [1] to [7]. In the present invention, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] An epoxy resin obtained by reacting a phenolic resin represented by the following formula (1) with epihalohydrin.
[0009] [ka]
[0010] (In formula (1), each of the multiple R1's independently represents an alkyl group having 1 to 4 carbon atoms. Each of the multiple m's independently represents an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.) [2] An epoxy resin represented by the following formula (2).
[0011] [ka]
[0012] (X in formula (2) is a monovalent substituent obtained by removing one hydrogen atom from the benzene ring of formula (2a) or a divalent linking group obtained by removing two hydrogen atoms, or a monovalent substituent obtained by removing one hydrogen atom from the benzene ring of formula (2b) or a divalent linking group obtained by removing two hydrogen atoms, and in formulas (2a) and (2b), each of the multiple R1s independently represents a C1-4 alkyl group. Each of the multiple R2s independently represents a hydrogen atom or a methyl group. Each of the multiple m's independently represents an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.) [3] The epoxy resin according to item [2] above, wherein in the formula (2), the molar ratio of (2a) to (2b) is (2a):(2b)=5:1 to 2:1. [4] 4. The curable resin composition according to claim 3, comprising the epoxy resin according to any one of the preceding items [1] to [3] and a curing agent. [5] A cured product obtained by subjecting the curable resin composition according to the above item [4] to a curing reaction. [6] A carbon fiber reinforced composite material obtained by curing the curable resin composition according to the above item [4]. [7] [7] A phenolic resin represented by the following formula (1).
[0013] [ka]
[0014] (In formula (1), each of the multiple R1's independently represents an alkyl group having 1 to 4 carbon atoms. Each of the multiple m's independently represents an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.) Effect of the Invention
[0015] According to the present invention, it is possible to provide an epoxy resin, a curable resin composition, and a carbon fiber reinforced composite material obtained by curing the epoxy resin or the curable resin composition, the cured product of which has excellent heat resistance. [Brief description of the drawings]
[0016] [Figure 1] 1 is a GPC chart of the phenol resin of Example 1. [Diagram 2] 1 is a GPC chart of the epoxy resin of Example 2. [Diagram 3] 1 is an NMR chart of the epoxy resin of Example 2. [Figure 4] 1 is a GPC chart of the epoxy resin of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The epoxy resin of the present embodiment is obtained by reacting a phenol resin represented by the following formula (1) with epihalohydrin.
[0018] [ka]
[0019] (In formula (1), each of the multiple R1's independently represents an alkyl group having 1 to 4 carbon atoms. Each of the multiple m's independently represents an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.)
[0020] In the above formula (1), R1 is represented by an alkyl group having 1 to 4 carbon atoms, and from the viewpoint of reactivity when used as a raw material and bending properties of a cured product, preferred examples include a methyl group, an ethyl group, a propyl group, a butyl group, a t-butyl group, etc. Among these, when R1 is a t-butyl group, a good balance between heat resistance and low water absorption is achieved, which is a particularly preferred embodiment.
[0021] In the formula (1), the value of n can be calculated from the number average molecular weight determined by gel permeation chromatography (GPC, detector: RI) measurement or the area ratio of each separated peak. n is preferably a real number of 1 to 3, and more preferably a real number of 1.1 to 3.
[0022] The epihalohydrin is readily available on the market. The amount of epihalohydrin used is usually 2.0 to 10 mol, preferably 3.0 to 8.0 mol, and more preferably 3.5 to 6.0 mol, per mol of hydroxyl groups in the raw material phenol mixture.
[0023] In the reaction between the phenolic resin represented by the formula (1) and epihalohydrin, an alkali metal hydroxide can be used as a catalyst for promoting the epoxidation step. Examples of alkali metal hydroxides that can be used include sodium hydroxide and potassium hydroxide. A solid or an aqueous solution thereof can be used, but in this embodiment, a solid formed into a flake shape is preferably used in terms of solubility and handling. The amount of alkali metal hydroxide used is usually 0.90 to 1.5 mol, preferably 0.95 to 1.25 mol, more preferably 0.99 to 1.15 mol, per mol of hydroxyl groups in the raw phenol mixture.
