Epoxy resin, curable resin composition, and cured product
The epoxy resin with a controlled molecular structure addresses the brittleness and water absorption issues of thermosetting resins, providing CFRP materials with higher elastic modulus and improved mechanical properties.
Patent Information
- Application Number
- JP2023055548
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Thermosetting resins used in CFRP materials are brittle with low bending strength and toughness, and there is a need for higher elastic modulus and lower water absorption to enhance material performance and prevent dimensional changes due to moisture absorption.
An epoxy resin represented by a specific formula with controlled molecular structure and properties, combined with a curing agent, to form a curable resin composition that improves mechanical properties and reduces water absorption.
The epoxy resin achieves high elastic modulus and low water absorption, resulting in improved CFRP materials with enhanced mechanical strength and resistance to moisture-induced dimensional changes.
Smart Images

Figure 2024143064000013 
Figure 2024143064000014 
Figure 2024143064000015
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin, a curable resin composition, and a cured product. [Background technology]
[0002] By curing epoxy resins with various curing agents, they become cured products with excellent mechanical properties, water resistance, chemical resistance, heat resistance, and electrical properties, and are used in a wide range of fields such as adhesives, paints, laminates, molding materials, and casting materials. Carbon fiber reinforced composite materials (CFRP), which are made by impregnating and curing reinforcement fibers with epoxy resin and a curing agent as a matrix resin, can be given properties such as light weight and high strength, and in recent years they have been widely used in aircraft structural members, wind turbine blades, automobile exterior panels, and computer applications such as IC trays and laptop computer housings, and demand for them is increasing. In particular, they are used as matrix resins for aircraft applications, taking advantage of the light weight and high strength properties of the molded products.
[0003] CFRP materials are required to have high mechanical strength, but thermosetting resins such as epoxy resins used in the matrix resin of CFRP are generally brittle and have low bending strength, toughness, adhesiveness, etc. Therefore, a method of adding a highly tough thermoplastic resin to a thermosetting resin to compensate for the characteristics has been widely adopted (Patent Documents 1 to 3). Specifically, the bending strength and toughness of prepregs are improved by combining particles of thermoplastic resins such as polyethersulfone, polyetherimide, and polyamide with a thermosetting resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 60-243113 [Patent Document 2] Patent No. 09-100358 [Patent Document 3] JP 2013-155330 A [Patent Document 4] JP 2007-211254 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a strong demand for thermosetting resins with a higher elastic modulus in order to obtain CFRP materials with even higher performance. This is because when a high-elasticity thermosetting resin fills and bonds the spaces between the carbon fibers, stress is transmitted to adjacent CF filaments through the thermosetting resin, allowing many CF filaments to contribute to the expression of material strength, thereby achieving high strength as a composite material. In addition, there is a demand for thermosetting resins with even lower water absorption to prevent dimensional changes and deterioration of mechanical strength due to moisture absorption.
[0006] Patent Document 4 describes a low water-absorbent epoxy resin. However, the epoxy resin described in Patent Document 4 does not have performance that satisfies the characteristics required by the recent market.
[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide an epoxy resin having a high elastic modulus and excellent low water absorption, and a curable resin composition containing the epoxy resin. [Means for solving the problem]
[0008] That is, the present invention is as shown in the following [1] to [5]. Note that in this application, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] An epoxy resin represented by the following formula (1).
[0009] [ka]
[0010] (In formula (1), a plurality of R1 independently represent a hydrocarbon group having 1 to 10 carbon atoms. R2 represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. n is the average value of the repeating number and is a real number satisfying 1 < n < 15.) [2] The epoxy resin according to the preceding item [1], wherein R1 in the formula (1) is a methyl group. [3] A curable resin composition comprising the epoxy resin according to the preceding item [1] or [2] and a curing agent. [4] The curable resin composition according to the preceding item [3], which is for carbon fiber reinforced plastics. [5] A cured product obtained by curing the curable resin composition according to the preceding item [3] or [4]. [Effect of the Invention]
[0011] According to the present invention, it is possible to provide an epoxy resin having a high elastic modulus and excellent low water absorption, and a curable resin composition containing the epoxy resin. [Brief Description of the Drawings]
[0012] [Figure 1] It is a high performance liquid chromatography chart of the epoxy resin of Synthesis Example 2. [Diagram 2] It is a GPC chart of the epoxy resin of Synthesis Example 2. [Diagram 3] It is a high performance liquid chromatography chart of the epoxy resin of Comparative Synthesis Example 2. [Figure 4] It is a high performance liquid chromatography chart of the epoxy resin of Comparative Synthesis Example 4. [Embodiments for Carrying Out the Invention]
[0013] The epoxy resin of the present embodiment is represented by the following formula (1).
