Connection electric wire and manufacturing method for connection electric wire

By immersing wire connections in sequential curable resin layers with controlled viscosities and curing, the method addresses inefficiencies in existing sealing technologies, enhancing productivity and adhesion in harsh environments.

JP2024143133APending Publication Date: 2024-10-11FURUKAWA ELECTRIC CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023055647
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for forming sealing layers on wire connections require multiple steps and curing processes, leading to increased manufacturing time, cost, and reduced productivity, with adhesion issues in harsh environments, and vulnerability to water infiltration.

Method used

A method involving immersing the connection portion in a first curable resin liquid, then in a second curable resin liquid while the first is uncured, followed by sequential curing to form a mixed region between the layers, enhancing adhesion and sealing effectiveness.

Benefits of technology

The method reduces manufacturing steps and time, improves productivity, and ensures robust sealing even in harsh conditions, maintaining adhesion under thermal shock and gasoline immersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143133000001_ABST
    Figure 2024143133000001_ABST
Patent Text Reader

Abstract

To provide an electric connecting wire that can reduce the number of manufacturing steps or manufacturing time, has excellent productivity, and is capable of sufficiently sealing (protecting) a connection portion even in a harsh environment, and a manufacturing method thereof.SOLUTION: A manufacturing method for a connecting electric wire in which a connection portion where conductors of multiple insulated electric wires are connected to each other is sealed with an insulating sealing layer, the manufacturing method for the connecting electric wire includes, in this order, the steps of immersing the connection portion in a first curable resin liquid, immersing the connection portion to which the first curable resin liquid is attached in a second curable resin liquid while the first curable resin liquid attached to the connection portion is in an uncured state, and curing the first curable resin liquid and the second curable resin liquid attached to the connection portion.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electric connection wire and a method for manufacturing the electric connection wire. [Background technology]

[0002] In wiring an insulated electric wire, when a branch wire is branched off from a trunk wire, trunk wires are connected in series, or a pine-needle connection is made, the insulating coating layer covering the insulated electric wire is peeled off and the exposed conductor is connected to form a connection. The formed connection is protected by wrapping its outer periphery with insulating tape or by covering it with a connection member such as a splice unit. In particular, when the connection is required to be waterproof, the connection is sealed with an insulating resin or the like to form a sealing layer. In forming the sealing layer, a method has been proposed in which two types of resin liquids (resin materials, resin compositions) with different viscosities are used to fill the gaps between the insulated wires or conductors with resin without leaving any gaps. Specifically, a method is known in which the connection part is immersed in a resin liquid with a lower viscosity, the resin liquid is allowed to penetrate into the small gaps between the insulated wires or conductors with the low-viscosity resin liquid, the resin liquid is hardened, and then the connection part is immersed in a resin liquid with a higher viscosity, and the resin liquid is hardened to form the sealing layer.

[0003] For example, Patent Document 1 proposes a technique for bundling a plurality of electric wires from which the covering has been removed to expose a plurality of core wires, and welding the plurality of core wires to form a welded portion for waterproofing between the plurality of core wires. This waterproofing method involves waterproofing the welded portion with a first sealant having a viscosity of 1 Pa·sec or less, and then waterproofing the welded portion with a second sealant having a viscosity of 10 to 70 Pa·sec. In this method, after the surface of the silicone rubber constituting the first sealant has hardened, the welded portion is immersed in the silicone rubber constituting the second sealant.

[0004] Patent Document 2 discloses a manufacturing method for a wire harness having a splice portion in which conductors are connected to each other and a sealing layer that seals the splice portion, the manufacturing method including a connecting step of connecting the conductors to each other to form the splice portion, a first resin material application step of immersing the splice portion in a first resin material having a first viscosity in an uncured state and then removing the first resin material, a first curing step of curing the first resin material applied to the splice portion, a second resin material application step of immersing the splice portion in a second resin material having a second viscosity in an uncured state and then removing the second resin material, and a second curing step of curing the second resin material applied to the splice portion, wherein the first viscosity is in the range of 10 to 50 mPa s and the second viscosity is set to be higher than the first viscosity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-9334 A [Patent Document 2] JP 2022-167488 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the methods described in Patent Documents 1 and 2, the connection part is immersed in a low-viscosity resin liquid, and then the low-viscosity resin liquid is cured before being immersed in a high-viscosity resin liquid. If the resin liquid is a moisture-curable resin liquid or silicone rubber, the resin liquid must be left to stand at least until the surface of the resin liquid is cured, which causes problems in securing storage space and stagnation of work, and thus increases manufacturing costs. In addition, if the resin liquid is an ultraviolet-curable resin liquid, a new ultraviolet irradiation process must be added to cure the low-viscosity resin liquid, which increases the number of processes, resulting in increased manufacturing costs and longer production times, resulting in reduced productivity. Furthermore, when resin liquids having different viscosities or different curing reactions are used as described above to sequentially form sealing layers by individually curing each resin liquid, there are limitations to improving the adhesion between the inner resin and the outer resin. In particular, in harsh environments such as thermal shock or immersion in gasoline, the inner resin and the outer resin are prone to peeling at their interface, and there is a problem that water, etc. can penetrate into the sealing layer from the peeled surface.

[0007] In view of the above problems, the present invention aims to provide a connecting wire that can reduce the number of manufacturing steps or manufacturing time, has excellent productivity, and can adequately seal (protect) the connection portion even in harsh environments, and a manufacturing method thereof. [Means for solving the problem]

[0008] As a result of intensive research by the present inventors to solve the above problems, in manufacturing a connecting wire having a sealing layer formed on a connecting portion, the connecting portion is immersed in a first curable resin liquid, and while the first curable resin liquid attached to the connecting portion is in an uncured state, the connecting portion to which the first curable resin liquid is attached is immersed in a second curable resin liquid, and then the first curable resin liquid and the second curable resin liquid attached to the connecting portion are cured. By curing the first curable resin liquid and the second curable resin liquid, a mixed region of both curable resins is formed between the layer made of the first curable resin formed by curing the first curable resin liquid and the layer made of the second curable resin formed by curing the second curable resin liquid, thereby increasing the adhesion between the two layers, and it has been found that a connecting wire that can seal and protect the connecting portion at a sufficiently high level even in harsh environments can be obtained with excellent productivity. The present invention has been completed through further research based on these findings.