[0024] In order to promote the above reaction, a quaternary ammonium salt such as tetramethylammonium chloride, tetramethylammonium bromide, trimethylbenzylammonium chloride, etc. may be added as a catalyst. The amount of the quaternary ammonium salt used is usually 0.1 to 15 g, preferably 0.2 to 10 g, per mole of hydroxyl groups in the raw material phenol mixture.
[0025] The reaction temperature is usually 30 to 90° C., preferably 35 to 80° C. In particular, in this embodiment, for higher purity epoxidation, a temperature of 50° C. or higher is preferred, and particularly 60° C. or higher is preferred. The reaction time is usually 0.5 to 10 hours, preferably 1 to 8 hours, and particularly preferably 1 to 3 hours. If the reaction time is too short, the reaction will not proceed to completion, and if the reaction time is too long, by-products will be produced, which is undesirable.
[0026] The reaction product of these epoxidation reactions is washed with water or heated under reduced pressure to remove epihalohydrin and solvent. Furthermore, in order to obtain an epoxy resin with a smaller amount of hydrolyzable halogen, the recovered epoxy resin can be dissolved in a ketone compound having 4 to 7 carbon atoms (e.g., methyl isobutyl ketone, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc.) as a solvent, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is added to carry out the reaction to ensure ring closure. In this case, the amount of the alkali metal hydroxide used is usually 0.01 to 0.3 mol, preferably 0.05 to 0.2 mol, per mol of hydroxyl group in the raw material phenol mixture used in the epoxidation. The reaction temperature is usually 50 to 120°C, and the reaction time is usually 0.5 to 2 hours.
[0027] After the reaction is completed, the salt formed is removed by filtration, washing with water, or the like, and the solvent is then distilled off under heating and reduced pressure to obtain the epoxy resin of the present embodiment.
[0028] The epoxy resin obtained by the reaction of the phenol resin represented by the above formula (1) with epihalohydrin is represented by the following formula (2).
[0029] [ka]
[0030] X in formula (2) is a monovalent substituent obtained by removing one hydrogen atom from the benzene ring of formula (2a) or a divalent linking group obtained by removing two hydrogen atoms from the benzene ring of formula (2a), or a monovalent substituent obtained by removing one hydrogen atom from the benzene ring of formula (2b) or a divalent linking group obtained by removing two hydrogen atoms from the benzene ring of formula (2b).
[0031] The values and preferred ranges of R1, m, and n in formulas (2a) and (2b) are the same as those in formula (1). Each of the multiple R2s independently represents a hydrogen atom or a methyl group, and when it is a hydrogen atom, it is a particularly preferred embodiment because the melt viscosity is low.
[0032] In the formula (2), the molar ratio of (2a) to (2b) is not particularly limited, but in terms of the balance of heat resistance, softening point, and melt viscosity, it is preferable that (2a):(2b)=5:1 to 2:1, and more preferably 5:1 to 3:1. The molar ratio of (2a) to (2b) can be analyzed by NMR. Specifically, it can be analyzed by the method described in the examples below.
[0033] The epoxy resin represented by the formula (2) can be represented, for example, as shown in the following formula (3).
[0034] [ka]
[0035] The values and preferred ranges of R1, R2, m, and n in formula (3) are the same as those in formula (2) above.
[0036] The epoxy equivalent of the epoxy resin of the present embodiment is preferably 160 g / eq. or more and 320 g / eq. or less, and more preferably 260 g / eq. or more and less than 280 g / eq. When the epoxy equivalent is 200 g / eq. or more, the heat resistance is good.
[0037] The epoxy resin of the present embodiment preferably has a resinous form having a softening point, and the softening point is preferably from 40° C. to 100° C., and more preferably from 80° C. to 100° C. A softening point of 40° C. or higher means that the molecular weight distribution is appropriate or that there is no residual solvent, etc., and the heat resistance is good, and problems such as poor curing and voids during molding can be suppressed, while a softening point of 100° C. or lower provides good handling when kneaded with other resins.
