Composite material, powder material and method for producing composite material
By attaching a metal or metalloid oxide ceramic with specific pore structures to nitride ceramics, the composite material achieves enhanced dispersibility and thermal conductivity, addressing the affinity and modification issues of nitride ceramics in resin combinations.
Patent Information
- Application Number
- JP2023056147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Nitride ceramics have low affinity with resins and poor dispersibility due to few surface functional groups, limiting the effectiveness of surface modification when combined with oxide ceramics, as seen in existing technologies.
A composite material is created by attaching a metal or metalloid oxide ceramic to the surface of nitride ceramics, with pores of 2 nm or less between particles, and a pore surface area ratio of 30% or more for pore diameters up to 10 nm, enhancing surface modification and dispersibility.
The composite material exhibits improved dispersibility in resins and maintains thermal conductivity by ensuring a high concentration of functional groups on the nitride ceramic surface, facilitating better adhesion and modification.
Smart Images

Figure 2024143455000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to composite materials, powder materials, and methods for making composite materials. [Background technology]
[0002] Semiconductor elements for electric power (so-called power devices) have become indispensable for the efficient use of electrical energy. There is also an increasing demand for semiconductor elements for lighting (so-called high-power LED devices) used in energy-saving, long-life, high-brightness, high-power LED lamps. In general, the amount of heat generated by power devices increases as their density increases. Nitride ceramics, which have excellent thermal conductivity, are known as inorganic materials for dissipating this heat.
[0003] Nitride ceramics have few surface functional groups and low affinity (wettability) with resins, etc., and therefore, for example, are poorly dispersible in resins. One possible solution to this problem is to coat the surface of the nitride ceramics with an oxide ceramic that has many hydroxyl groups. In relation to the above technology, Patent Document 1 discloses silica-coated metal nitride particles in which sintered silica particles (oxide ceramic particles) are directly bonded to the surfaces of metal nitride particles (nitride ceramic particles) to coat them almost without gaps. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-101510 A Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Document 1, silica particles are directly bonded to and coated on the nitride ceramic. Therefore, the oxide ceramics that can be used in the technique disclosed in Patent Document 1 are limited to materials that directly bond to the nitride ceramic. In addition, according to the inventor's research, it was found that when the above technique is applied to a combination of nitride ceramics and oxide ceramics with low affinity, the oxide ceramics cannot be maintained attached to the nitride ceramics due to poor wettability between the nitride ceramics and the oxide ceramics, and the surface modification effect cannot be obtained satisfactorily.
[0006] The technology disclosed herein has been created in view of the above, and aims to provide a composite material that has a surface modification effect achieved by the adhesion of oxide ceramics to the surface of nitride ceramics, typically a surface modification effect represented by the addition of functional groups, and, in another aspect, a method for producing the composite material. [Means for solving the problem]
[0007] The composite material disclosed herein is a composite material comprising a nitride ceramic and a metal or semi-metal oxide ceramic adhered to a surface of the nitride ceramic, wherein the oxide ceramic is an aggregate of a plurality of particles, and has pores with a pore diameter of 2 nm or less between the particles of the oxide ceramic, and the proportion of the pore surface area of the composite material having a pore diameter of 2 nm or less to the total pore surface area of the composite material having a pore diameter of 10 nm or less calculated by a nonlocalized density functional (NLDFT) method is 30% or more.
[0008] In the above composite material, the oxide ceramics attached to the surface of the nitride ceramics exist as an aggregate of a plurality of particles, with pores between the particles having a pore diameter of 2 nm or less. As described above, the ratio of the surface area of the pores in the composite material having a pore diameter of 2 nm or less to the surface area of the pores having a diameter of 10 nm or less is 30% or more. By attaching the oxide ceramics to the surface of the nitride ceramics in the above-mentioned configuration, the surface of the nitride ceramics can be more suitably modified (typically by increasing the functional groups) with a small amount of the oxide ceramics.
[0009] In a preferred embodiment of the composite material disclosed herein, the ratio of the surface area of pores of the composite material having a pore diameter of 1 nm or less to the surface area of pores of the composite material having a pore diameter of 2 nm or less is 20% or more. With this configuration, it is more preferable that the surface of the nitride ceramics can be modified (typically by increasing the number of functional groups) with a small amount of oxide ceramics.
[0010] In a preferred embodiment of the composite material disclosed herein, the pore surface area per unit mass of the oxide ceramic in the composite material having a pore diameter of 2 nm or less is 10 m 2 / g or more. According to this configuration, the oxide ceramic preferably exists as an aggregate of a plurality of particles in the composite material.
[0011] In a preferred embodiment of the composite material disclosed herein, the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. In a preferred embodiment of the composite material disclosed herein, the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. This configuration makes it possible to provide a composite material in which the oxide ceramic is attached in the form of an aggregate of a plurality of particles.
[0012] In a preferred embodiment of the composite material disclosed herein, the nitride ceramic contains at least one compound or mixture selected from the group consisting of aluminum nitride and boron nitride. With this configuration, it is possible to provide a composite material in which the effect of increasing surface functional groups is favorably exhibited.
[0013] As another aspect of the technology disclosed herein, there is provided a powder material containing the composite material in powder form. According to this configuration, since the composite material having the above configuration is in powder form, it is possible to provide a powder material that can be suitably composited with other materials.
[0014] In a preferred embodiment of the composite material disclosed herein, when the composite material is mixed with a separate phase of water and a non-polar solvent, 70 wt % or more of the composite material is present in the aqueous phase. With this configuration, the oxide ceramics are appropriately attached to the surface of the nitride ceramics, and therefore the surface modification effect can be favorably obtained.
[0015] The composite material disclosed herein has a large number of functional groups (typically hydroxyl groups) on the surface of the composite material, and therefore has good dispersibility in resins, and can therefore be suitably used as a filler for resin materials that have good dispersibility in resins.
[0016] As another aspect of the technology disclosed herein, a method for producing a composite material is provided. The method for producing a composite material disclosed herein is a method for producing a composite material including a nitride ceramic and an oxide ceramic of a metal or metalloid attached to the surface of the nitride ceramic, and includes a step of attaching a resinate containing a metal or metalloid, which is a raw material of the oxide ceramic, to the nitride ceramic, and a step of decomposing the resinate, in which the oxide ceramic is an aggregate of a plurality of particles in the composite material, and between the particles of the oxide ceramic there are pores with a pore diameter of 2 nm or less, and the ratio of the surface area of the pores of the composite material with a pore diameter of 2 nm or less to the surface area of the pores of the composite material with a pore diameter of 10 nm or less determined by a nonlocalized density functional (NLDFT) method is 30% or more. This method provides a method for producing a composite material that can suitably modify the surface of the nitride ceramic (typically increase functional groups) with a small amount of the oxide ceramic.
