Composite magnetic material, powder core, and power choke coil
A composite magnetic material with amphiphilically coated inorganic insulating particles and a thermosetting resin addresses the challenge of maintaining high relative magnetic permeability and withstand voltage, enhancing performance in powder magnetic cores and power choke coils.
Patent Information
- Application Number
- JP2023056700
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing composite magnetic materials face a challenge in maintaining high relative magnetic permeability while improving withstand voltage, as the addition of electrically insulating components often leads to agglomeration and reduced filling rates of soft magnetic alloy particles.
A composite magnetic material comprising iron-based soft magnetic alloy particles, inorganic insulating particles coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group, and a thermosetting resin is used, where the insulating particles are dispersed to prevent agglomeration and enhance filling rates, thereby improving both relative magnetic permeability and withstand voltage.
The solution effectively maintains high relative magnetic permeability and significantly enhances withstand voltage, making it suitable for applications in powder magnetic cores and power choke coils.
Smart Images

Figure 2024143808000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composite magnetic material, a powder magnetic core, and a power choke coil, and more particularly to a composite magnetic material, a powder magnetic core including a hardened material of the composite magnetic material, and a power choke coil. [Background technology]
[0002] Patent Document 1 discloses a composite magnetic body that contains, for example, a metal magnetic powder and a thermosetting resin, and the filling rate of the metal magnetic powder is 65% by volume to 90% by volume. It also describes that the composite magnetic body may further contain an electrically insulating material other than the thermosetting resin, and that the electrically insulating material is in the form of plate-like or needle-like particles. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-305108 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a composite magnetic material capable of improving voltage resistance while suppressing a decrease in relative permeability.
[0005] Another object of the present disclosure is to provide a powder magnetic core and a power choke coil that can improve voltage resistance while suppressing a decrease in relative permeability. [Means for solving the problem]
[0006] A composite magnetic material according to an embodiment of the present disclosure includes iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. The surfaces of the inorganic insulating particles are coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. The hydrophobic group has a hydrocarbon chain. The hydrophilic group includes at least one of a phosphate group and a phosphate salt.
[0007] The powder magnetic core of the present disclosure contains a cured product of the composite magnetic material.
[0008] The power choke coil of the present disclosure includes a hardened composite magnetic material and a coil conductor, the coil conductor being covered by the hardened composite magnetic material. Effect of the Invention
[0009] According to the present disclosure, there is an advantage that the withstand voltage can be improved while suppressing a decrease in relative permeability. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a molded body including a composite magnetic material according to an embodiment. [Diagram 2] Fig. 2A is a schematic exploded perspective view showing an example of a magnetic element including the powder magnetic core according to the embodiment, and Fig. 2B is a schematic perspective view showing an example of a magnetic element including the powder magnetic core in Fig. 2A. [Diagram 3] Fig. 3A is a cross-sectional view taken along line XX showing an example of a power choke coil according to an embodiment of the present invention, and Fig. 3B is a perspective view showing an outline of the power choke coil according to the embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view showing a modification of the power choke coil of the above embodiment. [Diagram 5] FIG. 5 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 2, and Example 1. [Figure 6] FIG. 6 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 3, and Example 2. [Figure 7] FIG. 7 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 4, Example 3, and Example 4. [Figure 8] FIG. 8 is a graph showing the relationship between the magnetic field and the relative permeability in Comparative Example 1, Comparative Example 5, and Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] 1. Overview Hereinafter, one embodiment of the present disclosure will be described. Note that the following embodiment is merely one of various embodiments of the present disclosure. The following embodiment can be modified in various ways depending on the design as long as the object of the present disclosure can be achieved.
[0012] The composite magnetic material of the present embodiment contains iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. The surface of each inorganic insulating particle is coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. The hydrophobic group has a hydrocarbon chain. The hydrophilic group has at least one of a phosphoric acid group and a phosphate salt.
[0013] According to the composite magnetic material of the present embodiment, even if the composite magnetic material contains inorganic insulating particles, which are an electrically insulating component, it is possible to improve the withstand voltage while suppressing a decrease in relative permeability. The reason for this is presumed to be as follows. However, the present embodiment is not bound by the explanation of the reasons below.
[0014] Conventionally, when a component having electrical insulation is blended in a composite magnetic material, the component having electrical insulation tends to aggregate in the compact, which reduces the filling rate of the soft magnetic alloy particles and the like, and as a result, the relative magnetic permeability of the compact tends to decrease. Furthermore, the aggregation of the component having electrical insulation tends to reduce the withstand voltage. In contrast, the inorganic insulating particles of this embodiment are coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. Specifically, the components on the surface of the inorganic insulating particles are bound to at least one of the phosphoric acid group and the phosphate salt, which are hydrophilic groups, by acid-base interaction, and the amphiphilic molecules are adsorbed on the surface of the inorganic insulating particles. Then, on the opposite side of the adsorption side (i.e., the side where the hydrophilic group is adsorbed) on the surface of the inorganic insulating particles, a hydrocarbon chain, which is a hydrophobic group, exists. Therefore, the inorganic insulating particles are less likely to aggregate with each other. Since the inorganic insulating particles are less likely to aggregate and are easily dispersed in the compact of the composite magnetic material, it is easier to increase the filling rate of the iron-based soft magnetic alloy particles in the hardened product of the composite magnetic material. It is considered that when the filling rate of the iron-based soft magnetic alloy particles is increased, the proportion of the iron-based soft magnetic alloy particles that have an effect on the magnetic force increases relatively, and therefore the relative permeability can be improved. Furthermore, the inorganic insulating particles coated with amphiphilic molecules are interposed between the iron-based soft magnetic alloy particles in a state in which they are less likely to aggregate with each other in the hardened composite magnetic material. Therefore, the electrical resistivity of the hardened composite magnetic material can be increased. It is considered that this can improve the insulation resistance, i.e., the withstand voltage, of the molded body made from the composite magnetic material.
[0015] The composite magnetic material of the present embodiment can be hardened to form a hardened product, and since it has excellent relative magnetic permeability and voltage resistance as described above, it can be suitably used to produce electronic components such as powder cores and magnetic elements such as power choke coils.
[0016] 2.Details The composite magnetic material, the powder magnetic core, and the power choke coil according to this embodiment will be described in detail below.
[0017] (1) Composite magnetic material As already described, the composite magnetic material of the present embodiment contains iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. Details of the components that can be contained in the composite magnetic material will be described.
[0018] (Iron-based soft magnetic alloy particles) The iron-based soft magnetic alloy particles have electrical conductivity and are dispersed in the composite magnetic material.
[0019] The iron-based soft magnetic alloy particles are soft magnetic alloy particles containing iron (Fe) as the main atom. Here, the main atom refers to the atom that has the highest mass ratio in terms of mass among the atoms contained in the soft magnetic alloy particles. For example, it is preferable that the iron atom is 50 mass% or more of the mass of all atoms contained in the iron-based soft magnetic alloy particles.