[0038] The melt viscosity (150°C) of the epoxy resin of this embodiment is preferably 0.01 to 1.0 Pa·s. If the viscosity is higher than 1.0 Pa·s, problems will arise with fluidity, causing problems with flow and embeddability during pressing. If the viscosity is less than 0.01 Pa·s, the molecular weight will be too small and heat resistance will be insufficient. In the prepreg molding method for carbon fiber reinforced composite materials, low tackiness is desired, so the melt viscosity (150°C) is preferably 0.5 to 1.0 Pa·s.
[0039] In the synthesis method of the phenolic resin represented by the formula (1) above, when furfural is reacted (condensed) with a phenol, the amount of the phenol is preferably in the range of 1.5 to 20 moles, particularly preferably 3 to 10 moles, per mole of furfural.
[0040] Examples of the phenols include catechols, resorcinols, and hydroquinones as disubstituted phenols, and phenol as monosubstituted phenols. These may be used alone or in combination of two or more kinds.
[0041] Examples of the solvent include, but are not limited to, methanol, ethanol, propanol, isopropanol, toluene, xylene, etc., and these may be used alone or in combination of two or more. When a solvent is used, the amount of the solvent used is usually 5 to 500 parts by weight, preferably 10 to 300 parts by weight, based on 100 parts by weight of phenol.
[0042] In the above condensation reaction, it is preferable to use a base catalyst. Although condensation polymerization is possible with an acid catalyst, the reaction between furfurals also occurs, resulting in a large amount of by-products. In addition, there is a method using an organometallic compound, but it is disadvantageous in terms of cost. Specific examples of the base catalyst include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide, alkali metal alkoxides such as sodium methoxide, sodium ethoxide, potassium methoxide, potassium ethoxide, and potassium-tert-butoxide, and alkaline earth metal alkoxides such as magnesium methoxide and magnesium ethoxide, but are not limited to these, and the catalyst may be used alone or in combination of two or more kinds. The amount of the catalyst used is usually 0.005 to 2.0 times the moles, preferably 0.01 to 1.1 times the moles, relative to 1 mole of phenol.
[0043] The condensation reaction in the presence of these base catalysts is preferably carried out in the range of 40 to 180° C., particularly preferably in the range of 80 to 165° C., and the reaction time can usually be selected in the range of 0.5 to 10 hours. The reaction product thus obtained is neutralized so that the system becomes neutral, or repeatedly washed with water in the presence of a solvent, and then the water is separated and drained, and the solvent and unreacted materials are removed under heating and reduced pressure to obtain the phenolic resin represented by the formula (I).
[0044] The phenolic resin represented by the formula (1) can be used as a raw material for a curable resin composition in combination with an epoxy resin and a curing accelerator. It can also be used as an olefin resin by reacting it with a cyanate resin raw material, a benzoxazine raw material, chloromethylstyrene, etc., and reacting it with vinylbenzyl ether, allyl halide, methallyl halide, etc.
[0045] The curable resin composition of the present embodiment contains the epoxy resin of the present embodiment and a curing agent. The curable resin composition of the present embodiment preferably has a heat resistance (Tg) of 200 to 300°C. If the heat resistance is less than 200°C, it is difficult to apply the composition to components that require heat resistance, such as those around an aircraft engine, and the resin softens during use, significantly reducing mechanical strength, which is undesirable as it can lead to damage to the material. In addition, the heat resistance of an epoxy resin is generally correlated with the crosslink density, and the higher the crosslink density, the higher the heat resistance. In other words, if the heat resistance exceeds 300°C, the crosslink density increases, which is undesirable as the mechanical strength of the cured product becomes brittle.
[0046] Examples of the curing agent that can be used in the curable resin composition of the present embodiment include amine-based curing agents, acid anhydride-based curing agents, amide-based curing agents, and phenol-based curing agents.