[0017] In a preferred embodiment of the manufacturing method disclosed herein, in the decomposition step, heat treatment is performed at 800° C. or less. This configuration suitably suppresses sintering of the oxide ceramics, increases the specific surface area of the oxide ceramics, and allows an aggregate of multiple particles of the oxide ceramics to adhere onto the nitride ceramics. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a partially enlarged view that illustrates a composite material according to one embodiment. [Diagram 2] FIG. 2 is an FE-SEM image (magnification: 50,000) relating to Example 1. [Diagram 3] FIG. 3 is an FE-SEM image (magnification: 50,000) relating to Example 2. [Figure 4] FIG. 4 is an FE-SEM image (magnification: 50,000) relating to Example 3. [Diagram 5] FIG. 5 is an FE-SEM image (100,000x) of Example 8. [Figure 6] FIG. 6 is an FE-SEM image (100,000x) of Example 9. [Figure 7] FIG. 7 is an FE-SEM image (magnification: 50,000) relating to Example 10. [Figure 8] FIG. 8 is an FE-SEM image (magnification: 50,000) relating to Example 11. [Figure 9] FIG. 9 is an FE-SEM image (100,000x) of Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] An embodiment of the present technology will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present technology can be understood as design matters for a person skilled in the art based on the conventional technology in the relevant field. The present technology can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. In this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)", it means "A or more and B or less", and also includes the meanings of "more than A and less than B", "more than A and B or less", and "more than A and less than B".
[0020] Fig. 1 is a schematic partially enlarged view showing a composite material 100 according to one embodiment. As shown in Fig. 1, the composite material 100 disclosed herein includes a nitride ceramic 10, an oxide ceramic 20 attached to the surface of the nitride ceramic 10, and pores 11. The composite material 100 may also include other components not shown.
[0021] The nitride ceramic 10 is a base material (core) of the composite material 100. The nitride ceramic 10 is, for example, aluminum nitride (AlN), boron nitride (BN), silicon nitride (Si 3 N 4), gallium nitride (GaN), etc., and the nitride ceramic 10 is preferably aluminum nitride, boron nitride, or a mixture thereof. From the viewpoint of favorably exhibiting the effect of increasing functional groups on the surface of the nitride ceramic 10 by the oxide ceramic, it is particularly preferable to use boron nitride as the nitride ceramic 10. Since boron nitride has few surface functional groups, the effect of increasing functional groups by the attachment of the oxide ceramic is high. Examples of boron nitride used in the nitride ceramic 10 include cubic boron nitride (cBN), hexagonal boron nitride (hBN), etc., and among them, hexagonal boron nitride is preferably used. The nitride ceramic 10 can be used alone or in combination of two or more types depending on the required characteristics and applications of the composite material 100.
[0022] The oxide ceramic 20 is attached to the surface of the nitride ceramic 10. As shown in FIG. 1, the oxide ceramic 20 is attached as an aggregate of multiple particles. Here, the oxide ceramic 20 is a porous body (porous structure) having many pores 11 between the particles of the oxide ceramic 20. With this structure, the functional group concentration is high in the portion where the oxide ceramic 20 is attached. Note that the "aggregate of multiple particles" in the specification refers to, for example, an agglomerate of particles or an incomplete sintered body (a body in which multiple particles are necked together).
[0023] The oxide ceramics 20 typically include metal or metalloid oxide ceramics. The oxide ceramics 20 preferably include at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. The oxide ceramics 20 also preferably include a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. According to this configuration, a high concentration of functional groups (mainly hydroxyl groups) is introduced to the surface of the oxide ceramics 20, making the surface easily hydrophilic and easily microparticulating. For this reason, it is suitable for use in that the oxide ceramics 20, which has a porous structure, can be easily formed. In addition, the term "metalloid" in the specification refers to a "metalloid element," typically referring to Si, B, Sb, and Te.
[0024] The oxide ceramics 20 are attached generally uniformly. It is preferable that the oxide ceramics 20 be attached (present widely) over a wide area of the surface of the nitride ceramics 10. This allows the effect of modifying the surface of the nitride ceramics 10 by the oxide ceramics 20, typically the effect of increasing functional groups, to be favorably exhibited.
[0025] It is preferable that at least a part of the composite material 100 has a surface exposed portion 12 where the surface of the nitride ceramic 10 is exposed. In other words, the surface exposed portion 12 indicates a portion where the oxide ceramic 20 is not attached to the surface of the nitride ceramic 10. This reduces the inhibition of the properties of the nitride ceramic 10 (e.g., thermal conductivity, etc.).
[0026] The surface exposure rate (%) of the nitride ceramic 10 in the composite material 100 is preferably 2% or more, 5% or more, 10% or more, 20% or more, 30% or more, or 40% or more. On the other hand, the surface exposure rate (%) of the nitride ceramic 10 in the composite material 100 is preferably 90% or less, 80% or less, 70% or less, 60% or less, or 50% or less. If the surface exposure rate is too low, it is not preferable because the expression of the properties of the nitride ceramic 10 (e.g., thermal conductivity, etc.) is suppressed. On the other hand, if the surface exposure rate is too high, it is not preferable because the surface modification effect of the oxide ceramic on the nitride ceramic 10 is reduced. Note that the "surface exposure rate of the nitride ceramic" in this specification can be measured, for example, based on the following procedure. First, a planar area of the composite material on an image is 100 μm 2 An SEM image containing the above information is obtained. By analyzing the obtained SEM image, the total area of the composite material and the area of the exposed nitride ceramic surface can be calculated using the following formula (I). Surface exposure rate (%) = (area of exposed nitride ceramic surface) / (total area of composite material) × 100 (I).
[0027] The adhesion rate (wt%) of the oxide ceramics 20 in the entire composite material 100 is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. On the other hand, the adhesion rate (wt%) of the oxide ceramics 20 is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the adhesion rate is too low, it is not preferable because the surface exposed portion of the nitride ceramics on the surface of the composite material 100 increases. On the other hand, if the adhesion rate is too high, it is not preferable because the expression of the properties such as thermal conductivity of the nitride ceramics 10 is suppressed. The adhesion rate of the oxide ceramics 20 can be calculated by the following formula (II). Adhesion rate of oxide ceramics (wt%) = weight of oxide ceramics (g) / (weight of nitride ceramics (g) + weight of oxide ceramics (g)) (II)
[0028] In the composite material 100 disclosed herein, the oxide ceramic 20 is an aggregate of a plurality of particles. According to this configuration, the interface (contact surface) between the nitride ceramic 10 and the oxide ceramic 20 attached to the surface of the nitride ceramic 10 is small. Therefore, even if the affinity (typically wettability) between the oxide ceramic 20 and the nitride ceramic 10 is poor, the oxide ceramic 20 is maintained in a state of being attached to the nitride ceramic 10. As a result, the surface of the nitride ceramic 10 is modified without being affected by the affinity between the oxide ceramic 20 and the nitride ceramic 10, resulting in improved affinity (wettability) with resins and the like. In addition, the composite material 100 disclosed herein has pores 11 with a pore diameter of 2 nm or less between the particles of the oxide ceramic 20. According to this configuration, the particle diameter of each particle forming the aggregate of a plurality of particles of the oxide ceramic 20 is small, and the surface can be suitably modified by the attachment of a small amount of the oxide ceramic. The composite material 100 is characterized in that the ratio of the surface area of pores in the composite material 100 having a pore diameter of 2 nm or less to the surface area of pores in the composite material 100 having a pore diameter of 10 nm or less, determined by the Non Localized Density Functional Theory (NLDFT) method, is 30% or more. When the pore diameter of the pores 11 in the composite material 100 is 2 nm or less, the surface properties are similar to those of non-porous oxide ceramics (Reference: M. Fuji, J. Soc. Powder Technol., Japan, 40, 355-363 (2003)). Therefore, this configuration allows the surface of the nitride ceramics 10 to be efficiently modified.
