Polarizer, polarizing plate, and image display device
A liquid crystal polarizer with a crack suppression layer of gelled thixotropic material addresses cracking issues in high-temperature environments, ensuring polarizer stability.
Patent Information
- Application Number
- JP2023055939
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Liquid crystal polarizers are prone to cracking in high-temperature environments.
A polarizer comprising a liquid crystal alignment solidified layer with a crack suppression layer made of a gelled thixotropic material, such as a metal compound colloid, is used to prevent cracking.
The configuration effectively suppresses cracks in high-temperature environments, maintaining the polarizer's integrity and functionality.
Smart Images

Figure 2024143323000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizer, a polarizing plate, and an image display device. [Background technology]
[0002] In image display devices (e.g., liquid crystal display devices, organic EL display devices, inorganic EL display devices), a polarizing plate is often arranged on at least one side of the image display panel due to the image formation method. The polarizing plate typically includes a polarizer. As one form of polarizer, a polarizer in which a liquid crystal compound is oriented and the oriented state is fixed (hereinafter referred to as a liquid crystal polarizer) is known. A liquid crystal polarizer is characterized by being thinner than a polyvinyl alcohol polarizer and being less susceptible to discoloration since it does not use iodine. Furthermore, since the liquid crystal polarizer is formed without stretching, it has excellent smoothness and surface stability. On the other hand, a problem with liquid crystal polarizers is that they are prone to cracking in high temperature environments. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-092825 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned problems in the prior art, and a main object of the present invention is to provide a liquid crystal polarizer in which cracks in a high-temperature environment are suppressed. [Means for solving the problem]
[0005] [1] A polarizer according to an embodiment of the present invention is configured as an oriented and solidified layer of a liquid crystal compound containing a dichroic dye, and has a crack suppression layer on one of its main surfaces. The crack suppression layer is a gelled layer of a thixotropic material. [2] In the above [1], the thixotropic material is a colloidal solution. [3] In the above [2], the colloid is a metal compound colloid, a phyllosilicate colloid or an amide colloid. [4] In the above [2] or [3], the colloid is a metal compound colloid, and the metal compound colloid is at least one selected from the group consisting of an alumina colloid, a silica colloid, a zirconia colloid, a titania colloid, and a tin oxide colloid. [5] In the above [3] or [4], the metal compound colloid is an alumina colloid. [6] In any one of the above [1] to [5], the thickness of the crack suppression layer is 30 nm to 1000 nm. [7] According to another aspect of the present invention, there is provided a polarizing plate comprising the polarizer according to any one of [1] to [6] above and a protective layer disposed on at least one main surface of the polarizer. [8] According to yet another aspect of the present invention, there is provided an image display device comprising the polarizer according to any one of [1] to [6] above or the polarizing plate according to [7] above. Effect of the Invention
[0006] According to the embodiment of the present invention, a polarizer in which cracks in a high-temperature environment are suppressed can be realized. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of a polarizer according to one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0009] A. Polarizer Representative embodiments of the present invention will be described below with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to make the drawings easier to see and understand, the drawings are drawn typically or conceptually, and thickness, length, width, shape, size, ratio, etc. may differ from the actual ones, and there may be no correspondence between the drawings.
[0010] A-1. Overview of polarizers FIG. 1 is a schematic cross-sectional view of a polarizer according to one embodiment of the present invention. The polarizer 10 in the illustrated example has a polarizer body 11 having two main surfaces and a crack suppression layer 12 formed on one of the main surfaces of the polarizer body 11. The crack suppression layer 12 is a gelling layer of a thixotropic material. With such a configuration, cracks in the polarizer in a high-temperature environment can be suppressed. Since the gelling layer of the thixotropic material is strong, it is presumed that it can adequately protect the polarizer body in a high-temperature environment, and as a result, cracks in the polarizer in a high-temperature environment can be suppressed. However, such a mechanism is merely presumed, and the presumption is not intended to limit the interpretation of the embodiment of the present invention, and the embodiment of the present invention is not bound by such a mechanism.
