Composite material, powder material and method for producing composite material
A composite material with nitride ceramics coated by a porous oxide ceramic addresses the thermal conductivity loss in nitride ceramics by adsorbing water vapor, preserving thermal conductivity and preventing hydrolysis.
Patent Information
- Application Number
- JP2023056144
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Nitride ceramics coated with silica to enhance water resistance compromise their thermal conductivity due to the absence of gaps, leading to impaired performance.
A composite material is developed with nitride ceramics coated by a metal or metalloid oxide ceramic having pores with diameters of 10 nm or less, which adsorb water vapor, maintaining thermal conductivity while preventing hydrolysis.
The composite material effectively suppresses the reaction between nitride ceramics and moisture, ensuring favorable thermal conductivity characteristics by allowing exposed surface portions and adsorbing water vapor, thus maintaining the properties of nitride ceramics.
Smart Images

Figure 2024143452000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to composite materials, powder materials, and methods for making composite materials. [Background technology]
[0002] Semiconductor elements for electric power (so-called power devices) have become indispensable for the efficient use of electrical energy. There is also an increasing demand for semiconductor elements for lighting (so-called high-power LED devices) used in energy-saving, long-life, high-brightness, high-power LED lamps. In general, the amount of heat generated by power devices increases as their density increases. Nitride ceramics, which have excellent thermal conductivity, are known as inorganic materials for dissipating this heat.
[0003] However, nitride ceramics (typically aluminum nitride, boron nitride, etc.) react with moisture in the air and undergo hydrolysis. For example, Patent Document 1 discloses silica-coated metal nitride particles in which the surfaces of metal nitride particles (nitride ceramic particles) are covered with silica particles with almost no gaps in order to improve water resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-101510 A Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Document 1, the nitride ceramic is covered with silica particles with almost no gaps, which impairs the thermal conductivity of the nitride ceramic.
[0006] The technology disclosed herein has been created in view of the above, and aims to provide a composite material that suppresses the reaction between nitride ceramics and moisture while allowing the nitride ceramics to exhibit suitable thermal conductivity characteristics. In another aspect, the technology also aims to provide a powder material containing the composite material and a method for producing the composite material. [Means for solving the problem]
[0007] The composite material disclosed herein includes a nitride ceramic and a metal or metalloid oxide ceramic attached to the surface of the nitride ceramic. In the composite material, the pore volume per unit mass of the oxide ceramic, when the pore diameter of the oxide ceramic is 10 nm or less, is less than 0.01 cm, as determined by a nonlocalized density functional (NLDFT) method. 3 / g or more.
[0008] In the above composite material, the pore volume per unit mass of the oxide ceramic when the pore diameter of the oxide ceramic is 10 nm or less is 0.01 cm 3 / g or more. According to this configuration, the pores of the oxide ceramics have the role of adsorbing (trapping) water vapor in the air, thereby suppressing the reaction between the nitride ceramics and moisture. Furthermore, since the oxide ceramics have a water vapor adsorption effect, it is not necessary to cover the nitride ceramics completely, and therefore it is possible to ensure an exposed surface portion on the surface of the nitride ceramics to which the oxide ceramics are not attached. By ensuring the exposed surface portion, the thermal conductivity of the nitride ceramics can be suitably expressed. Therefore, it is possible to provide a composite material that both suppresses the reaction between the nitride ceramics and moisture and expresses the thermal conductivity characteristics of the nitride ceramics.
[0009] In a preferred embodiment of the composite material disclosed herein, the oxide ceramic has a maximum peak pore size in a differential pore volume distribution of 10 nm or less. With this configuration, the composite material can adsorb water vapor effectively even in a low humidity environment.
[0010] In a preferred embodiment of the composite material disclosed herein, the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. In a preferred embodiment of the composite material disclosed herein, the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. This configuration makes it possible to provide a composite material to which an oxide ceramic having a suitable porous structure is attached.
[0011] According to another aspect of the technology disclosed herein, there is provided a powder material containing the composite material in powder form, which can suppress the reaction between the nitride ceramics and moisture while allowing the nitride ceramics to exhibit its properties.
[0012] In a preferred embodiment of the powder material disclosed herein, when the powder material is mixed with a separate phase of water and a non-polar solvent, 70% by weight or more of the powder material is present in the water phase. With this configuration, the oxide ceramics are preferably attached to the surface of the nitride ceramics, so that water vapor can be preferably adsorbed.
[0013] As another aspect of the technology disclosed herein, there is provided a method for producing a composite material. The method for producing a composite material disclosed herein is a method for producing a composite material including a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, and includes the steps of attaching a resinate containing a metal or metalloid as a raw material for the oxide ceramic to the nitride ceramic, and decomposing the resinate. Here, in the composite material, the oxide ceramic has a pore volume of 0.01 cm per unit mass of the oxide ceramic when the pore diameter of the oxide ceramic is 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method. 3 / g or more. This method therefore makes it possible to obtain a composite material that both inhibits the reaction between the nitride ceramic and moisture and allows the nitride ceramic to exhibit its properties.
[0014] In a preferred embodiment of the manufacturing method disclosed herein, in the decomposition step, heat treatment is performed at 800° C. or less. This configuration effectively suppresses sintering of the oxide ceramics, increases the specific surface area of the oxide ceramics, and allows porous oxide ceramic particles to adhere to the nitride ceramics. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a partially enlarged view that illustrates a composite material according to one embodiment. [Diagram 2] FIG. 2 is a schematic enlarged partial view showing a composite material according to another embodiment. [Diagram 3] FIG. 3 is an FE-SEM image (magnification: 50,000) relating to Example 1. [Figure 4] FIG. 4 is an FE-SEM image (magnification: 50,000) relating to Example 2. [Diagram 5] FIG. 5 is an FE-SEM image (magnification: 50,000) relating to Example 3. [Figure 6] FIG. 6 is an FE-SEM image (100,000x) of Example 8. [Figure 7] FIG. 7 is an FE-SEM image (100,000x) of Example 9. [Figure 8] FIG. 8 is an FE-SEM image (magnification: 50,000) relating to Example 10. [Figure 9] FIG. 9 is an FE-SEM image (magnification: 50,000) relating to Example 11. [Figure 10] FIG. 10 is an FE-SEM image (100,000x) of Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] An embodiment of the present technology will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present technology can be understood as design matters for a person skilled in the art based on the conventional technology in the relevant field. The present technology can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. In this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)", it means "A or more and B or less", and also includes the meanings of "more than A and less than B", "more than A and B or less", and "more than A and less than B".