[0029] In this specification, the "pore surface area of a composite material having a pore diameter of 10 nm or less obtained by the non-localized density functional (NLDFT) method" can be obtained by obtaining a nitrogen adsorption isotherm at -196°C and analyzing it by the NLDFT method. For example, the particle surface portion of the nitride ceramic is observed in advance with a scanning electron microscope or a transmission electron microscope, and after confirming that there are no pores in the required analysis range (for example, 200 nm or less, 100 nm or less, 50 nm or less, 20 nm or less, 10 nm or less, 5 nm or less, 1 nm or less), the above measurement can be performed on the entire composite material to measure the pore diameter and pore volume between particles of the oxide ceramic. In addition, after obtaining a nitrogen adsorption isotherm for the entire composite material, the composite material is subjected to ultrasonic dispersion to remove the oxide ceramic, and then the nitrogen adsorption isotherm of the nitride ceramic is obtained again and removed, so that the measurement can be performed. In addition, after obtaining a nitrogen adsorption isotherm for the entire composite material, either the nitride ceramic or the oxide ceramic of the composite material is dissolved and removed, and a nitrogen adsorption isotherm for either is obtained again, and the measurement can be performed by excluding the nitride ceramic or the oxide ceramic. Note that the pore volume per unit mass of the oxide ceramic when the pore diameter of the composite material is in a different numerical range can also be determined by this method ... can also be determined by the nitrogen adsorption isotherm for the nitride ceramic, s The analysis was performed using the α s Even if there is no clear inflection in the plot and a second straight line cannot be created, it can be determined that the nitride ceramic is non-porous. If it can be confirmed that the nitride ceramic particles are non-porous or that they have no pores within the analysis range, the "pore size, pore volume, and pore surface area of the composite material" can be regarded as the "pore size, pore volume, and pore surface area of the oxide ceramic."
[0030] The ratio of the pore surface area of the composite material 100 having a pore diameter of 2 nm or less to the pore surface area of the composite material 100 having a pore diameter of 10 nm or less by the NLDFT method is 30% or more, and preferably 40% or more, 50% or more, or 60% or more. As described above, when the pore diameter of the pores 11 of the composite material 100 is 2 nm or less, the surface property is similar to that of non-porous oxide ceramics. In detail, for pores having a pore diameter of 2 nm or less, components in the environment such as water vapor fill the micropores (micropore filling) under normal environment (typically in the air). In the composite material 100 having such a configuration, a certain number or more of the pores having a pore diameter of 2 nm or less are occupied by the pores having a pore diameter of 10 nm or less. This makes it possible to efficiently modify the surface of the nitride ceramic 10, and to suppress the inhibition of heat conduction by micropore filling (micropore filling).
[0031] The composite material 100 may have pores 11 with a pore diameter of 10 nm or more. For example, when the composite material 100 and a resin are mixed, it is not difficult to infiltrate the resin into the pores 11 with a pore diameter of 10 nm or more, more preferably 20 nm or more, 50 nm or more, 100 nm or more, or 200 nm or more, so the problem of heat conduction inhibition is small. According to the NLDFT method, the ratio of the pore surface area of the composite material 100 with a pore diameter of 2 nm or less to the pore surface area of the composite material 100 with a pore diameter of 20 nm or less is preferably 30% or more, 40% or more, 50% or more, or 60% or more. The ratio of the pore surface area of the composite material 100 with a pore diameter of 2 nm or less to the pore surface area of the composite material 100 with a pore diameter of 50 nm or less is preferably 30% or more, 40% or more, 50% or more, or 60% or more. The ratio of the surface area of pores in the composite material 100 having a pore diameter of 2 nm or less to the surface area of pores in the composite material 100 having a pore diameter of 100 nm or less is preferably 30% or more, 40% or more, 50% or more, or 60% or more. The ratio of the surface area of pores in the composite material 100 having a pore diameter of 2 nm or less to the surface area of pores in the composite material 100 having a pore diameter of 200 nm or less is preferably 30% or more, 40% or more, 50% or more, or 60% or more.
[0032] The ratio of the surface area of pores in the composite material 100 having a pore diameter of 1 nm or less to the surface area of pores in the composite material 100 having a pore diameter of 2 nm or less according to the NLDFT method is preferably 20% or more, more preferably 30% or more, 40% or more, 50% or more, or 60% or more. With this configuration, the composite material 100 has even smaller pores 11 (micropores) among the pores 11 having a diameter of 2 nm or less. This makes it possible to suppress the inhibition of thermal conduction.
[0033] According to the NLDFT method, the ratio of the surface area of pores in the composite material 100 having a diameter of 5 nm or less to the surface area of pores having a diameter of 10 nm or less is preferably 50% or more, more preferably 60% or more, 70% or more, 80% or more, or 90% or more. With this configuration, the pores 11 having a diameter of 5 nm or less occupy a large number of the surface area of pores having a diameter of 10 nm or less. This allows the surface modification of the nitride ceramic 10 to be efficiently achieved.
[0034] The surface area (m2) of pores with a diameter of 2 nm or less in the composite material 100 per unit mass of the oxide ceramic 20, measured by the NLDFT method, 2 / g) is 10m 2 / g or more is preferable, and 20m 2 / g or more, 30m 2 / g or more, 50m 2 / g or more, 100m 2 The surface area of pores with a pore diameter of 1 nm or less in the composite material 100 per unit mass of the oxide ceramic 20 is preferably 10 m 2 / g or more, 20m 2 / g or more, 30m 2 / g or more, 40m 2 / g or more, 80m 2 When the composite material 100 is in the above-mentioned numerical range, it indicates that the oxide ceramic 20 has a certain amount of pores, that is, the oxide ceramic 20 is not highly densified and preferably exists as an aggregate of a plurality of particles.
[0035] The pore surface area (m2) of the composite material 100 with a pore diameter of 2 nm or less per unit mass of the oxide ceramic 20 in the composite material 100 with a pore diameter of 2 nm or less was calculated by the NLDFT method. 2 Although there is no particular upper limit to the mass ratio of the oxide ceramic 20 adhered to the nitride ceramic 10, it is preferable that the upper limit is 10,000 m / g in order to maintain the strength of the oxide ceramic 20 adhered to the nitride ceramic 10 and to suppress the falling off of the oxide ceramic 20. 2 / g or less is preferable, and 5000m 2 / g or less, 3000m 2 / g or less, 2000m 2 / g or less, 1000m 2 / g or less is more preferable.
[0036] The peak pore diameter in the pore diameter distribution of the composite material 100 by the NLDFT method is preferably 5 nm or less, more preferably 3 nm or less, 2.5 nm or less, 2.2 nm or less, or 2 nm or less, in the differential pore volume distribution. This indicates that the pores 11 of the oxide ceramics 20 are generally composed of small particles of the oxide ceramics 20, that is, the majority of the particles of the oxide ceramics 20 have small particle diameters and are relatively densely assembled. This forms a thin and dense oxide ceramic film on the surface of the nitride ceramics 10, and the surface is efficiently modified. The differential pore volume distribution can be obtained by acquiring a nitrogen adsorption isotherm at -196°C and analyzing it by the NLDFT method. The lower limit of the peak pore diameter in the pore diameter distribution of the composite material 100 is not particularly limited, but is preferably 0.35 nm or more, for example. The lower limit of the pore diameter analysis by nitrogen adsorption is 0.35 nm.