[0011] A-2. Polarizer body The polarizer body (hereinafter, sometimes simply referred to as a polarizer) 11 is typically configured as an orientation-solidified layer of a liquid crystal compound containing a dichroic dye (hereinafter, referred to as a liquid crystal orientation-solidified layer). By configuring the polarizer as a liquid crystal orientation-solidified layer, a polarizer that is thin, difficult to discolor, and has excellent smoothness and surface stability can be realized. In this specification, the term "liquid crystal orientation-solidified layer" refers to a layer in which liquid crystal compounds are oriented in a predetermined direction within the layer and the orientation state is fixed. The term "liquid crystal orientation-solidified layer" is a concept that includes an orientation-solidified layer obtained by curing a liquid crystal monomer. In one embodiment of the liquid crystal orientation-solidified layer, the dichroic dye is aligned in accordance with the orientation of the rod-shaped liquid crystal compound, and as a result, an absorption axis is generated in substantially the same direction as the orientation direction of the liquid crystal compound.
[0012] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is preferably 35% to 48%, more preferably 37% to 45%, and even more preferably 39% to 43%. The degree of polarization of the polarizer is preferably 95.0% to 99.9%, more preferably 97.0% to 99.9%, and even more preferably 98.5% to 99.9%.
[0013] The thickness of the polarizer is preferably 2 μm to 8 μm, more preferably 3 μm to 7 μm, and further preferably 3 μm to 6 μm. By forming the polarizer using a liquid crystal compound, such a very thin thickness can be realized.
[0014] A-2-1. Liquid crystal compounds As the liquid crystal compound, any suitable liquid crystal compound can be adopted as long as it can express sufficient dichroism (light selective absorption performance) to function as a polarizer in a predetermined orientation state in combination with a dichroic dye. The liquid crystal compound is preferably polymerizable (i.e., liquid crystal monomer). If the liquid crystal compound is polymerizable, the orientation state of the liquid crystal compound can be fixed by aligning the liquid crystal compound and then polymerizing it. Here, the polymer formed by polymerization is non-liquid crystal. Therefore, the formed liquid crystal alignment solidified layer does not undergo transition to a liquid crystal phase, a glass phase, or a crystalline phase due to temperature changes specific to liquid crystal compounds, for example. As a result, the liquid crystal alignment solidified layer becomes a polarizer with extremely excellent stability that is not affected by temperature changes.
[0015] The mechanism by which the liquid crystal compound exhibits liquid crystallinity may be thermotropic or lyotropic, and the liquid crystal phase may be nematic or smectic.
[0016] The temperature range in which a liquid crystal compound exhibits liquid crystallinity varies depending on the type of the compound. Specifically, the temperature range is preferably 10°C to 120°C, more preferably 20°C to 110°C, and most preferably 30°C to 100°C.
[0017] In one embodiment, the liquid crystal compound is a liquid crystal monomer represented by formula (1). R1-A1-Y1-A2-Y2-A3-R2 (1) In formula (1), R1 and R2 each independently represent a chain organic group; At least one chain organic group of R1 and R2 represents a -(CH2)n-CH2-polymerizable group or a -O-(CH2)n-CH2-polymerizable group, where n is an integer of 1 to 24; A1 and A3 each independently represent a partial structure represented by formula (2), a divalent organic group, or a single bond; A2 represents a partial structure represented by formula (2) or a divalent organic group; -Y1- and -Y2- each independently represent a single bond, -C(=O)O-, -OC(=O)-, -C(=S)O-, -OC(=S)-, -C(=O)S-, -SC(=O)-, -CH2CH2-, -CH=CH-, -C(=O)NH-, -NHC(=O)-, -C2O-, -OCH2-, -CH2S-, or -SCH2-; One of A1 and A3 is a partial structure represented by formula (2) or a divalent organic group; At least one of A1, A2, and A3 is a partial structure represented by formula (2). -Cy-X2-C≡CX- ···(2) In formula (2), Cy represents a hydrocarbon ring group or a heterocyclic group; -X- represents -C(=O)O-, -OC(=O)-, -C(=S)O-, -OC(=S)-, -C(=O)S-, -SC(=O)-, -CH2CH2-, -CH=CH-, -C(=O)NH-, -NHC(=O)-, -CH2O-, -OCH2-, -CH2S-, or -SCH2-; -X2- represents a single bond, -C(=O)O-, -OC(=O)-, -C(=S)O-, -OC(=S)-, -C(=O)S-, -SC(=O)-, -CH2CH2-, -CH=CH-, -C(=O)NH-, -NHC(=O)-, -CHO-, -OCH2-, -CH2S-, or -SCH2-.