[0009] That is, the above problems were solved by the following means. <1> A method for manufacturing a connecting electric wire in which a connection portion in which conductors of a plurality of insulated electric wires are connected to each other is sealed with an insulating sealing layer, comprising the steps of: Immersing the connection portion in a first curable resin liquid; a step of immersing the connection portion to which the first curable resin liquid is attached in a second curable resin liquid while the first curable resin liquid attached to the connection portion is in an uncured state; and curing the first and second curable resin liquids applied to the connection portion, in this order. <2> The viscosity of the first curable resin liquid is 51 to 1000 mPa·s. <1> A method for producing the connecting wire according to claim 1. <3> The viscosity of the second curable resin liquid is higher than the viscosity of the first curable resin liquid. <1> or <2> A method for producing the connecting wire according to claim 1. <4> The viscosity of the first curable resin liquid is 1 to 9 mPa s, The viscosity of the second curable resin liquid is higher than the viscosity of the first curable resin liquid. <1> A method for producing the connecting wire according to claim 1. <5> The second curable resin liquid contains a photocurable resin. <1> ~ <4> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <6> The first curable resin liquid contains a photocurable resin. <1> ~ <5> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <7> The first curable resin liquid contains a moisture curable resin. <1> ~ <6> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <8> The second curable resin liquid is filled into a protective member before use. <1> ~ <7> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <9> The connecting wire is a wire harness. <1> ~ <8> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <10> A connecting wire in which a connection portion where conductors of a plurality of insulated wires are connected to each other is sealed with an insulating sealing layer, The sealing layer has a layer made of a first cured resin and a layer made of a second cured resin covering the layer made of the first cured resin, and has a mixed region of the first cured resin and the second cured resin between the layer made of the first cured resin and the layer made of the second cured resin. <11> The second curable resin includes a photocurable resin. <10> The connecting wire described in <12> The first curable resin includes a photocurable resin. <10> or <11> The connecting wire described in <13> The first curable resin includes a moisture curable resin. <10> ~ <12> 2. A connecting wire according to any one of claims 1 to 11. <14> The sealing layer is covered with a protective member. <10> ~ <13> 2. A connecting wire according to any one of claims 1 to 11. <15> The connecting wire is a wire harness. <10> ~ <14> 2. A connecting wire according to any one of claims 1 to 11.

[0010] In the present invention, a numerical range expressed using "to" means a range including the numerical values ​​before and after it as the lower limit and upper limit. Effect of the Invention

[0011] According to the method for producing an electric connection wire of the present invention, it is possible to obtain an electric connection wire capable of sealing and protecting a connection portion at a sufficiently high level even in a harsh environment with excellent productivity. The electric connection wire of the present invention is capable of sealing and protecting a connection portion at a sufficiently high level even in a harsh environment, and is also excellent in productivity. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram showing an embodiment of a connecting wire of the present invention. [Diagram 2] 1A to 1C are explanatory diagrams illustrating an embodiment of a method for producing an electric connector according to the present invention. [Diagram 3] FIG. 4 is an explanatory diagram illustrating an example of a method for producing a connector wire, which is not the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Preferred embodiments of the present invention will be described below, but the present invention is not limited to the following embodiments except as defined in the present invention.

[0014] [Connecting wire] The connecting wire of the present invention has conductors of multiple insulated wires connected together at connection parts (splice parts), and the connection parts are sealed with an insulating sealing layer. The sealing layer has a layer made of a first cured resin and a layer made of a second cured resin covering the layer made of the first cured resin, and has a mixed region of the first cured resin and the second cured resin between the layer made of the first cured resin and the layer made of the second cured resin.

[0015] Hereinafter, a preferred embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiments shown below, except as specified in the present invention. In addition, the description of the connecting wires and the like described with reference to the drawings below is not limited to the forms shown in the drawings, but is applied as a description of the configuration or invention-specific matters of the present invention.

[0016] FIG. 1 is a schematic diagram showing one embodiment of the connection wire of the present invention. In the connection wire 1 of the present invention, the covering parts 12 (insulating covering layer) at the ends of a plurality of insulated electric wires 10 are peeled off, and the exposed conductor parts 11 are connected to each other to form a connection part 13. The connection part 13 is sealed by an insulating sealing layer 20. In this specification, the region from the connection part to the conductor part where the connection part is not formed and the covering part is collectively referred to as the "connection part, etc." In addition, in the connection part, etc., all of the conductors in the part where the insulating covering layer is peeled off may form a connection part (it is not necessary to have a conductor part where a connection part is not formed). In the present invention, "the connection part where the conductors of a plurality of insulated electric wires are connected to each other is sealed by an insulating sealing layer" means that the region including the connection part is sealed by an insulating sealing layer. In other words, it means that the above-mentioned connection part, etc. are sealed by an insulating sealing layer. Although FIG. 1 shows a state in which conductors 11 are connected to each other using crimp terminals 14 to form connection portion 13, the method of connecting conductors 11 to each other is not particularly limited in the present invention.

[0017] The components of the electric connecting wire of the present invention will be described in detail below.

[0018] <Insulated wire> The insulated wire used in the electric connecting wire of the present invention is not particularly limited, and for example, an insulated wire normally used for a wire harness for an automobile can be used. The insulated wire has a conductor and an insulating coating layer that covers the outer periphery of the conductor.