[0037] The pore surface area (m2) of the oxide ceramics 20 measured by the NLDFT method per unit BET surface area of the nitride ceramics in the composite material 100 with a pore diameter of 2 nm or less 2 / m 2 ) is 0.1m 2 / m 2 More than 0.2m is preferable. 2 / m 2 More than 0.5m 2 / m 2 More than 0.7m 2 / m 2 More than 1m 2 / m 2 The above is more preferable. According to this configuration, the oxide ceramic 20 has pores on the nitride ceramic 10 to a certain degree of surface area, that is, the oxide ceramic 20 is not highly densified and is preferably present as an aggregate of multiple particles. In this specification, the term "BET surface area" refers to the specific surface area of a powder (solid) by gas adsorption, which is measured using nitrogen (N 2 The adsorption isotherms measured by a gas adsorption method using 1,2-dichloroethane (1,2-dichloroethane) gas were analyzed by the BET method.
[0038] The pore surface area (m2) of the composite material 100 measured by the NLDFT method per unit BET surface area of the nitride ceramics when the pore diameter of the composite material 100 is 2 nm or less. 2 / m 2 ) is not particularly limited, but from the viewpoint of maintaining the strength of the oxide ceramics 20 attached to the nitride ceramics 10 and suppressing falling off, it is preferable to set the upper limit to 1000 m 2 / m 2 Less than 500m is preferable 2 / m 2 Below, 200m 2 / m 2 Below, 100m 2 / m 2 Below, 50m 2 / m 2 The following is more preferred:
[0039] The pore volume (cm) of the composite material 100 with a pore diameter of 2 nm or less per unit mass of the oxide ceramic 20 obtained by the NLDFT method 3 / g) is 0.01 cm 3 / g or more, preferably 0.02 cm 3 / g or more, 0.03cm 3 / g or more, 0.04cm 3 / g or more, 0.08cm 3 / g or more. With such a pore volume, the surface modification effect of the oxide ceramic 20 is suitably exhibited.
[0040] There is no particular upper limit for the pore volume of the composite material 100, but α s Pore volume (cm) per unit mass of oxide ceramics 20 determined by the 3 / g) is, for example, 10 cm 3 / g or less, preferably 5 cm 3 / g or less, 2cm 3 / g or less, 1cm 3 / g or less, 0.5cm 3 / g or less. With such a pore volume, the strength of the oxide ceramic 20 attached to the nitride ceramic 10 is maintained and falling off is suppressed. s The pore volume by the α method was calculated by obtaining a nitrogen adsorption isotherm at -196°C in the same manner as the analysis by the NLDFT method described above. s It can be obtained by analyzing the α s The surface area can also be calculated using the method.
[0041] The adhesion weight of oxide ceramics 20 per unit BET surface area of nitride ceramics (g / m 2 ) is set to 0.001 g / m from the viewpoint of allowing the oxide ceramics 20 to adhere widely onto the nitride ceramics 10 and to perform suitable surface modification. 2 More than 0.002g / m 2 More than 0.003g / m 2 More than 0.005g / m 2 More than 0.007g / m 2 The deposition weight (g / m) of the oxide ceramic 20 per unit BET surface area of the nitride ceramic is preferably 2 ) is set at 1 g / m from the viewpoint of optimally expressing the thermal conductivity properties of nitride ceramics. 2 Below 0.5g / m 2 Below, 0.1g / m 2 Below 0.05g / m 2 The following is preferred:
[0042] In addition, the deposition volume (nm2) of oxide ceramics per unit BET surface area of nitride ceramics 3 / nm 2 ) is set to 0.2 nm so that the oxide ceramic 20 can be widely attached onto the nitride ceramic 10 and the surface can be suitably modified. 3 / nm 2 or more, 0.5nm 3 / nm 2 Above, 1nm 3 / nm 2 Above, 1.5nm 3 / nm 2 Above, 2nm 3 / nm 2 More preferably, the deposition volume (nm2) of the oxide ceramic 20 per unit BET surface area of the nitride ceramic 3 / nm 2 ) is set to 100 nm from the viewpoint of favorably exhibiting the thermal conductivity characteristics of the nitride ceramic 20. 3 / nm 2 Below, 80nm 3 / nm 2 Below, 50nm 3 / nm 2 Below, 30nm 3 / nm 2 Below, 20nm 3 / nm 2 The following is preferred:
[0043] In some preferred embodiments, the composite material 100 may be used as a powder material, in which the composite material is contained in a powder form. More specifically, the composite material 100 exists in a powder form and is used as a powder material. The powder material may be used, for example, as a filler for a resin member such as a thermally conductive sheet.
[0044] In some preferred embodiments, the composite material 100 is used as a filler for a resin member. Conventionally, when a composite material having pores is used as a filler for a resin member, voids (typically air) remain in the pores in the composite material, which may impair the thermal conductivity of nitride ceramics. On the other hand, for pores with a pore diameter of 2 nm or less, components in the environment such as water vapor fill the micropores under normal conditions (typically in the atmosphere), so that the thermal conductivity impediment caused by the pores is suppressed. In addition, the composite material 100 of this embodiment has a ratio of the surface area of pores with a pore diameter of 2 nm or less to the surface area of pores with a pore diameter of 10 nm or less of the composite material 100 obtained by the NLDFT method of 30% or more. Therefore, by using the composite material disclosed herein as a filler for a resin member, it is possible to suppress the impediment of thermal conductivity.
[0045] When the entire powder material is taken as 100 wt%, the powder material may contain, for example, 80 wt% or more of composite material 100, preferably 85 wt% or more of composite material 100, more preferably 90 wt% or more of composite material 100, even more preferably 95 wt% or more of composite material 100, and particularly preferably 98 wt% or more or 99 wt% or more of composite material 100.
[0046] In this embodiment, the average particle size of the composite material 100 in the powder material is not particularly limited and can be appropriately changed depending on the purpose and mode of use. The average particle size of the composite material 100 in the powder material is typically nano to millimeter size, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the composite material 100 in the powder material is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less. In this specification, the "average particle size" refers to the particle size obtained by the arithmetic average of circle equivalent diameters obtained by image analysis of at least 100 particles in an image obtained using an optical microscope or a scanning electron microscope (SEM).
[0047] In some preferred embodiments, when the separated phase of water and non-polar solvent and the powdered composite material 100 are stirred, 70 wt% or more (hereinafter also referred to as "the majority") of the composite material 100 is present in the aqueous phase, more preferably 75 wt% or more, 80 wt% or more. When the composite material 100 has the above-mentioned properties, it is found that the nitride ceramic surface tends to be modified by the oxide ceramic. That is, in a composite material having such properties, it is found that the oxide ceramic is attached to a certain amount or more of the nitride ceramic surface. The above evaluation (hereinafter also referred to as "water-non-polar solvent preference evaluation") is, for example, first, the powdered composite material, water, and the non-polar solvent are placed in a container (e.g., a glass bottle, etc.) and stirred (e.g., shaken by hand, using a shaker, etc.). After that, the container is left to stand, and it is confirmed whether the majority of the composite material is present in the aqueous phase or the non-polar solvent phase. Such confirmation can be performed by visual inspection. The non-polar solvent used in the water-non-polar solvent preference evaluation can be any of hexane, heptane, octane, nonane, and decane. When evaluating the water-non-polar solvent preference, the solvent and the container of the composite material may be subjected to a dispersion treatment such as ultrasonic dispersion to such an extent that the surface properties are not changed due to the falling off of the oxide ceramics. In addition, the ratio of the composite material in the separated phase of water and non-polar solvent can be determined, for example, by removing either the water phase or the non-polar solvent phase (in other words, separating the water phase and the non-polar solvent phase), drying and removing the solvent of the other phase, measuring the weight of the composite material contained in that phase, and calculating the ratio of the weight to the weight of the total composite material (the weight of the entire composite material put into the container).