[0047] In the curable resin composition of the present embodiment, an amine curing agent is preferred, since it can achieve a good balance between the resin viscosity of the curable resin composition and the heat resistance of the cured resin. Amine-based hardeners include 3,3'-diaminodiphenyl sulfone (3,3'-DDS), 4,4'-diaminodiphenyl sulfone (4,4'-DDS), diaminodiphenylmethane (DDM), 3,3'-diisopropyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenylmethane, 3,3'-diisopropyl-5,5'-diethyl-4,4' -diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetraisopropyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-diisopropyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetra-t-butyl-4,4'-diaminodiphenylmethane, diaminodiphenyl ether (DADPE), bisaniline, benzyldimethylaniline, 2-(dimethylaminomethyl)phenol (DMP-10), 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), 2-ethylhexanoic acid ester of 2,4,6-tris(dimethylaminomethyl)phenol, and the like can be used. Further examples include aniline novolak, orthoethylaniline novolak, aniline resins obtained by reacting aniline with xylylene chloride, and aniline resins obtained by polycondensation of aniline with substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.).
[0048] Examples of the acid anhydride curing agent include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.
[0049] Examples of the amide-based curing agent include dicyandiamide, or a polyamide resin synthesized from a dimer of linoleic acid and ethylenediamine.
[0050] Phenol-based hardeners include polyhydric phenols (bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, terpene diphenol, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 3,3',5,5'-tetramethyl-(1,1'-biphenyl)-4,4'-diol, hydroquinone, resorcin, naphthalene diol, tris-(4-hydroxyphenyl)methane, and 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, etc.); phenols (e.g., phenol, alkyl-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, and dihydroxynaphthalene, etc.); and aldehydes (formaldehyde, acetaldehyde, benzaldehyde, p-hydroxybenzaldehyde, o-hydroxyphenyl, phenylmethylsulfonyl ... phenolic resins obtained by condensation of the above-mentioned phenols with substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.); modified products of the above-mentioned phenols and / or the above-mentioned phenolic resins; and halogenated phenols such as tetrabromobisphenol A and brominated phenolic resins.
[0051] In the curable resin composition of this embodiment, it is one of the preferred embodiments to use the phenol resin represented by the formula (1) as the entire amount of the curing agent or as a part thereof.
[0052] In the curable resin composition of the present embodiment, the amount of the curing agent used is preferably 0.7 to 1.2 equivalents relative to 1 equivalent of the epoxy group of the epoxy resin. When the amount is less than 0.7 equivalents relative to 1 equivalent of the epoxy group or exceeds 1.2 equivalents, curing may be incomplete and good cured physical properties may not be obtained.
[0053] In addition, in the curable resin composition of the present embodiment, a curing accelerator may be blended as necessary. The gelation time can also be adjusted by using a curing accelerator. Examples of the curing accelerator that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5,4,0]undecene-7, phosphines such as triphenylphosphine, and metal compounds such as tin octylate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin as necessary.
[0054] In the curable resin composition of the present embodiment, other epoxy resins may be blended. Specific examples thereof include phenols (phenol, alkyl-substituted phenol, aromatic substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, etc.). , glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), polymers of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.), polymers of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzo phenolic resins obtained by polycondensation of phenols and substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.), polycondensates of bisphenols and various aldehydes, glycidyl ether epoxy resins obtained by glycidylating alcohols, alicyclic epoxy resins such as 4-vinyl-1-cyclohexene diepoxide and 3,4-epoxycyclohexylmethyl-3,4'-epoxycyclohexanecarboxylate, glycidyl amine epoxy resins such as tetraglycidyldiaminodiphenylmethane (TGDDM) and triglycidyl-p-aminophenol, and glycidyl ester epoxy resins, but are not limited to these, so long as they are commonly used epoxy resins.
[0055] The curable resin composition of the present embodiment may contain a known maleimide compound as necessary. Specific examples of the maleimide compound that can be used include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenylether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, biphenylaralkyl type maleimide, etc., but are not limited thereto. These may be used alone or in combination of two or more. When the maleimide compound is blended, a curing accelerator is blended if necessary. The above-mentioned curing accelerators, as well as radical polymerization initiators such as organic peroxides and azo compounds can be used.
[0056] The curable resin composition of the present embodiment can also adjust the gelation time by using a curing accelerator. Examples of curing accelerators that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5,4,0]undecene-7, phosphines such as triphenylphosphine, and metal compounds such as tin octylate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin, as necessary.