[0014] [Chemical Formula]
[0015] In formula (1), a plurality of R1s independently represent a hydrocarbon group having 1 to 10 carbon atoms, preferably a hydrocarbon group having 1 to 3 carbon atoms, and more preferably a methyl group. R2 represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, preferably a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms, and more preferably a hydrogen atom. n is the average value of the number of repetitions, and is preferably a real number of 1 < n < 15, more preferably 1 < n < 10, and particularly preferably 1 < n < 5.
[0016] Examples of the hydrocarbon group having 1 to 10 carbon atoms represented by R1 and R2 in formula (1) include an alkyl group, an allyl group, a phenyl group, and an alkoxy group. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group. Examples of the alkoxy group include a methoxy group or an ethoxy group.
[0017] In the above formula (1), the value of n can be calculated from the number average molecular weight determined by measuring the gel permeation chromatography (GPC, detector: RI) of the epoxy resin, or from the area ratio of each separated peak.
[0018] In this embodiment, the gel permeation chromatography analysis is measured under the following conditions. ·GPC (Gel Permeation Chromatography) analysis Manufacturer: Waters Columns: Guard column SHODEX GPC KF-601, KF-602 KF-602.5, KF-603 Flow rate: 0.5 ml / min. Column temperature: 40 °C Solvent used: THF (tetrahydrofuran) Detector: RI (differential refractive index detector)
[0019] The epoxy equivalent of the epoxy resin of this embodiment is preferably 240 g / eq. or more and 260 g / eq. or less, and more preferably 245 g / eq. or more and less than 255 g / eq. When the epoxy equivalent is 240 g / eq. or more, the heat resistance is good, and when it is 260 g / eq. or less, the strength is high.
[0020] The epoxy resin of the present embodiment is preferably in the form of a resin having a softening point, and the softening point is preferably 40° C. or more and 80° C. or less, and more preferably 60° C. or more and 70° C. or less. A softening point of 40° C. or more means that the molecular weight distribution is appropriate or that there is no residual solvent, etc., and problems such as poor curing and voids during molding can be suppressed. Conversely, a softening point of 80° C. or less provides good handling when kneading with other resins.
[0021] The ICI melt viscosity (150°C) is preferably 0.01 to 0.15 Pa·s, and more preferably 0.01 to 0.10 Pa·s. Viscosities higher than 0.15 Pa·s are undesirable because they cause problems with fluidity, flowability during pressing, and embeddability.
[0022] The epoxy resin represented by the above formula (1) can be obtained by reacting a phenol resin represented by the following formula (2) with epihalohydrin.
[0023] [ka]
[0024] The values and preferred ranges of R1, R2, and n in the formula (2) are the same as those in the formula (1).
[0025] The epihalohydrin is readily available on the market. The amount of epihalohydrin used is usually 2.0 to 10 mol, preferably 3.0 to 8.0 mol, and more preferably 3.5 to 6.0 mol, per mol of hydroxyl groups in the raw material phenol mixture.
[0026] In the above reaction, an alkali metal hydroxide can be used as a catalyst for promoting the epoxidation step. Examples of alkali metal hydroxides that can be used include sodium hydroxide, potassium hydroxide, etc., and a solid or an aqueous solution thereof can be used. In this embodiment, however, it is particularly preferable to use a solid formed into a flake shape from the standpoint of solubility and handling. The amount of the alkali metal hydroxide used is usually 0.90 to 1.5 mol, preferably 0.95 to 1.25 mol, and more preferably 0.99 to 1.15 mol, per mol of hydroxyl groups in the raw material phenol mixture.
