Compound, composition containing that compound, and production methods of them
A novel synthesis method for masked nitrile oxide compounds addresses safety and cost issues, enabling efficient and safe production of compounds for improved crosslinking in thermoplastic elastomers.
Patent Information
- Application Number
- JP2023055559
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for synthesizing masked nitrile oxide compounds face challenges with unstable diisocyanide compounds, high-risk materials, safety issues, and high manufacturing costs, particularly due to the use of ethyl nitroacetate and ion exchange resins.
A compound represented by general formula (1) is synthesized through a method involving the reaction of alkyl nitroacetate with a base and a compound having two or more leaving groups, optimizing handling, safety, and reducing costs by avoiding unstable materials and expensive steps.
The new compound and composition enable safe, cost-effective production of masked nitrile oxide compounds, facilitating improved crosslinking reactions in thermoplastic elastomer compositions with enhanced properties.
Smart Images

Figure 2024143073000001 
Figure 2024143073000002 
Figure 2024143073000003
Abstract
Description
[Technical field]
[0001] The present invention relates to compounds, compositions containing the compounds, and methods for their preparation. [Background technology]
[0002] Compositions in which polypropylene resins are blended with olefin- or styrene-based copolymer rubbers are widely used in the fields of vehicle components, home appliance components, office automation equipment components, medical components, miscellaneous goods, etc. Since their compression set and oil resistance are highly dependent on the crosslink density of the copolymer rubber, which is the dispersed phase, it is necessary to increase the crosslink density in order to improve these properties. In recent years, the use of a nitrile oxide compound having at least one nitrile oxide group in the molecule as a crosslinking agent has been proposed as a method for improving the crosslink density of a resin composition (Patent Document 1).
[0003] The nitrile oxide group is a functional group with the unique property of undergoing addition to multiple bonds without a catalyst. Therefore, it is widely used as a tool for click chemistry to easily introduce functional groups to multiple bonds. On the other hand, it is well known that isolation of nitrile oxide compounds is generally difficult due to their instability. To overcome this problem, compounds in which the nitrile oxide group is conjugated and stabilized by stabilizing groups such as large steric hindrance or aromatic rings are known. However, the introduction of stabilizing groups such as groups with steric hindrance or groups containing aromatic rings for stabilization is a major constraint on synthesis, and the bulky stabilizing groups may weaken the reactivity of the nitrile oxide group. In contrast, there are masked nitrile oxide compounds that generate nitrile oxide groups in a system by an operation such as heating (Non-Patent Document 1). Masked nitrile oxide compounds are stable compounds and do not require a stabilizing group for stabilizing the nitrile oxide group, so they can be easily synthesized. Furthermore, if they can be designed to generate nitrile oxide by heating, they will generate nitrile oxide groups, which are active species, under high temperature conditions during resin kneading, and these will react with the resin, making them suitable for resin modification (crosslinking).
[0004] As an example of the production of a masked nitrile oxide, in Patent Document 2, a masked nitrile oxide is synthesized from a compound having a nitromalonamide skeleton by potassium chloride of ethyl nitroacetate (step I-1), reacting the resulting potassium salt with isocyanide in glyme (step I-2), and then neutralizing with an ion exchange resin (step I-3), as shown in the following reaction formula (I).
[0005] [ka] [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2019 / 107450 [Patent Document 2] U.S. Patent No. 6,355,838 [Non-patent literature]
[0007] [Non-Patent Document 1] Nature Chemical Biology Vol.16,2020,497-506 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the synthesis method of Patent Document 2 has problems in terms of handling because it uses an unstable diisocyanide compound as a raw material. In addition, it is necessary to use ethyl nitroacetate, which has a high risk of explosion, as a raw material and convert it into a more reactive metal salt, which must be further reacted in high-temperature glyme for a long period of time, which also has safety problems. Furthermore, the subsequent neutralization requires treatment with an expensive ion exchange resin, which also has problems in terms of production cost. The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a compound that can be used as a masked nitrile oxide that is excellent in terms of handleability, safety, and production cost, a composition containing the compound, and methods for producing the compound and the composition. [Means for solving the problem]
[0009] As a result of intensive research aimed at achieving the above object, the present inventors have found a compound that can be used as a masked nitrile oxide that is excellent in terms of handling, safety, and production cost, a composition containing the compound, and a production method thereof, and have arrived at the present invention. That is, the present invention has the following aspects.
[0010] [1] A compound represented by the following general formula (1):
[0011] [ka]
[0012] In the general formula (1), multiple R a each independently represents a hydrocarbon group having 1 to 6 carbon atoms which may have a substituent; Y represents an n-valent organic group having 1 to 29 carbon atoms which may have a substituent and which may contain an oxygen atom, a nitrogen atom or a sulfur atom; and n is an integer of 2 to 10. [2] A composition comprising the compound according to [1]. [3] A thermoplastic elastomer composition obtained by dynamically crosslinking the composition described in [2]. Effect of the Invention
[0013] According to the present invention, it is possible to obtain a compound that can be used as a masked nitrile oxide that is excellent in terms of handling, safety, and production cost, a composition containing the compound, and a production method thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The following describes in detail the embodiments of the present invention, but the following description is a representative example of the embodiment of the present invention, and the present invention is not limited to these contents. In the present invention, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0015] The following definitions of terms apply throughout the specification and claims. "Polyethylene" is an ethylene homopolymer or ethylene-α-olefin copolymer having more than 50 mol% ethylene units. Polyethylene may have up to 1 mol% diene compound units. "Polypropylene" is a propylene homopolymer or a propylene-α-olefin copolymer having a proportion of propylene units greater than 50 mol %. Polypropylene may have up to 1 mol % of diene compound units. The phrase "substantially no solvent is added" means that no solvent is added other than the solvent that is inevitably mixed in during the production process. "Substantially free of solvent" means that the composition does not contain any solvent other than that inevitably mixed in during the manufacturing process. "Substantially free of solvent" means that the proportion of the solvent is 1 part by mass or less per 100 parts by mass of the total solid content (non-volatile content). Specific examples of the "solvent" include hydrocarbon solvents such as hexane, heptane, octane, toluene, and xylene, and polar solvents such as acetone, methanol, ethanol, and ethyl acetate. The "weight average molecular weight and number average molecular weight of a polymer" are molecular weights determined by gel permeation chromatography (GPC). The "number of carbon-carbon double bonds per polymer molecule" is calculated using the following formula. Number of carbon-carbon double bonds per polymer molecule [units / units] = Number of carbon-carbon double bonds per gram of polymer [mol / g] / Number average molecular weight of polymer [g / mol] The number of carbon-carbon double bonds per gram of polymer is 1 H-NMR and 13 This value was determined by C-NMR.