[0017] Fig. 1 is a schematic partially enlarged view showing a composite material 100 according to one embodiment. As shown in Fig. 1, the composite material 100 disclosed herein includes a nitride ceramic 10 and an oxide ceramic 20 attached to the surface of the nitride ceramic 10. The composite material 100 may also include other components not shown.
[0018] The nitride ceramic 10 is a base material (core) of the composite material 100. The nitride ceramic 10 is, for example, aluminum nitride (AlN), boron nitride (BN), silicon nitride (Si 3 N 4 ), gallium nitride (GaN), etc. Among them, from the viewpoint of favorably exhibiting the water vapor adsorption effect of the oxide ceramics, it is preferable that the nitride ceramic 10 is aluminum nitride, boron nitride, or a mixture of these. Examples of boron nitride used in the nitride ceramic 10 include cubic boron nitride (cBN), hexagonal boron nitride (hBN), etc., and among them, hexagonal boron nitride is preferably used. The nitride ceramic 10 can be used alone or in combination of two or more types depending on the required characteristics and applications of the composite material 100.
[0019] The oxide ceramic 20 in the composite material 100 disclosed herein is a porous body (porous structure) having a plurality of pores. The form of the porous structure of the oxide ceramic 20 is not particularly limited, and may be, for example, an aggregate of fine particles, or may be formed on the surface of oxide ceramic particles. In the specification, the term "aggregate of fine particles" refers to, for example, an aggregate of fine particles or an incomplete sintered body (fine particles are necked together). As shown in FIG. 1, by adopting such a form, pores 11 are formed between the fine particles of the oxide ceramic 20. By having a porous structure, the oxide ceramic 20 plays a role of adsorbing water vapor in the atmosphere (trapping it in the pores).
[0020] The oxide ceramics 20 typically include metal or metalloid oxide ceramics. The oxide ceramics 20 preferably include at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. The oxide ceramics 20 preferably include a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. According to this configuration, a high concentration of functional groups (mainly hydroxyl groups) is introduced to the surface of the oxide ceramics 20, making the surface easily hydrophilic and easily atomized. For this reason, it is suitable for use in that it is easy to form the oxide ceramics 20 having a porous structure. In the specification, the term "metalloid" refers to a "metalloid element," typically Si, B, Sb, and Te.
[0021] The oxide ceramics 20 are attached to the surface of the nitride ceramics 10. For example, as shown in FIG. 1, the oxide ceramics 20 are attached as an aggregate of fine particles, although this is not limited thereto. Here, the oxide ceramics 20 are attached generally uniformly. It is preferable that the oxide ceramics 20 be attached (present widely) over a wide area of the surface of the nitride ceramics 10. This allows the oxide ceramics 20 to preferably exhibit the water vapor adsorption effect.
[0022] The form of the oxide ceramic 20 is not limited to that shown in Fig. 1, and may exist in various forms. Fig. 2 is a schematic partial enlarged view showing a composite material 100 according to another embodiment. As shown in Fig. 2, the oxide ceramic 20 is attached to the surface of the nitride ceramic 10 in the form of a film, and pores 11 are formed on the surface. The oxide ceramic 20 may be a thin film, or may be a bulk having a certain thickness as long as it does not significantly inhibit the thermal conductivity of the nitride ceramic 10.
[0023] It is preferable that at least a part of the composite material 100 has a surface exposed portion 12 where the surface of the nitride ceramic 10 is exposed. In other words, the surface exposed portion 12 indicates a portion where the oxide ceramic 20 is not attached to the surface of the nitride ceramic 10. This reduces the inhibition of the properties of the nitride ceramic 10 (e.g., thermal conductivity, etc.).
[0024] The surface exposure rate (%) of the nitride ceramic 10 in the composite material 100 is preferably 20% or more, 30% or more, or 50% or more. On the other hand, the surface exposure rate (%) of the nitride ceramic 10 in the composite material 100 is preferably 99% or less, 95% or less, 90% or less, 80% or less, or 70% or less. If the surface exposure rate is too low, it is not preferable because the expression of the properties of the nitride ceramic 10 (e.g., thermal conductivity, etc.) is suppressed. On the other hand, if the surface exposure rate is too high, it is not preferable because the nitride ceramic 10 reacts with moisture and hydrolysis proceeds. Note that the "surface exposure rate of the nitride ceramic" in this specification can be measured, for example, based on the following procedure. First, a surface area of the composite material on an image is 100 μm 2 An SEM image containing the above information is obtained. By analyzing the obtained SEM image, the total area of the composite material and the area of the exposed nitride ceramic surface can be calculated using the following formula (I). Surface exposure rate (%) = (area of exposed nitride ceramic surface) / (total area of composite material) × 100 (I).
