Powder material, and method for producing powder material
By adhering oxide ceramics to nitride ceramics with a specific surface area ratio, the powder material achieves enhanced wettability and dispersibility, addressing the wettability issues of nitride ceramics in resin applications.
Patent Information
- Application Number
- JP2023056145
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Nitride ceramics have poor wettability with resins due to low affinity with oxide ceramics, limiting their dispersibility and surface modification effectiveness, as seen in existing bonding methods like silica-coated metal nitride particles.
A powder material is created by adhering metal or metalloid oxide ceramics to nitride ceramics, with a specific surface area ratio (Rα) of 1.2 or more, ensuring oxide ceramics exist as fine particles, enhancing wettability and dispersibility in resins.
The modified nitride ceramics exhibit improved affinity with resins, enabling better dispersibility and surface functional group concentration, suitable for use as resin fillers.
Smart Images

Figure 2024143453000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to powder materials and methods for making powder materials. [Background technology]
[0002] Semiconductor elements for electric power (so-called power devices) have become indispensable for the efficient use of electrical energy. There is also an increasing demand for semiconductor elements for lighting (so-called high-power LED devices) used in energy-saving, long-life, high-brightness, high-power LED lamps. In general, the amount of heat generated by power devices increases as their density increases. Nitride ceramics, which have excellent thermal conductivity, are known as inorganic materials for dissipating this heat.
[0003] Nitride ceramics have few surface functional groups and low affinity (wettability) with resins, etc., and therefore, for example, are poorly dispersible in resins. One possible solution to this problem is to coat the surface of the nitride ceramics with an oxide ceramic that has many hydroxyl groups. In relation to the above technology, Patent Document 1 discloses silica-coated metal nitride particles in which sintered silica particles (oxide ceramic particles) are directly bonded to the surfaces of metal nitride particles (nitride ceramic particles) to coat them almost without gaps. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-101510 A Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Document 1, silica particles are directly bonded to and coated on the nitride ceramic. Therefore, the oxide ceramics that can be used in the technique disclosed in Patent Document 1 are limited to materials that directly bond to the nitride ceramic. In addition, according to the inventor's research, it was found that when the above technique is applied to a combination of nitride ceramics and oxide ceramics with low affinity, the oxide ceramics cannot be maintained attached to the nitride ceramics due to poor wettability between the nitride ceramics and the oxide ceramics, and the surface modification effect cannot be obtained satisfactorily.
[0006] The technology disclosed herein has been created in view of the above-mentioned points, and aims to provide a powder material that has a surface modification effect due to the adhesion of oxide ceramics to the nitride ceramic surface, typically a surface modification effect represented by the addition of functional groups. In addition, as another aspect, the technology disclosed herein aims to provide a method for producing the powder material. [Means for solving the problem]
[0007] The powder material disclosed herein includes a nitride ceramic and a metal or semi-metal oxide ceramic attached to a surface of the nitride ceramic, and the powder material has an α ratio of the specific surface area of the powder material to the specific surface area of the nitride ceramic in the powder material based on a BET method. s Ratio of specific surface area based on the method R α (Hereafter, simply "R α ") is 1.2 or more.
[0008] In the above powder materials, R αSince the ratio is 1.2 or more, the oxide ceramic is present in the form of fine particles on the surface of the nitride ceramic. With this configuration, the interface (contact surface) between the nitride ceramic and the oxide ceramic attached to the nitride ceramic surface is small. Therefore, even if the affinity (typically wettability) between the oxide ceramic and the nitride ceramic is poor, the oxide ceramic is maintained in a state of being attached to the nitride ceramic. This makes it possible to provide a powder material in which the surface of the nitride ceramic is modified without being affected by the affinity between the oxide ceramic and the nitride ceramic, resulting in improved affinity (wettability) with resin.
[0009] In a preferred embodiment of the powder material disclosed herein, the ratio of the α of the powder material to the specific surface area of the nitride ceramic in the powder material based on the BET method is s Ratio of specific surface area based on the method R α is 1.4 or more. According to this configuration, the oxide ceramics are more preferably present in the state of fine particles, and therefore the surface of the nitride ceramics is more preferably modified.
[0010] In a preferred embodiment of the powder material disclosed herein, when the powder material is mixed with a separate phase of water and a non-polar solvent, 70 wt % or more of the powder material is present in the water phase. With this configuration, the oxide ceramics are suitably attached to the surface of the nitride ceramics, so that the functional groups on the surface of the nitride ceramics can be suitably increased.
[0011] In a preferred embodiment of the powder material disclosed herein, the oxide ceramic has pores, and the contribution rate of the pores to the increase in the specific surface area of the powder material due to the adhesion of the oxide ceramic is calculated by the following formula: Contribution rate of pores to the increase in the specific surface area of the powder material (%) = (pore surface area per unit mass of the powder material) / (α of the powder material) sWhen calculated based on (specific surface area-BET specific surface area of nitride ceramic in powder material) x 100, the contribution rate of the pores to the increase in the specific surface area of the powder material due to the adhesion of the oxide ceramic is 20% or more. This makes it possible to increase the concentration of functional groups in the part where the oxide ceramic is adhered.
[0012] In a preferred embodiment of the powder material disclosed herein, the nitride ceramic contains at least one compound selected from the group consisting of aluminum nitride and boron nitride. With this configuration, the oxide ceramic is preferably attached, so that it is possible to provide a powder material that preferably exhibits the effect of increasing the surface functional groups.
[0013] In a preferred embodiment of the powder material disclosed herein, the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. In a preferred embodiment of the powder material disclosed herein, the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. With this configuration, functional groups are suitably introduced to the surface, making it possible to provide a powder material in which the effect of increasing surface functional groups is suitably expressed.
[0014] The powder material disclosed herein has a large number of functional groups on the surface of the powder material, and therefore has good dispersibility in resins, and can therefore be suitably used as a filler for resin materials that have good dispersibility in resins.