[0057] The curable resin composition of the present embodiment may further contain various additives as exemplified below, as necessary. However, the curable resin composition of the present embodiment is not limited to the additives below, and may contain various additives well known in the art, as necessary.
[0058] The curable resin composition of the present embodiment may further contain a flame retardant as necessary for the purpose of imparting flame retardancy. The flame retardant is not particularly limited, and examples thereof include phosphorus compounds such as red phosphorus, phosphoric acid esters, and triphenylphosphine oxide coated with a thermosetting resin such as a phenolic resin; nitrogen-containing compounds such as melamine, melamine derivatives, melamine-modified phenolic resins, compounds having a triazine ring, cyanuric acid derivatives, and isocyanuric acid derivatives; phosphorus and nitrogen-containing compounds such as cyclophosphazene; metal complex compounds such as dicyclopentadienyl iron; zinc compounds such as zinc oxide, zinc stannate, zinc borate, and zinc molybdate; metal oxides such as iron oxide and molybdenum oxide; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; and composite metal hydroxides represented by the following composition formula (A). Examples of the flame retardant include known organic or inorganic compounds and metal hydroxides containing halogen atoms, antimony atoms, nitrogen atoms, or phosphorus atoms.
[0059] The curable resin composition of the present embodiment may further contain an inorganic filler as necessary. Specific examples of the inorganic filler include fine powders of fused silica, crystalline silica, glass, alumina, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, mica, etc., or beads obtained by sphering these.
[0060] Inorganic fillers having a flame retardant effect may be used, such as aluminum hydroxide, magnesium hydroxide, composite metal hydroxides such as a composite hydroxide of magnesium and zinc, and zinc borate.
[0061] When the curable resin composition contains an inorganic filler, its content is not particularly limited as long as the effect of this embodiment can be obtained. The content of the inorganic filler is preferably 50% by weight or more in the total weight of the curable resin composition, more preferably 60% by weight to 95% by weight from the viewpoint of flame retardancy, and even more preferably 70% by weight to 90% by weight. By containing an inorganic filler, the thermal expansion coefficient, thermal conductivity, elastic modulus, etc. of the cured product can be improved to desired properties. When the content of the inorganic filler is 50% by weight or more, the effect of improving these properties can be obtained more effectively. Also, when it is 95% by weight or less, the viscosity increase of the curable resin composition is more suppressed, sufficient fluidity is easily obtained, and moldability is further improved.
[0062] The curable resin composition of the present embodiment may further contain an antioxidant as necessary. This can prevent oxidation of the cured product of the curable resin composition, and can suppress weight loss of the cured product even when left in a high-temperature environment. Electrical properties are further improved.
[0063] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, sulfur-based antioxidants, hindered amine-based antioxidants, etc. These antioxidants may be used alone or in combination of two or more.
[0064] When the curable resin composition contains an antioxidant, the content is not particularly limited as long as the weight loss suppression effect is achieved. From the viewpoint of the heat resistance (high Tg) of the curable resin composition, the content of the antioxidant is preferably 0.5 parts by weight to 20 parts by weight, more preferably 1 part by weight to 10 parts by weight, based on 100 parts by weight of the total amount of the epoxy resin. By making the content of the antioxidant 0.5 parts by weight or more, the effect of suppressing the weight loss of the cured product can be sufficiently obtained, and by making the content of the antioxidant 20 parts by weight or less, the heat resistance (high Tg) of the cured product is suppressed from decreasing.
[0065] The curable resin composition of the present embodiment may further contain a coupling agent as necessary. This improves the adhesion between the resin component and the inorganic filler, and improves the electrical properties. The coupling agent may be appropriately selected from compounds that are commonly used. Examples of the coupling agent include known coupling agents such as various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, styrylsilane, methacrylsilane, acrylicsilane, and sulfidosilane, titanium-based compounds, aluminum chelate compounds, and aluminum / zirconium-based compounds. Among these, silane-based compounds are preferred. These coupling agents may be used alone or in combination of two or more.
[0066] When the curable resin composition contains a coupling agent, the content is preferably 0.05 to 5.0 parts by weight, and more preferably 0.1 to 4.5 parts by weight, based on 100 parts by weight of the total amount of the inorganic filler. By making the content 0.05 parts by weight or more, the adhesion to the frame, etc. can be further improved.
