Curable resin composition

The curable resin composition with specific epoxy and acrylic compounds, along with an inorganic filler, addresses deformation and crack resistance issues, ensuring effective encapsulation in semiconductor applications.

JP2024143810APending Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023056706
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing curable resin compositions experience deformation during curing and have insufficient crack resistance, particularly at high temperatures, which is problematic for applications like wafer level packages.

Method used

A curable resin composition comprising a modified silicone epoxy compound, an alicyclic epoxy compound, and a novolac or trisphenolmethane type epoxy resin, along with a liquid acrylic polymer and inorganic filler, which reduces viscosity and suppresses deformation while enhancing crack resistance.

Benefits of technology

The composition achieves low viscosity, minimizes deformation during curing, and significantly improves crack resistance, especially at high temperatures, making it suitable for encapsulants in semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143810000001
    Figure 2024143810000001
  • Figure 2024143810000002
    Figure 2024143810000002
  • Figure 2024143810000003
    Figure 2024143810000003
Patent Text Reader

Abstract

To provide a curable resin composition which has low viscosity, suppresses deformation during curing, and gives a cured product having high crack resistance.SOLUTION: The curable resin composition contains an epoxy compound (A), an acrylic polymer (B), and an inorganic filler (C). The epoxy compound (A) contains a modified silicone-based epoxy compound (a1), an alicyclic epoxy compound (a2), and a compound (a3) being at least one of a novolac type epoxy compound and a trisphenolmethane type epoxy resin. The acrylic polymer (B) contains a liquid acrylic polymer (b1) which is liquid at 25°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a curable resin composition, and more particularly to a curable resin composition containing an epoxy compound. [Background technology]

[0002] Patent Document 1 describes that a resin composition containing an elastomer having a polycarbonate structure in its molecule, an epoxy resin, an inorganic filler, a phenoxy resin, and a carbodiimide compound is suppressed in warping and has excellent strength and adhesion. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-24774 A Summary of the Invention [Problem to be solved by the invention]

[0004] Provided is a curable resin composition which has low viscosity, is inhibited from deforming during curing, and gives a cured product with high crack resistance. [Means for solving the problem]

[0005] The curable resin composition according to one embodiment of the present disclosure contains an epoxy compound (A), an acrylic polymer (B), and an inorganic filler (C). The epoxy compound (A) contains a modified silicone-based epoxy compound (a1), an alicyclic epoxy compound (a2), and a compound (a3) ​​which is at least one of a novolac-type epoxy compound and a trisphenolmethane-type epoxy resin. The acrylic polymer (B) contains a liquid acrylic polymer (b1) which is liquid at 25°C. Effect of the Invention

[0006] According to one aspect of the present disclosure, there are advantages in that the curable resin composition has a low viscosity, deformation of a cured product of the curable resin composition is suppressed, and the crack resistance of the cured product can be increased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The following describes embodiments of the present disclosure. Note that the following embodiments are merely a portion of various embodiments of the present disclosure. In addition, the following embodiments can be modified in various ways depending on the design, etc., as long as the object of the present disclosure can be achieved. In addition, the mechanism of action described below is a speculation, and the present disclosure is not bound by the description of the mechanism of action below.

[0008] The curable resin composition (hereinafter also referred to as composition (X)) contains an epoxy compound (A), an acrylic polymer (B), and an inorganic filler (C). The epoxy compound (A) contains a modified silicone-based epoxy compound (a1), an alicyclic epoxy compound (a2), and a compound (a3) ​​which is at least one of a novolac-type epoxy compound and a trisphenolmethane-type epoxy resin. The acrylic polymer (B) contains a liquid acrylic polymer (b1) which is liquid at 25°C.

[0009] Therefore, the composition (X) can have a low viscosity. Also, deformation of the cured product due to dimensional change during curing of the composition (X) is suppressed. Furthermore, the crack resistance of the cured product of the composition (X) can be increased. That is, when a force is applied to the cured product, the cured product is less likely to crack. In the embodiment, the crack resistance of the cured product is increased, particularly at high temperatures such as 240°C. In other words, the fracture energy of the cured product at high temperatures, which is indicated by the area under the curve of the stress-strain curve measured in a bending test, is increased.