[0027] In order to promote the reaction, a quaternary ammonium salt such as tetramethylammonium chloride, tetramethylammonium bromide, trimethylbenzylammonium chloride, etc. may be added as a catalyst. The amount of the quaternary ammonium salt used is usually 0.1 to 15 g, preferably 0.2 to 10 g, per mole of hydroxyl groups in the raw material phenol mixture.
[0028] The reaction temperature is usually 30 to 90° C., preferably 35 to 80° C. In particular, in this embodiment, for higher purity epoxidation, a temperature of 50° C. or higher is preferred, and particularly 60° C. or higher is preferred. The reaction time is usually 0.5 to 10 hours, preferably 1 to 8 hours, and particularly preferably 1 to 3 hours. If the reaction time is too short, the reaction will not proceed to completion, and if the reaction time is too long, by-products will be produced, which is undesirable. The reaction product of these epoxidation reactions is washed with water or heated under reduced pressure to remove epihalohydrin and solvent. Furthermore, in order to obtain an epoxy resin with a smaller amount of hydrolyzable halogen, the recovered epoxy resin can be dissolved in a ketone compound having 4 to 7 carbon atoms (e.g., methyl isobutyl ketone, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc.) as a solvent, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is added to carry out the reaction to ensure ring closure. In this case, the amount of the alkali metal hydroxide used is usually 0.01 to 0.3 mol, preferably 0.05 to 0.2 mol, per mol of hydroxyl group in the raw material phenol mixture used in the epoxidation. The reaction temperature is usually 50 to 120°C, and the reaction time is usually 0.5 to 2 hours.
[0029] After the reaction is completed, the salt formed is removed by filtration, washing with water, or the like, and the solvent is then distilled off under heating and reduced pressure to obtain the epoxy resin of the present embodiment.
[0030] The phenol resin represented by the formula (2) can be obtained, for example, by a condensation reaction between furfural and a phenol. In this case, the phenol is preferably used in an amount of 1.5 to 20 moles, particularly preferably 3 to 10 moles, per mole of furfural.
[0031] Specific examples of phenols that can be used include cresol, xylenol, trimethylphenol, octylphenol, phenylphenol, diphenylphenol, guaiacol, hydroquinone, resorcin, catechol, and allylphenol, each of which is preferably used alone or in combination.
[0032] Examples of the solvent include, but are not limited to, methanol, ethanol, propanol, isopropanol, toluene, xylene, etc., and these may be used alone or in combination of two or more. When a solvent is used, the amount of the solvent used is usually 5 to 500 parts by weight, preferably 10 to 300 parts by weight, based on 100 parts by weight of phenol.
[0033] In the above condensation reaction, it is preferable to use a base catalyst. Although condensation polymerization is possible with an acid catalyst, the reaction between furfurals also occurs, resulting in a large amount of by-products. In addition, there is a method using an organometallic compound, but it is disadvantageous in terms of cost. Specific examples of the base catalyst include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide, alkali metal alkoxides such as sodium methoxide, sodium ethoxide, potassium methoxide, potassium ethoxide, and potassium-tert-butoxide, and alkaline earth metal alkoxides such as magnesium methoxide and magnesium ethoxide, but are not limited to these, and the catalyst may be used alone or in combination of two or more kinds. The amount of the catalyst used is usually 0.005 to 2.0 times the moles, preferably 0.01 to 1.1 times the moles, relative to 1 mole of phenol.
[0034] The condensation reaction in the presence of these base catalysts is preferably carried out in the range of 40 to 180° C., particularly preferably in the range of 80 to 165° C., and the reaction time can usually be selected in the range of 0.5 to 10 hours. The reaction product thus obtained is neutralized so that the system becomes neutral, or repeatedly washed with water in the presence of a solvent, and then the water is separated and drained, and the solvent and unreacted materials are removed under heating and reduced pressure to obtain the phenolic resin represented by the formula (2).