[0016] A first aspect of the present invention relates to a compound that can be used as a masked nitrile oxide compound and a method for producing the same. A second aspect of the present invention relates to a composition comprising the compound of the first aspect of the present invention and a method for producing the same. Each aspect of the present invention will be described in turn below.
[0017] <Compound (masked nitrile oxide compound)> The compound of the present invention (hereinafter also referred to as "masked nitrile oxide compound") is a compound that is converted into a compound having a nitrile oxide group (hereinafter also referred to as "masked nitrile oxide") in a system by an operation such as heating, and is a compound represented by the following general formula (1) (hereinafter also referred to as "compound (1)").
[0018] [ka]
[0019] In the general formula (1), multiple R a each independently represents a hydrocarbon group having 1 to 6 carbon atoms which may have a substituent; Y represents a linear or branched n-valent organic group having 1 to 29 carbon atoms which may have a substituent and which may contain an oxygen atom, a nitrogen atom or a sulfur atom; and n is an integer of 2 to 10.
[0020] R ais a hydrocarbon group having 1 to 6 carbon atoms which may have a substituent. Examples of the hydrocarbon group having 1 to 6 carbon atoms include linear, branched, or cyclic hydrocarbon groups having 1 to 6 carbon atoms, such as saturated hydrocarbon groups having 1 to 6 carbon atoms, unsaturated hydrocarbon groups having 3 to 6 carbon atoms, and aromatic hydrocarbon groups having 4 to 6 carbon atoms. Examples of the saturated hydrocarbon group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, and a hexyl group. Examples of the unsaturated hydrocarbon group having 3 to 6 carbon atoms include an allyl group. Examples of the aromatic hydrocarbon group having 4 to 6 carbon atoms include a phenyl group and a furyl group. Examples of the substituent include halogen atoms such as F, Cl, Br and I; alkyl groups having 1 to 10 carbon atoms; alkoxy groups having 1 to 10 carbon atoms; hydroxyl groups; amino groups; cyano groups; and carboxy groups. Among these, from the viewpoints of availability and ease of handling, saturated hydrocarbon groups having 1 to 6 carbon atoms are preferred, saturated hydrocarbon groups having 1 to 3 carbon atoms are more preferred, and a methyl group and an ethyl group are even more preferred.
[0021] Y is an n-valent organic group having 1 to 29 carbon atoms, which may have a substituent and may contain an oxygen atom, a nitrogen atom, or a sulfur atom. The n-valent organic group having 1 to 29 carbon atoms is preferably a divalent to octavalent organic group having 1 to 29 carbon atoms, more preferably a divalent to hexavalent organic group, still more preferably a divalent to trivalent organic group, and particularly preferably a divalent organic group. Examples of the divalent organic group having 1 to 29 carbon atoms include a linear, branched, or cyclic alkylene group having 1 to 29 carbon atoms, a linear, branched, or cyclic alkenylene group having 2 to 29 carbon atoms, and an arylene group having 4 to 29 carbon atoms. Examples of the linear, branched, or cyclic alkylene group having 1 to 29 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, a hexadecylene group, a heptadecylene group, an octadecylene group, a nonadecylene group, and an icosylene group. Examples of the linear, branched, or cyclic alkenylene group having 2 to 29 carbon atoms include an ethenylene group, a propenylene group, a butenylene group, a pentenylene group, a hexenylene group, a heptenylene group, an octenylene group, a nonenylene group, a decenylene group, an undecenylene group, a dodecenylene group, a tridecenylene group, a tetradecenylene group, a pentadecenylene group, a hexadecenylene group, a heptadecenylene group, an octadecenylene group, a nonadecenylene group, and an icosenylene group. Examples of the arylene group having 4 to 29 carbon atoms include a phenylene group, a naphthylene group, a biphenylylene group, and a heteroarylene group in which a carbon atom in an aromatic ring is substituted with an oxygen atom, a nitrogen atom, or a sulfur atom, such as a furylene group, a thienylene group, or a pyridinediyl group. Among these, from the viewpoints of availability and handleability, linear or branched alkylene groups having 1 to 29 carbon atoms and arylene groups having 4 to 29 carbon atoms are preferred, linear or branched alkylene groups having 1 to 20 carbon atoms and arylene groups having 6 to 20 carbon atoms are more preferred, and a methylene group, an ethylene group, a propylene group, a butylene group, a phenylene group, and a naphthylene group are even more preferred.
[0022] n is an integer of 2 to 10, preferably 2 to 8, more preferably 2 to 6, further preferably 2 or 3, and particularly preferably 2.