[0025] The adhesion rate (wt%) of the oxide ceramics 20 in the entire composite material 100 is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. On the other hand, the adhesion rate (wt%) of the oxide ceramics 20 is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the adhesion rate is too low, the moisture adsorption effect of the oxide ceramics 20 cannot be obtained favorably, which is undesirable. On the other hand, if the adhesion rate is too high, the expression of the thermal conductivity, etc. of the nitride ceramics 10 is suppressed, which is undesirable. The adhesion rate of the oxide ceramics 20 can be calculated by the following formula (II). Adhesion rate of oxide ceramics (wt%) = weight of oxide ceramics (g) / (weight of nitride ceramics (g) + weight of oxide ceramics (g)) (II)
[0026] The composite material 100 disclosed herein has a pore volume (cm) per unit mass of the oxide ceramic 20 when the pore diameter of the oxide ceramic 20 is 10 nm or less, which is calculated by the Non Localized Density Functional Theory (NLDFT) method. 3 / g) is 0.01 cm 3 / g or more. According to this configuration, the oxide ceramic 20 has porosity, and the pores of the oxide ceramic 20 have the role of suitably adsorbing (trapping) water vapor in the air. In addition, since the oxide ceramic 20 has the above-mentioned water vapor adsorption effect, it is not necessary to completely cover the nitride ceramic 10, and therefore it is possible to suppress inhibition of thermoelectric conduction, etc. of the nitride ceramic 10. Note that in this specification, the term "pore volume (cm) per unit mass of the oxide ceramic when the pore diameter of the oxide ceramic is 10 nm or less" is used. 3The pore size and pore volume of the oxide ceramics can be measured by obtaining a nitrogen adsorption isotherm at -196°C and analyzing it by the NLDFT method. For example, the particle surface of the nitride ceramics is observed in advance with a scanning electron microscope or a transmission electron microscope, and after confirming that there are no pores of 10 nm or less, the above measurement is performed on the entire composite material, whereby the pore size and pore volume of the oxide ceramics can be measured. In addition, after obtaining a nitrogen adsorption isotherm for the entire composite material, the composite material is subjected to ultrasonic dispersion to remove the oxide ceramics, and then the nitrogen adsorption isotherm of the nitride ceramics is obtained again and excluded, thereby making the measurement possible. In addition, after obtaining a nitrogen adsorption isotherm for the entire composite material, either the nitride ceramics or the oxide ceramics of the composite material is dissolved and removed, and either of the nitrogen adsorption isotherms is obtained again and excluded, thereby making the measurement possible. Note that the pore volume per unit mass of the oxide ceramics when the pore size of the oxide ceramics is in another numerical range can also be obtained by this method. In addition, the pore volume per unit mass of the oxide ceramics can be measured by calculating the pore size and pore volume per unit mass of the oxide ceramics when the pore size and pore volume per unit mass of the oxide ceramics are in another numerical range ... s The analysis was performed using the α s Even if there is no clear inflection in the plot and a second straight line cannot be created, it can be determined that the nitride ceramic is non-porous.
[0027] The pore volume (cm) per unit mass of the oxide ceramic 20 in the composite material 100 when the pore diameter of the oxide ceramic 20 is 10 nm or less, obtained by the NLDFT method 3 / g) is 0.01 cm 3 / g or more, preferably 0.02 cm 3 / g or more, 0.03cm 3 / g or more, 0.05cm 3 / g or more, 0.1cm 3 / g or more. With such a pore volume, the oxide ceramic 20 can adequately exhibit the water vapor adsorption effect. There is no particular upper limit to the pore volume, but it is preferably 10 cm 3 / g or less, preferably 5 cm 3 / g or less, 2cm 3 / g or less, 1cm 3 / g or less, 0.5cm 3 / g or less. With such a pore volume, the strength of the oxide ceramic 20 attached to the nitride ceramic 10 is maintained, and falling off is suppressed.
[0028] In addition, the smaller the pore diameter of the oxide ceramic 20, the more effectively it can adsorb water vapor even in a low humidity environment. Therefore, the pore volume (cm) per unit mass of the oxide ceramic 20 in the composite material 100 when the pore diameter of the oxide ceramic 20 is 5 nm or less is 3 / g) is preferably 0.01 cm 3 / g or more, more preferably 0.02 cm 3 / g or more, 0.04cm 3 / g or more, 0.06cm 3 / g or more, 0.08cm 3 / g or more. In addition, the pore volume (cm) per unit mass of the oxide ceramic 20 in the composite material 100 when the pore diameter of the oxide ceramic 20 is 2 nm or less is 3 / g) is preferably 0.01 cm 3 / g or more, more preferably 0.02 cm 3 / g or more, 0.03cm 3 / g or more, 0.04cm 3 / g or more, 0.08cm 3 / g or more.
[0029] The peak pore size in the pore size distribution of the oxide ceramics 20 is not particularly limited, but from the viewpoint of favorably adsorbing water vapor, the maximum peak in the differential pore volume distribution is preferably 10 nm or less. The peak pore size in the pore size distribution of the oxide ceramics 20 is more preferably 7 nm or less, 5 nm or less, 3 nm or less, or 2 nm or less. The smaller the pore size of the oxide ceramics 20, the more favorably it can adsorb water vapor even in a low humidity environment. The differential pore volume distribution can be obtained by acquiring a nitrogen adsorption isotherm at -196°C and analyzing it by the NLDFT method.
[0030] When the pore diameter of the oxide ceramic 20 is 10 nm or less, the pore volume of the oxide ceramic 20 per unit BET surface area of the nitride ceramic is 0.0005 cm 3 / m 2 More preferably, 0.001 cm 3 / m 2 More than 0.0015cm 3 / m 2 More than 0.002cm 3 / m 2 More than 0.004cm 3 / m 2 Furthermore, when the pore diameter of the oxide ceramic 20 is 5 nm or less, the pore volume of the oxide ceramic 20 per unit BET surface area of the nitride ceramic is 0.0005 cm 3 / m 2 More preferably, 0.0007 cm 3 / m 2 More than 0.001cm 3 / m 2 More than 0.002cm 3 / m 2 More than 0.003cm 3 / m 2 Furthermore, when the pore diameter of the oxide ceramic 20 is 2 nm or less, the pore volume of the oxide ceramic 20 per unit BET surface area of the nitride ceramic is 0.0002 cm 3 / m 2 More preferably, 0.0005 cm 3 / m 2 More than 0.0007cm 3 / m 2 More than 0.001cm 3 / m 2 More than 0.002cm 3 / m 2 The term "BET surface area" as used herein refers to the specific surface area of a powder (solid) measured by gas adsorption, using nitrogen (N 2 The adsorption isotherms measured by a gas adsorption method using 1,2-dichloroethane (1,2-dichloroethane) gas were analyzed by the BET method.