[0035] The phenolic resin represented by the formula (2) can be combined with a commonly available epoxy resin or curing accelerator to produce a curable resin composition. It can also be used as an olefin resin by reacting it with a cyanate resin raw material, a benzoxazine raw material, chloromethylstyrene, etc., and reacting it with vinylbenzyl ether, allyl halide, methallyl halide, etc.
[0036] The epoxy resin of the present embodiment can be mixed with a curing agent to form a curable resin composition. Examples of the curing agent that can be used include amine-based curing agents, acid anhydride-based curing agents, amide-based curing agents, and phenol-based curing agents.
[0037] In the curable resin composition of the present embodiment, an amine curing agent is preferred, since it can achieve a good balance between the resin viscosity of the curable resin composition and the heat resistance of the cured resin. Amine-based hardeners include 3,3'-diaminodiphenyl sulfone (3,3'-DDS), 4,4'-diaminodiphenyl sulfone (4,4'-DDS), diaminodiphenylmethane (DDM), 3,3'-diisopropyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diisopropyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-dimethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetraethyl-4,4'-diaminodiphenylmethane, 3,3'-diisopropyl-5,5'-diethyl-4,4' -diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetraisopropyl-4,4'-diaminodiphenylmethane, 3,3'-di-t-butyl-5,5'-diisopropyl-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetra-t-butyl-4,4'-diaminodiphenylmethane, diaminodiphenyl ether (DADPE), bisaniline, benzyldimethylaniline, 2-(dimethylaminomethyl)phenol (DMP-10), 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), 2-ethylhexanoic acid ester of 2,4,6-tris(dimethylaminomethyl)phenol, and the like can be used. Further examples include aniline novolak, orthoethylaniline novolak, aniline resins obtained by reacting aniline with xylylene chloride, and aniline resins obtained by polycondensation of aniline with substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.).
[0038] Examples of the acid anhydride curing agent include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.
[0039] Examples of the amide-based curing agent include dicyandiamide, or a polyamide resin synthesized from a dimer of linoleic acid and ethylenediamine.
[0040] Phenol-based hardeners include polyhydric phenols (bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, terpene diphenol, 4,4'-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, 3,3',5,5'-tetramethyl-(1,1'-biphenyl)-4,4'-diol, hydroquinone, resorcin, naphthalene diol, tris-(4-hydroxyphenyl)methane, and 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, etc.); phenols (e.g., phenol, alkyl-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, and dihydroxynaphthalene, etc.); and aldehydes (formaldehyde, acetaldehyde, benzaldehyde, p-hydroxybenzaldehyde, o-hydroxyphenyl, phenylmethylsulfonyl ... phenolic resins obtained by condensation of the above-mentioned phenols with substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.); modified products of the above-mentioned phenols and / or the above-mentioned phenolic resins; and halogenated phenols such as tetrabromobisphenol A and brominated phenolic resins.
[0041] In the curable resin composition of the present embodiment, it is preferable to use the phenol resin represented by the formula (2) as the entire amount of the curing agent or as a part thereof.
[0042] In the curable resin composition of the present embodiment, the amount of the curing agent used is preferably 0.7 to 1.2 equivalents relative to 1 equivalent of the epoxy group of the epoxy resin. When the amount is less than 0.7 equivalents relative to 1 equivalent of the epoxy group or exceeds 1.2 equivalents, curing may be incomplete and good cured physical properties may not be obtained.
[0043] In addition, in the curable resin composition of the present embodiment, a curing accelerator may be blended as necessary. The gelation time can also be adjusted by using a curing accelerator. Examples of the curing accelerator that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5,4,0]undecene-7, phosphines such as triphenylphosphine, and metal compounds such as tin octylate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin as necessary.
[0044] In the curable resin composition of the present embodiment, other epoxy resins may be blended. Specific examples thereof include phenols (phenol, alkyl-substituted phenol, aromatic substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) and various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, etc.). , glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), polymers of phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.), polymers of phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzo phenolic resins obtained by polycondensation of phenols and substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) or substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.), polycondensates of bisphenols and various aldehydes, glycidyl ether epoxy resins obtained by glycidylating alcohols, alicyclic epoxy resins such as 4-vinyl-1-cyclohexene diepoxide and 3,4-epoxycyclohexylmethyl-3,4'-epoxycyclohexanecarboxylate, glycidyl amine epoxy resins such as tetraglycidyldiaminodiphenylmethane (TGDDM) and triglycidyl-p-aminophenol, and glycidyl ester epoxy resins, but are not limited to these, so long as they are commonly used epoxy resins.