[0010] The composition (X) can be used to prepare an encapsulant, particularly in a wafer-level package. Wafer-level packages include wafer-level chip-size packages and fan-out wafer-level packages. The encapsulant is a member that covers a part or all of a chip component such as a die in a semiconductor device such as a wafer-level package to protect the chip component from the external environment. When manufacturing a wafer-level package, for example, the composition (X) is applied to a substrate so as to cover a plurality of dies mounted on the substrate at once, and then the composition (X) is cured, and then the substrate is cut together with the encapsulant to prepare a plurality of wafer-level packages. In addition, for example, the composition (X) is applied to a wafer before dicing, and then the composition (X) is cured, and then the wafer is cut together with the encapsulant to prepare a plurality of wafer-level packages. Since the composition (X) of the embodiment has a low viscosity, it is easy to apply it on a large-area substrate or wafer. In addition, since deformation of the cured product due to dimensional change during curing of the composition (X) is suppressed, even if the composition (X) is cured on a large-area wafer, deformation such as warping is unlikely to occur in the wafer and the cured product. Furthermore, since the cured product of the composition (X) has high crack resistance at high temperatures, when a wafer-level package including an encapsulant made from the composition (X) is mounted on a substrate or the like by a reflow process or the like, the encapsulant is unlikely to be damaged. In particular, when the wafer-level package is enlarged, cracks are usually likely to occur in the encapsulant, but in the embodiment, even if the wafer-level package is enlarged, cracks in the encapsulant can be suppressed. In addition, when a semiconductor device such as a wafer-level package includes multiple dies and these dies are encapsulated at once with an encapsulant, if the distance between adjacent dies is small, cracks are likely to occur in the encapsulant between adjacent dies when the encapsulant is heated in a reflow process or the like. However, in the embodiment, cracks in the encapsulant between the dies as described above are also unlikely to occur.

[0011] In addition, the use of the composition (X) of the embodiment is not limited to the use of preparing an encapsulant in a wafer level package. The composition (X) can be used to prepare an encapsulant for any semiconductor device, not limited to a wafer level package. The composition (X) can also be used to prepare any resin member other than the encapsulant for a semiconductor device.

[0012] The components of composition (X) will be described in detail below.

[0013] The composition (X) contains an epoxy compound (A). The epoxy compound (A) has one or more epoxy groups in the molecule. There is no limitation on the molecular size of the epoxy compound (A), and the epoxy compound (A) may contain any of a monomer, a dimer, a trimer, an oligomer, a prepolymer, and the like.

[0014] As described above, the epoxy compound (A) contains the modified silicone-based epoxy compound (a1), the alicyclic epoxy compound (a2), and the compound (a3) ​​which is at least one of a novolac-type epoxy compound and a trisphenolmethane-type epoxy resin (hereinafter also referred to as compound (a3)).

[0015] The modified silicone-based epoxy compound (a1) and the alicyclic epoxy compound (a2) can reduce the viscosity of the composition (X) and increase the glass transition temperature of the cured product. The increased glass transition temperature of the cured product can increase the crack resistance of the cured product at high temperatures.

[0016] The modified silicone epoxy compound (a1) has, for example, a siloxane skeleton and one or more epoxy group-containing groups bonded to the siloxane skeleton in one molecule. The epoxy group-containing group is an organic group containing an epoxy group, such as an epoxy group itself or a glycidoxyalkyl group. The modified silicone epoxy compound (a1) contains, for example, at least one of a compound having a siloxane skeleton and a glycidoxyalkyl group bonded to one end of the skeleton in one molecule, and a compound having a siloxane skeleton and a glycidoxyalkyl group bonded to both ends of the skeleton in one molecule. The modified silicone epoxy compound (a1) is preferably liquid at 25°C.

[0017] The alicyclic epoxy compound (a2) is a compound having at least one epoxy group in one molecule, and two carbon atoms in the cyclic ether constituting the epoxy group are present on a saturated or unsaturated carbon ring that does not have aromaticity. The alicyclic epoxy compound (a2) is preferably liquid at 25°C. The alicyclic epoxy compound (a2) contains at least one compound selected from the group consisting of, for example, 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, 3,4-epoxycyclohexylmethyl (3',4'-epoxy)cyclohexanecarboxylate, ε-caprolactone-modified 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, bis(3,4-epoxycyclohexyl)adipate, 1,2-epoxy-4-vinylcyclohexane, 1,4-cyclohexanedimethanol diglycidyl ether, epoxyethyldivinylcyclohexane, diepoxyvinylcyclohexane, 1,2,4-triepoxyethylcyclohexane, and limonene dioxide.

[0018] Among the compounds (a3), the novolac type epoxy compound contains at least one selected from the group consisting of, for example, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, naphthol novolac type epoxy resins, and dicyclopentadiene novolac type epoxy resins.