[0023] <<Method for producing a compound (method for producing a masked nitrile oxide compound)>> The method for producing the compound of the present invention (hereinafter also referred to as "method for producing a masked nitrile oxide compound") is a method for producing the compound (1), which includes reacting alkyl 2-nitroacetate with a base and then reacting it with a compound having two or more leaving groups X (step II-1), as represented by the following reaction formula (II).
[0024] [ka]
[0025] In reaction formula (II), multiple R a each independently represents a hydrocarbon group having 1 to 6 carbon atoms which may have a substituent; Y represents a linear or branched n-valent organic group having 1 to 29 carbon atoms which may have a substituent and which may contain an oxygen atom, a nitrogen atom, or a sulfur atom; each of a plurality of X's is independently a leaving group; and n is the same as n in general formula (1).
[0026] In reaction formula (II), R a As the group, R in the general formula (1) a Examples of the above-mentioned problems are the same as those mentioned above. In reaction formula (II), examples of Y include those similar to those mentioned for Y in general formula (1). In reaction formula (II), X is a leaving group. Examples of X include halogen atoms such as chlorine, bromine, and iodine, and sulfonates such as methanesulfonate (OMs) and p-toluenesulfonate (OTf). In reaction formula (II), n is the same as n in general formula (1).
[0027] In the above step II-1, the amount of the alkyl 2-nitroacetate charged is preferably 2 to 10 moles, more preferably 2 to 5 moles, per mole of the compound having two or more leaving groups X. If the amount of the alkyl 2-nitroacetate charged is equal to or greater than the lower limit, it is difficult to allow the compound having two or more leaving groups X to remain unreacted in the product. If the amount of the alkyl 2-nitroacetate charged is equal to or less than the upper limit, it is difficult to allow the alkyl 2-nitroacetate to remain unreacted in the product. The melting point of the 2-nitroalkyl acetate is preferably 200° C. or lower, more preferably −65 to 100° C., and more preferably −60 to 80° C. When the melting point of the 2-nitroalkyl acetate is equal to or higher than the lower limit, the 2-nitroalkyl acetate is easy to handle at room temperature. When the melting point of the 2-nitroalkyl acetate is equal to or lower than the upper limit, the 2-nitroalkyl acetate becomes liquid during the reaction, and the reaction can be easily carried out without adding a solvent. The melting point of the compound having two or more leaving groups X is preferably 200° C. or less, more preferably 0 to 100° C., and more preferably 5 to 80° C. When the melting point of the diamine is equal to or more than the lower limit, the compound is easy to handle at room temperature. When the melting point of the compound having two or more leaving groups X is equal to or less than the upper limit, the compound becomes liquid during the reaction, and the reaction can be easily carried out without adding a solvent.
[0028] Examples of the base include metal alkoxides such as potassium t-butoxide, potassium t-butoxide, sodium methoxide, and sodium ethoxide; and hydroxides of alkali metals or alkaline earth metals such as potassium hydroxide, sodium hydroxide, and cesium hydroxide. The amount of the base used is preferably 1.0 to 2.0 mol, more preferably 1.0 to 1.5 mol, and even more preferably 1.0 to 1.2 mol, relative to 1 mol of the charged amount of ethyl 2-nitroacetate. A solvent may be used, which may be selected based on the reaction temperature and the solubility of the materials, and examples of the solvent include organic solvents such as tetrahydrofuran. A metal chelating agent may be used. The metal chelating agent may be selected based on the type of metal ion contained in the base used, and examples of the metal chelating agent include 12-crown-4-ether, 15-crown-5-ether, and 18-crown-6-ether.
[0029] The above reaction is preferably carried out by heating. The heating temperature is preferably 80 to 200° C., more preferably 90 to 170° C., and even more preferably 100 to 150° C. If the heating temperature is equal to or higher than the lower limit, the alcohol by-produced as the reaction proceeds can be easily distilled off, making it easier to obtain the target product in high yield without leaving unreacted raw materials. If the heating temperature is equal to or lower than the upper limit, it is easier to prevent the raw materials and products from being decomposed by heat, and it is easier to suppress unnecessary energy supply by applying the minimum amount of heat necessary for the reaction to proceed. The heating time is preferably 1 to 20 hours, more preferably 2 to 10 hours, and even more preferably 3 to 8 hours. When the heating time is equal to or more than the lower limit, the reaction proceeds sufficiently, and the target product is easily obtained in high yield without leaving unreacted raw materials. When the heating time is equal to or less than the upper limit, the raw materials and the product are easily prevented from being decomposed by heat, and unnecessary energy supply is easily suppressed by applying the minimum amount of heat necessary for the reaction to proceed. The heating may be carried out with or without the addition of a solvent, but from the viewpoints of improving ease of handling, increasing productivity, and reducing the environmental load, it is preferable to carry out the heating substantially without adding a solvent.
[0030] After heating, the resulting reaction product may be washed with water, etc. Washing makes it easier to remove water-soluble reaction by-products, etc. After heating, recrystallization may be performed using a good solvent and a poor solvent. Examples of the good solvent include ethyl acetate and diethyl ether, and ethyl acetate is preferred from the viewpoints of ease of handling, safety, and production cost. Examples of the poor solvent include hexane, and hexane is preferred from the viewpoints of ease of handling, safety, environmental load, and production cost. The powder obtained by recrystallization may be dried. Drying may be performed by heating under reduced pressure. The heating temperature during drying is preferably 40 to 100°C, more preferably 50 to 90°C, and even more preferably 60 to 80°C. When the heating temperature during drying is equal to or higher than the lower limit, the solvent remaining in the powder is easily removed. When the heating temperature during drying is equal to or lower than the upper limit, the reaction product is easily prevented from being decomposed by heat. Recrystallization may be performed immediately after heating or after washing.