[0067] The method for preparing the curable resin composition of the present embodiment is not particularly limited, but each component may be mixed uniformly or may be prepolymerized. For example, a mixture containing the compound of the present embodiment is heated in the presence or absence of a curing accelerator or a polymerization initiator, and in the presence or absence of a solvent to form a prepolymer. Similarly, an amine compound, a compound having an ethylenically unsaturated bond, a maleimide compound, a cyanate ester compound, polybutadiene and its modified products, polystyrene and its modified products, inorganic fillers, and other additives may be added to form a prepolymer. The mixing or prepolymerization of each component is carried out using, for example, an extruder, a kneader, a roll, or the like in the absence of a solvent, and a reaction kettle with a stirrer in the presence of a solvent.
[0068] The curable resin composition of the present embodiment is obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but for example, the composition can be obtained by thoroughly mixing the epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, an additive, etc., using an extruder, a kneader, a roll, a planetary mixer, etc., until the mixture is uniform.
[0069] The obtained curable resin composition can be formed into various forms such as a resin sheet, a prepreg, etc. The prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or the resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.
[0070] The curable resin composition of the present embodiment may be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone as necessary to form a varnish-like composition (hereinafter, simply referred to as varnish), which may be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. The solvent used in this case is in an amount that occupies 10 to 70% by weight, preferably 15 to 70% by weight, of the mixture of the curable resin composition of the present embodiment and the solvent.
[0071] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heated and cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated when laminating the prepreg.
[0072] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods. For example, a resin transfer molding technique (RTM method) can be used in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to prepare a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is hardened, and then the mold is opened to remove the molded product. In addition, a type of RTM method, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process) method, and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-T 2005-527410, can be used, which more appropriately controls the resin injection process, especially the VaRTM method, by evacuating a resin supply tank to a pressure lower than atmospheric pressure, using cyclic compression, and controlling the net molding pressure. In addition, other methods that can be used include the film stacking method, in which the fiber substrate is sandwiched between resin sheets (films), the method of attaching powdered resin to the reinforcing fiber substrate to improve impregnation, the molding method (Powder Impregnated Yarn) that uses a fluidized bed or fluid slurry method in the process of mixing the resin into the fiber substrate, and the method of blending resin fibers into the fiber substrate.
[0073] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among them, acrylic carbon fibers having high tensile strength are preferably used. As the form of carbon fibers, twisted yarn, untwisted yarn, non-twisted yarn, etc. can be used, but untwisted yarn or non-twisted yarn is preferably used because it has a good balance between the formability and strength properties of the fiber-reinforced composite material.
[0074] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP. Examples of the applications include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, printed wiring boards (BGA substrates, build-up substrates, etc.), and electric / electronic parts, 3D printing, as well as additives for other resins, etc.
[0075] The adhesives include adhesives for civil engineering, construction, automobiles, general office use, medical use, and adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer boards such as build-up boards, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to various uses.
[0076] When the curable resin composition of this embodiment is applied to a semiconductor element encapsulant, the curable resin composition of this embodiment is placed on a lead frame equipped with a semiconductor element, a semiconductor package substrate, and molded by a melt casting method, a transfer molding method, an injection molding method, a compression molding method, or the like, and further heated at 80 to 200° C. for 2 to 10 hours to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like of ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.