[0015] As another aspect of the technology disclosed herein, there is provided a method for producing a powder material. The method for producing a powder material disclosed herein includes a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, the method including the steps of: attaching a resinate containing a metal or metalloid, which is a raw material for the oxide ceramic, to the nitride ceramic; and decomposing the resinate. The ratio of the α of the powder material to the specific surface area of the nitride ceramic in the powder material based on the BET method is determined. s Ratio of specific surface area based on the method R α is 1.2 or more. According to this configuration, it is possible to provide a method for producing a powder material in which the surface of the nitride ceramic is modified by the oxide ceramic, thereby improving the affinity (wettability) with the resin.
[0016] In a preferred embodiment of the manufacturing method disclosed herein, the decomposition step is performed at a temperature of 800° C. or less. This configuration effectively suppresses sintering of the oxide ceramics and increases the specific surface area of the oxide ceramics. α can be suitably increased. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a partially enlarged view that illustrates a powder material according to one embodiment. [Diagram 2] FIG. 2 is a schematic enlarged partial view showing a powder material according to another embodiment. [Diagram 3] FIG. 3 is an FE-SEM image (magnification: 50,000) relating to Example 1. [Figure 4] FIG. 4 is an FE-SEM image (magnification: 50,000) relating to Example 2. [Diagram 5] FIG. 5 is an FE-SEM image (magnification: 50,000) relating to Example 3. [Figure 6] FIG. 6 is an FE-SEM image (100,000x) of Example 8. [Figure 7] FIG. 7 is an FE-SEM image (100,000x) of Example 9. [Figure 8] FIG. 8 is an FE-SEM image (magnification: 50,000) relating to Example 10. [Figure 9] FIG. 9 is an FE-SEM image (magnification: 50,000) relating to Example 11. [Figure 10] FIG. 10 is an FE-SEM image (100,000x) of Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] An embodiment of the present technology will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present technology can be understood as design matters for a person skilled in the art based on the conventional technology in the relevant field. The present technology can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. In this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)", it means "A or more and B or less", and also includes the meanings of "more than A and less than B", "more than A and B or less", and "more than A and less than B".
[0019] Fig. 1 is a schematic partially enlarged view showing a powder material 100 according to an embodiment. As shown in Fig. 1, the powder material 100 disclosed herein contains a nitride ceramic 10 and an oxide ceramic 20 attached to the surface of the nitride ceramic 10. The powder material 100 may also contain other components not shown.
[0020] In this embodiment, the average particle size of the powder material 100 in the powder material is not particularly limited and can be appropriately changed depending on the purpose and mode of use. The average particle size of the powder material 100 in the powder material is typically nano to millimeter size, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the powder material 100 in the powder material is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less. In this specification, the "average particle size" refers to the particle size obtained by the arithmetic average of circle equivalent diameters obtained by image analysis of at least 100 particles in an image obtained using an optical microscope or a scanning electron microscope (SEM).
[0021] The nitride ceramic 10 is a base material (core) of the powder material 100. Examples of the nitride ceramic 10 include aluminum nitride (AlN), boron nitride (BN), silicon nitride (Si3N4), and gallium nitride (GaN). The nitride ceramic 10 is preferably aluminum nitride or boron nitride, or a mixture thereof. From the viewpoint of favorably exhibiting the effect of increasing the functional groups on the surface of the nitride ceramic 10 by the oxide ceramic, it is particularly preferable to use boron nitride as the nitride ceramic 10. Examples of the boron nitride used in the nitride ceramic 10 include cubic boron nitride (cBN) and hexagonal boron nitride (hBN), and among them, hexagonal boron nitride is preferably used. The nitride ceramic 10 can be used alone or in combination of two or more types depending on the required characteristics and applications of the powder material 100.
[0022] The oxide ceramics 20 typically include metal or metalloid oxide ceramics. The oxide ceramics 20 preferably include at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. The oxide ceramics 20 also preferably include a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. According to this configuration, a high concentration of functional groups (mainly hydroxyl groups) is introduced to the surface of the oxide ceramics 20, making the surface easily hydrophilic and easy to atomize. For this reason, it is suitable for use in that it is easy to form the oxide ceramics 20, which are fine particles. In the specification, the term "metalloid" refers to a "metalloid element," typically Si, B, Sb, and Te.
[0023] The oxide ceramic 20 adheres to the surface of the nitride ceramic 10. For example, as shown in FIG. 1, the oxide ceramic 20 adheres in the form of fine particles. Here, the oxide ceramic 20 adheres generally uniformly. It is preferable that the oxide ceramic 20 adheres (is widely present) over a wide area of the surface of the nitride ceramic 10. This makes it possible to preferably achieve the effect of modifying the surface of the nitride ceramic 10 by the oxide ceramic, typically the effect of increasing functional groups.
[0024] The form of the oxide ceramic 20 is not limited to that shown in FIG. 1, and may exist in various forms. FIG. 2 is a schematic partial enlarged view showing a powder material 100 according to another embodiment. In some preferred embodiments, as shown in FIG. 2, the oxide ceramic 20 is attached as an aggregate of fine particles. In this case, the oxide ceramic 20 becomes a porous body (porous structure) having a large number of pores. According to such a structure, the functional group concentration is high in the part where the oxide ceramic 20 is attached. In addition, the "aggregation of fine particles" in the specification indicates, for example, an aggregate of fine particles or an incomplete sintered body (fine particles are necked together). In addition, as shown in FIG. 2, the oxide ceramic 20 may have pores 11 between the fine particles. The form of the pores 11 of the oxide ceramic 20 is not particularly limited, and may be, for example, an aggregate of fine particles as shown in FIG. 2, or may be formed on the particle surface of the oxide ceramic.
[0025] At least a part of the powder material 100 may have a surface exposed portion 12 where the surface of the nitride ceramic 10 is exposed. In other words, the surface exposed portion 12 indicates a portion of the surface of the nitride ceramic 10 where the oxide ceramic 20 is not attached. This reduces the inhibition of the properties of the nitride ceramic 10 (e.g., thermal conductivity, etc.).