[0020] The iron-based soft magnetic alloy constituting the iron-based soft magnetic alloy particles can be an alloy having an appropriate composition, and may contain at least one atom selected from the group consisting of silicon (Si), chromium (Cr), and aluminum (Al) as an atom other than iron, for example. However, the atom other than iron is not limited to the above.
[0021] The soft magnetic alloy particles are particles of an alloy having soft magnetism in a particulate form. In the present disclosure, the particulate form of the soft magnetic alloy includes the particulate form of the soft magnetic alloy. The particulate form of the soft magnetic alloy particles can be determined by measuring the particle diameter and checking whether the particle diameter is 100 μm or less. The average particle diameter of the iron-based soft magnetic alloy particles in the present disclosure means the median diameter D50 (50% particle diameter). The average particle diameter of the iron-based soft magnetic alloy particles is obtained by measuring the particle size distribution of the iron-based soft magnetic alloy particles by a laser diffraction / scattering method and calculating the volume-based particle diameter that is 50% of the integrated value obtained from the particle size distribution. The average particle diameter of the iron-based soft magnetic alloy particles is, for example, 3 μm or more and 40 μm or less. When the average particle diameter of the iron-based soft magnetic alloy particles is within this range, it is easy to realize a high filling rate of the iron-based soft magnetic alloy particles in the compact of the composite magnetic material. In addition, when the average particle size of the iron-based soft magnetic alloy particles is 40 μm or less, even if the compact made of the composite magnetic material is used in a high frequency band, the loss in the compact (e.g., a magnetic core) can be reduced, and in particular, the overcurrent loss can be reduced. In addition, the iron-based soft magnetic alloy particles can include alloy particles of a plurality of particle groups each having a different particle size distribution. In this case, it is easier to increase the filling rate of the iron-based soft magnetic alloy in the compact of the composite magnetic material. As an example, the iron-based soft magnetic alloy particles may include alloy particles (A1) of a particle group having an average particle size of 3 μm or more and 20 μm or less, and alloy particles (A2) of a particle group having an average particle size of 20 μm or more and 40 μm or less. However, the average particle size of the iron-based soft magnetic alloy particles is not limited to the above.
[0022] Specific examples of iron-based soft magnetic alloys include soft magnetic iron-silicon (Fe-Si) alloys, soft magnetic iron-aluminum (Fe-Al) alloys, soft magnetic iron-aluminum-silicon (Fe-Al-Si) alloys, soft magnetic iron-silicon-chromium (Fe-Si-Cr) alloys, soft magnetic iron-chromium (Fe-Cr) alloys, soft magnetic iron-nickel (Fe-Ni) alloys, soft magnetic iron-silicon-boron (Fe-Si-B) alloys, soft magnetic iron-nitrogen (Fe-N) alloys, soft magnetic iron-carbon (Fe-C) alloys, soft magnetic iron-boron (Fe-B) alloys, soft magnetic iron-phosphorus (Fe-P) alloys, permendur (Fe-Co), soft magnetic iron-cobalt-vanadium (Fe-Co-V) alloys, Fe-based amorphous alloys, Fe-based nanocrystalline alloys, and the like.
[0023] The ratio of the iron-based soft magnetic alloy particles to the total solid content of the composite magnetic material is preferably 89% by mass or more and 99% by mass or less. If it is 89% by mass or more, it is possible to prevent the saturation magnetic flux density from decreasing when a compact (e.g., a magnetic core) is produced from the composite magnetic material. Also, if it is 99% by mass or less, it is easy to bond the iron-based soft magnetic alloy particles to each other, and it is easy to maintain the shape of the magnetic core. In the present disclosure, the total solid content of the composite magnetic material refers to the total amount of components excluding volatile components, such as solvents, among the components that can be contained in the composite magnetic material.
[0024] The iron-based soft magnetic alloy particles can be produced by an appropriate method, such as mechanical pulverization, molten metal powdering, physical pulverization, and chemical pulverization. Examples of mechanical pulverization include stamp milling, ball milling, and hammer milling. Examples of molten metal powdering include high-pressure water spraying (water atomization), ultra-high-pressure water spraying, gas atomization (gas atomization), rotating electrode, and vacuum spraying. Examples of physical or chemical pulverization include electrolysis, gas reduction, solid reduction, carbonyl, hydride decomposition, evaporation condensation, and amalgamation. However, the method of producing the iron-based soft magnetic alloy particles is not limited to the above-mentioned method. The iron-based soft magnetic alloy particles may be surface-treated in advance with an appropriate dispersant, modifier, or the like.
[0025] (Inorganic insulating particles) The inorganic insulating particles have electrical insulation properties. Specifically, the inorganic insulating particles are particles made of an inorganic material having electrical insulation properties. In this embodiment, the inorganic insulating particles are coated on the surface with amphiphilic molecules having a hydrophobic group and a hydrophilic group. Note that the inorganic material referred to here does not include the above-mentioned iron-based soft magnetic alloy.
[0026] An amphiphilic molecule is a compound having a hydrophobic group and a hydrophilic group. In this embodiment, the hydrophobic group comprises a hydrocarbon chain. The hydrophilic group comprises at least one of a phosphate group and a phosphate salt. The hydrocarbon chain in the hydrophilic group is a hydrocarbon group in which the hydrocarbons are linked in a linear or branched manner. The amphiphilic molecule may further have a group other than the above-mentioned hydrocarbon group as a hydrophobic group, and may further have a group other than a phosphate group and a phosphate salt as a hydrophilic group.
[0027] In the present embodiment, the inorganic insulating particles may be present between the iron-based soft magnetic alloy particles in the hardened composite magnetic material. That is, the inorganic insulating particles may be present in the hardened composite magnetic material in a dispersed state so that the iron-based soft magnetic alloy particles are unlikely to come into contact with each other. Therefore, in the hardened composite magnetic material, the inorganic insulating particles may contribute to improving the withstand voltage.
[0028] In the present disclosure, the inorganic insulating particles being particulate also includes being in powder form (powder). In addition, the average particle size of the inorganic insulating particles in the present disclosure means the median diameter D50 (50% particle size) as in the case of iron-based soft magnetic alloy particles. Specifically, the average particle size of the inorganic insulating particles is obtained by measuring the particle size distribution of the inorganic insulating particles by a laser diffraction / scattering method and calculating the volume-based particle size that is 50% of the integrated value obtained from the particle size distribution. The average particle size of the inorganic insulating particles is preferably 0.8 μm or more and 4 μm or less. In this case, the relative permeability and withstand voltage of the molded body can be further improved.