[0019] (conductor) The shape and material of the conductor of the insulated wire are not particularly limited as long as it functions as a conductor. For example, the conductor may have a shape and material used in insulated wires used in wire harnesses for automobiles. The conductor may be a single wire or a twisted wire, a bare wire, or a plated or enamel-coated wire. Metal materials forming the conductor include soft copper, copper alloy, aluminum, etc.

[0020] (insulating coating layer) The type of the insulating coating layer of the insulated wire is not particularly limited as long as it has the desired insulating properties. For example, insulating resins used in wire harnesses for automobiles can be used. The insulating coating layer is preferably an extrusion coating layer formed by extrusion coating an insulating thermoplastic resin or a composition containing the resin. The thickness of the insulating coating layer is not particularly limited, and is usually about 0.15 to 5 mm.

[0021] (Connection) In one embodiment of the connecting wire of the present invention, as shown in Figures 1 and 2, the insulating coating layer (coating portion) at the tip of the multiple insulated electric wires is peeled off to expose the conductors, and the conductors are connected to each other to form a connection portion. There are no particular limitations on the method of forming the connection portion, as long as the conductors are electrically connected to each other. For example, arc welding, laser welding, ultrasonic bonding, etc. may be used, or a crimp connection using a crimp terminal such as a P-type sleeve or a B-type sleeve may be used. Although Figures 1 to 3 show a state in which a plurality of insulated electric wires are connected in a pine-needle manner, the method of connecting the plurality of insulated electric wires in the electric connector of the present invention is not particularly limited, and straight connection or branch connection may be used.

[0022] <Sealing layer> The electric connecting wire of the present invention has a sealing layer that seals the connection portion, the sealing layer having a layer made of a first cured resin, a layer made of a second cured resin covering the first cured resin, and a mixed region of the first cured resin and the second cured resin.

[0023] (1st cured resin) The layer made of the first curing resin is a layer formed by sealing (covering) the connection part with an insulating resin. The type of the first curing resin is not particularly limited, and it is preferable to include, for example, a resin such as a photo (ultraviolet) curing resin, a moisture curing resin, an anaerobic curing resin, or a thermosetting resin.

[0024] Examples of the photo (ultraviolet) curable resin include a resin obtained by photocuring a composition having a photoradical polymerization initiator and a compound capable of radical polymerization by the action of the photoradical polymerization initiator (radical polymerizable compound), and a resin obtained by photocuring a composition having a photocationic polymerization initiator and a compound capable of cationic polymerization by the action of the photocationic polymerization initiator (cationic polymerizable compound).

[0025] Moreover, the light (ultraviolet) curable resin is more preferably a cured product of a dark curable resin that cures even in areas not directly exposed to light. Specifically, it is preferable for the dark curable resin to be a resin in which a long-life active compound is generated by light irradiation (ultraviolet irradiation), the active compound diffuses into the curable resin liquid, and acts on a radical polymerization initiator that is not directly exposed to light to generate radicals and cure the curable resin liquid.

[0026] Examples of the thermosetting resin include a resin obtained by thermally curing a composition having a thermal radical polymerization initiator and a radical polymerizable compound, and a resin obtained by thermally curing a composition having a thermal cationic polymerization initiator and a cationic polymerizable compound. The thermosetting resin may also be a cured product of a thermosetting phenolic resin, an epoxy resin, a urethane resin, a urea resin, an alkyd resin, or the like.

[0027] Anaerobic curing resins include resins that are stable in air and cure when exposed to metal ions in the absence of oxygen. The moisture-curing resin may be a resin that is cured by contacting with moisture in the air or the like.

[0028] Specific examples of the first cured resin include cyanoacrylate resin, acrylic resin, epoxy resin, silicone resin, urethane resin, polyamide resin, fluororesin, polyvinyl butyral resin, phenolic resin, polyimide resin, acrylic rubber, polyester resin, modified polyolefin resin, etc., and the cured resin may be composed of one or more of these. The first curing resin preferably contains the light (ultraviolet) curing resin or the moisture curing resin. The light (ultraviolet) curing resin is preferably an acrylic resin. The moisture curing resin is preferably a cyanoacrylate resin or a silicone resin, and more preferably a cyanoacrylate resin.

[0029] (Second cured resin) The layer made of the second cured resin is an insulating cured resin layer that covers the layer made of the first cured resin that seals the connection parts and the like. The resin used for the second curing resin can be the same as the first curing resin, and the preferred form is also the same. Furthermore, it is also preferable to use, for example, a thermosetting resin or a hot melt resin as the second curing resin. From the viewpoint of the thermal effect on the coating insulating layer of the insulated electric wire, it is preferable to use a resin having a softening point in the range of about 50 to 180°C as the hot melt resin, and in addition to polyolefin resins such as polyethylene and polypropylene, ethylene-vinyl acetate copolymers, ethylene-ethyl acrylate copolymers, and acid-modified polyolefins such as maleic acid can be suitably used. In the present invention and this specification, the "hot melt resin" means a resin in a state in which the hot melt resin is solidified by lowering the temperature after being thermally melted.

[0030] The first and second curable resins may be the same or different. For example, when the first curable resin is a light (ultraviolet) curable resin, by making the second curable resin also a light (ultraviolet) curable resin, the first curable resin and the second curable resin can be cured simultaneously by irradiation with light (ultraviolet). In addition, for example, when the first curing resin is a light (ultraviolet) curing resin or a moisture curing resin, for example, a heat-melting resin can be used as the second curing resin. From the viewpoint of adhesion with the first curing resin, the heat-melting resin is preferably a heat-melting resin having a polar group such as modified polyolefin, polyurethane, polyester, polyamide, etc., and from the viewpoint of heat resistance, a heat-melting resin such as modified polypropylene, polyester, polyamide, etc. is more preferable.