[0048] The applications of the composite material disclosed herein are not particularly limited, but it can be suitably used in applications requiring the thermal conductivity properties of nitride ceramics, such as inorganic materials for heat dissipation components (e.g., heat dissipation sheets for electronics applications).
[0049] The method for producing the composite material disclosed herein will be described below. The method for producing the composite material disclosed herein typically includes a resinate attachment step and a resinate decomposition step in this order. However, the method is not limited to this and may include other steps. Here, the method further includes a material preparation step prior to the resinate attachment step. Each step will be described below.
[0050] (1) Material preparation process In the material preparation step, a resinate containing a metal or metalloid as a raw material for the oxide ceramic, a nitride ceramic, and a solvent are prepared. Note that the nitride ceramic is the same as the nitride ceramic of the composite material described above, and therefore a description thereof will be omitted here.
[0051] The average particle size of the nitride ceramics prepared in the material preparation step is not particularly limited, but is, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the nitride ceramics is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less.
[0052] The resinate may be a conventionally known organometallic compound resinate containing at least one element selected from the group consisting of Al, Si, Zr, Ti, Ce, Y, Fe, and Zn. In addition, the resinate is preferably one that forms at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite in the resinate decomposition step described below. More preferably, the resinate contains a compound that forms a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. This allows the oxide ceramics to be formed with a suitable porous structure and to be attached to the surface of the nitride ceramics in the resinate decomposition step described below.
[0053] The metal or metalloid component contained in the resinate is the same as that of the oxide ceramic of the composite material described above, and therefore the description is omitted here. The content of the metal or metalloid component in the resinate may be 70 wt% or less, and preferably 60 wt% or less, 50 wt% or less, 40 wt% or less, or 30 wt% or less, calculated as oxide ceramics. As a result, the content of the metal or metalloid component in the resinate is low, and the oxide forms a suitable porous structure. On the other hand, the content of the metal or metalloid component in the resinate may be 2 wt% or more, and preferably 5 wt% or more, or 10 wt% or more, calculated as oxide.
[0054] The thermal decomposition temperature of the resinate is not particularly limited, but may be 150° C. or higher in the air, and is preferably 200° C. or higher, 300° C. or higher, or 400° C. or higher. The thermal decomposition temperature of the resinate may be 1000° C. or lower in the air, and is preferably 900° C. or lower, 800° C. or lower, or 700° C. or lower.
[0055] The solvent prepared in the material preparation step may be an aqueous solvent or an organic solvent. As the aqueous solvent, water (e.g., pure water, deionized water, etc.) or a mixed solution mainly made of water (e.g., a mixed solution of water and a lower alcohol) can be used. In this specification, a "mixed solution mainly made of water" refers to a mixed solution in which 50 vol% or more of the mixed solution is water. On the other hand, as the organic solvent, alcohols such as methanol and ethanol, ketones such as acetone and methyl ketone, esters such as ethyl acetate, etc. can be used.
[0056] (2) Resinate attachment process In the resinate attachment step, the resinate containing the oxide ceramic prepared in the material preparation step is attached to the nitride ceramic. Here, the process includes sub-steps (2-1) mixing step and (2-2) drying step.
[0057] (2-1) Mixing process In the mixing step, the resinate containing the oxide ceramic, the nitride ceramic, and the solvent are mixed together to obtain a mixture in which the resinate and the nitride ceramic are uniformly present in the solvent.
[0058] In the mixing step, a conventionally known stirring device, mixing device, etc. may be used. The mixing time in the mixing step is not particularly limited as long as the resinate and the nitride ceramics are uniformly present in the mixture. After the mixing step, a dispersion treatment such as ultrasonic dispersion may be performed to more suitably homogenize each component in the mixture.
[0059] The concentration of the nitride ceramic in the mixture is not particularly limited, but if the concentration is too low, it is not preferable from the viewpoint of cost balance. Therefore, the concentration of the nitride ceramic in the mixture is, for example, 10 g / l or more, preferably 100 g / l or more, or 300 g / l or more. On the other hand, if the concentration of the nitride ceramic is too high, there is a risk of the composite material agglomerating. Therefore, the concentration of the nitride ceramic in the mixture is, for example, 50000 g / l or less, preferably 10000 g / l or less, or 3000 g / l or less.
[0060] When calculated as the oxide ceramics in the resinate, the ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the nitride ceramics in the mixture is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. The ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the nitride ceramics in the mixture is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the ratio is too low, the oxide ceramics may not be sufficiently attached to the nitride ceramics to exhibit the functional group increasing effect. On the other hand, if the ratio is too high, the oxide ceramics may be excessively attached to the nitride ceramics, suppressing the expression of the characteristics of the nitride ceramics.
[0061] (2-2) Drying process In the drying step, the mixture obtained in the mixing step is dried to remove the solvent from the mixture, thereby obtaining a dried product in which the resinate is adhered to the surface of the nitride ceramic.
[0062] In the drying step, a conventionally known drying means may be used, for example, a hot air dryer, a low-humid air dryer, a vacuum dryer, various infrared dryers, an electromagnetic induction dryer, a microwave dryer, dry air, etc., or drying promotion means such as air blowing, decompression, heating, etc., may be used alone or in combination. Such means may be appropriately selected depending on the type and amount of the solvent in the mixture.
[0063] The drying temperature in the drying step (such as the set temperature of the drying device) may be appropriately selected depending on the type and amount of the solvent in the mixture, and may be set to, for example, 60° C. to 150° C., typically 80° C. to 120° C. The drying time may also be appropriately selected depending on the type and amount of the solvent in the mixture, and is not particularly limited.
[0064] (3) Resinate decomposition process In the resinate decomposition step, the resinate in the dried material obtained in the drying step is decomposed. As a result, oxide ceramics are generated as an aggregate of multiple particles as a resinate decomposition product. Here, the resinate decomposition step (thermal decomposition of the resinate) is performed by heat treatment. The dried material may be crushed before the resinate decomposition step. This operation can more effectively suppress the aggregation of the composite material after the resinate decomposition step.
[0065] The temperature of the heat treatment in the resinate decomposition step is preferably 800°C or less, 780°C or less, 750°C or less, 720°C or less, or 700°C or less. In this temperature range, sintering of the oxide ceramics is suitably suppressed, and the specific surface area of the oxide ceramics is increased. In other words, the oxide ceramics are prevented from becoming non-porous, and an oxide ceramics having a porous structure can be obtained. On the other hand, the lower limit of the heat treatment temperature is not particularly limited as long as it is equal to or higher than the decomposition temperature of the resinate, and is, for example, 200°C or more, and preferably 250°C or more, 300°C or more, or 350°C or more.
[0066] The atmosphere in the resinate decomposition step is not particularly limited as long as it can decompose the resinate. However, from the viewpoint of suitably removing organic component-derived residues (e.g., carbon, etc.) from the composite material, it is preferable to carry out the step in an oxidizing atmosphere (e.g., air, etc.).