[0029] It is preferable that the average particle size of the inorganic insulating particles and the average particle size of the iron-based soft magnetic alloy particles satisfy the following relationship. Ins , the average particle size of the iron-based soft magnetic alloy particles is D Cond When expressed as D Ins / D Cond It is preferable that the ratio represented by the following formula (1) is satisfied.
[0030] 0.09≦D Ins / D Cond ≦0.5 (1) The above ratio D Ins / D Cond If the ratio D is 0.09 or more, the inorganic insulating particles are more likely to penetrate and intervene between the iron-based soft magnetic alloy particles in the hardened composite magnetic material, and the packing rate of the iron-based soft magnetic alloy particles is more likely to be increased. Therefore, the relative permeability of the hardened material is more likely to be increased. Ins / D Cond If D is 0.5 or less, the withstand voltage can be further improved while maintaining a high filling rate of the iron-based soft magnetic alloy particles in the hardened composite magnetic material. Ins / D Cond It is more preferable that the ratio is 0.2 or more.
[0031] In the composite magnetic material, when the volume of the iron-based soft magnetic alloy particles is 100 (volume %), the ratio of the inorganic insulating particles to the total volume of the iron-based soft magnetic alloy particles is preferably 1.3 volume % or more and 4.0 volume % or less. When the ratio of the inorganic insulating particles is within the above range, the filling property of the iron-based soft magnetic alloy particles in the composite magnetic material can be improved. Therefore, the relative permeability of the compact of the composite magnetic material can be improved, and the withstand voltage can also be improved.
[0032] The inorganic material constituting the inorganic insulating particles can be an inorganic component having suitable insulating properties. The inorganic material includes at least one selected from the group consisting of talc (hydrated magnesium silicate), silica (silicon oxide), alumina (aluminum oxide), boron nitride, magnesium oxide, titanium oxide, zirconium oxide, and mica. The boron nitride preferably includes hexagonal boron nitride (h-BN).
[0033] In the present disclosure, the inorganic insulating particles having surfaces coated with amphipathic molecules can be prepared, for example, as follows. However, the method for preparing the inorganic insulating particles having surfaces coated with amphipathic molecules is not limited to the following method.
[0034] A particulate inorganic material having insulating properties as inorganic insulating particles and a dispersant are prepared.
[0035] The dispersant contains the above-mentioned amphipathic molecules. Therefore, the surfaces of the inorganic insulating particles are particularly easily covered with the amphipathic molecules. The dispersant is preferably, for example, a phosphate ester-based dispersant. The phosphate ester-based dispersant has amphipathic molecules, the hydrophobic group has a hydrocarbon chain, and the hydrophilic group has at least one of a phosphoric acid group and a phosphate salt. More specifically, the dispersant is, for example, a phosphate ester-based wetting dispersant.
[0036] Next, the inorganic insulating particles, the dispersant, and, if necessary, a solvent such as an organic solvent are mixed, and the inorganic insulating particles are dispersed in the mixture. In this case, the ratio of the amphipathic molecules to 100% by mass of the inorganic insulating particles is preferably 10% by mass or more and 100% by mass or less. When the ratio of the amphipathic molecules is 10% by mass or more, the composite magnetic material molding can maintain a high relative permeability and improve the withstand voltage. Also, when the ratio of the amphipathic molecules is 100% by mass or less, the surface of the inorganic insulating particles can be covered with a sufficient amount of the amphipathic molecules, so that particularly excellent relative permeability and withstand voltage are easily achieved. It is more preferable that the ratio of the amphipathic molecules is 30% by mass or more. The upper limit of the ratio of the amphipathic molecules is not particularly limited, and is, for example, 100% by mass.
[0037] This results in inorganic insulating particles coated with amphiphilic molecules.
[0038] (thermosetting resin) The thermosetting resin functions as a so-called binder in the cured composite magnetic material. That is, the thermosetting resin has a function of binding the iron-based soft magnetic alloy particles together in the cured composite magnetic material. However, in this embodiment, as described above, since inorganic insulating particles are interposed between the iron-based soft magnetic alloy particles in the cured composite magnetic material, the binding is not limited to the binding of all the iron-based soft magnetic alloy particles together.
[0039] The thermosetting resin can have electrical insulation properties, and therefore, when the composite magnetic material is cured, the thermosetting resin can penetrate to fill the gaps between the soft magnetic alloy particles, thereby improving the electrical insulation properties of the molded body of the composite magnetic material. Furthermore, the thermosetting resin can ensure moldability when molding the composite magnetic material to produce a cured product.
[0040] Examples of the thermosetting resin include, but are not limited to, epoxy resin, phenol resin, phenoxy resin, silicone resin, polyimide, and organic phosphoric acid compound.
[0041] Examples of epoxy resins include alkylphenol novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; naphthol novolac type epoxy resins; phenol aralkyl type epoxy resins having a phenylene skeleton, biphenylene skeleton, or the like; biphenyl aralkyl type epoxy resins; naphthol aralkyl type epoxy resins having a phenylene skeleton, biphenylene skeleton, or the like; multifunctional epoxy resins such as triphenol methane type epoxy resins and alkyl modified triphenol methane type epoxy resins; triphenyl methane type epoxy resins; tetrakisphenol ethane type epoxy resins; dicyclopentadiene type epoxy resins; and one or more components selected from the group consisting of ene-type epoxy resins; stilbene-type epoxy resins; bisphenol-type epoxy resins such as bisphenol A-type epoxy resins and bisphenol F-type epoxy resins; biphenyl-type epoxy resins; naphthalene-type epoxy resins; alicyclic epoxy resins; bromine-containing epoxy resins such as bisphenol A-type bromine-containing epoxy resins; glycidylamine-type epoxy resins obtained by reacting polyamines such as diaminodiphenylmethane or isocyanuric acid with epichlorohydrin; and glycidyl ester-type epoxy resins obtained by reacting polybasic acids such as phthalic acid or dimer acid with epichlorohydrin.
[0042] The thermosetting resin may be, for example, in a liquid state or in a solid state.
[0043] The composite magnetic material may contain a curable component other than the thermosetting resin, for example, a photocurable component.
[0044] The ratio of the thermosetting resin to the total amount of the iron-based soft magnetic alloy particles may be appropriately adjusted depending on the shape of the composite magnetic material, the type of the thermosetting resin, and the properties required for the molded body, but is, for example, 1% by mass or more and 10% by mass or less. Within this range, the electrical insulation of the molded body of the composite magnetic material is easily maintained.
[0045] The composite magnetic material may contain components other than those described above without departing from the scope of the present disclosure. For example, the composite magnetic material may contain additives as components other than those described above. Examples of additives include modifiers, lubricants, and hardeners.