[0031] The adhesion weight of oxide ceramics 20 per unit BET surface area of nitride ceramics (g / m 2 ) is 0.001 g / m from the viewpoint of suitably increasing the water vapor adsorption amount of the oxide ceramic 20. 2 More than 0.002g / m 2 More than 0.003g / m 2 More than 0.005g / m 2 More than 0.007g / m 2 The deposition weight (g / m) of the oxide ceramic 20 per unit BET surface area of the nitride ceramic is preferably 2 ) is set at 1 g / m from the viewpoint of optimally expressing the properties of nitride ceramics. 2 Below 0.5g / m 2 Below, 0.1g / m 2 Below 0.05g / m 2 The following is preferred:
[0032] In addition, the deposition volume (nm2) of oxide ceramics per unit BET surface area of nitride ceramics 3 / nm 2 ) is 0.2 nm from the viewpoint of suitably increasing the amount of water vapor adsorption of the oxide ceramic 20. 3 / nm 2 or more, 0.5nm 3 / nm 2 Above, 0.7nm 3 / nm 2 Above, 1nm 3 / nm 2 Above, 2nm 3 / nm 2 More preferably, the deposition volume (nm2) of the oxide ceramic 20 per unit BET surface area of the nitride is 3 / nm 2 ) is set to 100 nm from the viewpoint of favorably expressing the characteristics of the nitride ceramic 20. 3 / nm 2 Below, 50nm 3 / nm 2 Below, 40nm 3 / nm 2 Below, 30nm 3 / nm 2 Below, 20nm 3 / nm 2The following is preferred:
[0033] In some preferred embodiments, the composite material 100 may be used as a powder material, in which the composite material is in powder form. More specifically, the composite material 100 exists in powder form and is used as a powder material. The powder material may be used, for example, as a filler for a thermally conductive sheet or the like.
[0034] When the entire powder material is taken as 100 wt%, the powder material may contain, for example, 80 wt% or more of composite material 100, preferably 85 wt% or more of composite material 100, more preferably 90 wt% or more of composite material 100, even more preferably 95 wt% or more of composite material 100, and particularly preferably 98 wt% or more, or 99 wt% or more of composite material 100.
[0035] In this embodiment, the average particle size of the composite material 100 in the powder material is not particularly limited and can be appropriately changed depending on the purpose and mode of use. The average particle size of the composite material 100 in the powder material is typically nano to millimeter size, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the composite material 100 in the powder material is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less. In this specification, the "average particle size" refers to the particle size obtained by the arithmetic average of circle equivalent diameters obtained by image analysis of at least 100 particles in an image obtained using an optical microscope or a scanning electron microscope (SEM).
[0036] The applications of the composite material disclosed herein are not particularly limited, but it can be suitably used in applications requiring the thermal conductivity properties of nitride ceramics, such as inorganic materials for heat dissipation components (e.g., heat dissipation sheets for electronics applications).
[0037] In some preferred embodiments, when the separated phase of water and non-polar solvent and the powdered composite material 100 are stirred, 70 wt% or more (hereinafter also referred to as "the majority") of the composite material 100 is present in the aqueous phase, more preferably 75 wt% or more, 80 wt% or more. When the composite material 100 has the above-mentioned properties, it is found that the nitride ceramic surface tends to be modified by the oxide ceramic. That is, in a composite material having such properties, it is found that the oxide ceramic is attached to a certain amount or more of the nitride ceramic surface. The above evaluation (hereinafter also referred to as "water-non-polar solvent preference evaluation") is, for example, first, the powdered composite material, water, and the non-polar solvent are placed in a container (e.g., a glass bottle, etc.) and stirred (e.g., shaken by hand, using a shaker, etc.). After that, the container is left to stand, and it is confirmed whether the majority of the composite material is present in the aqueous phase or the non-polar solvent phase. Such confirmation can be performed by visual inspection. The non-polar solvent used in the water-non-polar solvent preference evaluation can be any of hexane, heptane, octane, nonane, and decane. When evaluating the water-non-polar solvent preference, the solvent and the container of the composite material may be subjected to a dispersion treatment such as ultrasonic dispersion to such an extent that the surface properties are not changed due to the falling off of the oxide ceramics. In addition, the ratio of the composite material in the separated phase of water and non-polar solvent can be determined, for example, by removing either the water phase or the non-polar solvent phase (in other words, separating the water phase and the non-polar solvent phase), drying and removing the solvent of the other phase, measuring the weight of the composite material contained in that phase, and calculating the ratio of the weight to the weight of the total composite material (the weight of the entire composite material put into the container).
[0038] The method for producing the composite material disclosed herein will be described below. The method for producing the composite material disclosed herein typically includes a resinate attachment step and a resinate decomposition step in this order. However, the method is not limited to this and may include other steps. Here, the method further includes a material preparation step prior to the resinate attachment step. Each step will be described below.
[0039] (1) Material preparation process In the material preparation step, a resinate containing a metal or metalloid as a raw material for the oxide ceramic, a nitride ceramic, and a solvent are prepared. Note that the nitride ceramic is the same as the nitride ceramic of the composite material described above, and therefore a description thereof will be omitted here.