[0067] The time for which the heat treatment is held at the top temperature in the resinate decomposition step is not particularly limited as long as the resinate can be completely decomposed, but the heat treatment can be carried out for, for example, about 0.1 to 2 hours.
[0068] After the heat treatment, the obtained composite material may be subjected to a crushing treatment. This makes the composite material in a powder form. Therefore, the obtained composite material can be suitably used as a powder material. The method for crushing the composite material in the crushing step is not particularly limited, and a conventionally known method can be used.
[0069] As described above, specific aspects of the technology disclosed herein include those described in the following sections.
[0070] Item 1: A composite material comprising a nitride ceramic and a metal or semi-metal oxide ceramic adhered to a surface of the nitride ceramic, wherein the oxide ceramic is an aggregate of a plurality of particles, the particles of the oxide ceramic have pores with a pore diameter of 2 nm or less between them, and the ratio of the surface area of pores of the composite material with a pore diameter of 2 nm or less to the surface area of pores of the composite material with a pore diameter of 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method, is 30% or more.
[0071] Item 2: The composite material according to item 1, wherein the ratio of the surface area of pores of the composite material having a pore diameter of 1 nm or less to the surface area of pores of the composite material having a pore diameter of 2 nm or less is 20% or more.
[0072] Item 3: The pore surface area per unit mass of the oxide ceramic in the composite material having a pore diameter of 2 nm or less is 10 m 2 Item 3. The composite material according to item 1 or 2, wherein the elastic modulus is 1 / g or more.
[0073] Item 4: The composite material according to any one of Items 1 to 3, wherein the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.
[0074] Item 5: The composite material according to any one of Items 1 to 4, wherein the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia.
[0075] Item 6: The composite material according to any one of Items 1 to 5, wherein the nitride ceramic contains at least one compound or mixture selected from the group consisting of aluminum nitride and boron nitride.
[0076] Item 7: A powder material comprising the composite material according to item 1 or 2 in powder form.
[0077] Item 8: The composite material according to any one of Items 1 to 7, wherein when a separate phase of water and a nonpolar solvent is stirred with the composite material, 70 wt % or more of the composite material is present in the aqueous phase.
[0078] Item 9: The composite material according to any one of Items 1 to 8, which is a filler of a resin material.
[0079] Item 10: A method for producing a composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, the method comprising the steps of: attaching a resinate containing a metal or metalloid, which is a raw material for the oxide ceramic, to the nitride ceramic; and decomposing the resinate; wherein in the composite material, the oxide ceramic is an aggregate of a plurality of particles, and between the particles of the oxide ceramic there are pores having a pore diameter of 2 nm or less, and the proportion of the pore surface area of the composite material having a pore diameter of 2 nm or less to the pore surface area of the composite material having a pore diameter of 10 nm or less determined by a nonlocalized density functional (NLDFT) method is 30% or more.
[0080] Item 11: The method for producing a composite material according to Item 10, wherein the decomposition step comprises heat treatment at 800° C. or less.
[0081] Test examples relating to the technology disclosed herein will be described below, but such test examples are not intended to limit the technology.
[0082] <Preparation of evaluation samples> In this test example, evaluation samples according to the following Examples 1 to 12 were prepared.
[0083] (Example 1) First, 10 ml of ethanol was added to 7.0 g (0.5 g in terms of silica) of an ethanol solution of tris(2-ethylhexanoic acid)ethoxysilane as a resinate (7.15 wt% in terms of silica, thermal decomposition temperature in air 350°C) and dissolved. 9.5 g of nonporous boron nitride powder (Tokuyama Corporation, S03) was added thereto and stirred. Then, a dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. This resulted in a composite material in which 5 wt % of amorphous silica particles were attached to boron nitride. The composite material thus obtained was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 1.
[0084] (Example 2) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 700°C, at a heating rate of 5°C / min for 1 hour. As a result, a powdered composite material was obtained as an evaluation sample according to Example 2, in which 5 wt% of amorphous silica particles were attached to boron nitride.
[0085] (Example 3) The procedure was the same as in Example 2, except that silicon resinate (Si 13%, silica equivalent 27.8 wt%, decomposition temperature in air 617°C) was used as the Si resinate, and 12 ml of ethanol was added to 1.80 g of the Si resinate (silica equivalent 0.5 g) and dissolved. As a result, a powdered composite material was obtained as an evaluation sample according to Example 3, in which 5 wt% of amorphous silica particles were attached to the boron nitride.
[0086] (Example 4) The procedure was the same as in Example 3, except that 0.36 g of Si resinate (0.1 g in terms of silica) and 9.9 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample according to Example 4, in which 1 wt% of amorphous silica particles were attached to the boron nitride.
[0087] (Example 5) The procedure was the same as in Example 3, except that 0.72 g of Si resinate (0.2 g in terms of silica) and 9.8 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 5, in which 2 wt% of amorphous silica particles were attached to the boron nitride.
[0088] (Example 6) The procedure was the same as in Example 3, except that 3.60 g of Si resinate (1.0 g in terms of silica) and 9.0 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample according to Example 6, in which 10 wt% of amorphous silica particles were attached to the boron nitride.
[0089] (Example 7) First, 12 ml of ethanol was added to 1.08 g (0.2 g in terms of alumina) of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemicals) (18.47 wt% in terms of alumina, decomposition temperature in air 295°C) as Al resinate, and dissolved. 19.8 g of non-porous aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) was added thereto and stirred. Then, dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. As a result, a composite material in which 1 wt % of amorphous alumina particles were attached to aluminum nitride was obtained. The obtained composite material was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 7.
[0090] (Example 8) The procedure was the same as in Example 7, except that 5.4 g of Al resinate (1.0 g in terms of alumina) and 19.0 g of aluminum nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 8, in which 5 wt% of amorphous alumina particles were attached to the aluminum nitride.
[0091] (Example 9) The powdered composite material according to Example 8, which had been fired and crushed, was further fired in an air atmosphere at a temperature of 650°C, at a heating rate of 10°C / min, for 0.5 hours. This resulted in a composite material in which 5 wt% of γ-alumina particles were attached to aluminum nitride. The resulting composite material was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 9.
[0092] (Example 10) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 900°C, at a heating rate of 5°C / min for 1 hour. This resulted in a powdered composite material as an evaluation sample according to Example 10 in which 5 wt% of amorphous silica particles were attached to boron nitride.
[0093] (Example 11) The boron nitride powder (S03, manufactured by Tokuyama Corporation) used in Example 1 was used as an evaluation sample without adhering oxide ceramics.
[0094] (Example 12) The aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) used in Example 7 was used as it was as an evaluation sample without adhering oxide ceramics.
[0095] <Evaluation test> The above composite material was subjected to the following evaluation tests.
[0096] (1) Pore analysis Each sample was pretreated in a vacuum at 250°C for 1 hour, and then subjected to a specific surface area measurement device (model number: Belsorp-max (registered trademark)) manufactured by Microtrack-Bell, Inc., to obtain a nitrogen adsorption isotherm at -196°C. The following analysis was then performed using analysis software (BELLMaster Version 7.3.2.0).