[0046] The modifier or lubricant can improve the dispersibility of the iron-based soft magnetic alloy particles in the hardened composite magnetic material, or modify the surface of the iron-based soft magnetic alloy particles. Examples of the modifier include coupling agents and surfactants. Examples of the coupling agent include at least one component selected from the group consisting of silane coupling agents, titanium-based coupling agents, titanium alkoxides, and titanium chelates. Examples of the surfactant include ionic surfactants and nonionic surfactants.
[0047] The lubricant may be, for example, an organometallic soap, and the organometallic soap may be, for example, at least one component selected from the group consisting of zinc stearate, calcium stearate, magnesium stearate, and barium stearate. Note that the modifier and the lubricant are not limited to the above components.
[0048] The curing agent is not particularly limited as long as it is a component capable of curing the thermosetting resin. In the present disclosure, the curing agent also includes a curing accelerator, a curing catalyst, and a curing assistant. Specific examples of the curing agent include phenol-based curing agents, acid anhydride-based curing agents, aliphatic amine-based curing agents, and aromatic amine-based curing agents, as well as imidazole-based curing accelerators, tertiary amines, and phosphorus compounds.
[0049] (2) Preparation of composite magnetic materials and compacts The composite magnetic material of this embodiment can be prepared, for example, as follows.
[0050] First, iron-based soft magnetic alloy particles, inorganic insulating particles that have been coated so as to have amphiphilic molecules on their surfaces (hereinafter, sometimes referred to as "coated inorganic insulating particles"), and a thermosetting resin are prepared. The iron-based soft magnetic alloy particles may be previously surface-treated with an appropriate dispersant, modifier, lubricant, etc., as necessary.
[0051] Then, for example, the iron-based soft magnetic alloy particles and the coated inorganic insulating particles are added to a kneadable container, mixed, and dispersed uniformly.
[0052] Next, the iron-based soft magnetic alloy particles and the coated inorganic insulating particles are mixed, and then the thermosetting resin is further added, and additives, solvents, etc. are further added as necessary, and the mixture is kneaded. When adding the thermosetting resin, the thermosetting resin may be added to the iron-based soft magnetic alloy particles and the coated inorganic insulating particles in a state where it is dissolved in a solvent in advance. In addition, a suitable kneading device can be used for kneading. The conditions for kneading may be appropriately adjusted depending on the type of thermosetting resin, the melting start temperature, etc., and for example, the heating temperature can be set to a temperature lower than the temperature at which the thermosetting resin starts to harden. In this way, a composite magnetic material is obtained.
[0053] The kneaded composite magnetic material may be dried by heating it at an appropriate temperature. When a solvent such as an organic solvent is added during kneading, it is preferable to dry the composite magnetic material by heating it at a temperature at which the solvent can volatilize.
[0054] The dried composite magnetic material may be pulverized by a suitable pulverizing device or the like to obtain a powdered composite magnetic material. The pulverization may be performed by a stamp mill method, a ball mill method, a hammer mill method, or the like. The composite magnetic material may be pulverized and then classified to obtain a composite magnetic material having a suitable particle size. The particle size of the composite magnetic material may be, for example, 100 μm or more and 500 μm or less, but is not limited thereto.
[0055] Thus, the shape or properties of the composite magnetic material are not particularly limited. When the composite magnetic material is in powder form (powder), it is easy to improve moldability. Therefore, the powder of the composite magnetic material is particularly suitable for use as a material for producing a compact, for example. To produce a compact, first, the powder composite magnetic material is placed in a mold and pressure-molded into an appropriate shape. The conditions for pressing can be adjusted as appropriate, but for example, a pressure of 1 ton / cm 2 More than 10ton / cm 2 It can be more than that.
[0056] Next, the composite magnetic material after pressure molding is heated to harden the thermosetting resin. The heating temperature and heating time may be appropriately adjusted depending on the type of thermosetting resin, but the heating temperature is, for example, 150° C. to 300° C., and the heating time is, for example, 1 minute to 10 hours.
[0057] In this disclosure, a composite magnetic material molded article includes a cured composite magnetic material.
[0058] FIG. 1 shows a schematic cross-sectional view of a molded body 1 made from the composite magnetic material of this embodiment. As shown in FIG. 1, the molded body 1 contains iron-based soft magnetic alloy particles 2, inorganic insulating particles 3, and a cured product 4 of a thermosetting resin. That is, the molded body 1 contains the composite magnetic material described above. In addition, inorganic insulating particles 3 are interposed between the iron-based soft magnetic alloy particles 2. In addition, the surface of each inorganic insulating particle 3 is covered with amphiphilic molecules having a hydrophobic group having a hydrocarbon chain and at least one hydrophilic group of a phosphoric acid group and a phosphate salt. Therefore, the molded body containing the composite magnetic material can realize an improvement in withstand voltage while suppressing a decrease in relative permeability.
[0059] (Characteristics of Molded and Cured Products) The initial relative magnetic permeability of the cured composite magnetic material is the relative magnetic permeability when no magnetic field is applied (i.e., magnetic field of 0 kA / m). The initial relative magnetic permeability of the composite magnetic material in the present disclosure and the relative magnetic permeability when a magnetic field is applied can be measured and calculated by the method described in the following Example "(2-1) Evaluation 1: Initial relative magnetic permeability and relative magnetic permeability".
[0060] The withstand voltage of the cured composite magnetic material is preferably 70 V / mm or more. In this case, when the cured composite magnetic material is used as a magnetic core of an inductor component, the leakage current of the magnetic core can be effectively reduced. The withstand voltage of the cured composite magnetic material in this disclosure can be measured and calculated by the method described in the following Example "(2-2) Evaluation 2: Withstand voltage".
[0061] As described above, the composite magnetic material of the present embodiment is capable of improving the relative permeability and the withstand voltage of the molded body even if it contains an electrically insulating component. Therefore, the composite magnetic material of the present embodiment can be suitably used for manufacturing a magnetic element and a magnetic core provided in the magnetic element by molding the magnetic element into a desired shape, for example, by pressing the magnetic element.
[0062] For example, the composite magnetic material can be used to manufacture magnetically responsive electronic components, such as inductor components that are magnetic elements. Examples of inductor components include inductors, noise filters, reactors, and transformers. In addition, the use of the magnetic element is not particularly limited, but examples include noise filter components and impedance matching circuit components. The inductor component includes, for example, a coil-shaped conductor portion and a coating layer that coats the coil-shaped conductor portion. Therefore, an inductor component can be manufactured by using a molded body made of the composite magnetic material as the coating layer. In particular, the molded body 1 of the composite magnetic material of this embodiment can be suitably used for the dust core 10 and the power choke coil 110. However, it is not intended that the use of the composite magnetic material is limited to the above.
[0063] Preferred aspects of the dust core 10 and power choke coil 110 of this embodiment will be described with reference to the drawings (FIGS. 2A to 4).
[0064] (3)Powder magnetic core The powder magnetic core 10 is used, for example, in a magnetic element having a magnetic core. The powder magnetic core 10 is also called a dust core.