[0026] The surface exposure rate (%) of the nitride ceramic 10 in the powder material 100 is preferably 2% or more, 5% or more, 10% or more, 20% or more, 30% or more, or 40% or more. On the other hand, the surface exposure rate (%) of the nitride ceramic 10 in the powder material 100 is preferably 90% or less, 80% or less, 70% or less, 60% or less, or 50% or less. If the surface exposure rate is too low, it is not preferable because the expression of the characteristics of the nitride ceramic 10 (e.g., thermal conductivity, etc.) is suppressed. On the other hand, if the surface exposure rate is too high, it is not preferable because the surface modification effect of the oxide ceramic on the nitride ceramic 10 is reduced. Note that the "surface exposure rate of the nitride ceramic" in this specification can be measured, for example, based on the following procedure. First, a powder material having a planar area of 100 μm on an image is measured. 2An SEM image containing the above information is obtained. By analyzing the obtained SEM image, the total area of the powder material and the area of the exposed nitride ceramic surface can be calculated using the following formula (I). Surface exposure rate (%) = (area of exposed nitride ceramic surface) / (total area of powder material) × 100 (I).
[0027] The adhesion rate (wt%) of the oxide ceramics 20 in the entire powder material 100 is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. On the other hand, the adhesion rate (wt%) of the oxide ceramics 20 is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the adhesion rate is too low, the surface of the nitride ceramics 10 is exposed in a large amount, which is not preferable. On the other hand, if the adhesion rate is too high, it is not preferable because the expression of the thermal conductivity and other properties of the nitride ceramics 10 is suppressed. The adhesion rate of the oxide ceramics 20 can be calculated by the following formula (II). Adhesion rate of oxide ceramics (wt%) = weight of oxide ceramics (g) / (weight of nitride ceramics (g) + weight of oxide ceramics (g)) (II)
[0028] The powder material 100 disclosed herein is a powder material having a specific surface area of 10 based on the BET method. s Ratio of specific surface area based on the method R α (Hereafter, simply "R α In the following description, the specific surface area based on the BET method is referred to as the "BET specific surface area," and α s For the specific surface area based on the α s This is called the "specific surface area". αIn the powder material 100 having a .alpha. of 1.2 or more, the oxide ceramics 20 are present in the form of fine particles on the surface of the nitride ceramics 10. This reduces the interface (contact surface) between the nitride ceramics 10 and the oxide ceramics 20 attached to the surface of the nitride ceramics 10. Therefore, even if the affinity (typically wettability) between the oxide ceramics 20 and the nitride ceramics 10 is poor, the oxide ceramics 20 can be maintained in a state of being attached to the nitride ceramics 10. This allows the surface of the nitride ceramics 10 to be modified without being affected by the affinity between the oxide ceramics 20 and the nitride ceramics 10, resulting in improved affinity (wettability) with the resin. Note that in this specification, the term ".alpha. s The "specific surface area" is the adsorption isotherm measured by the gas adsorption method using nitrogen (N2) gas as the adsorbate, expressed as α s In this specification, the term "BET specific surface area" refers to a value obtained by analyzing an adsorption isotherm measured by a gas adsorption method using nitrogen (N2) gas as an adsorbate, in accordance with the "Method of measuring the specific surface area of powders (solids) by gas adsorption" specified in JIS Z 8830:2013 (ISO9277:2010), using the BET method. The "BET surface area" described below also refers to a value obtained by analyzing the same method. α The "specific surface area of the nitride ceramic based on the BET method" used in the calculation may be an analytical value of the nitride ceramic after removing the oxide ceramic from the powder material, or may be an analytical value of the nitride ceramic before the oxide ceramic is attached.
[0029] The α of powder material 100 to the BET specific surface area of nitride ceramics 10 s Specific surface area ratio R α is 1.2 or more, and preferably 1.4 or more, 1.5 or more, 1.7 or more, 2 or more, or 3 or more. On the other hand, the α of the powder material 100 to the BET specific surface area of the nitride ceramic 10 s Specific surface area ratio R αThere is no particular upper limit to the ratio, but if this ratio is excessively high, the thermal conductivity characteristics of the nitride ceramic 10 may be suppressed. s Specific surface area ratio R α is preferably 100 or less, 50 or less, 30 or less, or 20 or less.
[0030] In some preferred embodiments, when the separated phase of water and non-polar solvent and the powder material 100 in a powder state are stirred, 70 wt% or more (hereinafter also referred to as "the majority") of the powder material 100 is present in the water phase, more preferably 75 wt% or more, 80 wt% or more. When the powder material 100 has the above-mentioned properties, it is found that the nitride ceramic surface tends to be modified by the oxide ceramic. That is, in a powder material having such properties, it is found that the oxide ceramic is attached to a certain amount or more of the nitride ceramic surface. The above evaluation (hereinafter also referred to as "water-non-polar solvent preference evaluation") is, for example, first, the powder material in a powder form, water, and a non-polar solvent are placed in a container (e.g., a glass bottle, etc.) and stirred (e.g., shaken by hand, using a shaker, etc.). After that, the container is left to stand, and it is confirmed whether the majority of the powder material is present in the water phase or the non-polar solvent phase. Such confirmation can be performed by visual inspection. The non-polar solvent used in the water-non-polar solvent preference evaluation can be any of hexane, heptane, octane, nonane, and decane. When evaluating the water-non-polar solvent preference, the solvent and the container of the powder material may be subjected to a dispersion treatment such as ultrasonic dispersion to such an extent that the surface properties are not changed due to the falling off of the oxide ceramics. In addition, the ratio of the powder material in the separated phase of water and non-polar solvent can be determined, for example, by removing either the water phase or the non-polar solvent phase (in other words, separating the water phase and the non-polar solvent phase), drying and removing the solvent of the other phase, measuring the weight of the powder material contained in that phase, and calculating the ratio of the weight to the weight of the total powder material (the weight of the entire powder material put into the container).