[0018] Specific examples of the liquid crystal monomer represented by formula (1) include the following. [ka] [ka]
[0019] Liquid crystal compounds are described, for example, in Japanese Patent No. 6798600, JP 2022-181212 A, JP 2022-176121 A, and WO 2019 / 182133 A. The descriptions in these publications are incorporated herein by reference.
[0020] A-2-2. Dichroic dye A dichroic dye is a substance or compound that absorbs at least a part of the wavelengths in the visible light region (380 nm to 780 nm) and exhibits dichroism. A representative dichroic dye is an azo dye. An azo dye has at least one azo group (-N=N-) in the molecule. The number of azo groups in the molecule of an azo dye is preferably 1 or more, more preferably 2 or more. On the other hand, the number of azo groups in the molecule of an azo dye is preferably 6 or less, more preferably 4 or less, and even more preferably 3 or less. If the number of azo groups is within such a range, an azo dye having excellent solubility in a solvent, compatibility with a liquid crystal compound, and color tone can be obtained.
[0021] In one embodiment, the dichroic dye may be black. If the dichroic dye is black, a black polarizer can be obtained. As a result, adverse effects on the color tone of the image display device can be suppressed. The black dye can be prepared, for example, by mixing a red dye and a blue dye, or a red dye, a yellow dye, and a blue dye in an appropriate ratio. When mixing a red dye and a blue dye, the compounding ratio (weight ratio) of the red dye / blue dye is preferably 1 / 200 to 5 / 1, more preferably 1 / 100 to 4 / 1, and even more preferably 1 / 10 to 3 / 1. When mixing a red dye, a yellow dye, and a blue dye, the compounding ratio (weight ratio) of the red dye is preferably 0.1 to 5, more preferably 0.5 to 2, and the compounding ratio (weight ratio) of the blue dye is preferably 0.1 to 5, more preferably 0.2 to 2, and even more preferably 0.5 to 2, when the yellow dye is taken as the standard (1). With such a configuration, a desired black color tone can be realized in the polarizer.
[0022] Specific examples of yellow dyes (yellow dichroic dyes) suitable for use in the embodiment of the present invention include the following. [ka]
[0023] Specific examples of the red dye (red dichroic dye) suitable for use in the embodiment of the present invention include the following. [ka] [ka]
[0024] Specific examples of blue dyes (blue dichroic dyes) suitable for use in the embodiments of the present invention include the following. [ka]
[0025] The amount of the dichroic dye is preferably 1 to 50 parts by weight, more preferably 2 to 40 parts by weight, based on 100 parts by weight of the liquid crystal compound. With such a composition, the liquid crystal compound tends to be polymerized without disturbing the alignment of the liquid crystal compound. When the dichroic dye is a mixture of dyes of each color, the amount of the dichroic dye is the total amount of the dyes of each color.
[0026] Examples of dichroic dyes include those described in Japanese Patent No. 6076528, Japanese Patent No. 6798600, JP-A-2013-228706,
[0067] to
[0071] , Japanese Patent No. 2013-227532,
[0008] to
[0026] , Japanese Patent No. 2013-209367,
[0008] to
[0015] , Japanese Patent No. 2013-14883,
[0045] to
[0058] , and Japanese Patent No. 2013-109090,
[0012] ~
[0029] ,
[0009] ~
[0017] of JP 2013-101328 A,
[0051] ~
[0065] of JP 2013-37353 A,
[0049] ~
[0073] of JP 2012-63387 A,
[0016] ~
[0018] of JP 11-305036 A,
[0009] ~
[0011] of JP 2001-133630 A,
[0030] of JP 2011-215337 A 】~
[0169] ,
[0021] ~
[0075] of JP 2010-106242 A,
[0011] ~
[0025] of JP 2010-215846 A,
[0017] ~
[0069] of JP 2011-048311 A,
[0013] ~
[0133] of JP 2011-213610 A,
[0074] ~
[0246] of JP 2011-237513 A,
[0005] to
[0051] ,
[0005] to
[0041] of International Publication No. 2016 / 060173,
[0008] to
[0062] of International Publication No. 2016 / 136561,
[0014] to
[0033] of International Publication No. 2017 / 154835,
[0014] to
[0033] of International Publication No. 2017 / 154695, and
[0013] to
[0037] of International Publication No. 2017 / 195833. The descriptions in these publications are incorporated herein by reference.