[0065] The powder magnetic core 10 includes a green compact 1 (cured product) of the composite magnetic material described above. The powder magnetic core 10 of this embodiment is a green compact obtained by, for example, pressure-molding the composite magnetic material described above and heating it.
[0066] The shape of the powder magnetic core 10 may be set according to an appropriate shape for use in electronic components such as magnetic elements, and is not particularly limited; for example, it may be a cylindrical shape, a polygonal prism shape, a toroidal shape, a disk shape, or the like.
[0067] Specifically, the powder magnetic core 10 shown as an example in Fig. 2A is formed with a coil conductor portion 20 in which a copper wire is wound so as to have an air core, and has a protrusion 102 that passes through the air core of the coil conductor portion 20, and has a main body portion 101 that covers the periphery of the wound portion of the coil conductor portion 20. In Fig. 2A, the coil conductor portion 20 is, for example, an edgewise coil formed by winding a rectangular copper wire, but is not limited to this.
[0068] 2A shows an exploded perspective view of a choke coil 100 in which a coil conductor 20 is sandwiched between two powder cores 10 (11, 12) having similar shapes from above and below the air core with a protruding portion 102 disposed so as to pass through the air core of the coil conductor 20. That is, the choke coil 100 is produced from the coil conductor 20 and the powder cores 10 (11, 12) (see FIG. 2B). Of the coil conductor 20 sandwiched between the powder cores 11, 12, a tip portion 200 (a first tip portion 201 and a second tip portion 202) may protrude from each of the powder cores 11, 12 when the powder cores 11, 12 are stacked, but the first tip portion 201 and the second tip portion 202 may serve as terminals (connection terminals) that can be connected to an external circuit. The connection terminal can be produced by stacking the powder cores 11, 12 with the coil conductor 20 sandwiched between them, and then bending the tip portions 201, 202 of the coil conductor 20 in opposite directions. As shown in Fig. 2B, the housing 50 may be formed by stacking the powder cores 11, 12 with the coil conductor 20 sandwiched between them, and then molding the powder cores 11, 12 with resin so as to cover the entire main body 101 of the powder core 10 (11, 12).
[0069] (4) Power choke coil A power choke coil is a passive element that stores electric energy flowing between terminal portions as magnetic energy. Specifically, the power choke coil 110 includes, for example, a coil conductor portion 20. The coil conductor portion 20 has two terminal portions (a first end 211 and a second end 212) (see FIG. 3A). The power choke coil 110 can generate magnetic energy by a current flowing between the first terminal 211 and the second terminal portion 212 in the coil conductor portion 20. The coil conductor portion 20 is, for example, an edgewise coil formed by winding a rectangular copper wire.
[0070] As described above, the composite magnetic material can impart high relative permeability and voltage resistance to the compact 1, and therefore can be suitably used to manufacture the power choke coil 110. The power choke coil 110 of this embodiment includes a hardened composite magnetic material and a coil conductor portion 20. The coil conductor portion 20 is covered with the hardened composite magnetic material. Note that the hardened composite magnetic material is the compact 1 of the composite magnetic material, and therefore may be the above-mentioned dust core 10.
[0071] The choke coil 100 as shown in FIG. 2B above can be considered to be a type of power choke coil 110, but in the power choke coil 110 shown in FIGS. 3A and 3B, the composite magnetic material and the coil conductor portion 20 are integrally molded. Specifically, as shown in the cross-sectional view of FIG. 3A, in the power choke coil 110, the coil conductor portion 20 is embedded inside the molded body 1 by being covered with the composite magnetic material and molded. That is, the choke coil 100 shown in FIGS. 2A and 2B is a coil-assembled magnetic element in which the composite magnetic material molded body (powder core 10) and the coil conductor portion 20 are prepared separately and assembled, whereas the power choke coil 110 shown in FIGS. 3A and 3B can be considered to be a coil-embedded magnetic element in which the composite magnetic material and the coil conductor portion 20 are integrally molded so as to include the coil conductor portion 20.
[0072] As shown in FIGS. 3A and 3B, power choke coil 110 includes coil conductor portion 20 having an air core inside compact 1, and is applicable to applications in which a large current flows, and can be made compact.
[0073] The coil conductor portion 20 has a first end 211 and a second end 212. The first end 211 and the second end 212 are connected to the respective connection terminals 30. Specifically, the first end 211 is connected to the first connection terminal 31, and the second end 212 is connected to the second connection terminal 32. The air-core portion of the coil conductor portion 20 is filled with a hardened product (green body 1) of the composite magnetic material, and therefore, the part of the coil conductor portion 20 that was air-core can become a magnetic path.
[0074] The connection terminals 30 (first connection terminal 31 and second connection terminal 32) are connected to external electrodes, allowing current to flow through the power choke coil 110. When a current flows through the power choke coil 110, a magnetic field is generated, but since the magnetic path contains the composite magnetic material molding 1, the relative permeability is less likely to decrease, and the power choke coil 110 can effectively convert electrical energy into magnetic energy and store the magnetic energy. The power choke coil 110 also has excellent voltage resistance.
[0075] As shown in FIG. 3B, the housing 51 may be formed by molding the outer surfaces of the hardened composite magnetic material (molded body 1) and the first end 211 and the second end 212 of the coil conductor portion 20 with an appropriate resin.
[0076] (Modification) 3A and 3B, the power choke coil 110 shown in FIG. 4 is also a coil-buried type magnetic element in which a composite magnetic material and a coil conductor portion 20 are integrally formed. In the power choke coil 110 shown in FIG. 4, for example, a coil wire, specifically, a winding coil 20A, is used as the coil conductor portion 20. In the power choke coil 110, the winding coil 20A and the composite magnetic material are integrally formed. The winding coil 20A has a first end and a second end (not shown), and the first end and the second end of the winding coil 20A are connected to the respective connection terminals 30, so that a current can be passed through the power choke coil 110. The power choke coil 110 of this modification also has a low relative permeability and excellent voltage resistance.
[0077] (5) Summary As is apparent from the above-described embodiments, the present disclosure includes the following aspects. In the following, reference symbols are given in parentheses only to clarify the correspondence with the embodiments.
[0078] The composite magnetic material according to the first aspect contains iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin. The surface of each of the inorganic insulating particles is coated with amphiphilic molecules having a hydrophobic group and a hydrophilic group. The hydrophobic group includes a hydrocarbon chain, and the hydrophilic group includes at least one of a phosphoric acid group and a phosphate salt.
[0079] According to this embodiment, it is possible to improve the withstand voltage while making it difficult for the relative magnetic permeability of the molded body to decrease.
[0080] In the composite magnetic material according to the second aspect, in the first aspect, the average particle size of the inorganic insulating particles and the average particle size of the iron-based soft magnetic alloy particles satisfy the relationship of formula (1).