[0031] The alkyl 2-nitroacetate may be a commercially available product or may be synthesized from commercially available raw materials. Commercially available products include methyl 2-nitroacetate and ethyl 2-nitroacetate. The compound having two or more leaving groups X may be a commercially available product, or may be synthesized from commercially available raw materials. Examples of commercially available products include bis(haloalkyl)benzenes such as 1,4-bis(bromomethyl)benzene and 1,4-bis(iodomethyl)benzene; and dihaloalkanes such as 1,2-dibromobutane, 1,3-dibromopropane, and 1,4-dibromobutane. Examples of compounds synthesized from commercially available raw materials include purchased glycol, glycerol, trimethylolpropane, 1,4-di(hydroxymethyl)benzene, and 1,3,5-tris(hydroxymethyl)benzene, and the like, and the hydroxyl groups of these compounds are mesylated or tosylated to convert them into leaving groups by a known method.
[0032] ≪Composition≫ The composition of the present invention contains the compound (1) according to the first aspect of the present invention. The compound (1) is preferably used as a crosslinking agent (C) for reacting with a polymer (B) having a double bond, which will be described later, by a treatment such as heating to form a crosslinked structure. The compound (1) may be used alone or in combination of two or more kinds.
[0033] The composition of the present invention may further contain at least one selected from the group consisting of a polyolefin (A), a polymer (B) having a double bond, a crosslinking agent (C) containing the compound (1) and optionally containing a compound other than the compound (1), a softener for hydrocarbon-based rubber (D), and other components other than the components (A) to (D) in addition to the compound (1). Among these, the composition of the present invention preferably contains a polymer (B) having a double bond in addition to the compound (1), and more preferably contains a polyolefin (A) and a polymer (B) having a double bond. Each component will be described below.
[0034] [Polyolefin (A)] The polyolefin (A) is a polymer of an aliphatic hydrocarbon compound having a double bond, such as ethylene, propylene, butadiene, isoprene, etc., or a hydrogenated product thereof. Examples of the polyolefin (A) include polypropylene-based resins, polyethylene-based resins, polybutene-based resins, etc. Among these, polypropylene-based resins (hereinafter also referred to as "polypropylene-based resin (A1)") are preferred from the viewpoint of heat resistance.
[0035] The polypropylene resin (A1) is a polyolefin resin having a propylene unit content of 50 mass% or more relative to all monomer units. In the composition of the present invention, the polypropylene resin (A1) contributes to moldability.
[0036] The type of polypropylene resin (A1) is not particularly limited, and any of propylene homopolymers, propylene random copolymers, propylene block copolymers, and the like can be used.
[0037] When the polypropylene-based resin (A1) is a propylene random copolymer, examples of the monomer copolymerized with propylene include ethylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. When the polypropylene-based resin (A1) is a propylene block copolymer, examples include propylene block copolymers obtained by multi-stage polymerization, more specifically, propylene block copolymers obtained by polymerizing polypropylene in the first stage and polymerizing a propylene-ethylene copolymer in the second stage.
[0038] The content of propylene units in the polypropylene resin (A1) is preferably 60% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more. When the content of propylene units is equal to or more than the lower limit, the heat resistance and rigidity tend to be good. On the other hand, the upper limit of the content of propylene units in the polypropylene resin (A1) is not particularly limited, and is usually 100% by mass. The content of propylene units in the polypropylene resin (A1) can be determined by infrared spectroscopy.
[0039] The polypropylene resin (A1) has a melt flow rate (MFR) of usually 0.05 g / 10 min or more at 230° C. and a load of 21.2 N, and from the viewpoint of fluidity, it is preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more. On the other hand, the polypropylene resin (A1) has a MFR of usually 100 g / 10 min or less, and from the viewpoint of moldability, it is preferably 70 g / 10 min or less, more preferably 50 g / 10 min or less, and particularly from the viewpoint of fragility, it is even more preferably 30 g / 10 min or less.
[0040] The polypropylene resin (A1) can be produced by a known polymerization method using a known olefin polymerization catalyst. For example, a multi-stage polymerization method using a Ziegler-Natta catalyst can be used. For this multi-stage polymerization method, a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. can be used, and two or more of these methods can be combined to produce the resin.
[0041] In addition, the polypropylene resin (A1) may be a commercially available product. The commercially available polypropylene resin may be procured from the manufacturers listed below and may be appropriately selected. Available commercial products include Novatec® PP from Japan Polypropylene, Prim Polypro® from Prime Polymer, Sumitomo Noblen® from Sumitomo Chemical, polypropylene block copolymer from SunAllomer, Moplen® from LyondellBasell, ExxonMobil PP from ExxonMobil, Formolene® from Formosa Plastics, Borealis PP from Borealis, SEETEC PP from LG Chemical, ASI POLYPROPYLENE from A. Schulman, INEOS PP from INEOS Olefins & Polymers, Braskem PP from Braskem, Samsung Total from SAMSUNG TOTAL PETROCHEMICALS, Sabic® PP from Sabic, TOTAL PETROCHEMICALS Polypropylene from TOTAL PETROCHEMICALS, and YUPLENE® from SK.
[0042] The polyolefin (A) may be used either alone or in combination of two or more different types having different propylene unit contents, different types of monomer units contained, different physical properties, and the like.