[0027] A-2-3. Method for forming polarizer A polarizer (liquid crystal alignment solidified layer) can be formed, for example, by applying a solution (liquid crystal composition) in which a liquid crystal compound (preferably a liquid crystal monomer), a dichroic dye, and optionally a photopolymerization initiator are dissolved in any suitable solvent to a predetermined alignment substrate, heating the liquid crystal monomer to bring it into a liquid crystal state and aligning the liquid crystal monomer, fixing the alignment by cooling, and polymerizing or crosslinking the liquid crystal monomer by irradiating it with light.
[0028] As the alignment substrate, any appropriate resin film (typically, a stretched resin film) can be used as long as it has a predetermined alignment regulating force. As the resin constituting the alignment substrate, any appropriate resin can be used as long as it is not dissolved in the solvent of the liquid crystal composition and has heat resistance when heated to align the liquid crystal monomer. Specific examples include cycloolefin-based resins (e.g., norbornene-based resins). The alignment regulating force can be imparted typically by rubbing alignment, stretched substrate alignment, or photoalignment. Stretched substrate alignment or photoalignment is preferred.
[0029] A-3. Crack suppression layer As described above, the crack suppression layer 12 is a gelation layer of a thixotropic material. Thixotropy refers to a phenomenon in which when a fluid is subjected to shear (e.g., stirring, pumping, coating), the viscosity decreases over time, and when the shear is stopped and the fluid is left stationary, the viscosity returns to the original value. Therefore, a thixotropic material is a material whose viscosity decreases under shear stress to become a highly fluid sol (liquid state), and when left stationary, becomes a gel (solid state). As is clear from the nature of a thixotropic material, when a sol under shear (e.g., by stirring) is applied to a polarizer body, the applied film spontaneously gels to become a gelation layer. Therefore, by using a thixotropic material, no additional steps or operations such as heating, ultraviolet irradiation (crosslinking or curing), lamination, or transfer are required when forming the crack suppression layer. Therefore, the crack suppression layer can be formed very simply and efficiently. Furthermore, the crack suppression layer can be formed without adversely affecting the polarizer body (e.g., by heat or ultraviolet light). In addition, since no adhesive layer is required for lamination or transfer, this can contribute to making polarizers (ultimately polarizing plates and image display devices) thinner.
[0030] A thixotropic material is typically a colloidal solution, which typically is a sol under shear and gels on standing. A colloidal solution typically contains a liquid medium (dispersion medium) and colloidal particles dispersed in the liquid medium.
[0031] Representative examples of the dispersion medium include water or an organic solvent. Specific examples of the organic solvent include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol, butanediol, pentanediol, 2-methyl-2,4-pentanediol, diethylene glycol, dipropylene glycol, and ethylene glycol monopropyl ether; ketones such as methyl ethyl ketone and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; esters such as ethyl acetate, butyl acetate, and γ-butyrolactone; and ethers such as tetrahydrofuran and 1,4-dioxane.
[0032] Examples of colloids (colloid particles) include metal compound colloids, phyllosilicate colloids, and amide (acid amide) colloids. The colloids (colloid particles) are preferably metal compound colloids. Examples of metal compound colloids include alumina colloids, silica colloids, zirconia colloids, titania colloids, and tin oxide colloids. These may be used alone or in combination. The metal compound colloids are preferably alumina colloids.