[0031] The sealing layer may have an insulating protective member (such as an insulating cap) on its outermost layer, and the sealing layer may be covered with the protective member. When the sealing layer has the protective member, the connection parts and the like can be protected more effectively. The material constituting the protective member is not particularly limited, and materials generally used in forming a sealing layer can be used. Protective members available on the market can also be used. For example, protective materials such as (crosslinked) polyethylene, polypropylene, vinyl chloride, polyethylene terephthalate, and polycarbonate are preferable. When crosslinked polyethylene is used as the protective member, it can be shrunk by heating with a hot dryer or the like. Therefore, the outer diameter of the protective member can be reduced by inserting the conductor part of the connecting wire into the crosslinked polyethylene protective member and then heating and shrinking it, which not only improves the vehicle mountability but also reduces the amount of resin filled in the protective member. In addition, since the inside of the protective member may be filled with a second curable resin liquid and may be used as is to form a sealing layer and then cured, for example, when the second curable resin is a light (ultraviolet) curable resin, it is preferable to use a material with high light transmittance such as polyethylene, polypropylene, etc. In addition, when the second curable resin is a heat-melting resin, it is preferable to use a material with high heat resistance such as cross-linked polyethylene, polyethylene terephthalate, polycarbonate, etc.

[0032] (mixed area) In the electric wire connection of the present invention, the sealing layer has a mixed region in which the first cured resin and the second cured resin are mixed between the layer made of the first cured resin and the layer made of the second cured resin. In the electric wire connection of the present invention, the layer made of the first cured resin and the layer made of the second cured resin forming the sealing layer do not have a clear interface between the layers. In other words, the first cured resin and the second cured resin are each diffused into the layer on the other side in a gradational manner. Since the sealing layer has a mixed region of the first cured resin and the second cured resin, there is no clear interface between the layer made of the first cured resin and the layer made of the second cured resin, and the adhesion between the layer made of the first cured resin and the layer made of the second cured resin is improved. As a result, if the connecting wire of the present invention is used as an automobile wire harness, for example, it can exhibit good durability against thermal shock and immersion in gasoline in a harsh in-vehicle environment.

[0033] <How to analyze mixed areas> The state of the mixed region in the sealing layer can be confirmed by Raman spectroscopy or FT-IR mapping analysis of a thin section of a portion that may form a mixed region (for example, a thin section perpendicular to the longitudinal direction of the insulated wire directly above the connection portion). When a signal derived from the first cured resin is detected on the second cured resin side beyond the range assumed to be the layer made of the first cured resin by such an analysis method, it is determined that the "mixed region is present." The "range assumed to be the layer made of the first cured resin" can be derived, for example, from the viscosity of the first curable resin liquid, and the range of the first cured resin obtained by immersing the connection part or the like in the first curable resin liquid, taking it out, and curing it can also be the "range assumed to be the layer made of the first cured resin." For example, if the range assumed to be the layer made of the first cured resin based on the viscosity of the first cured resin liquid is a range of 20 to 200 μm from the outermost surface of the connection part (the conductor surface or the crimp terminal surface), and a signal derived from the first cured resin (for example, a signal derived from a cyano group when the first cured resin is a cyanoacrylate resin) is detected beyond that range (for example, 5 μm or more beyond that range), it can be determined that there is a mixed region in which the first cured resin and the second cured resin are mixed.

[0034] In addition, when the first curable resin liquid is applied to the connection part by dip coating, in which the connection part is immersed in a container filled with the first curable resin liquid and then pulled up, the thickness of the resin liquid is determined by the viscosity of the liquid and the surface tension at the gas-liquid interface if the pulling speed is sufficiently slow and the viscosity is low. Therefore, the following relational expression is established for the thickness (h, unit: m).

[0035] TIFF2024143133000002.tif20170

[0036] In the above formula (1), the parameters are as follows: U: Pulling speed (m / s) η: Viscosity of the curable resin liquid (Pa s = kg m / s) ρ: Density of the curable resin liquid (kg / m 3 ) γ: Surface tension of curable resin liquid (N / m) g: Gravitational acceleration (m / s 2 )

[0037] Therefore, the thickness of the resin liquid calculated by the above (Formula 1) can also be set as the above "range assumed to be the layer made of the first cured resin".

[0038] The connecting wire of the present invention is preferably used for a wire harness (preferably an automobile wire harness). In the present invention and this specification, the wire harness is a general term for a bundle of electric wires arranged in various places of a vehicle, such as an engine room, an instrument panel, and inside a door, according to environmental performance.

[0039] [Method of manufacturing connection wire] The manufacturing method of the connecting electric wire of the present invention (hereinafter also referred to as the manufacturing method of the present invention) comprises, in this order, a step of immersing the connecting portion in a first curable resin liquid, a step of immersing the connecting portion to which the first curable resin liquid is attached in a second curable resin liquid while the first curable resin liquid attached to the connecting portion is in an uncured state, and a step of curing the first curable resin liquid and the second curable resin liquid attached to the connecting portion. In the manufacturing method of the present invention, the details of the insulated wire and the connection part of the insulated wire used are as described above.