[0043] [Polymer having double bonds (B)] The polymer (B) having a double bond is a polymer having at least one double bond in the molecule. Among the polyolefins (A), those having a double bond are classified as the polymer (B) having a double bond. Here, the double bond includes a carbon-carbon double bond, a carbon-nitrogen double bond, a carbon-oxygen double bond, etc., and among them, a carbon-carbon double bond is preferable. Examples of the polymer (B) having a double bond include polymers having at least one double bond in the molecule, such as polyolefins, urethane resins, acrylic resins, polyester resins, etc. Among these, polyolefins having at least one double bond in the molecule are preferred, and ethylene-α-olefin-non-conjugated diene copolymers (hereinafter also referred to as "ethylene-α-olefin-non-conjugated diene copolymers (B1)") are more preferred from the viewpoints of compatibility with polyolefin (A) and rubber elasticity.
[0044] The content of ethylene units in the ethylene-α-olefin-non-conjugated diene copolymer (B1) is preferably 50% by mass or more, more preferably 55% by mass or more, and on the other hand, preferably 90% by mass or less, more preferably 80% by mass or less, based on the total amount of monomer units constituting the ethylene-α-olefin-non-conjugated diene copolymer (B1). The content of ethylene units in the above range is preferable for imparting appropriate flexibility.
[0045] Examples of the α-olefin units in the ethylene-α-olefin-non-conjugated diene copolymer (B1) include propylene units, 1-butene units, 3-methyl-1-butene units, 1-pentene units, 4-methyl-1-pentene units, 1-hexene units, 4-methyl-1-hexene units, 1-heptene units, 1-octene units, and 1-decene units. Among these, propylene units, 1-butene units, and 1-hexene units are preferred. The ethylene-α-olefin-non-conjugated diene copolymer (B1) may contain only one type of these α-olefin units, or two or more types.
[0046] The content of α-olefin units in the ethylene-α-olefin-non-conjugated diene copolymer (B1) is preferably 10% by mass or more, more preferably 20% by mass or more, and on the other hand, preferably 45% by mass or less, more preferably 35% by mass or less, based on the total amount of monomer units constituting the ethylene-α-olefin-non-conjugated diene copolymer (B1). The content of α-olefin units in the above range is preferable for imparting appropriate flexibility.
[0047] Examples of the non-conjugated diene units in the ethylene-α-olefin-non-conjugated diene copolymer (B1) include dicyclopentadiene units, 1,4-hexadiene units, cyclooctadiene units, methylenenorbornene units, ethylidenenorbornene units, vinylidenenorbornene units, etc. Among these, the inclusion of ethylidenenorbornene units and / or vinylidenenorbornene units is preferred because it can provide the ethylene-α-olefin-non-conjugated diene copolymer (B1) with an appropriate crosslinking structure. The ethylene-α-olefin-non-conjugated diene copolymer (B1) may contain only one type of these non-conjugated diene units or two or more types.
[0048] The content of non-conjugated diene units in the ethylene-α-olefin-non-conjugated diene copolymer (B1) is preferably 1 mass% or more, more preferably 3 mass% or more, and on the other hand, preferably 10 mass% or less, more preferably 8 mass% or less, based on the total amount of monomer units constituting the ethylene-α-olefin-non-conjugated diene copolymer (B1). A content of non-conjugated diene units of not less than the above lower limit is preferred from the viewpoint of increasing the degree of crosslinking of the composition, and a content of not more than the above upper limit is preferred from the viewpoint of moldability.
[0049] The content of each structural unit in the ethylene / α-olefin / non-conjugated diene copolymer (B1) can be determined by infrared spectroscopy.
[0050] The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated diene copolymer (B1) calculated as polypropylene by gel permeation chromatography (GPC) is preferably 300,000 or more, more preferably 350,000 or more, and even more preferably 400,000 or more. The Mw of the ethylene-α-olefin-non-conjugated diene copolymer (B1) is preferably 1,000,000 or less, more preferably 900,000 or less, and even more preferably 800,000 or less. It is preferable from the viewpoint of appearance that the Mw of the ethylene-α-olefin-non-conjugated diene copolymer (B1) is the above upper limit value or less, and it is preferable from the viewpoint of preventing bleed-out that the Mw is the above lower limit value or more.
[0051] The measurement conditions for the GPC method for the ethylene-α-olefin-non-conjugated diene copolymer (B1) are as follows. Equipment :Waters 150C Column: Shodex AD806MS x 3 (8.0 mm inner diameter x 300 mm length) Detector: IR (dispersive, 3.42 μm) Solvent: o-dichlorobenzene Temperature: 140℃ Flow rate: 1.0mL / min Injection volume: 200μL Calibration sample: Polydisperse standard polyethylene Calibration method: Polypropylene conversion using the Mark-Houwink formula
[0052] The polymer (B) having a double bond may be used either alone or in combination of two or more types differing in the monomer units contained therein, their contents, physical properties, and the like.
[0053] [Crosslinker (C)] The compound (1) is used as a crosslinking agent (C) for reacting with a polymer (B) having a double bond by treatment such as heating to form a crosslinked structure. The crosslinking agent (C) contains the compound (1) and may further contain a compound other than the compound (1). Examples of the compound other than the compound (1) include masked nitrile oxide compounds and nitrile oxide compounds other than the compound (1).
[0054] (Masked nitrile oxide compounds other than compound (1)) Examples of the masked nitrile oxide compound other than the compound (1) include the compound represented by the general formula (1) above, a Examples of the compound (1) include a compound having a divalent organic group between the carbon atom at the α-position and the carbon atom at the β-position of the carbonyl group.
[0055] [Hydrocarbon-based rubber softeners (D)] In the composition and its production method of the present invention, it is preferable to use a hydrocarbon-based rubber softener (D) in order to soften the resulting composition and increase its flexibility and elasticity, as well as to improve the processability and flowability of the resulting composition.