[0045] The curable resin composition of the present embodiment can be mixed with known additives as necessary.Specific examples of additives that can be used include polybutadiene and its modified products, modified products of acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, maleimide-based compounds, cyanate ester-based compounds, silicone gel, silicone oil, and inorganic fillers such as silica, alumina, calcium carbonate, quartz powder, aluminum powder, graphite, talc, clay, iron oxide, titanium oxide, aluminum nitride, asbestos, mica, and glass powder, surface treatment agents for fillers such as silane coupling agents, release agents, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.
[0046] The curable resin composition of the present embodiment may contain a known maleimide compound as necessary. Specific examples of the maleimide compound that can be used include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenylether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, biphenylaralkyl type maleimide, etc., but are not limited thereto. These may be used alone or in combination of two or more. When the maleimide compound is blended, a curing accelerator is blended if necessary. The above-mentioned curing accelerators, as well as radical polymerization initiators such as organic peroxides and azo compounds can be used.
[0047] The curable resin composition of the present embodiment is obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but for example, the composition can be obtained by thoroughly mixing the epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, an additive, etc., using an extruder, a kneader, a roll, a planetary mixer, etc., until the mixture is uniform.
[0048] The obtained curable resin composition can be formed into various forms such as a resin sheet, a prepreg, etc. The prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or the resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.
[0049] The curable resin composition of the present embodiment may be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone as necessary to form a varnish-like composition (hereinafter, simply referred to as varnish), which may be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. The solvent used in this case is in an amount that occupies 10 to 70% by weight, preferably 15 to 70% by weight, of the mixture of the curable resin composition of the present embodiment and the solvent.
[0050] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heated and cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated when laminating the prepreg.
[0051] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods. For example, a resin transfer molding technique (RTM method) can be used in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to prepare a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is hardened, and then the mold is opened to remove the molded product. In addition, a type of RTM method, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process) method, and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-T 2005-527410, can be used, which more appropriately controls the resin injection process, especially the VaRTM method, by evacuating a resin supply tank to a pressure lower than atmospheric pressure, using cyclic compression, and controlling the net molding pressure. In addition, other methods that can be used include the film stacking method, in which the fiber substrate is sandwiched between resin sheets (films), the method of attaching powdered resin to the reinforcing fiber substrate to improve impregnation, the molding method (Powder Impregnated Yarn) that uses a fluidized bed or fluid slurry method in the process of mixing the resin into the fiber substrate, and the method of blending resin fibers into the fiber substrate.
[0052] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among them, acrylic carbon fibers having high tensile strength are preferably used. As the form of carbon fibers, twisted yarn, untwisted yarn, non-twisted yarn, etc. can be used, but untwisted yarn or non-twisted yarn is preferably used because it has a good balance between the formability and strength properties of the fiber-reinforced composite material.
[0053] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP. Examples of the applications include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, printed wiring boards (BGA substrates, build-up substrates, etc.), and electric / electronic parts, 3D printing, as well as additives for other resins, etc.
[0054] The adhesives include adhesives for civil engineering, construction, automobiles, general office use, medical use, and adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer boards such as build-up boards, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to various uses.
[0055] The cured product of the curable resin composition of the present embodiment preferably has a flexural modulus of 2.5 GPa to 5.0 GPa, more preferably 3.0 GPa or more and 4.0 GPa or more. If the flexural modulus is less than 2.5 GPa, the rigidity of the carbon fiber composite material is insufficient, which leads to a decrease in reliability, and is not preferred. Also, if the flexural modulus is more than 5.0 GPa, the material becomes brittle, which is not preferred.
[0056] When the curable resin composition of this embodiment is applied to a semiconductor element encapsulant, the curable resin composition of this embodiment is placed on a lead frame equipped with a semiconductor element, a semiconductor package substrate, and molded by a melt casting method, a transfer molding method, an injection molding method, a compression molding method, or the like, and further heated at 80 to 200° C. for 2 to 10 hours to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like of ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.