[0077] When the curable resin composition of the present embodiment is applied to a printed wiring board application, a prepreg can be obtained by heating and melting the composition to reduce the viscosity and impregnating the composition into reinforcing fibers such as glass fibers and polyamide fibers. Specific examples of the composition include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, and / or organic fibers, but are not particularly limited thereto. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. In addition, as the weaving method of the woven fabric, plain weave, sash weave, twill weave, and the like are known, and these known weaves can be appropriately selected and used according to the intended application and performance. In addition, woven fabrics that have been subjected to fiber opening treatment or glass woven fabrics that have been surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. Moreover, the varnish can be impregnated into reinforcing fibers and dried by heating to obtain a prepreg, which can be used to prepare a copper clad laminate (CCL). The obtained prepreg and CCL can be hot-press molded to prepare a laminate using the curable resin composition of the present embodiment. The laminate is not particularly limited as long as it has one or more prepregs, and may have any other layers. Moreover, a sheet-shaped adhesive can be obtained by applying the varnish onto a release film, removing the solvent under heating, and performing B-stage formation. This sheet-shaped adhesive can be used as an interlayer insulating layer in a multilayer board or an adhesive sheet when mounting a semiconductor. The curable resin composition of the present embodiment can also be suitably used for special board materials such as package boards (substrates) and HDI (high density interconnect). EXAMPLES
[0078] The present invention will be described in more detail below with reference to synthesis examples and examples. The materials, processing contents, processing procedures, etc. shown below can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Various analytical methods used in the examples are described below.
[0079] Various analytical methods were carried out under the following conditions. Epoxy equivalent It is measured according to the method described in JIS K-7236, and the unit is g / eq. ·Softening point The measurement was performed according to JIS K-7234 and the unit is °C. Melt Viscosity ICI melt viscosity (125°C) measured by the cone-plate method, the unit is Pa·s.
[0080] ·GPC (gel permeation chromatography) measurement Manufacturer:Waters Column: Guard column SHODEX GPC KF-601, KF-602 KF-602.5, KF-603 Flow rate: 0.5ml / min. Column temperature: 40℃ Solvent used: THF (tetrahydrofuran) Detector: RI (Differential Refraction Detector)
[0081] ·NMR measurement Equipment: AVANCE NEO 600MHz (Bruker) Measurement method: 13C (CDCl3) Accumulation count: 10000
[0082] [Example 1] In a flask equipped with a stirrer, a reflux condenser, and a stirrer, 55 parts by weight of 4-t-butylcatechol, 151 parts by weight of toluene, and 11 parts by weight of 30% aqueous sodium hydroxide solution were charged, stirred and dissolved, and then heated to 110°C, where 16 parts by weight of furfural was dropped over 1 hour. The mixture was then reacted at 110°C for 3 hours. When the temperature was raised, the water that had distilled out was removed from the system. After reaching 110°C, the mixture was cooled to 60°C, 30 parts by weight of water was charged, and 0.4 parts by weight of phosphoric acid and 7 parts by weight of 35% hydrochloric acid were added to neutralize the mixture. After repeated washing with water, unreacted phenol was distilled off under reduced pressure with heating to obtain 66 parts by weight of a phenolic resin represented by the following formula (1) (R1 is a t-butyl group, m is 1, and n is 1.2). The results of GPC are shown in Figure 1.
[0083] [ka]
[0084] [Example 2] 62 parts by weight of the phenolic resin obtained in Example 1 were charged into a reaction vessel with 230 parts by weight of epichlorohydrin (ECH, hereinafter the same), 3 parts by weight of tetramethylammonium chloride (TMAC, hereinafter the same), and 4 parts by weight of water, and the mixture was heated, stirred, dissolved, and then reacted for 8 hours while maintaining the temperature at 50°C. Then, 24 parts by weight of flake-shaped sodium hydroxide was charged in portions over 90 minutes, and the mixture was reacted for 90 minutes while maintaining the temperature at 50°C. Then, the mixture was repeatedly washed with water to remove by-product salts and TMAC, and the excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure, and 188 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 50°C, and 7 parts by weight of a 30% aqueous sodium hydroxide solution was added, and the mixture was reacted for 1 hour, after which the reaction solution was repeatedly washed with water until the washing liquid became neutral. Next, methyl isobutyl ketone was distilled off from the oil layer under reduced pressure with heating to obtain 51 parts by weight of an epoxy resin represented by the following formula (2) (R1 is a t-butyl group, R2 is a hydrogen atom, m is 1, and n is 1.6. The molar ratio of (2a) to (2b) is (2a):(2b)=4.3:1). The properties of the obtained epoxy resin are shown in Table 1. The results of GPC are shown in Figure 2, and the results of NMR are shown in Figure 3. The lower part of Figure 3 is an enlarged view of the vicinity of 30 to 60 ppm. The molar ratio of (2a) to (2b) was calculated from the area ratio of 50.24-50.44 ppm and 50.63-50.66 ppm in Figure 3.