[0040] The average particle size of the nitride ceramics prepared in the material preparation step is not particularly limited, but is, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the nitride ceramics is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less.
[0041] The resinate may be a conventionally known organometallic compound resinate containing at least one element selected from the group consisting of Al, Si, Zr, Ti, Ce, Y, Fe, and Zn. In addition, the resinate is preferably one that forms at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite in the resinate decomposition step described below. More preferably, the resinate contains a compound that forms a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. This allows the oxide ceramics to be formed with a suitable porous structure in the resinate decomposition step described below and to adhere to the surface of the nitride ceramics.
[0042] The metal or metalloid component contained in the resinate is the same as that of the oxide ceramic of the composite material described above, and therefore the description is omitted here. The content of the metal or metalloid component in the resinate may be 70 wt% or less, and preferably 60 wt% or less, 50 wt% or less, 40 wt% or less, or 30 wt% or less, calculated as oxide ceramics. As a result, the content of the metal or metalloid component in the resinate is low, and thus an oxide ceramic with a suitable porous structure is formed. On the other hand, the content of the metal or metalloid component in the resinate may be 2 wt% or more, and preferably 5 wt% or more, or 10 wt% or more, calculated as oxide.
[0043] The thermal decomposition temperature of the resinate is not particularly limited, but may be 150° C. or higher in the air, and is preferably 200° C. or higher, 300° C. or higher, or 400° C. or higher. The thermal decomposition temperature of the resinate may be 1000° C. or lower in the air, and is preferably 900° C. or lower, 800° C. or lower, or 700° C. or lower.
[0044] The solvent prepared in the material preparation step may be an aqueous solvent or an organic solvent. As the aqueous solvent, water (e.g., pure water, deionized water, etc.) or a mixed solution mainly made of water (e.g., a mixed solution of water and a lower alcohol) can be used. In this specification, a "mixed solution mainly made of water" refers to a mixed solution in which 50 vol% or more of the mixed solution is water. On the other hand, as the organic solvent, alcohols such as methanol and ethanol, ketones such as acetone and methyl ketone, esters such as ethyl acetate, etc. can be used.
[0045] (2) Resinate attachment process In the resinate attachment step, the resinate containing the oxide ceramic prepared in the material preparation step is attached to the nitride ceramic. Here, the process includes sub-steps (2-1) mixing step and (2-2) drying step.
[0046] (2-1) Mixing process In the mixing step, the resinate containing the oxide ceramic, the nitride ceramic, and the solvent are mixed together to obtain a mixture in which the resinate and the nitride ceramic are uniformly present in the solvent.
[0047] In the mixing step, a conventionally known stirring device, mixing device, etc. may be used. The mixing time in the mixing step is not particularly limited as long as the resinate and the nitride ceramics are uniformly present in the mixture. After the mixing step, a dispersion treatment such as ultrasonic dispersion may be performed to more suitably homogenize each component in the mixture.
[0048] The concentration of the nitride ceramic in the mixture is not particularly limited, but if the concentration is too low, it is not preferable from the viewpoint of cost balance. Therefore, the concentration of the nitride ceramic in the mixture is, for example, 10 g / l or more, preferably 100 g / l or more, or 300 g / l or more. On the other hand, if the concentration of the nitride ceramic is too high, there is a risk of the composite material agglomerating. Therefore, the concentration of the nitride ceramic in the mixture is, for example, 50000 g / l or less, preferably 10000 g / l or less, or 3000 g / l or less.
[0049] When calculated as the oxide ceramics in the resinate, the ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the nitride ceramics in the mixture is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. The ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the nitride ceramics in the mixture is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the ratio is too low, the oxide ceramics may not be attached to the nitride ceramics in a sufficient amount to obtain a sufficient moisture adsorption effect. On the other hand, if the ratio is too high, the oxide ceramics may be excessively attached to the nitride ceramics, suppressing the expression of the characteristics of the nitride ceramics.
[0050] (2-2) Drying process In the drying step, the mixture obtained in the mixing step is dried to remove the solvent from the mixture, thereby obtaining a dried product in which the resinate is adhered to the surface of the nitride ceramic.
[0051] In the drying step, a conventionally known drying means may be used, for example, a hot air dryer, a low-humid air dryer, a vacuum dryer, various infrared dryers, an electromagnetic induction dryer, a microwave dryer, dry air, etc., or drying promotion means such as air blowing, decompression, heating, etc., may be used alone or in combination. Such means may be appropriately selected depending on the type and amount of the solvent in the mixture.
[0052] The drying temperature in the drying step (such as the set temperature of the drying device) may be appropriately selected depending on the type and amount of the solvent in the mixture, and may be set to, for example, 60° C. to 150° C., typically 80° C. to 120° C. The drying time may also be appropriately selected depending on the type and amount of the solvent in the mixture, and is not particularly limited.
[0053] (3) Resinate decomposition process In the resinate decomposition step, the resinate in the dried material obtained in the drying step is decomposed. This produces oxide ceramics with a porous structure as a resinate decomposition product. Here, the resinate decomposition step (thermal decomposition of the resinate) is carried out by heat treatment. Here, the oxide ceramics can be in the form of an aggregate of fine particles. The dried material may be crushed before the resinate decomposition step. This operation can more effectively suppress the aggregation of the composite material after the resinate decomposition step.
[0054] The temperature of the heat treatment in the resinate decomposition step is preferably 800°C or less, 780°C or less, 750°C or less, 720°C or less, or 700°C or less. In this temperature range, sintering of the oxide ceramics is suitably suppressed, and the specific surface area of the oxide ceramics is increased. In other words, the oxide ceramics is prevented from becoming non-porous, and an oxide ceramics having a porous structure can be obtained. On the other hand, the lower limit of the heat treatment temperature is not particularly limited as long as it is equal to or higher than the decomposition temperature of the resinate, and is, for example, 200°C or more, and preferably 250°C or more, 300°C or more, or 350°C or more.