[0033] The concentration of colloid particles in the colloid solution is preferably 0.1% by weight to 30.0% by weight, more preferably 0.15% by weight to 20.0% by weight, and even more preferably 0.15% by weight to 15.0% by weight. If the concentration of colloid particles is within this range, a gelled layer (crack suppression layer) having appropriate mechanical strength can be formed.
[0034] The colloidal particles may have any suitable shape, including, for example, a spherical shape, an oval spherical shape, a needle shape, a rod shape, a fibrous shape, and an amorphous shape.
[0035] The size of the colloidal particles can be appropriately set depending on the purpose, shape, etc. For example, when the colloidal particles are spherical, the average primary particle diameter is preferably 1 nm to 200 nm, more preferably 20 nm to 180 nm, and further preferably 50 nm to 120 nm. For example, when the colloidal particles are elongated (e.g., needle-like, rod-like, fibrous), the average aspect ratio (major axis / minor axis) is preferably 30 to 5000, more preferably 100 to 3000; the average minor axis is preferably 1 nm to 10 nm, more preferably 2 nm to 5 nm; and the average major axis is preferably 100 nm to 10000 nm, more preferably 500 nm to 7000 nm. If the size of the colloidal particles is too large, the transparency and fluidity may be insufficient. If the size of the colloidal particles is too small, the storage stability may be insufficient.
[0036] The pH of the colloidal solution may be, for example, 2.5 to 4.0, or, for example, 3.0 to 3.6. If necessary, a pH adjuster may be used. The colloidal solution can be made neutral by using a pH adjuster. As a result, chemical adverse effects on the polarizer body can be suppressed. Examples of pH adjusters include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonia, ethylamine, tetramethylammonium hydroxide, and urea.
[0037] The viscosity of the colloidal solution (25° C.) is preferably 300 mPa·s or less, and more preferably 1 mPa·s to 200 mPa·s. If the viscosity of the colloidal solution is in this range, a gelled layer (crack suppression layer) having a desired thickness can be formed.
[0038] The colloidal solution may contain additives. Examples of additives include dispersion stabilizers, coupling agents, and antistatic agents. The type, number, combination, and amount of additives may be appropriately set depending on the purpose.
[0039] The colloidal solution typically does not contain a binder resin. In other words, the colloidal solution typically does not have an adhesive function. The colloidal solution, which is a thixotropic material, has a spontaneous film-forming function (gelling function), so there is no need to use a binder resin. As a result, there is no need to apply heat and / or active energy rays (e.g., ultraviolet rays) to harden the binder resin, so that adverse effects on the polarizer body can be avoided when forming the crack suppression layer.
[0040] The metal compound colloid is preferably an alumina colloid as described above. Therefore, the thixotropic material is preferably an alumina sol. Alumina includes aluminum hydroxides (alumina hydrates) such as gibbsite, bayerite, boehmite, pseudoboehmite, diaspore, and amorphous, as well as alumina crystals of γ, η, δ, ρ, κ, θ, χ, and α types. The alumina is preferably boehmite or pseudoboehmite.
[0041] Commercially available colloidal solutions may be used. Specific examples of commercially available products include "Aluminasol-F1000" (alumina colloid) manufactured by Kawaken Fine Chemicals Co., Ltd., "BYK-AQUAGEL 7100" (phyllosilicate colloid) manufactured by BYK, and "Disparlon" (amide colloid) manufactured by Kusumoto Chemicals Co., Ltd.
[0042] The thickness of the crack suppression layer is preferably 30 nm to 1000 nm, more preferably 50 nm to 700 nm, still more preferably 80 nm to 600 nm, particularly preferably 100 nm to 500 nm, and particularly preferably 120 nm to 400 nm. When the thickness of the crack suppression layer is within this range, it is possible to simultaneously achieve a thin polarizer (and thus a polarizing plate) and suppress cracks in the polarizer.
[0043] B. Polarizing plate FIG. 2 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 has a polarizer 10, a first protective layer 20 arranged on one main surface of the polarizer 10, and a second protective layer 30 arranged on the other main surface of the polarizer 10. The polarizer 10 is a polarizer according to the embodiment of the present invention described in the above section A. One of the first protective layer 20 and the second protective layer 30 may be omitted. In this case, the protective layer on the crack suppression layer side may be omitted, and the protective layer on the opposite side to the crack suppression layer may be omitted. One of the first protective layer and the second protective layer may be an alignment substrate used in the manufacture of the above polarizer.