[0085] [ka]
[0086] [Comparative Example 1] An epoxy resin having a representative structure represented by the following formula (A) was synthesized according to Production Example 1 of JP 2007-211254 A. The properties of the obtained epoxy resin are shown in Table 1. The results of GPC of the epoxy resin are shown in FIG.
[0087] [ka]
[0088] [Table 1]
[0089] [Example 3, Comparative Example 2] The epoxy resins obtained in Example 2 and Comparative Example 1 were used as the base resin, and 3,3', The components were mixed using 5,5'-tetraethyl-4,4'-diaminodiphenylmethane (abbreviation: TEDDM, manufactured by Tokyo Chemical Industry Co., Ltd., active hydrogen equivalent: 78 g / eq.) in the weight ratio shown in Table 2, and cured at 180°C for 6 hours to produce a cured product.
[0090] The physical properties were measured under the following conditions. <Heat resistance (Tg) measurement conditions> Dynamic viscoelasticity measuring instrument: TA-instruments, DMA-2980 Measurement temperature range: -30~280℃ Heating rate: 2℃ / min Tg: The peak point of Tan δ was taken as Tg. <5% weight loss temperature measurement conditions> Equipment: TG-DTA6220 (SII) Sample: 200 mesh on 5-10mg Heating rate: 10℃ / min Gas purge: Air 200ml / min
[0091] [Table 2]
[0092] The results in Table 2 confirm that the cured products of the examples of the present invention have excellent heat resistance.
Claims
1. An epoxy resin obtained by reacting a phenolic resin represented by the following formula (1) with epihalohydrin. [Formula 1] (In formula (1), there are multiple R 1 Each independently represents a C1-4 alkyl group. Each of the multiple m's is independently an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.)
2. An epoxy resin represented by the following formula (2): [chemical 2] (X in formula (2) is a monovalent substituent obtained by removing one hydrogen atom from the benzene ring of formula (2a) or a divalent linking group obtained by removing two hydrogen atoms from the benzene ring of formula (2b), or a monovalent substituent obtained by removing one hydrogen atom from the benzene ring of formula (2b) or a divalent linking group obtained by removing two hydrogen atoms from the benzene ring of formula (2b), and in formulas (2a) and (2b), 1 Each independently represents a C1-4 alkyl group. 2 Each independently represents a hydrogen atom or a methyl group. Each of the multiple m's is independently an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.)
3. The epoxy resin according to claim 2, wherein in the formula (2), the molar ratio of (2a) to (2b) is (2a):(2b)=5:1 to 2:
1.
4. The curable resin composition according to claim 3, comprising the epoxy resin according to any one of claims 1 to 3 and a curing agent.
5. A cured product obtained by subjecting the curable resin composition according to claim 4 to a curing reaction.
6. A carbon fiber reinforced composite material obtained by curing the curable resin composition according to claim 4.
7. A phenolic resin represented by the following formula (1): [C3] (In formula (1), there are multiple R 1 Each independently represents a C1-4 alkyl group. Each of the multiple m's is independently an integer of 0 to 2. n is the average number of repetitions and is a real number of 1 to 3.)
Citation Information
Patent Citations
Manufacture of flame retardant polymer resin
JP1982167311A
Resin sealed semiconductor device
JP1985097649A
Thermosetting resin composition and its cured product
JP2000319345A
Epoxy resin composition and method for producing epoxy resin
JP2007211254A
Method of preparing epoxy resin
JP2008019449A
Cited By
Epoxy resin mixture, curable resin composition and cured product thereof
JP7814623B2
Epoxy resins, curable resin compositions, and cured products thereof, as well as carbon fiber reinforced composite materials
JP7894530B2
Epoxy resin mixture, curable resin composition and cured product thereof
JPWO2025169747A1
Epoxy resin, curable resin composition, cured products thereof, and carbon fiber-reinforced composite material
JPWO2025169748A1
Epoxy resin mixture, curable resin composition and cured product thereof
WO2025169747A1