[0031] In some preferred embodiments, the oxide ceramics 20 preferably have a porous structure having pores 11. In this case, the contribution rate (%) of the pores to the increase in the specific surface area of the powder material 100 due to the adhesion of the oxide ceramics 20 (hereinafter also referred to as the "contribution rate of the pores to the increase in the specific surface area") is, for example, 20% or more, and preferably 30% or more, 40% or more, 50% or more, 70% or more, or 80% or more. In the specification, the "contribution rate of the pores to the increase in the specific surface area" can be calculated by the following formula (III). Contribution rate of pores to the increase in specific surface area (%) = (pore surface area per unit mass of powder material) / (α of powder material) s Specific surface area – BET specific surface area of nitride ceramics in powder material) × 100… Equation (III)
[0032] Pore volume per unit mass of oxide ceramics 20 (cm 3 / g) is preferably 0.002 cm from the viewpoint of suitably increasing the specific surface area of the powder material 100 and suitably increasing the surface functional groups of the powder material 100. 3 / g or more, more preferably 0.005 cm 3 / g or more, 0.01cm 3 / g or more, 0.015cm 3 / g or more, 0.02cm 3 On the other hand, the pore volume (cm) per unit mass of the oxide ceramic 20 is 3 / g) is preferably 2 cm or less from the viewpoint of maintaining the strength of the oxide ceramic 20 attached onto the nitride ceramic 10 and suppressing the fall-off of the oxide ceramic 20. 3 / g or less, more preferably 1 cm 3 / g or less, 0.7cm 3 / g or less or 0.5cm 3 / g or less.
[0033] The porosity (%) of the oxide ceramics 20 is preferably 1% or more, more preferably 1.5% or more, 2% or more, 3% or more, or 5% or more, from the viewpoint of favorably increasing the specific surface area of the powder material 100 and favorably increasing the surface functional groups of the powder material 100. The porosity (%) of the oxide ceramics 20 is preferably 80% or less, more preferably 75% or less, 70% or less, or 60% or less, from the viewpoint of maintaining the strength of the oxide ceramics 20 attached to the nitride ceramics 10 and suppressing the oxide ceramics 20 from falling off. In this specification, the "porosity of the oxide ceramics" refers to a value obtained by the following formula (IV) using the pore volume per unit mass of the oxide ceramics of the above oxide ceramics. Porosity of oxide ceramics (%) = Pore volume per unit mass of oxide ceramics (cm 3 / g) / {Oxide ceramics pore volume per unit mass of oxide ceramics (cm 3 / g) + (1 / density of oxide ceramics (g / cm 3 ))}×100...Formula (IV)
[0034] The average pore size (nm) of the oxide ceramics 20 is not particularly limited, but is preferably 15 nm or less, more preferably 10 nm or less, 8 nm or less, 5 nm or less, or 2 nm or less. Such a numerical range indicates that the particle size of the oxide ceramics 20 forming the porous structure on the nitride ceramics 10 is small, that is, that the oxide ceramics 20 can be present thinly on the nitride ceramics 10. This makes it possible to efficiently introduce functional groups onto the surface of the nitride ceramics 10 with a small amount of the oxide ceramics 20. In this specification, the "average pore size of the oxide ceramics" refers to the above-mentioned α s The pore volume of the oxide ceramic and the pore surface area of the oxide ceramic obtained by the plot method are used to obtain the value according to the following formula (V). Average pore diameter of oxide ceramics (nm) = 4 × pore volume per unit mass of oxide ceramics / pore surface area per unit mass of oxide ceramics...Equation (V) Although there is no particular lower limit to the average pore size of the oxide ceramic 20, it is preferable that the average pore size is, for example, 0.35 nm or more. The lower limit of measurement for pore size analysis by nitrogen gas adsorption method is 0.35 nm.
[0035] Pore surface area of oxide ceramics 20 per unit BET surface area of nitride ceramics (m 2 / m 2 ) is 0.1m 2 / m 2 More than 0.2m 2 / m 2 More than 0.3m 2 / m 2 More than 0.5m 2 / m 2 More than 1m 2 / m 2 The above is preferred.
[0036] The adhesion weight of oxide ceramics 20 per unit BET surface area of nitride ceramics (g / m 2 ) is 0.001 g / m from the viewpoint of suitably increasing the surface functional groups of the powder material 100. 2 More than 0.002g / m 2 More than 0.003g / m 2 More than 0.005g / m 2 More than 0.007g / m 2 The deposition weight (g / m) of the oxide ceramic 20 per unit BET surface area of the nitride ceramic is preferably 2 ) is set at 1 g / m from the viewpoint of optimally expressing the properties of nitride ceramics. 2 Below 0.5g / m 2 Below, 0.1g / m 2 Below 0.05g / m 2 The following is preferred:
[0037] In addition, the deposition volume (nm2) of oxide ceramics per unit BET surface area of nitride ceramics 3 / nm 2 ) is preferably 0.2 nm from the viewpoint of suitably increasing the specific surface area of the powder material 100. 3 / nm 2 or more, 0.5nm3 / nm 2 Above, 0.7nm 3 / nm 2 Above, 1nm 3 / nm 2 Above, 2nm 3 / nm 2 More preferably, the deposition volume (nm2) of the oxide ceramic 20 per unit BET surface area of the nitride is 3 / nm 2 ) is set to 100 nm from the viewpoint of favorably exhibiting the characteristics of the nitride ceramic 10. 3 / nm 2 Below, 50nm 3 / nm 2 Below, 40nm 3 / nm 2 Below, 30nm 3 / nm 2 Below, 20nm 3 / nm 2 The following is preferred:
[0038] In some preferred embodiments, the powder material 100 has an increased number of functional groups on the surface due to the oxide ceramics 20 attached to the surface of the nitride ceramics 10. This provides good wettability and dispersibility with resin. Therefore, the powder material disclosed herein can be suitably used as a filler for resin materials that have good wettability and dispersibility with resin.
[0039] The applications of the powder material disclosed herein are not particularly limited, but it can be suitably used in applications requiring the thermal conductivity properties of nitride ceramics, such as inorganic materials for heat dissipation components (e.g., heat dissipation sheets for electronics applications).
[0040] The method for producing the powder material disclosed herein will be described below. The method for producing the powder material disclosed herein typically includes a resinate adhesion step and a resinate decomposition step in this order. However, the method is not limited to this and may include other steps. Here, the method further includes a material preparation step prior to the resinate adhesion step. Each step will be described below.
[0041] (1) Material preparation process In the material preparation step, a resinate containing a metal or metalloid as a raw material for the oxide ceramic, a nitride ceramic, and a solvent are prepared. Note that the nitride ceramic is similar to the nitride ceramic of the powder material described above, and therefore a description thereof will be omitted here.