[0040] Fig. 2 shows one embodiment of the manufacturing method of the present invention. Fig. 3 shows one example of a manufacturing method of a connecting electric wire that is not the manufacturing method of the present invention. In the present invention, the number of insulated electric wires to be connected is not particularly limited. Note that Figs. 2 and 3 are based on the assumption that both the first curable resin liquid and the second curable resin liquid are light (ultraviolet) curable resins. FIG. 2(A) shows a process of immersing the connection portion 13 of the insulated electric wire 10 in the first curable resin liquid 21. FIG. 2(B) shows the first curable resin liquid 21 attached to the connection portion 13 after the connection portion 13 is immersed in the first curable resin liquid 21 and then removed from the first curable resin liquid 21 in an uncured state. FIG. 2(C) shows a process of immersing the first curable resin liquid 21 in the second curable resin liquid in an uncured state, in which the first curable resin liquid 21 is immersed in an insulating cap 26 filled with the second curable resin liquid 23. FIG. 2(D) shows a state in which a mixed region 25 of the resin is formed between a layer made of the first curable resin 22 and a layer made of the second curable resin 24 in the sealing layer after the first curable resin liquid and the second curable resin liquid are cured together by UV irradiation. On the other hand, in FIG. 3 showing an example of a manufacturing method of a connecting wire that is not the manufacturing method of the present invention, FIG. 3(A) is the same as FIG. 2(A), but as shown in FIG. 3(B), the first curable resin liquid 21 is cured by UV irradiation before being immersed in the second curable resin liquid 23. Then, as shown in FIG. 3(C), the first curable resin 22 cured by UV irradiation is immersed in an insulating cap 26 filled with the second curable resin liquid 23, and then the second curable resin liquid 23 is cured. Therefore, the first curable resin 22 and the second curable resin 24 do not mix with each other, and a clear interface is formed between the layer made of the first curable resin 22 and the layer made of the second curable resin 24, and a mixed region 25 of these resins is not formed. Each step of the production method of the present invention will be described in detail below.

[0041] <Step of immersing in first curable resin liquid> In the manufacturing method of the present invention, the layer made of the first curing resin in the sealing layer of the resulting connecting electric wire is formed by immersing the connection part, etc., in a first curing resin liquid. The resin contained in the first curing resin liquid may be a curing resin (resin composition) that is cured to form the first curing resin. That is, for example, a photo (ultraviolet) curing resin, a moisture curing resin, an anaerobic curing resin, a thermosetting resin, etc. may be used. The connection parts and the like are preferably immersed in the first curable resin liquid so that the covering part is covered with the first curable resin liquid by 5 mm or more from the boundary with the exposed conductor part.

[0042] The viscosity of the first curable resin liquid is not particularly limited. It can be preferably 51 to 1000 mPa·s, or can be 1 to 9 mPa·s. If the viscosity is 51 to 1000 mPa·s, when the connection part or the like is immersed in the first curable resin liquid and then removed, the first curable resin liquid is retained at the immersed portion, and excessive dripping can be suppressed. Also, if the viscosity is 1 to 9 mPa·s, excess first curable resin liquid attached to the connection part or the like quickly flows off, and excessive dripping can be suppressed.

[0043] In the present invention, the viscosity of the curable resin liquid is the viscosity at the temperature of the resin liquid at the time when the connection part is immersed. The viscosity at the temperature can be measured, for example, by a B-type viscometer (for example, manufactured by Eiko Seiki Co., Ltd., product name: Digital Viscometer DVNext). A B-type viscometer is a type of rotational viscometer in which a rotor called a spindle rotor is immersed in the liquid and rotated by a motor to measure the flow resistance. When using a B-type viscometer, the measurement can be performed by adjusting the rotation speed (0.01 to 250 rpm) so that the torque range (%) is within the range of 10 to 100% using a spindle attached to the digital viscometer DVNext (model number: LV DVNX). In addition, for example, when the curable resin liquid is a commercially available product, the viscosity can be the viscosity described in the pamphlet of the commercially available product. Furthermore, the temperature may be, for example, room temperature in the manufacture of the connecting wire of the present invention, and when a photo-(ultraviolet) curable resin, moisture curable resin, or anaerobic curable resin is used as the curable resin liquid, the viscosity may be the viscosity at 25°C.

[0044] The manufacturing method of the present invention does not include a step of curing the first curable resin liquid after immersing the connection part, etc. in the first curable resin liquid and taking it out, and before immersing it in the second curable resin liquid. Therefore, at the stage of immersing in the second curable resin liquid, the first curable resin liquid is in an uncured state. By immersing the first curable resin liquid in the second curable resin liquid while it is still uncured, a part of the first curable resin liquid diffuses into the second curable resin liquid, and a part of the second curable resin liquid diffuses into the first curable resin liquid (a part of the first curable resin liquid and a part of the second curable resin liquid mix together), and then curing it, a mixed region in which the first curable resin and the second curable resin are mixed can be formed. In addition, since the manufacturing method of the present invention does not include a step of curing the first curable resin liquid before immersion in the second curable resin liquid, it is possible to move to the step of immersing in the second curable resin liquid immediately after immersion in the first curable resin liquid, and problems such as securing storage space and stagnation of work do not occur, and productivity can be significantly improved. In particular, for example, when the first curable resin and the second curable resin are both light (ultraviolet) curable resins, the first curable resin liquid and the second curable resin liquid can be cured at the same time by irradiating ultraviolet rays after immersion in the second curable resin liquid.

[0045] The "state in which the first curable resin liquid is uncured" means, for example, when the first curable resin liquid is a light (ultraviolet) curable resin, the state of the curable resin liquid in a state in which light (ultraviolet) irradiation is not performed. In addition, for example, when the first curable resin liquid is a moisture curable resin, it means a state in which at least the surface curing has not progressed completely. In addition, since the moisture curable resin progresses in a curing reaction by contacting with water in the air, when the first curable resin liquid is a moisture curable resin, the time from immersion in the first curable resin liquid to immersion in the second curable resin liquid can be appropriately set according to the humidity of the working environment, and for example, the time is preferably within 5 minutes, more preferably within 3 minutes, even more preferably within 2 minutes, even more preferably within 1 minute, even more preferably within 30 seconds, even more preferably within 20 seconds, and even more preferably within 10 seconds. If it is within the above preferred range, the first curable resin liquid can be left in an uncured state.