[0057] When the curable resin composition of the present embodiment is applied to a printed wiring board application, a prepreg can be obtained by heating and melting the composition to reduce the viscosity and impregnating the composition into reinforcing fibers such as glass fibers and polyamide fibers. Specific examples of the composition include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, and / or organic fibers, but are not particularly limited thereto. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. In addition, as the weaving method of the woven fabric, plain weave, sash weave, twill weave, and the like are known, and these known weaves can be appropriately selected and used according to the intended application and performance. In addition, woven fabrics that have been subjected to fiber opening treatment or glass woven fabrics that have been surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. Moreover, the varnish can be impregnated into reinforcing fibers and dried by heating to obtain a prepreg, which can be used to prepare a copper clad laminate (CCL). The obtained prepreg and CCL can be hot-press molded to prepare a laminate using the curable resin composition of the present embodiment. The laminate is not particularly limited as long as it has one or more prepregs, and may have any other layers. Moreover, a sheet-shaped adhesive can be obtained by applying the varnish onto a release film, removing the solvent under heating, and performing B-stage formation. This sheet-shaped adhesive can be used as an interlayer insulating layer in a multilayer board or an adhesive sheet when mounting a semiconductor. The curable resin composition of the present embodiment can also be suitably used for special board materials such as package boards (substrates) and HDI (high density interconnect).
[0058] The water absorption is preferably 2.0% or less, more preferably 1.5% or less, and particularly preferably 1.2% or less. If the water absorption exceeds 2.0%, the cured product absorbs moisture, causing the material to significantly soften and reduce mechanical strength, which is undesirable. EXAMPLES
[0059] The present invention will be described in more detail below with reference to synthesis examples and examples. The materials, processing contents, processing procedures, etc. shown below can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Various analytical methods used in the examples are described below.
[0060] Various analytical methods were carried out under the following conditions. Epoxy equivalent It is measured according to the method described in JIS K-7236, and the unit is g / eq. ·Softening point The measurement was performed according to JIS K-7234 and the unit is °C. Melt Viscosity ICI melt viscosity (150°C) measured by the cone-plate method, the unit is Pa·s.
[0061] ·GPC (gel permeation chromatography) analysis Manufacturer:Waters Column: Guard column SHODEX GPC KF-601, KF-602 KF-602.5, KF-603 Flow rate: 0.5ml / min. Column temperature: 40℃ Solvent used: THF (tetrahydrofuran) Detector: RI (Differential Refraction Detector)
[0062] High performance liquid chromatography (HPLC) measurement Shimadzu Corporation Liquid Delivery Unit LC-20AD Shimadzu Corporation Photodiode array detector SPD-M20A Shimadzu Corporation Column Oven CTO-20A Column: Intersil ODS-2, 5 μm, 4.6 × 250 mm, 40 °C MobilPhaseA: Acetonitrile (AN) MobilPhaseB: Water (W) Time Program: (Synthesis Example 2) 0-10min.AN / W=60% / 40% → 100% / 0% 10-20min.AN / W=100% / 0% (Comparative Synthesis Examples 2 and 4) 0-28min.AN / W=50% / 50% → 100% / 0% 28-40min.AN / W=100% / 0% Flow Rate: 1.0mL / min. Detection: UV 274nm, PDA
[0063] [Synthesis Example 1] In a flask equipped with a stirrer, a reflux condenser, and a stirrer, 500 parts by weight of para-cresol, 87.5 parts by weight of water, and 37.5 parts by weight of sodium hydroxide were charged, stirred, dissolved, and heated to 110°C, where 100 parts by weight of furfural was dropped over 1 hour. After that, the mixture was reacted at 110°C for 3 hours, and then heated to 145°C. During the temperature increase, the water distilled out was removed from the system. After reaching 145°C, the mixture was cooled to 80°C, 100 parts by weight of water was charged, and 4 parts by weight of phosphoric acid and 79 parts by weight of 35% hydrochloric acid were added to neutralize. After repeated washing with water, unreacted phenol was distilled off under reduced pressure with heating to obtain 219 parts by weight of a phenolic resin represented by the following formula (3A).