[0055] The atmosphere in the resinate decomposition step is not particularly limited as long as it can decompose the resinate. However, from the viewpoint of suitably removing organic component-derived residues (e.g., carbon, etc.) from the composite material, it is preferable to carry out the step in an oxidizing atmosphere (e.g., air, etc.).
[0056] The time for which the heat treatment is held at the top temperature in the resinate decomposition step is not particularly limited as long as the resinate can be completely decomposed, but the heat treatment can be carried out for, for example, about 0.1 to 2 hours.
[0057] After the heat treatment, the obtained composite material may be subjected to a crushing treatment. This makes the composite material in a powder form. Therefore, the obtained composite material can be suitably used as a powder material. The method for crushing the composite material in the crushing step is not particularly limited, and a conventionally known method can be used.
[0058] As described above, specific aspects of the technology disclosed herein include those described in the following sections.
[0059] Item 1: A composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to the surface of the nitride ceramic, wherein the pore volume per unit mass of the oxide ceramic in the pore diameter of 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method, is 0.01 cm 3 / g or more.
[0060] Item 2: The composite material according to item 1, wherein the oxide ceramic has a maximum peak pore size in a differential pore volume distribution of 10 nm or less.
[0061] Item 3: The composite material according to item 1 or 2, wherein the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.
[0062] Item 4: The composite material according to any one of Items 1 to 3, wherein the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia.
[0063] Item 5: A powder material comprising the composite material according to any one of items 1 to 4 in powder form.
[0064] Item 6: The powder material according to item 5, wherein when a separate phase of water and a non-polar solvent is stirred with the powder material, 70 wt % or more of the powder material is present in the aqueous phase.
[0065] Item 7: A method for producing a composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, comprising the steps of: attaching a resinate containing a metal or metalloid, which is a raw material for the oxide ceramic, to the nitride ceramic; and decomposing the resinate. In the composite material, the pore volume per unit mass of the oxide ceramic in the pore diameter of the oxide ceramic of 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method, is 0.01 cm 3 / g or more.
[0066] Item 8: The method for producing a composite material according to Item 7, wherein the decomposition step comprises heat treatment at 800° C. or less.
[0067] Test examples relating to the technology disclosed herein will be described below, but such test examples are not intended to limit the technology.
[0068] <Preparation of evaluation samples> In this test example, evaluation samples according to the following Examples 1 to 12 were prepared.
[0069] (Example 1) First, 10 ml of ethanol was added to 7.0 g (0.5 g in terms of silica) of an ethanol solution of tris(2-ethylhexanoic acid)ethoxysilane as a resinate (7.15 wt% in terms of silica, thermal decomposition temperature in air 350°C) and dissolved. 9.5 g of nonporous boron nitride powder (Tokuyama Corporation, S03) was added thereto and stirred. Then, a dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. This resulted in a composite material in which 5 wt % of amorphous silica particles were attached to boron nitride. The composite material thus obtained was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 1.
[0070] (Example 2) The procedure was the same as in Example 1, except that the dried product was calcined in an air atmosphere at a temperature of 700°C, at a heating rate of 5°C / min for 1 hour. As a result, a powdered composite material was obtained as an evaluation sample according to Example 2, in which 5 wt% of amorphous silica particles were attached to the boron nitride.
[0071] (Example 3) The procedure was the same as in Example 2, except that silicon resinate (Si 13%, silica equivalent 27.8 wt%, decomposition temperature in air 617°C) was used as the Si resinate, and 12 ml of ethanol was added to 1.80 g of the Si resinate (silica equivalent 0.5 g) and dissolved. As a result, a powdered composite material was obtained as an evaluation sample according to Example 3, in which 5 wt% of amorphous silica particles were attached to the boron nitride.
[0072] (Example 4) The procedure was the same as in Example 3, except that 0.36 g of Si resinate (0.1 g in terms of silica) and 9.9 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample according to Example 4, in which 1 wt% of amorphous silica particles were attached to the boron nitride.
[0073] (Example 5) The procedure was the same as in Example 3, except that 0.72 g of Si resinate (0.2 g in terms of silica) and 9.8 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 5, in which 2 wt% of amorphous silica particles were attached to the boron nitride.
[0074] (Example 6) The procedure was the same as in Example 3, except that 3.60 g of Si resinate (1.0 g in terms of silica) and 9.0 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 6, in which 10 wt% of amorphous silica particles were attached to the boron nitride.
[0075] (Example 7) First, 12 ml of ethanol was added to 1.08 g (0.2 g in terms of alumina) of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemicals) (18.47 wt% in terms of alumina, decomposition temperature in air 295°C) as Al resinate, and dissolved. 19.8 g of non-porous aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) was added thereto and stirred. Then, dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. As a result, a composite material was obtained in which 1 wt % of amorphous alumina particles were attached to aluminum nitride. The obtained composite material was crushed in a mortar to obtain a powdered composite material as an evaluation sample of Example 7.
[0076] (Example 8) The procedure was the same as in Example 7, except that 5.4 g of Al resinate (1.0 g in terms of alumina) and 19.0 g of aluminum nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 8, in which 5 wt% of amorphous alumina particles were attached to the aluminum nitride.
[0077] (Example 9) The powdered composite material according to Example 8, which had been fired and crushed, was further fired in an air atmosphere at a temperature of 650°C, at a heating rate of 10°C / min, for 0.5 hours. This resulted in a composite material in which 5 wt% of γ-alumina particles were attached to the aluminum nitride. The resulting composite material was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 9.
[0078] (Example 10) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 900° C., at a heating rate of 5° C. / min for 1 hour. This resulted in a powdered composite material as an evaluation sample according to Example 10, in which 5 wt % of amorphous silica was attached to boron nitride.