[0056] Examples of the hydrocarbon-based rubber softener (D) include mineral oil-based softeners and synthetic resin-based softeners, but mineral oil-based softeners are preferred from the viewpoint of compatibility with other components. Mineral oil-based softeners are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons, and paraffinic hydrocarbons, and those in which 50% or more of the total carbon atoms are paraffinic hydrocarbons are called paraffinic oils, those in which 30 to 45% of the total carbon atoms are naphthenic hydrocarbons are called naphthenic oils, and those in which 35% or more of the total carbon atoms are aromatic hydrocarbons are called aromatic oils. Of these, it is preferable to use paraffin-based oil. The hydrocarbon rubber softener (D) may be used alone or in combination of two or more kinds.
[0057] The kinetic viscosity of the hydrocarbon-based rubber softener (D) at 40° C. is preferably 20 centistokes (cSt) or more, more preferably 50 cSt or more, and is preferably 800 cSt or less, more preferably 600 cSt or less. The kinetic viscosity can be measured by the method of JIS K2283.
[0058] The flash point (COC method) of the hydrocarbon rubber softener (D) is preferably at least 200° C., more preferably at least 250° C. The flash point can be measured by the method of JIS K2265.
[0059] In addition, when a hydrocarbon-based rubber softener (D) is used, the hydrocarbon-based rubber softener (D) and the polymer having a double bond (B) may be pre-mixed and used as an oil-extended rubber before mixing the polyolefin (A) and the polymer having a double bond (B).
[0060] A known method can be used for producing oil-extended rubber (oil extension method). Examples of the oil extension method include a method of mechanically kneading the polymer (B) having a double bond and the softener (D) for hydrocarbon-based rubber using a mixing roll or a Banbury mixer to extend the oil, a method of adding a predetermined amount of the softener (D) for hydrocarbon-based rubber to the polymer (B) having a double bond and then removing the solvent by a method such as steam stripping, and a method of stirring a mixture of the polymer (B) having a double bond and the softener (D) for hydrocarbon-based rubber in the form of crumbs with a Henschel mixer or the like to impregnate the mixture.
[0061] Oil-extended rubber is commercially available, and can be selected from JSR EPR manufactured by JSR Corporation, Mitsui EPT (registered trademark) manufactured by Mitsui Chemicals, Inc., Esprene (registered trademark) manufactured by Sumitomo Chemical Co., Ltd., Keltan (registered trademark) manufactured by LANXESS, KEP (registered trademark) manufactured by KUMHO POLYCHEM, and NODEL (registered trademark) manufactured by DOW.
[0062] [Other ingredients] In addition to the polyolefin (A), the polymer having a double bond (B), the crosslinking agent (C) containing the compound (1), and the hydrocarbon-based rubber softener (D), other components may be used in the composition of the present invention depending on the purpose, as long as the effects of the present invention are not impaired.
[0063] Examples of other components include various additives such as fillers, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, metal deactivators, molecular weight regulators, antibacterial agents, antifungal materials, and fluorescent brightening agents, thermoplastic resins and elastomers other than the polyolefin (A) and the polymer having a double bond (B), and surfactants. These may be used alone or in combination of two or more. The total content of each component relative to the total mass of the composition does not exceed 100 mass%.
[0064] Examples of the filler include glass fiber, hollow glass spheres, carbon fiber, talc, calcium carbonate, mica, potassium titanate fiber, silica, titanium dioxide, carbon black, etc. When a filler is used, it is usually used in an amount of 0.1 to 50 parts by mass per 100 parts by mass of the total of components (A) to (D).
[0065] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, thioether-based antioxidants, etc. When an antioxidant is used, it is usually used in the range of 0.01 to 3.0 parts by mass per 100 parts by mass of the total of the components (A) to (D).
[0066] Examples of thermoplastic resins other than polyolefin (A) and polymer having a double bond (B) include polyphenylene ether-based resins; polyamide-based resins such as nylon 6 and nylon 66; polyester-based resins such as polyethylene terephthalate and polybutylene terephthalate; polyoxymethylene-based resins such as polyoxymethylene homopolymer and polyoxymethylene copolymer; polymethyl methacrylate-based resins, and polyolefin resins (excluding those corresponding to polyolefin (A) and polymer having a double bond (B)). Examples of elastomers other than the elastomer obtained by crosslinking a mixture containing polyolefin (A), polymer (B) having a double bond, and masked nitrile oxide compound include styrene-based elastomers such as styrene-butadiene copolymer rubber and styrene-isoprene copolymer rubber; polyester-based elastomers; and polybutadiene.
[0067] The surfactant may be an anionic surfactant, a nonionic surfactant, or a cationic surfactant.
[0068] The other components may be mixed into the raw material mixture before the dynamic heat treatment described below, or may be mixed into the composition after the dynamic heat treatment.