[0097] (1-1) Specific surface area analysis by BET method In each of Examples 1 to 10, the specific surface area of the nitride ceramics was analyzed by the BET method using the above-mentioned analysis software. 2 / g, the adhesion weight of oxide ceramics per unit BET surface area of nitride ceramics (g / m 2 ) and the deposition volume of oxide ceramics per unit BET surface area of nitride ceramics (nm 3 / nm 2) was calculated. Similarly, the BET specific surface areas of the nitride ceramics of Examples 11 and 12 measured by this method were taken as the values of the boron nitride powder and aluminum nitride powder used in each Example. The BET specific surface area values of the boron nitride powder and aluminum nitride powder used in each Example were 1.3 m 2 / g, 3.2m 2 / g. The densities of the attached oxide ceramics, amorphous alumina, γ-alumina, and amorphous silica, were 3.0 g / cm3, respectively. 3 , 3.7g / cm 3 , 2.2g / cm 3 The results are shown in Table 1.
[0098] [Table 1]
[0099] (1-2) Pore volume analysis using NLDFT method In each of Examples 1 to 10, the pore size distribution was created under the following conditions using the above-mentioned analysis software. Curve Interpolation: Cubic Spline Curve Model: Cylinder Adsorbent: Metal oxide Fitting method: Tikhonov normalization, smoothing Using the obtained pore size distribution, the pore volume (cm) per unit mass of the composite material with a pore size of 2 nm or less was calculated. 3 The pore volume per unit mass of the oxide ceramics (cm 3 / g) and the pore volume per unit BET surface area of the powder consisting of nitride ceramic particles in the composite material (cm 3 / m 2 ) was also calculated. Furthermore, the pore diameter of the maximum peak in the differential pore volume distribution was calculated. The results are shown in Table 1. In Example 10, the obtained nitrogen adsorption isotherm was analyzed by the above-mentioned analysis software. s As a result of the analysis using the method, α sThere was no clear inflection in the plot, so a second straight line could not be created. Therefore, Example 10 was determined to be non-porous, and is therefore underlined.
[0100] (1-3) Pore surface area analysis using NLDFT method Using the pore size distribution obtained by the analysis of (1-2) above, the pore surface area (m) per unit mass of the composite material with pore sizes of 200 nm or less, 100 nm or less, 50 nm or less, 20 nm or less, 10 nm or less, 5 nm or less, 2 nm or less, and 1 nm or less was calculated for Examples 1 to 9. 2 The pore volume per unit mass of the oxide ceramics (m 2 / g) and the pore volume per unit BET surface area of the powder consisting of nitride ceramic particles in the composite material (m 2 / m 2 The results are shown in Tables 2-1 and 2-2.
[0101] In addition, the percentages (%) of the pore surface area per pore diameter based on the pore diameter distribution of the composite material were calculated for "pores with diameters of 200 nm or less and pores with diameters of 2 nm or less," "pores with diameters of 100 nm or less and pores with diameters of 2 nm or less," "pores with diameters of 50 nm or less and pores with diameters of 2 nm or less," "pores with diameters of 20 nm or less and pores with diameters of 2 nm or less," "pores with diameters of 1 ... nm or less," and "pores with diameters of 10 nm or less and pores with diameters of 5 nm or less." The results are shown in Table 3.
[0102] [Table 2-1]
[0103] [Table 2-2]
[0104] [Table 3]
[0105] (1-4)α s Analysis by the method In each of Examples 1 to 12, α was measured using the above-mentioned analysis software. s A plot was created. s When creating the plot, the criterion α s For the curves, silica was selected for Examples 1-6 and 10, alumina for Examples 7-9 and 12, and GCB (graphitized carbon black) for Example 11. The obtained α s From the plot, an approximate line passing through the origin and a line with a high α s From the plot of the area, an approximation line with a smaller slope was created, and the specific surface area, pore volume, and external surface area of the composite material were calculated from the above two approximation lines. s For samples where there was no clear inflection in the plot and no second straight line could be created, the samples were judged to be non-porous, and only the specific surface area was calculated. α The pore surface area, the average pore diameter (nm) of the oxide ceramics, the contribution rate (%) of the pores to the increase in specific surface area, and the porosity (%) of the oxide ceramics were calculated. R α = (α of the composite material s specific surface area) / (BET specific surface area of nitride ceramics)...Equation (a) Pore surface area = α of composite material s Specific surface area – the external surface area per unit mass of a composite material… Equation (b) Average pore diameter of oxide ceramics (nm) = 4 × pore volume per unit mass of oxide ceramics / pore surface area per unit mass of oxide ceramics...Equation (c) Contribution rate of pores to the increase in specific surface area (%) = (pore surface area per unit mass of composite material) / (α of composite material s specific surface area – BET specific surface area of nitride ceramic in composite material) × 100... formula (d) Porosity of oxide ceramics (%) = Pore volume per unit mass of oxide ceramics (cm 3 / g) / {Oxide ceramics pore volume per unit mass of oxide ceramics (cm 3 / g) + (1 / density of oxide ceramics (g / cm 3 ))}×100...Equation (e) Regarding the "density of oxide ceramics" in formula (e), the densities of amorphous alumina, γ-alumina, and amorphous silica are 3.0 g / cm3. 3 , 3.7g / cm 3 , 2.2g / cm 3 The pore surface area and pore volume were calculated as the values per unit mass of the composite material, the values per unit mass of the oxide ceramic, and the values per unit BET surface area of the nitride ceramic in the composite material. The results are shown in Table 4.
[0106] [Table 4]
[0107] As shown in Table 1, in Examples 1 to 9, the BET specific surface area of the nitride ceramic in the composite material after the oxide ceramic was attached was increased compared to the BET specific surface area of the nitride ceramic before the oxide ceramic was attached. On the other hand, in Example 10, the increase in the BET specific surface area of the nitride ceramic in the composite material before and after the oxide ceramic was attached was not observed very much. In addition, when comparing Examples 1 and 10, the BET specific surface area of the nitride ceramic in Example 10 was smaller than that of Example 1, even though the oxide attachment weight was the same. This suggests that the oxide ceramic attached to the nitride ceramic in Example 10 is non-porous, that is, the oxide ceramic does not exist as an aggregate of multiple particles.
[0108] As shown in Table 2-2, it was confirmed that Examples 1 to 9 had pores with a pore diameter of 2 nm or less. Furthermore, as shown in Table 3, in Examples 1 to 9, the ratio of the pore surface area of the composite material with a pore diameter of 2 nm or less to the pore surface area of the composite material with a pore diameter of 10 nm or less (the item "2 nm or less / 10 nm or less" in Table 3) was 30% or more in all examples. From this, it can be seen that in Examples 1 to 9, pores of 2 nm or less are suitably formed by the oxide ceramics adhered to the nitride ceramics. Therefore, it is considered that in the composite materials of Examples 1 to 9, functional groups are imparted to the surface of the nitride ceramics, and the surface is suitably modified. On the other hand, in Example 10, as described above, α s Analysis by the method confirmed that the material was non-porous.
[0109] Furthermore, as shown in Table 3, in Examples 1 to 9, the ratio of the surface area of pores of the composite material with a pore diameter of 1 nm or less to the surface area of pores of the composite material with a pore diameter of 2 nm or less (the item "1 nm or less / 2 nm or less" in Table 3) was 20% or more in all Examples. This shows that in Examples 1 to 9, the oxide ceramics adhered to the nitride ceramics favorably forms pores of 1 nm or less, which are even smaller than the pores of 2 nm or less.