[0064] [ka]
[0065] [Synthesis Example 2] 77 parts by weight of the phenolic resin obtained in Synthesis Example 1 were charged into a reaction vessel with 229 parts by weight of epichlorohydrin (ECH, hereinafter the same), 40 parts by weight of dimethyl sulfoxide (DMSO, hereinafter the same), and 13 parts by weight of water, and after heating, stirring, and dissolving, 23 parts by weight of flake-shaped sodium hydroxide was charged in portions over 1.5 hours while maintaining the temperature at 55°C. Thereafter, the reaction was further carried out at 55°C for 1.5 hours and at 70°C for 30 minutes. Next, washing with water was repeated to remove DMSO and by-product salts, and then excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure, and 217 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, and 22 parts by weight of methanol, 22 parts by weight of water, and 5 parts by weight of 30% aqueous sodium hydroxide solution were added, and the reaction was carried out for 1 hour, after which the reaction solution was repeatedly washed with water until the washing liquid became neutral. Next, methyl isobutyl ketone was distilled off from the oil layer under heating and reduced pressure to obtain 68 parts by weight of an epoxy resin represented by the following formula (3B). The epoxy equivalent of the obtained epoxy resin was 251 g / eq, the softening point was 63.9°C, the ICI melt viscosity (150°C) was 0.06 Pa s, and n in the following formula (3B) was 1.9. The HPLC results are shown in Figure 1, and the GPC results in Figure 2.
[0066] [ka]
[0067] [Comparative Synthesis Example 1] In a flask equipped with a stirrer, a reflux condenser, and a stirrer, 254 parts by weight of phenol, 63 parts by weight of water, and 27 parts by weight of sodium hydroxide were charged, stirred, dissolved, and heated to 110°C, where 44 parts by weight of furfural were dropped over 2 hours. After that, the mixture was reacted at 110°C for 3 hours, and then heated to 145°C. During the temperature increase, the water distilled out was removed from the system. After reaching 145°C, the mixture was cooled to 80°C, 63 parts by weight of water was charged, and 4 parts by weight of phosphoric acid and 63 parts by weight of 35% hydrochloric acid were added to neutralize. After repeated washing with water, unreacted phenol was distilled off under reduced pressure with heating to obtain 107 parts by weight of a phenolic resin represented by the following formula (4A).
[0068] [ka]
[0069] [Comparative Synthesis Example 2] 78 parts by weight of the phenolic resin obtained in Comparative Synthesis Example 1 were charged into a reaction vessel with 254 parts by weight of epichlorohydrin (ECH, hereinafter the same), 64 parts by weight of dimethyl sulfoxide (DMSO, hereinafter the same), and 13 parts by weight of water. After heating, stirring, and dissolving, 23 parts by weight of flake-shaped sodium hydroxide were charged in portions over 2 hours while maintaining the temperature at 45°C. Then, the reaction was further carried out at 45°C for 2 hours and at 70°C for 60 minutes. Next, washing with water was repeated to remove by-product salts and dimethyl sulfoxide, and excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure, and 218 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, 7 parts by weight of 30% aqueous sodium hydroxide solution was added, and the reaction was carried out for 1 hour. The reaction solution was then repeatedly washed with water until the washing liquid became neutral. Next, methyl isobutyl ketone was distilled off from the oil layer under reduced pressure with heating to obtain 97 parts by weight of the epoxy resin represented by formula (4). The epoxy equivalent of the obtained epoxy resin was 211 g / eq, the softening point was 44°C, the ICI melt viscosity (150°C) was 0.06 Pa s, and n in the following formula (4B) was 2.1. The HPLC results are shown in Figure 3.