[0069] [Content of each ingredient] The content of each component in the composition of the present invention will be described below. The content of compound (1) is preferably from 0.1 to 20 mass %, more preferably from 0.1 to 5 mass %, and even more preferably from 0.1 to 2 mass %, of the total amount of the composition. When the composition of the present invention contains polyolefin (A), the content of polyolefin (A) is preferably from 1 to 70 mass %, more preferably from 10 to 50 mass %, and even more preferably from 20 to 40 mass %, of the total amount of the composition. When the composition of the present invention contains the polymer (B) having a double bond, the content of the polymer (B) having a double bond is preferably 10 to 90 mass %, more preferably 30 to 90 mass %, and even more preferably 50 to 90 mass % of the total amount of the composition. The content of the crosslinking agent (C) in the composition of the present invention is preferably from 0.1 to 30 mass %, more preferably from 0.1 to 10 mass %, and even more preferably from 0.1 to 5 mass %, of the total amount of the composition. When the composition of the present invention contains a crosslinking agent other than compound (1) as the crosslinking agent (C), the content of the crosslinking agent other than compound (1) is preferably 0.1 to 20 mass%, more preferably 0.1 to 5 mass%, and even more preferably 0.1 to 2 mass%, of the total amount of the composition. When the composition of the present invention contains a hydrocarbon-based rubber softener (D), the content of the hydrocarbon-based rubber softener (D) is preferably 0.1 to 50 mass %, more preferably 1 to 40 mass %, and even more preferably 10 to 40 mass % of the total amount of the composition. When the composition of the present invention contains components other than the components (A) to (D), the content of the optional components is preferably 0.1 to 50 mass%, more preferably 0.1 to 40 mass%, and even more preferably 0.1 to 20 mass%, of the total amount of the composition. The compositions of the present invention are preferably substantially solvent-free.
[0070] The amount of the compound (1) used is preferably 0.05 parts by mass or more, more preferably 0.2 parts by mass or more, based on 100 parts by mass of the polymer (B) having a double bond, in order to sufficiently advance the crosslinking reaction. On the other hand, from the viewpoint of controlling the crosslinking reaction, it is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less. Specifically, it is preferably 0.05 to 10 parts by mass, more preferably 0.2 to 8 parts by mass, and even more preferably 0.2 to 6 parts by mass.
[0071] When polyolefin (A) and polymer (B) having a double bond are used, the amount of polymer (B) having a double bond is preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 65% by mass or more, from the viewpoint of flexibility, based on the total of polyolefin (A) and polymer (B) having a double bond (100% by mass). Also, from the viewpoint of moldability, it is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. Specifically, it is preferably 55 to 95% by mass, more preferably 60 to 90% by mass, and even more preferably 65 to 85% by mass.
[0072] When polyolefin (A) and polymer (B) having a double bond are used, the mass ratio represented by [amount of polyolefin (A)] / [amount of polymer (B) having a double bond] is preferably 5 / 95 to 45 / 55, and more preferably 10 / 90 to 40 / 60, from the viewpoints of crosslinking characteristics and rubber elasticity.
[0073] When using a hydrocarbon-based rubber softener (D) and a polymer (B) having a double bond, the amount of the hydrocarbon-based rubber softener (D) used is preferably 1 part by mass or more, more preferably 10 parts by mass or more, even more preferably 20 parts by mass or more, and particularly preferably 30 parts by mass or more, based on 100 parts by mass of the polymer (B) having a double bond, from the viewpoint of flexibility. On the other hand, from the viewpoint of production stability, it is preferably 350 parts by mass or less, more preferably 300 parts by mass or less. Specifically, it is preferably 1 to 350 parts by mass, more preferably 10 to 300 parts by mass, and even more preferably 20 to 300 parts by mass.
[0074] When a crosslinking agent (C) other than the compound (1) and a polymer (B) having a double bond are used, the amount of the crosslinking agent (C) other than the compound (1) used is preferably 0.05 parts by mass or more, more preferably 0.2 parts by mass or more, relative to 100 parts by mass of the polymer (B) having a double bond, in order to sufficiently proceed with the crosslinking reaction. On the other hand, from the viewpoint of controlling the crosslinking reaction, it is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less. Specifically, it is preferably 0.05 to 10 parts by mass, more preferably 0.2 to 8 parts by mass, and even more preferably 0.2 to 6 parts by mass.
[0075] In the composition of the present invention, the gel fraction of the polymer (B) having a double bond is preferably 0 to 50%, more preferably 0 to 30%, and even more preferably 0 to 10%. When the gel fraction of the polymer (B) having a double bond is within the above range, the handleability of the composition is easily improved. The gel fraction can be measured by the method described in the Examples.
[0076] <Method for producing composition> The method for producing the composition of the present invention comprises mixing the compound (1) of the first aspect of the present invention with at least one selected from the group consisting of a polyolefin (A), a polymer having a double bond (B), a compound other than the compound (1) as a crosslinking agent (C), a hydrocarbon-based rubber softener (D), and other components, as necessary.
[0077] <Thermoplastic elastomer composition> The thermoplastic elastomer composition of the present invention is obtained by dynamically crosslinking the composition according to the second embodiment of the present invention by subjecting it to a dynamic heat treatment. The crosslinked structure in the thermoplastic elastomer composition is preferably formed by a reaction between the compound (1) and the polymer (B) having a double bond, and forms an islands-in-a-sea structure in which rubber particles having the crosslinked structure are dispersed in a matrix of the polyolefin (A).
[0078] In the thermoplastic elastomer composition of the present invention, the gel fraction of the polymer (B) having double bonds after crosslinking (i.e., the rubber particles) is preferably 10 to 100%, more preferably 20 to 100%, and even more preferably 30 to 100%. When the gel fraction of the polymer (B) having double bonds after crosslinking is equal to or more than the above lower limit, the crosslink density is easily increased, and a molded product having excellent compression set and oil resistance is easily obtained. When the gel fraction of the polymer (B) having double bonds after crosslinking is equal to or less than the above upper limit, the handleability of the thermoplastic elastomer composition is easily improved. The gel fraction can be measured by the method described in the Examples.
[0079] <Method for producing thermoplastic elastomer composition> The thermoplastic elastomer composition of the present invention comprises dynamically crosslinking the composition of the second aspect of the present invention by dynamically heat treating it to obtain a thermoplastic elastomer.