[0079] (Example 11) The boron nitride powder (S03, manufactured by Tokuyama Corporation) used in Example 1 was used as an evaluation sample without being coated with oxide ceramics.
[0080] (Example 12) The aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) used in Example 7 was used as it was as an evaluation sample without adhering oxide ceramics.
[0081] <Evaluation test> The above composite material was subjected to the following evaluation tests.
[0082] (1) Pore analysis Each sample was pretreated in a vacuum at 250°C for 1 hour, and then subjected to a specific surface area measurement device (model number: Belsorp-max (registered trademark)) manufactured by Microtrack-Bell, Inc., to obtain a nitrogen adsorption isotherm at -196°C. The following analysis was then performed using analysis software (BELLMaster Version 7.3.2.0).
[0083] (1-1) Specific surface area analysis In each of Examples 1 to 10, the specific surface area of the nitride ceramics was analyzed by the BET method using the above-mentioned analysis software. 2 / g, the adhesion weight of oxide ceramics per unit BET surface area of nitride ceramics (g / m 2 ) and volume (nm 3 / nm 2) was calculated. Similarly, the BET specific surface areas of the nitride ceramics of Examples 11 and 12 measured by this method were taken as the values of the boron nitride powder and aluminum nitride powder used in each Example. The BET specific surface area values of the boron nitride powder and aluminum nitride powder used in each Example were 1.3 m 2 / g, 3.2m 2 / g. The densities of the attached oxide ceramics, amorphous alumina, γ-alumina, and amorphous silica, were 3.0 g / cm3, respectively. 3 , 3.7g / cm 3 , 2.2g / cm 3 The results are shown in Table 1.
[0084] (1-2) Pore volume analysis In each of Examples 1 to 9, the pore size distribution was created under the following conditions using the above-mentioned analysis software. Curve Interpolation: Cubic Spline Curve Model: Cylinder Adsorbent: Metal oxide Fitting method: Tikhonov normalization, smoothing Using the obtained pore size distribution, the pore volume (cm) per unit mass of the composite material with pore sizes of 10 nm or less, 5 nm or less, and 2 nm or less was calculated. 3 The pore volume per unit mass of the oxide ceramic (cm 3 / g) and the pore volume per unit BET surface area of the powder consisting of nitride ceramic particles in the composite material (cm 3 / m 2 The results are shown in Table 1. In Example 10, the nitrogen adsorption isotherm obtained was analyzed using the above-mentioned analysis software to determine α s As a result of the analysis using the method, α s There was no clear inflection in the plot, so a second straight line could not be created. Therefore, Example 10 was determined to be non-porous, and is therefore underlined.
[0085] [Table 1]
[0086] As shown in Table 1, in Examples 1 to 9, the BET specific surface area of the nitride ceramic in the composite material after the oxide ceramic was attached was increased compared to the BET specific surface area of the nitride ceramic before the oxide ceramic was attached. On the other hand, in Example 10, there was little increase in the BET specific surface area of the nitride ceramic in the composite material before and after the oxide ceramic was attached. In addition, when comparing Examples 1 and 10, the BET specific surface area of the nitride ceramic in Example 10 was smaller than that of Example 1, even though the weight of the oxide ceramic attached was the same. This suggests that the oxide ceramic attached to the nitride ceramic in Example 10 is non-porous.
[0087] As shown in Table 1, in all of the results in Examples 1 to 9, the pore volume per unit mass of the oxide ceramics in which the pore diameter of the oxide ceramics is 10 nm or less is 0.01 cm 3 On the other hand, in Example 10, as described above, α s Analysis by the method confirmed that the material was non-porous.
[0088] In addition, as shown in Table 1, when Example 1 and Example 2 are compared, in Example 1, in which the firing temperature in the resinate decomposition step was 400° C., the pore volume per unit mass of the oxide ceramic in the pores having a diameter of 10 nm or less was 0.32 cm 3 , compared to Example 2, in which the firing temperature was 700° C. 3 / g, which was large.
[0089] (2) Water vapor adsorption measurement For each of Examples 1 to 6, 10, and 11, pretreatment was carried out in a vacuum at 250°C for 1 hour, and then the samples were subjected to a specific surface area measurement device (model number: Belsorp-max (registered trademark)) manufactured by Microtrack-Bel, and a water vapor adsorption isotherm at 25°C was obtained. Based on the obtained water vapor adsorption isotherm, the water vapor adsorption amount (cm) per unit mass of the composite material was calculated when the relative pressure in the water vapor adsorption isotherm was 0.1, 0.2, and 0.3. 3(STP) / g) were also calculated. The amount of water vapor adsorption per unit mass of oxide (cm 3 (STP) / g) and the water vapor adsorption per unit BET surface area (cm 3 (STP) / m 2 ) and the water vapor adsorption per unit BET surface area of the composite (cm 3 (STP) / m 2 The results are shown in Table 2.
[0090] [Table 2]
[0091] Comparing Examples 1 to 6 with Example 11, Examples 1 to 6 had a higher water vapor adsorption amount per unit mass of the composite material in all low relative pressure regions of 0.1, 0.2, and 0.3. This shows that the composite material exhibits a favorable water vapor adsorption effect even at low humidity. Comparing Examples 10 and 11, Example 10, in which nonporous oxide ceramics are locally attached, had a higher water vapor adsorption amount per unit mass of the composite material than Example 11, in which no oxide ceramics are attached. However, it is considered that the adsorbed water vapor in Example 10 is not trapped in the pores of the oxide ceramics, but exists on the surfaces of the oxide ceramics and nitride ceramics. Therefore, in Example 10, there is a risk that the adsorbed moisture will react with the nitride ceramics. In addition, comparing Examples 1 to 6 with Example 10, Examples 1 to 6 had a higher water vapor adsorption amount per unit mass of the oxide ceramics. This suggests that water vapor is trapped in the pores of the oxide ceramics in Examples 1 to 6.