[0046] <Step of immersing in second curable resin liquid> In the manufacturing method of the present invention, the layer made of the second curable resin in the sealing layer of the resulting connecting electric wire is formed by immersing the connection part to which the first curable resin liquid is attached in the second curable resin liquid while the first curable resin liquid is in an uncured state, and then curing it. The resin contained in the second curable resin liquid may be a curable resin (resin composition) that is cured to form the second curable resin. That is, for example, a photo (ultraviolet) curable resin, a moisture curable resin, an anaerobic curable resin, a thermosetting resin, a heat-melting (hot melt) resin, etc. may be used. The immersion in the second curable resin liquid is preferably performed to a position where the first curable resin liquid adhering to the connection parts and the like is completely covered.

[0047] The viscosity of the second curable resin liquid is not particularly limited, and is preferably higher than the viscosity of the first curable resin liquid from the viewpoint of preventing dripping. For example, the viscosity is preferably 200 mPa·s or more higher than the viscosity of the first curable resin liquid, more preferably 400 mPa·s or more higher, and also preferably 600 mPa·s or more higher. The viscosity of the second curable resin liquid is preferably 400 to 10,000 mPa·s, more preferably 500 to 8,000 mPa·s, even more preferably 600 to 7,000 mPa·s, and even more preferably 700 to 6,000 mPa·s.

[0048] The second curable resin liquid may be filled in, for example, an insulating protective member (insulating cap, etc.). This allows the second curable resin liquid to be cured together with the protective member, and the sealing layer can be effectively protected by the protective member. The material of the protective member is not particularly limited, and the above-mentioned protective members can be used, for example.

[0049] <Step of curing the first curable resin liquid and the second curable resin liquid> The method for curing the first and second curable resin liquids can be appropriately set depending on the types of the first and second curable resin liquids. For example, when the first curable resin liquid and the second curable resin liquid are both light (ultraviolet) curable resins, the first curable resin liquid and the second curable resin liquid can be cured at the same time by irradiating light (ultraviolet) rays, so that the time required for manufacturing can be shortened. In addition, when the first curable resin liquid is a moisture curable resin and the second curable resin liquid is a light (ultraviolet) irradiable resin, if the second curable resin liquid is cured by irradiating light (ultraviolet) rays to the second curable resin liquid to stabilize the shape of the sealing layer, the first curable resin inside will naturally harden over time while maintaining the shape of the sealing layer. In addition, when the first curable resin liquid is a moisture curable resin and the second curable resin liquid is a heat-melting resin, if the second curable resin liquid is cured by cooling the second curable resin liquid to stabilize the shape of the sealing layer, the first curable resin inside will naturally harden over time while maintaining the shape of the sealing layer. For example, when the second curable resin liquid is a heat-fusible resin liquid, the first curable resin liquid is preferably a curable resin having a wide usable temperature range (e.g., −40 to 100° C., −40 to 120° C., −40 to 150° C., −40 to 200° C., etc.).

[0050] The manufacturing method of the present invention can provide the electric connector of the present invention. The structure, characteristics and physical properties of the obtained electric connector are as described above. EXAMPLES

[0051] The present invention will be described in more detail based on the following examples and comparative examples, but the present invention is not limited to these.

[0052] Details of the resins used in this example were as follows: <First curable resin liquid> Cyanoacrylate adhesive (moisture-curing, impact-resistant and heat-resistant instant adhesive, product name: ThreeBond 1782 (referred to as "1782" in the table below), viscosity: 80.0 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture-curing, impact-resistant and heat-resistant instant adhesive, product name: ThreeBond 1783 (referred to as "1783" in the table below), viscosity: 800 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (photocurable instant adhesive, product name: ThreeBond 1771E (referred to as "1771E" in the table below), viscosity: 2.0 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (photocurable instant adhesive, product name: ThreeBond 1773E (referred to as "1773E" in the table below), viscosity: 150 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3042 (referred to as "3042" in the table below), viscosity: 20 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3094B (referred to as "3094B" in the table below), viscosity: 150 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3042B (referred to as "3042B" in the table below), viscosity: 500 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3013B (referred to as "3013B" in the table below), viscosity: 1.0 Pa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3051E (referred to as "3051E" in the table below), viscosity: 1.5 Pa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture curing, instant adhesive for bonding metal, product name: ThreeBond 1702B (referred to as "1702B" in the table below), viscosity: 35.0 mPa s, manufactured by ThreeBond Co., Ltd.) The above viscosities are all measured at room temperature (25° C.). <Second hardening resin liquid> Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3006D (referred to as "3006D" in the table below), viscosity: 2.0 Pa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (photocurable adhesive (moisture curable type), product name: ThreeBond 3177 (referred to as "3177" in the table below), viscosity: 1200 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3042B (referred to as "3042B" in the table below), viscosity: 500 mPa s, manufactured by ThreeBond Co., Ltd.) Hot melt adhesive (main component: polyamide resin, product number: TEC7785-12 (referred to as "7785-12" in the table below), softening point: 155°C, viscosity (180°C): 5500mPa s, manufactured by Sanyo Life Materials Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3042 (referred to as "3042" in the table below), viscosity: 20 mPa s, manufactured by ThreeBond Co., Ltd.) The viscosity of the acrylate adhesive is measured at room temperature (25°C), and the viscosity of the hot melt adhesive is measured at 180°C.