[0080] In the present invention, the term "dynamic heat treatment" means kneading in a molten or semi-molten state. This dynamic heat treatment is preferably performed by melt kneading, and as a mixing and kneading device for this purpose, for example, a non-open type Banbury mixer, a mixing roll, a kneader, or a twin-screw extruder is used. Among these, it is preferable to use a twin-screw extruder. A preferred embodiment of the production method using a twin-screw extruder is to supply each component to a raw material supply port (hopper) of a twin-screw extruder having a plurality of raw material supply ports and perform dynamic heat treatment.
[0081] The temperature for the dynamic heat treatment is usually 160 to 280° C., preferably 165 to 250° C., and more preferably 170 to 220° C. The time for the dynamic heat treatment is usually 0.1 to 30 minutes.
[0082] [Molded products / Applications] The thermoplastic elastomer composition of the present invention can be formed into a molded article by various molding methods usually used for compositions, such as injection molding, extrusion molding, blow molding, and compression molding, and among these, injection molding and extrusion molding are preferred. After these molding processes, the material may be subjected to secondary processing such as lamination molding and thermoforming to form a molded product.
[0083] The thermoplastic elastomer composition and its production method of the present invention can be used in a wide range of fields, including the automotive field (seals, cushions, boots, etc.), the construction field (gaskets, packings, etc.), and various other miscellaneous goods fields, such as sporting goods (grips for golf clubs and tennis rackets, etc.), industrial parts (hose tubes, gaskets, etc.), home appliance parts (hoses, packings, etc.), medical parts (medical containers, gaskets, packings, etc.), food parts (containers, packings, etc.), medical device parts, electric wires, and other miscellaneous goods. EXAMPLES
[0084] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples.
[0085] In the following description, "parts" and "%" indicate "parts by mass" and "% by mass", respectively.
[0086] The raw materials and evaluation methods used in the following examples are as follows. ≪Raw materials≫ Polyolefin (A): Propylene-based polymer (manufactured by Japan Polypropylene Corporation, product name: Novatec MA3Q). Polymer having double bonds (B): ethylene-α-olefin-non-conjugated diene copolymer (manufactured by Dow, product name: NORDEL IP4760P). Antioxidant (1): Hindered phenol-based antioxidant (manufactured by BASF Japan Ltd., product name: Irganox1010). Antioxidant (2): Phosphite-based antioxidant (manufactured by BASF Japan Ltd., product name: Irgafos168). Masked nitrile oxide compound (C1): A masked nitrile oxide compound represented by the following formula (C1).
[0087] [ka]
[0088] [Production Example 1] Production of masked nitrile oxide compound (C1) A masked nitrile oxide compound (C1) was obtained with reference to a known method (International Publication No. 2001 / 07400).
[0089] Compound (C1) 1 H-NMR spectrum: 1 H-NMR (400MHz, CDCl3): δ7.18(d,4H),5.33(m,2H),4.29(m,4H),3.50(m,4H),1.27(m,6H)
[0090] Evaluation method <Gel fraction> The obtained thermoplastic elastomer composition was weighed into a 60-mesh wire net whose mass had been measured in advance, placed in a Soxhlet extractor, and extracted with xylene for 4 hours while adjusting the temperature so that the reflux was 12 minutes per time. After cooling the wire net after extraction, it was dried in a vacuum dryer at 80°C for 4 hours, and the mass of the wire net was measured. The mass percentage of the xylene extraction residue relative to the sample before xylene extraction was converted into the content of the polymer (B) having a double bond, and evaluated as the gel fraction of the polymer (B) having a double bond in the thermoplastic elastomer composition. A larger gel fraction of the polymer (B) having a double bond in the composition means that the crosslinking reaction has progressed to a greater extent.
[0091] [Example 1] 22.5 parts of polypropylene resin (A), 70 parts of ethylene-α-olefin-non-conjugated diene copolymer (B), 0.1 part of antioxidant (1), and 0.1 part of antioxidant (2) were blended and melt-kneaded for 2 minutes at 225°C using a benchtop kneader MC15HT (manufactured by Xplore Instruments). Then, 7.5 parts of polypropylene resin (A) and 1 part of masked nitrile oxide compound (C1) were added, and the mixture was melt-kneaded for 3 minutes at 225°C and dynamically crosslinked to obtain a thermoplastic elastomer composition. The gel fraction was calculated according to the above procedure. The gel fraction was 43%. This shows that the masked nitrile oxide compound of the present invention is excellent in terms of handling, safety, and production cost. In addition, the masked nitrile oxide compound of the present invention is converted into a compound having a nitrile oxide group in the system by heat treatment, and the crosslinking reaction with the polymer (B) having a double bond proceeds, and thus the masked nitrile oxide compound shows excellent crosslinking properties (gel fraction).
Claims
1. A compound represented by the following general formula (1): [Case 1] In the general formula (1), a plurality of R a each independently represents a hydrocarbon group having 1 to 6 carbon atoms which may have a substituent; Y represents an n-valent organic group having 1 to 29 carbon atoms which may have a substituent and which may contain an oxygen atom, a nitrogen atom or a sulfur atom; and n is an integer of 2 to 10.
2. A composition comprising the compound of claim 1.
3. A thermoplastic elastomer composition obtained by dynamically crosslinking the composition according to claim 2.
Citation Information
Patent Citations
Thermoplastic elastomer composition
JP2013203832A
Compound, compound as synthetic precursor of that compound, composition, and production methods of them
JP2024143203A
Carboxylic acid derivatives and adhesion molecule inhibitors containing the same as the active ingredient
WO2001007400A1
Reagents for heat activated polymer crosslinking
WO2002006391A1
Thermoplastic elastomer composition and method for preparing same
WO2020241575A1