[0081] 0.09≦Average particle size of inorganic insulating particles / Average particle size of iron-based soft magnetic alloy particles≦0.5 (1)
[0082] According to this embodiment, the relative magnetic permeability of the molded body can be further increased, and the withstand voltage can be further improved.
[0083] A composite magnetic material according to a third aspect is the composite magnetic material of the first or second aspect, wherein the inorganic insulating particles have an average particle size of 0.8 μm or more and 4 μm or less.
[0084] According to this embodiment, the relative magnetic permeability and the withstand voltage of the molded body can be further improved.
[0085] The composite magnetic material according to a fourth aspect is any one of the first to third aspects, wherein the volume ratio of the inorganic insulating particles to the total volume of the iron-based soft magnetic alloy particles is 1.3 volume % or more and 4.0 volume % or less.
[0086] According to this embodiment, the molded body can maintain a high relative magnetic permeability, and the withstand voltage can be further improved.
[0087] The composite magnetic material according to a fifth aspect is any one of the first to fourth aspects, wherein the proportion of the amphiphilic molecules with respect to the total mass of the inorganic insulating particles is 10 mass % or more and 100 mass % or less.
[0088] According to this embodiment, the composite magnetic material molding can maintain a high relative magnetic permeability and improve the withstand voltage. In addition, if the proportion of the amphiphilic molecules is 100 mass % or less, the surfaces of the inorganic insulating particles can be covered with a sufficient amount of the amphiphilic molecules, so that it is easy to realize particularly excellent relative magnetic permeability and withstand voltage.
[0089] The composite magnetic material of the sixth aspect is any one of the first to fifth aspects, wherein the inorganic insulating particles include coated particles obtained by adding the amphiphilic molecules in a ratio of 10% by mass or more and 100% by mass or less to 100% by mass of the inorganic insulating particles.
[0090] According to this embodiment, the composite magnetic material molding can maintain a high relative magnetic permeability and improve the withstand voltage. In addition, if the proportion of the amphiphilic molecules is 100 mass % or less, the surfaces of the inorganic insulating particles can be covered with a sufficient amount of the amphiphilic molecules, so that it is easy to realize particularly excellent relative magnetic permeability and withstand voltage.
[0091] A powder magnetic core (10) according to a seventh aspect includes a cured product of the composite magnetic material according to any one of the first to sixth aspects.
[0092] According to this embodiment, a powder magnetic core (10) can be obtained that can simultaneously improve the withstand voltage while making it difficult for the relative permeability to decrease.
[0093] A power choke coil (110) according to an eighth aspect includes the hardened composite magnetic material according to any one of the first to sixth aspects, and a coil conductor portion (20). The coil conductor portion (20) is covered with the hardened composite magnetic material.
[0094] According to this embodiment, a power choke coil (110) can be obtained that can simultaneously improve the withstand voltage while making it difficult for the relative permeability to decrease. EXAMPLES
[0095] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to the following examples.
[0096] (1) Experiment 1 (Preparation of composite magnetic material) [Comparative Example 1] As iron-based soft magnetic alloy particles (hereinafter also referred to as "alloy particles"), Fe-Si-Cr-based metal powder (FeSiCr-based metal powder) with an average particle diameter D50 of 9 μm was prepared. 4 mass% of epoxy resin as a thermosetting resin and MEK (methyl ethyl ketone) as an organic solvent were mixed with 100 mass% of the prepared alloy particles. In Comparative Example 1, no inorganic insulating particles were added. After kneading the mixture, the solvent was removed by drying at 50°C for 30 minutes to prepare a composite magnetic material (dried product).
[0097] The dried product was pulverized in a pulverizer and then classified to obtain a powder of a composite magnetic material having a particle size of 100 μm to 500 μm.
[0098] Next, the powder is added to a compression molding die and compressed at a pressure of 2t / cm 2 The compacts were molded under the following conditions. For the evaluation described later, a toroidal shaped compact and a disk shaped compact were prepared as quasi-test pieces. The compacts of each quasi-test piece were then heated at 175°C for 3 hours to harden them, producing hardened products of the composite magnetic material. In this way, a toroidal shaped hardened product test piece and a disk shaped hardened product test piece were obtained. The density of the hardened product test pieces and the filling rate (volume %) of the alloy particles are shown in Table 1 as "density (g / cm3)", respectively. 3 The density of the hardened test piece was calculated by dividing the mass of the test piece by the volume of the test piece measured with a micrometer. The alloy particle filling rate was calculated from the following formula (2). The same applies below. In the following formula (2), the density of the test piece is expressed as d Mea , the true density of the alloy particles is d Met , the true density of the inorganic insulating particles is d Ins , the true density of the thermosetting resin is d Res , the packing ratio of the alloy particles is a MetIn the composite magnetic material, the mass percent of inorganic insulating particles is M with respect to 100 mass percent of alloy particles. Ins , the mass% of the thermosetting resin is M Res , the mass percent of the amphiphilic molecules is M Amp , respectively.
[0099] a Met =d Mea ×(100 / d Met ) / (100+M Ins +M Res +M Amp ) × 100 ... (2)
[0100] [Example 1, Comparative Example 2] In Example 1, FeSiCr-based metal powder with an average particle size (D50) of 9 μm was prepared as the alloy particles. In addition, talc with an average particle size D50 of 2 μm was prepared as the inorganic insulating particles, and 33 mass% of a phosphate ester-based wetting and dispersing agent and an appropriate amount of MEK as an organic solvent were added to 100 mass% of the inorganic insulating particles and stirred to subject the inorganic insulating particles to a surface treatment, thereby preparing coated inorganic insulating particles.
[0101] Next, the alloy particles and the coated inorganic insulating particles were mixed, and then 4% by mass of epoxy resin as a thermosetting resin and MEK as an organic solvent were mixed with 100% by mass of the alloy particles. Then, after kneading the mixture, the solvent was removed by drying at 50°C for 30 minutes to prepare a composite magnetic material (dried material). The dried material was pulverized in a pulverizer and then classified to obtain a powder of the composite magnetic material having a particle size of 100 μm to 500 μm.
[0102] In Comparative Example 2, the inorganic insulating particles were talc like in Example 1, but the inorganic insulating particles were not surface-treated. Otherwise, the materials were mixed, kneaded, dried, pulverized, and classified in the same manner as in Example 1 to obtain a powder of a composite magnetic material having a particle size of 100 μm to 500 μm.
[0103] Next, the powders of the composite magnetic materials of Example 1 and Comparative Example 2 were compression molded under the same conditions as Comparative Example 1 to prepare a toroidal shaped compact and a disk shaped compact as quasi-test pieces, and the compacts as quasi-test pieces were hardened by heating at 175°C for 3 hours. As a result, a toroidal shaped hardened product test piece and a disk shaped hardened product test piece were obtained. The density of the hardened product test pieces and the filling rate (volume%) of the alloy particles are as shown in Table 1.