[0019] The compound (a3) ​​contains, for example, a compound (a31) represented by the following formula. In the formula, n is a natural number indicating the number of repeating units in the molecule. That is, the compound (a3) ​​contains, for example, at least one of a phenol novolac type epoxy resin and a trisphenol methane type epoxy resin.

[0020] [ka]

[0021] The compound (a3) ​​improves the crack resistance of the cured product at high temperatures. It is presumed that the compound (a3) ​​increases the crosslink density of the cured product. Although (a3) ​​tends to increase the viscosity of the composition (X), in the embodiment, the viscosity of the composition (X) can be reduced because the composition (X) contains the modified silicone epoxy compound (a1), the alicyclic epoxy compound (a2) and the liquid acrylic polymer (b1).

[0022] The ratio of the modified silicone epoxy compound (a1) to the epoxy compound (A) is preferably 5% by mass or more and 30% by mass or less. If the ratio is 5% by mass or more, there is an advantage that the viscosity of the composition (X) can be further reduced. If the ratio is 30% by mass or less, there is an advantage that the glass transition temperature of the cured product is less likely to decrease. The ratio is more preferably 8% by mass or more, and even more preferably 12% by mass or more. The ratio is more preferably 25% by mass or less, and even more preferably 20% by mass or less.

[0023] The ratio of the alicyclic epoxy compound (a2) to the epoxy compound (A) is preferably 30% by mass or more and 80% by mass or less. If the ratio is 30% by mass or more, there is an advantage that the glass transition temperature of the cured product can be increased. If the ratio is 80% by mass or less, there is an advantage that it is easy to achieve both a low viscosity of the composition (X) and a high fracture energy of the cured product. The ratio is more preferably 40% by mass or more, and even more preferably 50% by mass or more. The ratio is more preferably 75% by mass or less, and even more preferably 70% by mass or less.

[0024] The ratio of compound (a3) ​​to epoxy compound (A) is preferably 5% by mass or more and 30% by mass or less. If the ratio is 5% by mass or more, the crack resistance of the cured product at high temperatures can be further improved. If the ratio is 30% by mass or less, the increase in viscosity of composition (X) can be suppressed. The ratio is more preferably 8% by mass or more, and even more preferably 12% by mass or more. The ratio is more preferably 25% by mass or less, and even more preferably 20% by mass or less.

[0025] The total ratio of the modified silicone epoxy compound (a1), the alicyclic epoxy compound (a2), and the compound (a3) ​​to the epoxy compound (A) is, for example, 70% by mass or more and 100% by mass or less. That is, the epoxy compound (A) may contain only the modified silicone epoxy compound (a1), the alicyclic epoxy compound (a2), and the compound (a3), and the epoxy compound (A) may further contain an epoxy compound (a4) that is not any of the modified silicone epoxy compound (a1), the alicyclic epoxy compound (a2), and the compound (a3). The total ratio of the modified silicone epoxy compound (a1), the alicyclic epoxy compound (a2), and the compound (a3) ​​to the epoxy compound (A) is preferably 80% by mass or more, more preferably 85% by mass or more.

[0026] When the epoxy compound (A) contains an epoxy compound (a4), the epoxy compound (a4) contains at least one selected from the group consisting of, for example, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, aralkyl type epoxy resins, biphenol type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, biphenyl type epoxy resins, anthracene type epoxy resins, epoxidized products of condensates of phenols with aromatic aldehydes having a phenolic hydroxyl group, triglycidyl isocyanurate, and naphthylene ether skeleton-containing epoxy resins.

[0027] The epoxy compound (A) is preferably liquid at 25° C. However, so long as the epoxy compound (A) is liquid as a whole, the epoxy compound (A) may contain a component that is not liquid.

[0028] The acrylic polymer (B) has a main chain made of a polymer of a monomer containing a compound having a (meth)acryloyl group (acrylic compound). The (meth)acryloyl group is a generic term for an acryloyl group and a methacryloyl group, that is, at least one of an acryloyl group and a methacryloyl group. The acrylic compound is, for example, an ester of (meth)acrylic acid and an alkyl alcohol having 1 to 10 carbon atoms. The acrylic polymer (B) may or may not have a group having a radically polymerizable unsaturated bond such as a (meth)acryloyl group in the molecule.