[0044] The first protective layer and the second protective layer are made of any suitable resin film. Representative materials for the resin film include cellulose resins such as triacetyl cellulose (TAC), cycloolefin resins such as polynorbornene, (meth)acrylic resins, polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene, and polycarbonate resins. Representative examples of (meth)acrylic resins include (meth)acrylic resins having a lactone ring structure. (Meth)acrylic resins having a lactone ring structure are described in, for example, JP-A-2000-230016, JP-A-2001-151814, JP-A-2002-120326, JP-A-2002-254544, and JP-A-2005-146084. These publications are incorporated herein by reference. From the viewpoint of ease of processing into irregular shapes, etc., cellulose-based resins are preferred, and TAC is more preferred. From the viewpoint of obtaining a polarizing plate having low moisture permeability and excellent durability, cycloolefin-based resins and (meth)acrylic resins are preferred.
[0045] The thickness of each of the first protective layer and the second protective layer is preferably from 10 μm to 80 μm, more preferably from 12 μm to 40 μm, and further preferably from 15 μm to 35 μm.
[0046] In one embodiment, the protective layer (inner protective layer) disposed on the image display panel side when the polarizing plate 100 is applied to an image display device has optical isotropy. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 10 nm or less, preferably 7 nm or less, more preferably 5 nm or less; and the thickness direction retardation Rth(550) is -10 nm to 10 nm, preferably -7 nm to 7 nm, more preferably -5 nm to 5 nm. In another embodiment, the inner protective layer is a retardation layer having any appropriate retardation value. In this case, the in-plane retardation Re(550) of the retardation layer is, for example, 120 nm to 160 nm. "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C, and is calculated by the formula: Re=(nx-ny)×d. "Rth(550)" is the thickness direction retardation measured with light of 550 nm wavelength at 23°C, and is calculated by the formula: Re = (nx - nz) x d. Here, "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).
[0047] C. Image display device The polarizer described in the above item A or the polarizing plate described in the above item B can be applied to an image display device. Therefore, an image display device including such a polarizer or polarizing plate can also be included in the embodiment of the present invention. Representative examples of the image display device include a liquid crystal display device, an organic electroluminescence (EL) display device, and an inorganic EL display device. EXAMPLES
[0048] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties in the examples are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.
[0049] (1) Thickness The polarizer obtained in each example was cut, and the cross section of the polarizing plate was observed using a scanning electron microscope (manufactured by JEOL Ltd., "JSM7100F") to measure the thickness of the crack suppression layer.
[0050] (2) Cracks in the polarizer The polarizers obtained in the examples and comparative examples were heated from room temperature to 140°C at a heating rate of 30°C / min. The polarizers were observed under a polarizing microscope while being heated, and the temperature at which cracks occurred was measured. A cooling and heating stage for microscopes manufactured by Linkam was used for heating.
[0051] [Example 1] 28.57 parts of a liquid crystal compound represented by the following formula (I-1), 0.43 parts of an azo dye represented by the following formula (II-1), 0.29 parts of an azo dye represented by the following formula (II-2), 0.29 parts of a photopolymerization initiator (manufactured by BASF, product name "IRGACURE369"), and 0.43 parts of a leveling agent (manufactured by BYK-Chemie, product name "BYK-361N") were added to 69.99 parts of cyclopentanone, heated and stirred at 80°C, and then filtered using a syringe equipped with a syringe filter (manufactured by Membrane Solutions, PTFE13045, aperture 0.45 μm), thereby preparing a liquid crystal composition. [ka] [ka] [ka]
[0052] The liquid crystal composition was applied to the surface of a biaxially stretched norbornene film ("ZEONORFILM" manufactured by ZEON Corporation, thickness: 52 μm, Re(550): 50 nm, Ra of the liquid crystal composition coating surface: 1.2 nm) as an alignment substrate using a bar coater, dried by heating at 120° C. for 2 minutes, and then cooled to the liquid crystal phase and exposed to an exposure dose of 500 mJ / cm 2 . 2The resulting laminate of the alignment substrate and the polarizer had a thickness of about 4.5 μm.