[0104] [Example 2, Comparative Example 3] In Example 2, a powder of a composite magnetic material was produced under the same conditions as in Example 1, except that the inorganic insulating particles in Example 1 were changed to silica having an average particle diameter D50 of 4 μm, and the amount of a phosphate ester-based wetting dispersant used in surface treatment of the inorganic insulating particles was changed to 35 mass %.
[0105] In Comparative Example 3, a powder of a composite magnetic material was produced under the same conditions as in Comparative Example 2, except that the inorganic insulating particles in Comparative Example 2 were changed to silica having an average particle size D50 of 4 μm.
[0106] Next, the powders of the composite magnetic materials of Example 2 and Comparative Example 3 were compression molded under the same conditions as Comparative Example 1 to prepare a toroidal shaped compact and a disk shaped compact as quasi-test pieces, and the compacts as quasi-test pieces were hardened by heating at 175°C for 3 hours. As a result, a toroidal shaped hardened product test piece and a disk shaped hardened product test piece were obtained. The density of the hardened product test pieces and the filling rate (volume%) of the alloy particles are as shown in Table 1.
[0107] [Examples 3-4, Comparative Example 4] In Example 3, a powder of a composite magnetic material was produced under the same conditions as Example 1, except that the inorganic insulating particles in Example 1 were changed to alumina having an average particle diameter D50 of 3 μm, and the amount of a phosphate ester-based wetting dispersant used in surface treatment of the inorganic insulating particles was changed to 23 mass %.
[0108] In Example 4, powder of a composite magnetic material was produced under the same conditions as in Example 3, except that the amount of the phosphate ester-based wetting and dispersing agent in Example 3 was changed to 35 mass %.
[0109] In Comparative Example 4, powder of a composite magnetic material was produced under the same conditions as in Comparative Example 2, except that the inorganic insulating particles in Comparative Example 2 were changed to alumina having an average particle size D50 of 3 μm.
[0110] Next, the powders of the composite magnetic materials of Examples 3-4 and Comparative Example 4 were compression molded under the same conditions as Comparative Example 1 to prepare a toroidal shaped compact and a disk shaped compact as quasi-test pieces, and the compacts as quasi-test pieces were hardened by heating at 175°C for 3 hours. As a result, a toroidal shaped hardened product test piece and a disk shaped hardened product test piece were obtained. The density of the hardened product test pieces and the filling rate (volume%) of the alloy particles are as shown in Table 1.
[0111] [Example 5, Comparative Example 5] In Example 5, a powder of a composite magnetic material was produced under the same conditions as in Example 1, except that the inorganic insulating particles in Example 1 were changed to boron nitride (hexagonal boron nitride) having an average particle diameter D50 of 3 μm, and the amount of a phosphate ester-based wetting and dispersing agent used in surface treatment of the inorganic insulating particles was changed to 41 mass %.
[0112] In Comparative Example 5, powder of a composite magnetic material was produced under the same conditions as in Comparative Example 2, except that the inorganic insulating particles in Comparative Example 2 were changed to boron nitride (hexagonal boron nitride) having an average particle size D50 of 3 μm.
[0113] Next, the powders of the composite magnetic materials of Example 5 and Comparative Example 5 were compression molded under the same conditions as Comparative Example 1 to prepare a toroidal shaped compact and a disk shaped compact as quasi-test pieces, and the compacts as quasi-test pieces were hardened by heating at 175°C for 3 hours. As a result, a toroidal shaped hardened product test piece and a disk shaped hardened product test piece were obtained. The density of the hardened product test pieces and the filling rate (volume%) of the alloy particles are as shown in Table 1.
[0114] (2) Evaluation of Experiment 1 (2-1) Evaluation 1: Initial relative permeability and relative permeability In each of the Examples and Comparative Examples, a test piece of the cured product of a toroidal shaped compact having dimensions of outer diameter φ14 mm, inner diameter φ10 mm, and thickness of approximately 2 mm was wound with 30 turns of silver-plated soft copper wire having a diameter of φ0.6 mm and a coating thickness of 0.15 mm, and then connected to an LCR meter to measure the inductance at 10 kHz and a current of 0 A. From the obtained results, the relative permeability was calculated based on the following formula (3). In formula (3), L is inductance [H], μ0 is the permeability of a vacuum [H / m], μi is the relative permeability, le is the magnetic path length [m], and Ae is the cross-sectional area [m 2 ] and n indicate the number of turns of the coil, and the letters in [ ] are units. The values calculated using this are shown in Table 1.
[0115] L = (μi) × (μ0) × n 2 ×Ae / le···(3) Next, in order to measure the inductance when a magnetic field was applied, a DC bias current was applied to the above-mentioned test piece with a copper wire wound under the same conditions, and the inductance was measured at 10 kHz using an LCR meter in the same manner as for the initial relative permeability.
[0116] The DC current required for the applied magnetic field was calculated based on the following formula (4): In formula (4), Hx is the applied magnetic field [A / m], le is the magnetic path length [m], Ix is the applied current [A], and n is the number of turns of the coil, and the words in brackets [] are units.
[0117] Hx = n / le × Ix (4) Table 1 shows the relative permeability when no magnetic field is applied (0 kA / m) (also called initial relative permeability) and the relative permeability when the magnetic field is 12.4 kA / m. Graphs showing the relationship between the applied magnetic field and the relative permeability are shown in Figs. 5 to 8. In Figs. 5 to 8, the horizontal axis is the magnetic field [kA / m] and the vertical axis is the relative permeability. Fig. 5 shows the results of Comparative Example 1, Comparative Example 2, and Example 1. Fig. 6 shows the results of Comparative Example 1, Comparative Example 3, and Example 2. Fig. 7 shows the results of Comparative Example 1, Comparative Example 4, Example 3, and Example 4. Fig. 8 shows the results of Comparative Example 1, Comparative Example 5, and Example 5.
[0118] (2-2) Rating 2: Withstand voltage In each example and comparative example, a test piece of a disk-shaped cured product having a diameter of φ12 mm and a thickness of about 1 mm was clamped with a probe on both sides near the center, and a DC voltage of 10 V was applied in stages using an ultra-high resistance / micro ammeter. The discharge time was 1 second, and the charge time was 10 seconds. From the "voltage [V] at which the leakage current became 10 mA or more" obtained from this, the withstand voltage was calculated based on the following formula (5). In formula (5), Ex is the withstand voltage [V / mm], Ez is the "voltage at which the leakage current became 10 mA or more" [V], d is the thickness [mm] of the test piece, and the words in [] are units. The results are shown in the "Withstand voltage (V / mm)" column in Table 1.