[0042] The average particle size of the nitride ceramics prepared in the material preparation step is not particularly limited, but is, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the nitride ceramics is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less.
[0043] The resinate may be a conventionally known organometallic compound resinate containing at least one element selected from the group consisting of Al, Si, Zr, Ti, Ce, Y, Fe, and Zn. In addition, the resinate is preferably one that forms at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite in the resinate decomposition step described below. More preferably, the resinate contains a compound that forms a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. This allows the resinate to form fine oxide ceramic particles and adhere to the surface of the nitride ceramic in the resinate decomposition step described below.
[0044] The metal or metalloid component contained in the resinate is the same as that of the oxide ceramics of the powder material described above, and therefore the description will be omitted here. The content of the metal or metalloid component in the resinate may be 70 wt% or less, and preferably 60 wt% or less, 50 wt% or less, 40 wt% or less, or 30 wt% or less, calculated as oxide ceramics. As a result, the content of the metal or metalloid component in the resinate is low, and thus an oxide ceramics that is preferably fine particles is formed. On the other hand, the content of the metal or metalloid component in the resinate may be 2 wt% or more, and preferably 5 wt% or more, or 10 wt% or more, calculated as oxide.
[0045] The thermal decomposition temperature of the resinate is not particularly limited, but may be 150° C. or higher in the air, and is preferably 200° C. or higher, 300° C. or higher, or 400° C. or higher. The thermal decomposition temperature of the resinate may be 1000° C. or lower in the air, and is preferably 900° C. or lower, 800° C. or lower, or 700° C. or lower.
[0046] The solvent prepared in the material preparation step may be an aqueous solvent or an organic solvent. As the aqueous solvent, water (e.g., pure water, deionized water, etc.) or a mixed solution mainly made of water (e.g., a mixed solution of water and a lower alcohol) can be used. In this specification, a "mixed solution mainly made of water" refers to a mixed solution in which 50 vol% or more of the mixed solution is water. On the other hand, as the organic solvent, alcohols such as methanol and ethanol, ketones such as acetone and methyl ketone, esters such as ethyl acetate, etc. can be used.
[0047] (2) Resinate attachment process In the resinate attachment step, the resinate containing the oxide ceramic prepared in the material preparation step is attached to the nitride ceramic. Here, the process includes sub-steps (2-1) mixing step and (2-2) drying step.
[0048] (2-1) Mixing process In the mixing step, the resinate containing the oxide ceramic, the nitride ceramic, and the solvent are mixed together to obtain a mixture in which the resinate and the nitride ceramic are uniformly present in the solvent.
[0049] In the mixing step, a conventionally known stirring device, mixing device, etc. may be used. The mixing time in the mixing step is not particularly limited as long as the resinate and the nitride ceramics are uniformly present in the mixture. After the mixing step, a dispersion treatment such as ultrasonic dispersion may be performed to more suitably homogenize each component in the mixture.
[0050] The concentration of the nitride ceramic in the mixture is not particularly limited, but if the concentration is too low, it is not preferable from the viewpoint of cost balance. Therefore, the concentration of the nitride ceramic in the mixture is, for example, 10 g / l or more, preferably 100 g / l or more, or 300 g / l or more. On the other hand, if the concentration of the nitride ceramic is too high, there is a risk of the powder material agglomerating. Therefore, the concentration of the nitride ceramic in the mixture is, for example, 50000 g / l or less, preferably 10000 g / l or less, or 3000 g / l or less.
[0051] When calculated as the oxide ceramics in the resinate, the ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the nitride ceramics in the mixture is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. The ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the nitride ceramics in the mixture is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the ratio is too low, the oxide ceramics may not be sufficiently attached to the nitride ceramics to exhibit the functional group increasing effect. On the other hand, if the ratio is too high, the oxide ceramics may be excessively attached to the nitride ceramics, suppressing the expression of the characteristics of the nitride ceramics.
[0052] (2-2) Drying process In the drying step, the mixture obtained in the mixing step is dried to remove the solvent from the mixture, thereby obtaining a dried product in which the resinate is adhered to the surface of the nitride ceramic.
[0053] In the drying step, a conventionally known drying means may be used, for example, a hot air dryer, a low-humid air dryer, a vacuum dryer, various infrared dryers, an electromagnetic induction dryer, a microwave dryer, dry air, etc., or drying promotion means such as air blowing, decompression, heating, etc., may be used alone or in combination. Such means may be appropriately selected depending on the type and amount of the solvent in the mixture.
[0054] The drying temperature in the drying step (such as the set temperature of the drying device) may be appropriately selected depending on the type and amount of the solvent in the mixture, and may be set to, for example, 60° C. to 150° C., typically 80° C. to 120° C. The drying time may also be appropriately selected depending on the type and amount of the solvent in the mixture, and is not particularly limited.
[0055] (3) Resinate decomposition process In the resinate decomposition step, the resinate in the dried product obtained in the drying step is decomposed. This produces fine oxide ceramic particles as a resinate decomposition product. Here, the resinate decomposition step (thermal decomposition of the resinate) is carried out by heat treatment. Here, the oxide ceramic particles can be in the form of fine particles. The dried product may be crushed before the resinate decomposition step. This operation can more effectively suppress the aggregation of the powder material after the resinate decomposition step.
[0056] The temperature of the heat treatment in the resinate decomposition step is preferably 800°C or less, 780°C or less, 750°C or less, 720°C or less, or 700°C or less. In this temperature range, sintering of the oxide ceramics is suitably suppressed, and the specific surface area of the oxide ceramics is increased. In other words, the oxide ceramics are prevented from becoming non-porous, and an oxide ceramics having a porous structure can be obtained. On the other hand, the lower limit of the heat treatment temperature is not particularly limited as long as it is equal to or higher than the decomposition temperature of the resinate, and is, for example, 200°C or more, and preferably 250°C or more, 300°C or more, or 350°C or more.