[0092] (3) Water-nonpolar solvent preference evaluation For each of Examples 1 to 12, approximately 200 mg of sample was placed in a glass bottle, 20 ml of pure water was added, the bottle was capped, and the bottle was shaken by hand. The bottle was then opened, 20 ml of n-hexane as a non-polar solvent was added, the bottle was capped again, and the bottle was shaken by hand. The glass bottle was then left to stand, and it was visually confirmed whether the majority of the sample (i.e., 70% or more) was present in the water phase or the non-polar solvent phase (hexane phase). For Examples 8 to 9 and 12, evaluation was performed in the same manner as described above, except that n-decane was used instead of n-hexane. The results are shown in Table 3.
[0093] [Table 3]
[0094] As shown in Table 3, it was confirmed that the majority of all samples in Examples 1 to 9 were present in the aqueous phase. This shows that the nitride ceramic surface was modified by the oxide ceramic, that is, the oxide ceramic was attached to a certain amount of the nitride ceramic surface. On the other hand, it was confirmed that the majority of the samples in Examples 10 and 11 were present in the non-polar solvent phase. Note that in Example 12, the sample was present throughout the solvent when visually observed, and the boundary between the aqueous phase and the non-polar solvent phase (n-decane phase) was not clear, so it was classified as "unclear."
[0095] (4) Surface morphology observation Each of Examples 1 to 12 was observed using a field emission scanning electron microscope (FE-SEM) manufactured by Hitachi High-Technologies Corporation. Backscattered electron images of some of the Examples are shown in Figures 3 to 10. Figure 3 is an FE-SEM image (50,000x) of Example 1. Figure 4 is an FE-SEM image (50,000x) of Example 2. Figure 5 is an FE-SEM image (50,000x) of Example 3. Figure 6 is an FE-SEM image (100,000x) of Example 8. Figure 7 is an FE-SEM image (100,000x) of Example 9. Figure 8 is an FE-SEM image (50,000x) of Example 10. Figure 9 is an FE-SEM image (50,000x) of Example 11. Figure 10 is an FE-SEM image (100,000x) of Example 12.
[0096] As shown in Figs. 9 and 10, the nitride ceramics without oxide ceramics were confirmed to have no irregularities on the surface and were non-porous. On the other hand, as shown in Figs. 3 to 7, in Examples 1 to 3, 8 and 9, fine irregularities were observed on the surface of the composite material, and it was confirmed that the oxide ceramics were attached to the surface of the nitride ceramics as an aggregate of fine particles and had a porous structure, and similarly, the surface exposure of the nitride ceramics was confirmed. Although not shown here, the adhesion of the oxide ceramics as an aggregate of fine particles, the formation of pores, and the surface exposure of the nitride ceramics were also confirmed in Examples 4 to 7. In Examples 1 to 9, by having a portion where the nitride ceramics is exposed on a part of the surface of the composite material, the thermal conductivity of the nitride ceramics can be suitably expressed from the exposed portion. Similarly, it is considered that other properties of the nitride ceramics can be expressed by such a configuration.
[0097] As shown in FIG. 8, in Example 10 where the oxide ceramics were highly densified, it was confirmed that the oxide ceramics were spherical on the (0001) plane (FIG. 8) of the nitride ceramics (boron nitride), which is stable and has few functional groups. This is believed to be because the oxide ceramics were repelled by the (0001) plane of the boron nitride during the densification process by sintering the oxide ceramics, resulting in the spherical shape shown in FIG. 8. When the oxide ceramics exist in a spherical state as shown in FIG. 8, the oxide ceramics tend to easily fall off from the surface of the nitride ceramics. On the other hand, in Example 10, it was confirmed that the oxide ceramics were concentrated in a band shape on the end face of the nitride ceramics (lower right of FIG. 8). This is believed to be because the end face of the boron nitride constituting the nitride ceramics is an area with many functional groups compared to the (0001) plane, and has a high affinity with the oxide ceramics. In addition, when the oxide ceramics are concentrated on the end face of the nitride ceramics as shown in Example 10 (FIG. 8), it is not preferable because it inhibits the thermal conduction of the nitride ceramics. Moreover, the surface of the nitride ceramic is excessively exposed, which is undesirable since there is a risk of the nitride ceramic reacting with water vapor.
[0098] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]
[0099] 10. Nitride Ceramics 11 Pore 12 Surface exposure 20 Oxide Ceramics 100 Composite materials
Claims
1. A composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, The pore volume per unit mass of the oxide ceramics having a pore diameter of 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method, is 0.01 cm 3 / g or more; Composite material.
2. The oxide ceramic has a maximum peak pore diameter of 10 nm or less in a differential pore volume distribution.
2. The composite material of claim 1.
3. The oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.
3. A composite material according to claim 1 or 2.
4. The oxide ceramic comprises a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia; 3. A composite material according to claim 1 or 2.
5. A powder material comprising the composite material according to claim 1 or 2 in powder form.
6. 6. The powder material of claim 5, wherein when the powder material is mixed with a separate phase of water and a non-polar solvent, 70 wt % or more of the powder material is present in the water phase.
7. 1. A method for producing a composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, comprising the steps of: A step of adhering a resinate containing a metal or semi-metal that is a raw material of the oxide ceramic to the nitride ceramic; and decomposing the resinate, In the composite material, the pore volume per unit mass of the oxide ceramic in the pore diameter of the oxide ceramic of 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method, is 0.01 cm 3 / g or more; Manufacturing methods for composite materials.
8. In the decomposition step, heat treatment is performed at 800° C. or less. A method for producing the composite material according to claim 7.
Citation Information
Patent Citations