[0070] [ka]
[0071] [Comparative Synthesis Example 3] According to Example 7 of JP 2001-64339 A, 432 parts by weight of orthocresol, 93 parts by weight of water, and 40 parts by weight of sodium hydroxide were charged into a flask equipped with a stirrer, a reflux condenser, and a stirrer, and after stirring and dissolving, the mixture was heated to 110°C, and 78 parts by weight of furfural was added dropwise over 2 hours. After that, the mixture was reacted at 110°C for 3 hours, and then the temperature was raised to 145°C. During the temperature rise, the water distilled out was removed from the system. After reaching 145°C, the mixture was cooled to 80°C, and 92 parts by weight of water was charged, and 6 parts by weight of phosphoric acid and 92 parts by weight of 35% hydrochloric acid were added to neutralize. After repeated washing with water, unreacted phenol was distilled off under reduced pressure with heating to obtain 210 parts by weight of a phenolic resin represented by the following formula (5A).
[0072] [ka]
[0073] [Comparative Synthesis Example 4] 94 parts by weight of the phenolic resin obtained in Comparative Synthesis Example 3 were charged into a reaction vessel with 248 parts by weight of epichlorohydrin (ECH, hereinafter the same), 44 parts by weight of dimethyl sulfoxide (DMSO, hereinafter the same), and 13 parts by weight of water. After heating, stirring, and dissolving, 25 parts by weight of flake-shaped sodium hydroxide were charged in portions over 2 hours while maintaining the temperature at 45°C. Then, the reaction was further carried out at 45°C for 2 hours and at 70°C for 60 minutes. Next, washing with water was repeated to remove by-product salts and dimethyl sulfoxide, and excess epichlorohydrin was distilled from the oil layer under heating and reduced pressure, and 256 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, 5 parts by weight of 30% aqueous sodium hydroxide solution was added, and the reaction was carried out for 1 hour. The reaction solution was then repeatedly washed with water until the washing liquid became neutral. Next, methyl isobutyl ketone was distilled off from the oil layer under heating and reduced pressure to obtain 116 parts by weight of an epoxy resin represented by the following formula (5B). The epoxy equivalent of the obtained epoxy resin was 231 g / eq, the softening point was 50.1°C, the ICI melt viscosity (150°C) was 0.06 Pa s, and n in the following formula (5B) was 1.6. The HPLC results are shown in Figure 4.
[0074] [ka]
[0075] The epoxy resins obtained in Synthesis Example 2 and Comparative Synthesis Examples 2 and 4 were used as the base resin, and 4,4'-methylenebis(2,6-diethylaniline) (abbreviation: M-DEA, manufactured by Tokyo Chemical Industry Co., Ltd., active hydrogen equivalent: 78 g / eq.) was used as the curing agent. These were mixed in the weight ratios shown in the formulation in Table 1, and cured at 160°C for 6 hours to produce cured products.
[0076] The physical properties were measured under the following conditions. <Flexural modulus measurement conditions> Measured according to JIS K-7074. <Water absorption rate> Water absorption rate: Weight increase rate (%) after boiling a disk-shaped test piece with a diameter of 5 cm and a thickness of 4 mm in 100°C water for 24 hours
[0077] [Table 1]
[0078] From the results in Table 1, it was confirmed that Example 1 had a high flexural modulus and was excellent in low water absorbency.
Claims
1. An epoxy resin represented by the following formula (1): [Formula 1] (In formula (1), there are multiple R 1 R independently represents a hydrocarbon group having 1 to 10 carbon atoms. 2 represents a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms. n is the average number of repetitions and is a real number in the range of 1<n<15.)
2. R in the formula (1) 1 2. The epoxy resin according to claim 1, wherein is a methyl group.
3. A curable resin composition comprising the epoxy resin according to claim 1 and a curing agent.
4. The curable resin composition according to claim 3, which is for use in carbon fiber reinforced plastics.
5. A cured product obtained by curing the curable resin composition according to claim 3 or 4.
Citation Information
Patent Citations
Preparation method of epoxy resin material filled with organic cross-linked resin as reinforcer
CN116162329A
Thermosetting resin composition and its cured product
JP2000319345A
Phenolic resin, epoxy resin, thermosetting resin composition, and production of resin
JP2001064339A
Phenolic resin, epoxy resin, epoxy resin composition, and cured product of the same
JP2008195843A
Epoxy resin composition having improved toughness
JP1985243113A