[0057] The atmosphere in the resinate decomposition step is not particularly limited as long as it can decompose the resinate, but it is preferable to carry out the step in an oxidizing atmosphere (e.g., air) in order to effectively remove residues derived from organic components (e.g., carbon, etc.) from the powder material.
[0058] The time for which the heat treatment is held at the top temperature in the resinate decomposition step is not particularly limited as long as the resinate can be completely decomposed, but the heat treatment can be carried out for, for example, about 0.1 to 2 hours.
[0059] After the heat treatment, the obtained powder material may be subjected to a crushing process. This makes the powder material into a powder form. Therefore, the obtained powder material can be suitably used as a powder material. The method for crushing the powder material in the crushing step is not particularly limited, and a conventionally known method can be used.
[0060] As described above, specific aspects of the technology disclosed herein include those described in the following sections.
[0061] Item 1: A powder material comprising a nitride ceramic and a metal or semimetal oxide ceramic attached to the surface of the nitride ceramic, wherein the ratio of the specific surface area of the nitride ceramic in the powder material based on the BET method to the specific surface area of the powder material is α s Ratio of specific surface area based on the method R α is not less than 1.2,
[0062] Item 2: The α of the powder material relative to the specific surface area of the nitride ceramic in the powder material based on the BET method s Ratio of specific surface area based on the method R α Item 2. The powder material according to item 1, wherein the powder material has a molecular weight of 1.4 or more.
[0063] Item 3: The powder material according to item 1 or 2, in which, when a separate phase of water and a nonpolar solvent is stirred with the powder material, 70 wt % or more of the powder material is present in the aqueous phase.
[0064] Item 4: The oxide ceramic has pores, and the contribution rate of the pores to the increase in the specific surface area of the powder material due to the adhesion of the oxide ceramic is calculated by the following formula: Contribution rate of pores to the increase in the specific surface area of the powder material (%) = (pore surface area per unit mass of the powder material) / (α of the powder material) s 4. The powder material according to any one of items 1 to 3, wherein, when calculated based on (specific surface area-BET specific surface area of nitride ceramic in powder material)×100, the contribution rate of the pores to an increase in the specific surface area of the powder material due to adhesion of the oxide ceramic is 20% or more.
[0065] Item 5: The nitride ceramic contains at least one compound selected from the group consisting of aluminum nitride and boron nitride; Item 5. The powder material according to any one of items 1 to 4.
[0066] Item 6: The powder material according to any one of Items 1 to 5, wherein the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.
[0067] Item 7: The powder material according to any one of Items 1 to 6, wherein the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia.
[0068] Item 8: The powder material according to any one of Items 1 to 7, which is a filler for a resin material.
[0069] Item 9: A method for producing a powder material containing a nitride ceramic and a metal or metalloid oxide ceramic attached to the surface of the nitride ceramic, comprising the steps of: attaching a resinate containing a metal or metalloid as a raw material for the oxide ceramic to the nitride ceramic; and decomposing the resinate. The ratio of the specific surface area of the powder material to the specific surface area of the nitride ceramic in the powder material based on the BET method is determined by the following steps: s Ratio of specific surface area based on the method R α A method for producing a powder material, wherein
[0070] Item 10: The method for producing a powder material according to Item 9, wherein the decomposition step includes a heat treatment at 800° C. or less.
[0071] Test examples relating to the technology disclosed herein will be described below, but such test examples are not intended to limit the technology.
[0072] <Preparation of evaluation samples> In this test example, evaluation samples according to the following Examples 1 to 12 were prepared.
[0073] (Example 1) First, 10 ml of ethanol was added to 7.0 g (0.5 g in terms of silica) of an ethanol solution of tris(2-ethylhexanoic acid)ethoxysilane as a resinate (7.15 wt% in terms of silica, thermal decomposition temperature in air 350°C) and dissolved. 9.5 g of nonporous boron nitride powder (Tokuyama Corporation, S03) was added thereto and stirred. Then, a dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. As a result, a powder material was obtained in which 5 wt % of amorphous silica particles were attached to boron nitride. The obtained powder material was crushed in a mortar to obtain a powder material as an evaluation sample according to Example 1.
[0074] (Example 2) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 700°C, at a heating rate of 5°C / min for 1 hour. As a result, a powder material was obtained as an evaluation sample according to Example 2, in which 5 wt% of amorphous silica particles were attached to the boron nitride.
[0075] (Example 3) The procedure was the same as in Example 2, except that silicon resinate (Si 13%, silica equivalent 27.8 wt%, decomposition temperature in air 617°C) was used as the Si resinate, and 12 ml of ethanol was added to 1.80 g of the Si resinate (silica equivalent 0.5 g) and dissolved. This resulted in a powder material as an evaluation sample according to Example 3, in which 5 wt% of amorphous silica particles were attached to the boron nitride.
[0076] (Example 4) The procedure was the same as in Example 3, except that 0.36 g of Si resinate (0.1 g in terms of silica) and 9.9 g of boron nitride powder were used. This resulted in a powder material as an evaluation sample according to Example 4, in which 1 wt% of amorphous silica particles were attached to the boron nitride.
[0077] (Example 5) The procedure was the same as in Example 3, except that 0.72 g of Si resinate (0.2 g in terms of silica) and 9.8 g of boron nitride powder were used. This resulted in a powder material as an evaluation sample for Example 5, in which 2 wt% of amorphous silica particles were attached to the boron nitride.
[0078] (Example 6) The procedure was the same as in Example 3, except that 3.60 g of Si resinate (1.0 g in terms of silica) and 9.0 g of boron nitride powder were used. This resulted in a powder material as an evaluation sample for Example 6, in which 10 wt% of amorphous silica particles were attached to the boron nitride.
[0079] (Example 7) First, 12 ml of ethanol was added to 1.08 g (0.2 g in terms of alumina) of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemicals) (18.47 wt% in terms of alumina, decomposition temperature in air 295°C) as Al resinate, and dissolved. 19.8 g of non-porous aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) was added thereto and stirred. Then, dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. As a result, a powder material was obtained in which 1 wt % of amorphous alumina particles were attached to aluminum nitride. The obtained powder material was crushed in a mortar to obtain a powder material as an evaluation sample according to Example 7.