[0053] An alumina colloid solution (manufactured by Kawaken Fine Chemicals Co., Ltd., product name "Aluminasol-F1000") was applied to the polarizer surface of the obtained laminate using a bar coater. The applied film gelled spontaneously, forming a crack-suppressing layer as a gelling layer. The thickness of the crack-suppressing layer was 169 nm. The polarizer with the crack-suppressing layer formed thereon was subjected to the evaluation in (2) above. The results are shown in Table 1.
[0054] [Example 2] A polarizer having a crack suppression layer formed thereon was produced in the same manner as in Example 1, except that the thickness of the crack suppression layer was set to 372 nm. The obtained polarizer was subjected to the same evaluations as in Example 1. The results are shown in Table 1.
[0055] [Comparative Example 1] The alignment substrate / polarizer laminate obtained in Example 1 was used as it was (that is, without forming a crack suppression layer) in the same manner as in Example 1. The results are shown in Table 1.
[0056] [Comparative Example 2] 50 parts of methylolmelamine was dissolved in pure water at a temperature of 30°C for 100 parts of a polyvinyl alcohol resin containing an acetoacetyl group (average degree of polymerization: 1200, degree of saponification: 98.5 mol%, degree of acetoacetylation: 5 mol%) to prepare an aqueous solution adjusted to a solid content of 3.7%. 18 parts of an aqueous solution of alumina colloid (average particle size 15 nm, solid content concentration 10%, positive charge) was added to 100 parts of this aqueous solution to prepare an aqueous solution of adhesive. The viscosity of the aqueous solution of adhesive was 9.6 mPa·s. This aqueous solution of adhesive was used instead of the alumina colloid solution of Example 1 to prepare a polarizer having an adhesive layer (thickness 199 nm). The obtained polarizer was subjected to the same evaluation as in Example 1. The results are shown in Table 1.
[0057] [Comparative Example 3] Except for changing the thickness of the adhesive layer to 442 nm, a polarizer having an adhesive layer was produced in the same manner as in Comparative Example 2. The obtained polarizer was subjected to the same evaluations as in Example 1. The results are shown in Table 1.
[0058] [Table 1]
[0059] As is clear from Table 1, the polarizers of the examples of the present invention suppress cracks in a high-temperature environment. It can be seen that the effect of suppressing cracks is more pronounced as the thickness of the crack-suppressing layer increases. Furthermore, as is clear from Comparative Examples 2 and 3, when the colloidal solution contains a binder resin (and therefore has an adhesive function), the effect of suppressing cracks is actually reduced. [Industrial Applicability]
[0060] The polarizer and polarizing plate according to the embodiment of the present invention are suitable for use in image display devices. [Explanation of symbols]
[0061] 10 Polarizer 11 Polarizer body 12 Crack suppression layer 20 First protective layer 30 Second layer of protection 100 Polarizing Plate
Claims
1. A polarizer including a crack suppression layer on one of its main surfaces, the polarizer being configured as an oriented and solidified layer of a liquid crystal compound including a dichroic dye, The crack suppression layer is a gelling layer of a thixotropic material; Polarizer.
2. The polarizer of claim 1 , wherein the thixotropic material is a colloidal solution.
3. The polarizer of claim 2 , wherein the colloid is a metal compound colloid, a phyllosilicate colloid, or an amide colloid.
4. 4. The polarizer according to claim 3, wherein the colloid is a metal compound colloid, and the metal compound colloid is at least one selected from the group consisting of an alumina colloid, a silica colloid, a zirconia colloid, a titania colloid, and a tin oxide colloid.
5. 5. The polarizer according to claim 4, wherein the metal compound colloid is an alumina colloid.
6. 2. The polarizer according to claim 1, wherein the crack suppression layer has a thickness of 30 nm to 1000 nm.
7. A polarizing plate comprising the polarizer according to claim 1 and a protective layer disposed on at least one main surface of the polarizer.
8. An image display device comprising the polarizing plate according to claim 7 .