[0119] Ex = (Ez-10) / d (5)
[0120] [Table 1]
[0121] As is clear from the above results, when comparing Comparative Example 1, in which no inorganic insulating particles were added, with Comparative Example 2-5, in which inorganic insulating particles that had not been surface-treated were added, it was shown that, as is clear from Figures 5 to 8 and Table 1, in Comparative Example 2-5, regardless of which inorganic insulating particles were used, the relative permeability was lower than that of Comparative Example 1.
[0122] In contrast, when comparing Comparative Example 1, in which no inorganic insulating particles were added, with Examples 1-5, in which coated inorganic insulating particles were added, as is clear from Figures 5 to 8 and Table 1, it was found that, although the filling rate of the alloy particles was reduced in Examples 1-5, in which coated inorganic insulating particles were added, the same relative permeability as in Comparative Example 1 was obtained regardless of which inorganic insulating particle was used. Furthermore, it was shown that, compared to Comparative Example 1, an extremely high withstand voltage could be achieved in Examples 1-5.
[0123] In addition, when the same type of inorganic insulating particles are used in comparison between Comparative Example 2-5 and Example 1-5, it is shown that a high relative magnetic permeability can be achieved by blending coated inorganic insulating particles.
[0124] Furthermore, in Example 1-5 in which coated inorganic insulating particles were added, it was shown that a high withstand voltage could be achieved by blending coated inorganic insulating particles, compared with the same type of inorganic insulating particles.
[0125] (3) Experiment 2 (Preparation of composite magnetic material) Next, for comparison with the above Experiment 1, the following experiment was conducted.
[0126] [Examples 6-21 and Comparative Examples 6-10] In Examples 6-21, as shown in Table 2 or Table 3, one or more of the “type” of inorganic insulating particles, the average particle diameter “D50 (μm)”, “addition amount (volume % relative to alloy particles)”, and “addition amount (mass % relative to inorganic insulating particles)” of the dispersant used to coat the surface of the inorganic insulating particles were changed from those in Example 1 described above, and a powder of the composite magnetic material was produced under the same conditions as in Example 1.
[0127] In addition, in Comparative Examples 6-10, as shown in Table 2 or Table 3, one or more of the “type” of inorganic insulating particles, the average particle diameter “D50 (μm)”, and the “addition amount (relative to alloy particles (volume %))” were changed from those in Comparative Example 2 described above, and powder of the composite magnetic material was produced under the same conditions as in Comparative Example 2.
[0128] The powders of the composite magnetic materials of Examples 6-21 and Comparative Examples 6-10 were compression molded under the same conditions as in Comparative Example 1 to produce a toroidal shaped compact and a disk shaped compact as quasi-test pieces. The quasi-test pieces were hardened by heating at 175°C for 3 hours to obtain a toroidal shaped hardened product test piece and a disk shaped hardened product test piece.
[0129] (4) Evaluation of Experiment 2 Under the same conditions as in "(2-1) Evaluation 1: Initial relative magnetic permeability and relative magnetic permeability" above, the inductance was measured for Example 6-21 and Comparative Example 6-10, and the initial relative magnetic permeability and relative magnetic permeability were calculated. The results are shown in Tables 2 and 3.
[0130] In addition, under the same conditions as in "Evaluation 2: Withstand voltage" above, for Example 6-21 and Comparative Example 6-10, the "voltage [V]" at which the leakage current reached 10 mA or more was measured, and the withstand voltage was calculated. The results are shown in Tables 2 and 3. For comparison, Tables 2 and 3 also show the results of the above-mentioned Experiment 1 (Examples 1-5 and Comparative Examples 1-5).
[0131] [Table 2]
[0132] [Table 3]
[0133] In Experiment 2, a comparison of Comparative Example 1 in which no inorganic insulating particles were added, Comparative Example 6-10 in which inorganic insulating particles not subjected to surface treatment were added, and Example 6-21 in which coated inorganic insulating particles were added showed the same tendency as in Experiment 1. That is, it was shown that, regardless of which inorganic insulating particle was used, Example 6-21 had a high relative permeability comparable to that of Comparative Example 1 and a high withstand voltage higher than that of Comparative Example 1. In addition, when Example 6-22 was compared with Comparative Example 6-10, which had the same type of inorganic insulating particles, Example 6-21 had a higher relative permeability and a higher withstand voltage than Comparative Example 6-10. [Explanation of symbols]
[0134] 1 Molded body 2. Iron-based soft magnetic alloy particles 3. Inorganic insulating particles 4. Cured thermosetting resin 10,11,12 Powder magnetic core 20 Coil conductor 110 Power choke coil
Claims
1. A composite magnetic material containing iron-based soft magnetic alloy particles, inorganic insulating particles, and a thermosetting resin, the surface of each of the inorganic insulating particles is coated with an amphiphilic molecule having a hydrophobic group and a hydrophilic group; The hydrophobic group comprises a hydrocarbon chain; The hydrophilic group comprises at least one of a phosphate group and a phosphate salt. Composite magnetic material.
2. The average particle size of the inorganic insulating particles and the average particle size of the iron-based soft magnetic alloy particles satisfy the relationship of formula (1). 0.09≦average particle size of inorganic insulating particles / average particle size of iron-based soft magnetic alloy particles≦0.5 (1) The composite magnetic material of claim 1 .
3. The average particle size of the inorganic insulating particles is 0.8 μm or more and 4 μm or less. The composite magnetic material according to claim 1 or 2.
4. The volume ratio of the inorganic insulating particles to the total volume of the iron-based soft magnetic alloy particles is 1.3 volume % or more and 4.0 volume % or less. The composite magnetic material according to claim 1 or 2.
5. A ratio of the amphiphilic molecules to the total mass of the inorganic insulating particles is 10 mass% or more and 100 mass% or less. The composite magnetic material according to claim 1 or 2.
6. The inorganic insulating particles include coated particles obtained by adding the amphiphilic molecules in a ratio of 10% by mass or more and 100% by mass or less to 100% by mass of the inorganic insulating particles. The composite magnetic material according to claim 1 or 2.
7. The composite magnetic material according to claim 1 or 2 includes a cured product of the composite magnetic material. Powder magnetic core.
8. A magnetic coil comprising the hardened composite magnetic material according to claim 1 or 2 and a coil conductor portion, The coil conductor portion is covered with a hardened product of the composite magnetic material. Power choke coil.
Citation Information
Patent Citations
Soft magnetic material, powder magnetic core, method for producing soft magnetic material, and method for producing powder magnetic core
JP2007211340A
Soft magnetic powder and inductor
JP2022060995A
Soft magnetic film
WO2014132880A1
Magnetic resin composition, magnetic sheet, and inductor component
WO2023149454A1
Composite magnetic material, magnetic element and manufacturing method of them
JP2002305108A