[0080] (Example 8) The procedure was the same as in Example 7, except that 5.4 g of Al resinate (1.0 g in terms of alumina) and 19.0 g of aluminum nitride powder were used. This resulted in a powder material serving as an evaluation sample according to Example 8, in which 5 wt % of amorphous alumina particles were attached to the aluminum nitride.
[0081] (Example 9) The powdered material according to Example 8, which had been fired and crushed, was further fired in an air atmosphere at a temperature of 650°C, at a heating rate of 10°C / min, for 0.5 hours. This resulted in a powder material in which 5 wt% of γ-alumina particles were attached to the aluminum nitride. The resulting powder material was crushed in a mortar to obtain a powder material as an evaluation sample according to Example 9.
[0082] (Example 10) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 900° C., at a heating rate of 5° C. / min for 1 hour. This resulted in a powder material serving as an evaluation sample according to Example 10 in which 5 wt % of amorphous silica was attached to boron nitride.
[0083] (Example 11) The boron nitride powder (S03, manufactured by Tokuyama Corporation) used in Example 1 was used as an evaluation sample without being coated with oxide ceramics.
[0084] (Example 12) The aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) used in Example 7 was used as it was as an evaluation sample without adhering oxide ceramics.
[0085] <Evaluation test> The above powder materials were subjected to the following evaluation tests.
[0086] (1) Pore analysis Each sample was pretreated in a vacuum at 250°C for 1 hour, and then subjected to a specific surface area measurement device (model number: Belsorp-max (registered trademark)) manufactured by Microtrack-Bell, Inc., to obtain a nitrogen adsorption isotherm at -196°C. The following analysis was then performed using analysis software (BELLMaster Version 7.3.2.0).
[0087] (1-1) Analysis by BET method In each of Examples 1 to 10, the specific surface area of the nitride ceramics was analyzed by the BET method using the above-mentioned analysis software. 2 / g, the adhesion weight of oxide ceramics per unit BET surface area of nitride ceramics (g / m 2 ) and volume (nm 3 / nm 2) was calculated. Similarly, the BET specific surface areas of the nitride ceramics of Examples 11 and 12 measured by this method were taken as the values of the boron nitride powder and aluminum nitride powder used in each Example. The BET specific surface area values of the boron nitride powder and aluminum nitride powder used in each Example were 1.3 m 2 / g, 3.2m 2 The densities of the attached oxide ceramics, amorphous alumina, γ-alumina, and amorphous silica, were 3.0 g / cm3 and 3.0 g / cm3, respectively. 3 , 3.7g / cm 3 , 2.2g / cm 3 The results are shown in Table 1.
[0088] (1-2)α s Analysis by the method In each of Examples 1 to 12, α was measured using the above-mentioned analysis software. s A plot was created. s When creating the plot, the criterion α s For the curves, silica was selected for Examples 1-6 and 10, alumina for Examples 7-9 and 12, and GCB (graphitized carbon black) for Example 11. The obtained α s From the plot, an approximate line passing through the origin and a line with a high α s From the plot of the area, an approximation line with a smaller slope was created, and the specific surface area, pore volume, and external surface area of the powder material were calculated from the above two approximation lines. s For samples where there was no clear inflection in the plot and no second straight line could be created, the samples were judged to be non-porous, and only the specific surface area was calculated. α The pore surface area, the average pore diameter (nm) of the oxide ceramics, the contribution rate (%) of the pores to the increase in specific surface area, and the porosity (%) of the oxide ceramics were calculated. R α = (α of powder material s specific surface area) / (BET specific surface area of nitride ceramics)...Equation (a) Pore surface area = α of powder material sSpecific surface area - the external surface area per unit mass of a powder material...Equation (b) Average pore diameter of oxide ceramics (nm) = 4 × pore volume per unit mass of oxide ceramics / pore surface area per unit mass of oxide ceramics...Equation (c) Contribution rate of pores to the increase in specific surface area (%) = (pore surface area per unit mass of powder material) / (α of powder material) s Specific surface area – BET specific surface area of nitride ceramics in powder material) × 100… formula (d) Porosity of oxide ceramics (%) = Pore volume per unit mass of oxide ceramics (cm 3 / g) / {Oxide ceramics pore volume per unit mass of oxide ceramics (cm 3 / g) + (1 / density of oxide ceramics (g / cm 3 ))}×100...Equation (e) Regarding the "density of oxide ceramics" in formula (e), the densities of amorphous alumina, γ-alumina, and amorphous silica are 3.0 g / cm3. 3 , 3.7g / cm 3 , 2.2g / cm 3 The pore surface area and pore volume were calculated based on the values per unit mass of the powder material, the values per unit mass of the oxide ceramics, and the values per unit BET surface area of the nitride ceramics in the powder material. The results are shown in Table 1.
[0089] [Table 1]
[0090] As shown in Table 1, in Examples 1 to 9, R α was 1.4 or more in all the examples. From this, it can be seen that in Examples 1 to 9, the oxide ceramics are suitably present on the nitride ceramics in the form of fine particles. Therefore, in the powder materials according to Examples 1 to 9, it is considered that functional groups are imparted to the surface of the nitride ceramics, and the surface is suitably modified. On the other hand, in Example 10, R αwas 1.31.
[0091] As shown in Table 1, in all of Examples 1 to 9, the contribution rate of pores to the increase in the specific surface area of the powder material was 50% or more, which was a good result. From this, it is considered that in the powder materials of Examples 1 to 9, the oxide ceramics are generally present as an aggregate of fine particles (porous body having pores).
[0092] (2) Water-nonpolar solvent preference evaluation For each of Examples 1 to 12, approximately 200 mg of sample was placed in a glass bottle, 20 ml of pure water was added, the bottle was capped, and the bottle was shaken by hand. The bottle was then opened, 20 ml of n-hexane as a non-polar solvent was added, the bottle was capped again, and the bottle was shaken by hand. The glass bottle was then left to stand, and it was visually confirmed whether the majority of the sample (i.e., 70% or more) was present in the water phase or the non-polar solvent phase (hexane phase). For Examples 8 to 9 and 12, evaluation was performed in the same manner as described above, except that n-decane was used instead of n-hexane. The results are shown in Table 2.