[0053] Example 1 Three 0.75 sq copper wires (insulated wires) with a total length of 200 mm and three 0.75 sq aluminum wires (insulated wires) with a total length of 200 mm were used, and the polyvinyl chloride (PVC) insulating coating layer was removed within a range of 15 mm from one end of each wire to expose the conductor. The conductors were then joined together using an ultrasonic joining machine (manufactured by Nippon Avionics Co., Ltd.) to form a connection. A cyanoacrylate adhesive (product name: ThreeBond 1782) shown in Table 1 below was used as the first curable resin liquid. An acrylate adhesive (product name: ThreeBond 3006D) shown in Table 1 below was used as the second curable resin liquid, and was filled in a polypropylene container (insulating cap) in advance. As shown in FIG. 2, the connection part was immersed in the first curable resin liquid to a position where the coated part was immersed by about 5 mm, and then immediately removed. Within 10 seconds after removal, the connection part was immersed in the second curable resin liquid in the same manner while still attached to the first curable resin liquid, and the polypropylene container was placed in a vacuum chamber under ultraviolet light with an intensity of 1000 mW / cm. 2 The second curable resin liquid was cured by irradiating ultraviolet light at 400 K for 30 seconds. Thus, a connecting electric wire was obtained, which is made of a plurality of insulated electric wires whose connecting parts are sealed with resin. The first curable resin liquid naturally hardens while the connecting electric wire obtained is left at room temperature. Therefore, the connecting electric wire of the present invention is obtained, in which a layer made of the first curable resin is formed in contact with the connecting parts, a layer made of the second curable resin is formed on the outside of the layer made of the first curable resin, and a mixed region in which the first curable resin and the second curable resin are mixed is formed between them.

[0054] (Examples 2 to 11) A connecting wire was produced by curing the first curable resin liquid and the second curable resin liquid in the same manner as in Example 1 above, except that the first curable resin liquid and the second curable resin liquid were the curable resin liquids shown in Table 1 below. The first curable resin liquid in Examples 2 and 3 naturally cures while the resulting connecting wire is left at room temperature, and the first curable resin liquid in Examples 4 to 11 cures together with the second curable resin liquid by ultraviolet irradiation.

[0055] Example 12 In the same manner as in Example 1, partial areas of the conductor portions of the three copper electric wires and the three aluminum electric wires were ultrasonically joined to form connection portions. As the first curable resin liquid, a cyanoacrylate adhesive (product name: ThreeBond 1783) shown in Table 1 below was used. As the second curable resin liquid, a hot melt adhesive (product name: TEC7785-12) shown in Table 1 below was dissolved in advance at 180°C and filled into a polyethylene terephthalate container (insulating cap). The connection part was immersed in the first curable resin liquid to a position where the coating part was immersed about 5 mm, and immediately removed. Within 10 seconds after removal, the connection part was similarly immersed in the second curable resin liquid with the first curable resin liquid attached thereto, and was left to stand at room temperature for 5 minutes while immersed in the polyethylene terephthalate container to cool. In this way, the first curable resin liquid and the second curable resin liquid were cured, and a layer made of the first curable resin was formed in contact with the connection part, and a layer made of the second curable resin was formed on the outside of the first curable resin, and a mixed region in which the first curable resin and the second curable resin are mixed was formed between them, to obtain a connecting wire of the present invention.

[0056] Comparative Example 1 The first curable resin liquid and the second curable resin liquid were the curable resin liquids shown in the following Table 1. A connecting wire was obtained in the same manner as in Example 1, except that the connecting portion was immersed in the first curable resin liquid, immediately removed, and then left to stand for 4 hours in an environment with a temperature of 23°C and a humidity of 50% to cure the first curable resin liquid, and then immersed in the second curable resin liquid. The hardening of the first hardenable resin liquid was not complete when left standing for 3 hours, but was complete when left standing for 4 hours.

[0057] (Comparative Examples 2 and 3) The first curable resin liquid and the second curable resin liquid were the curable resin liquids shown in Table 1 below. The connection part was immersed in the first curable resin liquid and immediately taken out, and then exposed to ultraviolet light with an intensity of 1000 mW / cm. 2 An electric connecting wire was obtained in the same manner as in Example 4, except that the first hardening resin liquid was hardened by irradiation with light at 40 V for 30 seconds and then immersed in the second hardening resin liquid.

[0058] (Analysis of mixed areas) For the connecting electric wires of Examples 1 to 5 and 12 and Comparative Example 1, the mixed region of the first cured resin and the second cured resin in the formed sealing layer was analyzed. The wire was cut in the radial direction near the boundary between the conductor part where the insulating coating layer had been removed and the part where the insulating coating layer was still present, and the cut surface was polished and then cleaned with an ultrasonic cleaner. The cut surface was then subjected to mapping measurement with a microscopic Raman spectrophotometer to visualize (Raman imaging) the distribution of the resin components of the first cured resin and the second cured resin. -1 By analyzing the distribution of Raman scattering intensity in the vicinity, the presence or absence of a mixed region of the first cured resin and the second cured resin was determined. In the electric wires of Examples 1 to 5 and 12, the distribution of Raman scattering intensity derived from the cyano group of the first cured resin was observed even at a position 1000 μm away from the conductor surface toward the outer surface of the sealing layer. On the other hand, in the electric wire of Comparative Example 1, the distribution of Raman scattering intensity derived from the cyano group of the first cured resin was observed only up to a range 23 μm away from the conductor surface toward the outer surface of the sealing layer, and the distance was almost the same as the thickness of the first cured resin from the conductor surface. This shows that the electric wires of Examples 1 to 5 and 12 have a mixed region of the first cured resin and the second cured resin, and the electric wire of Comparative Example 1 does not have the mixed region.

[0059] The following evaluation tests were carried out on each of the obtained connecting wires. The results are shown in Table 1 below.

[0060] (Thermal shock test) Each of the resulting connecting wires was heated at 125°C for 30 minutes and then cooled at -40°C for 30 minutes, which constituted one cycle. This cycle was repeated 500 times in total. Thereafter, the insulating cap of each connecting wire was fixed, and a tensile tester (manufactured by Shimadzu Corporation) was used to test whether peeling occurred within the sealing layer and whether the insulated wires were pulled out when the six insulated wires were pulled out at a speed of 100 mm / min and 80 N. This test was performed a total of five times, and the number of times the wires were pulled out was used to evaluate the thermal shock resistance according to the following evaluation criteria. -Evaluation criteria- ○: The insulated wire could not be pulled out in all five tests. △: The insulated wire was pulled out 1 to 3 times out of 5 tests. ×: The insulated wire was pulled out 4 to 5 times out of 5 tests.