[0110] As shown in Table 2-2, in Examples 1 to 9, the surface area of pores with a pore diameter of 2 nm or less in the composite material per unit mass of the oxide ceramic is 10 m 2 / g or more. Therefore, it is considered that in the composite materials of Examples 1 to 9, the oxide ceramic is present as an aggregate of a plurality of particles.
[0111] As shown in Table 4, in each of Examples 1 to 9, the pore volume (cm ) per unit mass of the oxide ceramic 20 3 / g) is 0.5 cm 3 / g or less. This shows that the oxide ceramics adhered to the composite materials according to Examples 1 to 9 maintain a strength sufficient to prevent them from falling off.
[0112] (2) Water-nonpolar solvent preference evaluation For each of Examples 1 to 12, approximately 200 mg of sample was placed in a glass bottle, 20 ml of pure water was added, the bottle was capped, and the bottle was shaken by hand. The bottle was then opened, 20 ml of n-hexane as a non-polar solvent was added, the bottle was capped again, and the bottle was shaken by hand. The glass bottle was then left to stand, and it was visually confirmed whether the majority of the sample (i.e., 70% or more) was present in the water phase or the non-polar solvent phase (hexane phase). For Examples 8 to 9 and 12, evaluation was performed in the same manner as described above, except that n-decane was used instead of n-hexane. The results are shown in Table 5.
[0113] [Table 5]
[0114] As shown in Table 5, it was confirmed that the majority of all samples in Examples 1 to 9 existed in the aqueous phase. This shows that the nitride ceramic surface was modified by the oxide ceramic, that is, the oxide ceramic was attached to a certain amount of the nitride ceramic surface. On the other hand, it was confirmed that the majority of the samples in Examples 10 and 11 existed in the non-polar solvent phase. Note that Example 12 was classified as "unclear" because, to the naked eye, the sample existed throughout the entire solvent, and it was not clear whether the majority of the sample existed in the aqueous phase or the non-polar solvent phase (n-decane phase).
[0115] (3) Surface morphology observation Each of Examples 1 to 12 was observed using a field emission scanning electron microscope (FE-SEM) manufactured by Hitachi High-Technologies Corporation. Backscattered electron images of some of the Examples are shown in Figures 2 to 9. Figure 2 is an FE-SEM image (50,000x) of Example 1. Figure 3 is an FE-SEM image (50,000x) of Example 2. Figure 4 is an FE-SEM image (50,000x) of Example 3. Figure 5 is an FE-SEM image (100,000x) of Example 8. Figure 6 is an FE-SEM image (100,000x) of Example 9. Figure 7 is an FE-SEM image (50,000x) of Example 10. Figure 8 is an FE-SEM image (50,000x) of Example 11. Figure 9 is an FE-SEM image (100,000x) of Example 12.
[0116] As shown in Figs. 8 and 9, the nitride ceramics without oxide ceramics were confirmed to have no irregularities on the surface and were non-porous. On the other hand, as shown in Figs. 2 to 6, in Examples 1 to 3, 8 and 9, fine irregularities were observed on the surface of the composite material, and it was confirmed that the oxide ceramics were attached to the surface of the nitride ceramics as an aggregate of multiple particles and had a porous structure, and similarly, the surface exposure of the nitride ceramics was confirmed. Although not shown here, the adhesion of the oxide ceramics as an aggregate of multiple particles, the formation of pores, and the surface exposure of the nitride ceramics were also confirmed in Examples 4 to 7. In Examples 1 to 9, by having a portion where the nitride ceramics is exposed on a part of the surface of the composite material, the thermal conductivity of the nitride ceramics can be suitably expressed from the exposed portion. Similarly, it is considered that other properties of the nitride ceramics can be expressed by such a configuration.
[0117] As shown in FIG. 7, in Example 10 where the oxide ceramics were highly densified, it was confirmed that the oxide ceramics were spherical on the (0001) plane (FIG. 7) of the nitride ceramics (boron nitride), which is stable and has few functional groups. This is believed to be because the oxide ceramics were repelled by the (0001) plane of the boron nitride during the densification process by sintering the oxide ceramics, resulting in the spherical shape shown in FIG. 7. When the oxide ceramics exist in a spherical state as shown in FIG. 7, the oxide ceramics tend to easily fall off from the surface of the nitride ceramics. On the other hand, in Example 10, it was confirmed that the oxide ceramics were concentrated in a band shape on the end face of the nitride ceramics (lower right of FIG. 7). This is believed to be because the end face of the boron nitride constituting the nitride ceramics is an area with many functional groups compared to the (0001) plane, and has a high affinity with the oxide ceramics. In addition, when the oxide ceramics are concentrated on the end face of the nitride ceramics as shown in Example 10 (FIG. 7), it is not preferable because it inhibits the thermal conduction of the nitride ceramics. Moreover, the surface of the nitride ceramic is excessively exposed, which is undesirable since there is a risk of the nitride ceramic reacting with water vapor.
[0118] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]
[0119] 10. Nitride Ceramics 11 Pore 12 Surface exposure 20 Oxide Ceramics 100 Composite materials
Claims
1. A composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, The oxide ceramic is an aggregate of a plurality of particles, The oxide ceramic has pores between the particles having a pore diameter of 2 nm or less, A composite material, wherein the proportion of the surface area of pores of the composite material having a pore diameter of 2 nm or less to the surface area of pores of the composite material having a pore diameter of 10 nm or less, as determined by a nonlocalized density functional (NLDFT) method, is 30% or more.
2. The proportion of the pore surface area of the composite material having a pore diameter of 1 nm or less to the pore surface area of the composite material having a pore diameter of 2 nm or less is 20% or more.
3. A composite material according to claim 1 or 2.
3. The pore surface area per unit mass of the oxide ceramic in the composite material having a pore diameter of 2 nm or less is 10 m 2 / g or more; 3. A composite material according to claim 1 or 2.
4. The oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.
3. A composite material according to claim 1 or 2.
5. The oxide ceramic comprises a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia; 3. A composite material according to claim 1 or 2.
6. The nitride ceramic contains at least one compound or mixture selected from the group consisting of aluminum nitride and boron nitride.
3. A composite material according to claim 1 or 2.
7. The composite material according to claim 1 or 2 is in powder form. powder material.
8. 3. The composite material according to claim 1, wherein when the composite material is mixed with a separate phase of water and a non-polar solvent, 70 wt % or more of the composite material is present in the aqueous phase.
9. A filler for resin materials, 3. A composite material according to claim 1 or 2.
10. 1. A method for producing a composite material comprising a nitride ceramic and a metal or metalloid oxide ceramic attached to a surface of the nitride ceramic, comprising the steps of: A step of adhering a resinate containing a metal or semi-metal that is a raw material of the oxide ceramic to the nitride ceramic; and decomposing the resinate, In the composite material, the oxide ceramic is an aggregate of a plurality of particles, The oxide ceramic has pores between the particles having a pore diameter of 2 nm or less, The ratio of the pore surface area of the composite material having a pore diameter of 2 nm or less to the pore surface area of the composite material having a pore diameter of 10 nm or less, which is determined by a nonlocalized density functional (NLDFT) method, is 30% or more. Manufacturing methods for composite materials.
11. In the decomposition step, heat treatment is performed at 800° C. or less. A method for producing the composite material according to claim 10.
Citation Information
Patent Citations