[0093] [Table 2]
[0094] As shown in Table 2, it was confirmed that the majority of all samples in Examples 1 to 9 were present in the aqueous phase. This indicates that the nitride ceramic surface was modified by the oxide ceramic, that is, that the oxide ceramic was attached to a certain amount of the nitride ceramic surface. On the other hand, it was confirmed that the majority of the samples in Examples 10 and 11 were present in the non-polar solvent phase. Note that Example 12 was classified as "unclear" because, to the naked eye, the sample was present throughout the entire solvent, and it was not clear whether the majority of the sample was present in the aqueous phase or the non-polar solvent phase (n-decane phase).
[0095] (3) Surface morphology observation Each of Examples 1 to 12 was observed using a field emission scanning electron microscope (FE-SEM) manufactured by Hitachi High-Technologies Corporation. Backscattered electron images of some of the Examples are shown in Figures 3 to 10. Figure 3 is an FE-SEM image (50,000x) of Example 1. Figure 4 is an FE-SEM image (50,000x) of Example 2. Figure 5 is an FE-SEM image (50,000x) of Example 3. Figure 6 is an FE-SEM image (100,000x) of Example 8. Figure 7 is an FE-SEM image (100,000x) of Example 9. Figure 8 is an FE-SEM image (50,000x) of Example 10. Figure 9 is an FE-SEM image (50,000x) of Example 11. Figure 10 is an FE-SEM image (100,000x) of Example 12.
[0096] As shown in Figs. 9 and 10, the nitride ceramics without oxide ceramics were confirmed to have no irregularities on the surface and were non-porous. On the other hand, as shown in Figs. 3 to 7, in Examples 1 to 3, 8 and 9, fine irregularities were observed on the surface of the powder material, and it was confirmed that the oxide ceramics were attached to the surface of the nitride ceramics as an aggregate of fine particles or an incomplete sintered body of fine particles, and had a porous structure. Similarly, in Examples 1 to 3, 8 and 9, the surface exposure of the nitride ceramics was confirmed. Although not shown here, in Examples 4 to 7, the attachment of the oxide ceramics as an aggregate of fine particles or an incomplete sintered body of fine particles, the formation of porosity, and the surface exposure of the nitride ceramics were confirmed. In Examples 1 to 9, the powder material has a part on the surface where the nitride ceramics are exposed, and the thermal conductivity of the nitride ceramics can be suitably expressed from the exposed part. Similarly, it is considered that other properties of the nitride ceramics can be expressed by such a configuration.
[0097] As shown in FIG. 8, in Example 10, in which the oxide ceramics were highly densified, it was confirmed that the oxide ceramics were spheroidized on the (0001) plane (FIG. 8) of the nitride ceramics (boron nitride), which is stable and has few functional groups. This is believed to be because the oxide ceramics were sintered too much, and in the process of densification by sintering, the oxide ceramics were repelled by the (0001) plane of boron nitride, resulting in the spheroidized form shown in FIG. 8. When the oxide ceramics exist in a spheroidized state as shown in FIG. 8, the oxide ceramics tend to easily fall off from the surface of the nitride ceramics. On the other hand, in Example 10, it was confirmed that the oxide ceramics were concentrated in a band shape on the end face of the nitride ceramics (lower right of FIG. 8). This is believed to be because the end face of boron nitride constituting the nitride ceramics is an area with more functional groups than the (0001) plane, and has a high affinity with oxides. Furthermore, when the oxide ceramic is concentrated on the end face of the nitride ceramic as shown in Example 10 (FIG. 8), this is not preferable because it inhibits the thermal conduction of the nitride ceramic.
[0098] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]
[0099] 10. Nitride Ceramics 11 Pore 12 Surface exposure 20 Oxide Ceramics 100 Powder material
Claims
1. A powder material comprising a nitride ceramic and a metal or semi-metal oxide ceramic attached to a surface of the nitride ceramic, The ratio of the specific surface area of the powder material based on the BET method of the nitride ceramic in the powder material to the α s Ratio of specific surface area based on the method R α is 1.2 or more, powder material.
2. The ratio of the specific surface area of the powder material based on the BET method of the nitride ceramic in the powder material to the α s Ratio of specific surface area based on the method R α is 1.4 or more, 2. The powder material according to claim 1.
3. 2. The powder material of claim 1, wherein when the powder material is mixed with a separate phase of water and a non-polar solvent, 70 wt % or more of the powder material is present in the water phase.
4. The oxide ceramic has pores, The contribution rate of the pores to the increase in the specific surface area of the powder material due to the adhesion of the oxide ceramics is calculated by the following formula: Contribution rate of pores to the increase in specific surface area of powder material (%) = (pore surface area per unit mass of powder material) / (α of powder material) s Specific surface area - BET specific surface area of nitride ceramics in powder material) x 100 When calculated based on the above, the contribution rate of the pores to the increase in the specific surface area of the powder material due to the adhesion of the oxide ceramic is 20% or more.
4. The powder material according to claim 2 or 3.
5. The nitride ceramic contains at least one compound selected from the group consisting of aluminum nitride and boron nitride.
4. The powder material according to claim 2 or 3.
6. The oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.
4. The powder material according to claim 2 or 3.
7. The oxide ceramic comprises a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia; 4. The powder material according to claim 2 or 3.
8. A filler for resin materials, 4. The powder material according to claim 2 or 3.
9. 1. A method for producing a powder material comprising a nitride ceramic and a metal or semi-metal oxide ceramic attached to a surface of the nitride ceramic, comprising: A step of adhering a resinate containing a metal or semi-metal that is a raw material of the oxide ceramic to the nitride ceramic; and decomposing the resinate, The ratio of the specific surface area of the powder material based on the BET method of the nitride ceramic in the powder material to the α s Ratio of specific surface area based on the method R α is 1.4 or more, A method for producing powder materials.
10. In the decomposition step, a heat treatment is performed at 800° C. or less. A method for producing the powder material according to claim 9.
Citation Information
Patent Citations
Metal nitride particle coated with silica, and manufacturing method thereof
JP2015101510A