[0061] (Gasoline immersion test) Each of the resulting connecting wires was immersed in automobile gasoline No. 2 (JIS K 2202 No. 2) for 60 minutes, and after being pulled out of the gasoline, was left to stand in the air at room temperature (25°C) for 24 hours. Then, the insulating cap of each connecting wire was fixed, and a tensile tester (manufactured by Shimadzu Corporation) was used to test whether peeling occurred within the sealing layer and whether the insulated wires were pulled out when the six insulated wires were pulled out at a speed of 100 mm / min and 80 N. This test was performed a total of five times, and the number of times the wires were pulled out was applied to the following evaluation criteria to evaluate the gasoline immersion resistance. -Evaluation criteria- ○: The insulated wire could not be pulled out in all five tests. △: The insulated wire was pulled out 1 to 3 times out of 5 tests. ×: The insulated wire was pulled out 4 to 5 times out of 5 tests.

[0062] (Watertightness test) For the connecting electric wires immediately after manufacture, the connecting electric wires after the above 500 cold / hot cycles (connecting electric wires before the tensile test), and the connecting electric wires after the above immersion in gasoline (connecting electric wires before the tensile test), one of the six insulated electric wires constituting the connecting electric wires was selected, air was pumped into it using a regulator, and the other five wires immersed in water in a tank were evaluated for air leakage. The air pressure was gradually increased from 0 kPa to 200 kPa, and the air pressure at the time of air leakage was recorded and evaluated according to the following evaluation criteria. In the table, "Initial water stoppage" is the evaluation result of the connecting electric wire immediately after manufacture, "Water stoppage after cold / hot cycles" is the evaluation result of the connecting electric wires after 500 cold / hot cycles, and "Water stoppage after gasoline immersion" is the evaluation result of the connecting electric wires after gasoline immersion. -Evaluation criteria- ×: Air leak occurred before the air pressure reached 50 kPa. △: No air leak occurred when the air pressure was 50 kPa, but air leak occurred before the air pressure reached 200 kPa. ○: No air leak occurred even when the air pressure reached 200 kPa.

[0063] [Table 1]

[0064] It is understood that the connecting wires of Comparative Examples 1 to 3 obtained by immersing the first curable resin liquid in the second curable resin liquid after curing the first curable resin liquid lose adhesion of the sealing layer due to thermal shock cycles and immersion in gasoline. In contrast, the connecting wires of Examples 1 to 12, which did not include a curing process for the first curable resin liquid, and were obtained by immersing the first curable resin liquid in an uncured state in the second curable resin liquid and curing it, sufficiently maintained the adhesion of the sealing layer even after being subjected to a thermal shock cycle and immersed in gasoline. [Explanation of symbols]

[0065] 1 Connecting wire 10 Insulated wire 11 Conductor 12 Covering part 13 Connection 14 Crimp terminal 20 Sealing layer 21 First hardening resin liquid 22 First cured resin 23 Second hardening resin liquid 24 Second cured resin 25 Mixed area 26 Insulating cap (protective material)

Claims

1. A method for manufacturing a connecting electric wire in which a connection portion in which conductors of a plurality of insulated electric wires are connected to each other is sealed with an insulating sealing layer, comprising the steps of: immersing the connection portion in a first curable resin liquid; a step of immersing the connection portion to which the first curable resin liquid is attached in a second curable resin liquid while the first curable resin liquid attached to the connection portion is in an uncured state; and curing the first and second curable resin liquids applied to the connection portion, in this order.

2. 2. The method for producing a connection wire according to claim 1, wherein the first curable resin liquid has a viscosity of 51 to 1000 mPa·s.

3. The method for producing an electric connection wire according to claim 2 , wherein the second hardening resin liquid has a higher viscosity than the first hardening resin liquid.

4. The viscosity of the first curable resin liquid is 1 to 9 mPa·s, The method for manufacturing an electric connection wire according to claim 1 , wherein the second hardening resin liquid has a higher viscosity than the first hardening resin liquid.

5. The method for manufacturing an electric connection wire according to claim 1 , wherein the second curable resin liquid includes a photocurable resin.

6. The method for producing an electric connection wire according to claim 5 , wherein the first curable resin liquid includes a photocurable resin.

7. The method for producing an electric connection wire according to claim 5 , wherein the first hardening resin liquid contains a moisture-hardening resin.

8. The method for manufacturing an electric connection wire according to any one of claims 1 to 7, wherein the second curable resin liquid is used by filling a protective member.

9. The method for producing an electric connection wire according to any one of claims 1 to 7, wherein the electric connection wire is a wire harness.

10. A connecting wire in which a connection portion where conductors of a plurality of insulated wires are connected to each other is sealed with an insulating sealing layer, The sealing layer has a layer made of a first cured resin and a layer made of a second cured resin covering the layer made of the first cured resin, and has a mixed region of the first cured resin and the second cured resin between the layer made of the first cured resin and the layer made of the second cured resin.

11. The electrical connection wire of claim 10 , wherein the second curable resin comprises a photocurable resin.

12. The electrical connection wire of claim 11 , wherein the first curable resin comprises a photocurable resin.

13. The electrical connection wire of claim 11 , wherein the first curable resin comprises a moisture curable resin.

14. The electric wire according to any one of claims 10 to 13, wherein the sealing layer is covered with a protective member.

15. The connection wire according to any one of claims 10 to 13, wherein the connection wire is a wire harness.

Citation Information

Patent Citations

  • Moisture-blocking structure and moisture-blocking method between conductors in welded part of wire

    JP2003009334A

  • Waterproofing structure of electric wire splice portion

    JP2009283341A

  • Method for producing wire harness, and the wire harness

    JP2011113692A

  • Connection structure and manufacturing method thereof

    JP2011238500A

  • Method om manufacturing wire with terminal

    JP2019175790A