[0029] The acrylic polymer (B) contains a liquid acrylic polymer (b1) that is liquid at 25° C. The liquid acrylic polymer (b1) increases the flexibility of the cured product, and therefore deformation such as warping of the cured product due to dimensional changes during curing of the composition (X) can be suppressed. In addition, the liquid acrylic polymer (b1) can reduce the viscosity of the composition (X).

[0030] The liquid acrylic polymer (b1) contains, for example, a polymer (b11) having a group having a radically polymerizable unsaturated bond. The polymer (b11) has a structure in which a group having a radically polymerizable unsaturated bond is bonded to one end or both ends of a main chain made of a polymer of a monomer containing an acrylic compound. The polymer (b11) has, for example, a structure shown in the following formula (1).

[0031] [ka]

[0032] In formula (1), Fn is a group having a radically polymerizable unsaturated bond, such as an acryloyl group, a methacryloyl group, or an allyl group. In formula (1), R is H or an alkyl group having 1 to 10 carbon atoms, and n is a number of 8 to 9,000.

[0033] The liquid acrylic polymer (b1) may contain, for example, a polymer (b12) that does not have a group having a radically polymerizable unsaturated bond.

[0034] Specific examples of the polymer (b11) include XMAP RC100C, RC200C, MM110C, and the like manufactured by Kaneka Corporation, and NISSO PB TE-2000 and TEAI-1000, and the like manufactured by Nippon Soda Co., Ltd.

[0035] Specific examples of the polymer (b12) include a compound having a polybutyl acrylate structure in the molecule, such as Clarity LA-2114 manufactured by Kuraray Co., Ltd., and UP-1000 manufactured by Toagosei Co., Ltd.

[0036] The weight average molecular weight of the liquid acrylic polymer (b1) is preferably 5000 or more and 40000 or less. If the weight average molecular weight is 5000 or more, deformation such as warping of the cured product can be further suppressed. If the weight average molecular weight is 40000 or less, the viscosity of the composition (X) can be further suppressed. If the weight average molecular weight is 8000 or more, it is more preferable, and if it is 10000 or more, it is more preferable. If the weight average molecular weight is 36000 or less, it is more preferable, and if it is 33000 or less, it is more preferable.

[0037] The weight average molecular weight is measured by GPC (gel permeation chromatography) using HLC-8329GPC manufactured by Tosoh Corporation, TSKgel SuperMultiprore HZ-M manufactured by Tosoh Corporation as the GPC column, and tetrahydrofuran as the GPC solvent, using a standard polystyrene conversion method.

[0038] The proportion of the liquid acrylic polymer (b1) is preferably 5% by mass or more and 25% by mass or less based on the total of the epoxy compound (A) and the acrylic polymer (B). If the proportion is 5% by mass or more, the warping of the cured product can be further reduced, and the crack resistance can be further improved. If the proportion is 20% by mass or less, there is an advantage that the viscosity of the composition (X) is less likely to increase. If the proportion is 7% by mass or more, it is more preferable, and if it is 10% by mass or more, it is even more preferable. If the proportion is 20% by mass or less, it is even more preferable, and if it is 15% by mass or less, it is even more preferable.

[0039] The acrylic polymer (B) may further contain a polymer (b2) other than the liquid acrylic polymer (b1), i.e., an acrylic polymer (b2) that is solid at 25° C. When the acrylic polymer (B) contains the acrylic polymer (b2), the proportion of the acrylic polymer (b2) is preferably 80% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less, based on the acrylic polymer (B).

[0040] The composition (X) contains an inorganic filler (C). The inorganic filler (C) can reduce the linear expansion coefficient of the cured product of the composition (X), and as a result, can suppress deformation such as warping of the cured product due to dimensional change during curing of the composition (X).

[0041] The inorganic filler (C) contains at least one selected from the group consisting of, for example, silica, alumina, barium sulfate, talc, clay, mica, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum borate, barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, barium zirconate, calcium zirconate, etc. Silica contains at least one selected from the group consisting of, for example, crystalline silica, non-crystalline silica, amorphous silica, fused silica, and crushed silica, etc.

[0042] The ratio of the inorganic filler (C) to the composition (X) is preferably 75% by mass or more and 90% by mass or less. When the ratio is 75% by mass or more, deformation of the cured product can be further suppressed. When the ratio is 90% by mass or less, an increase in the viscosity of the composition (X) can be suppressed. When the ratio is 78% by mass or more, it is more preferable, and when it is 81% by mass or more, it is even more preferable. When the ratio is 88% by mass or less, it is even more preferable, and when it is 87% by mass or less, it is even more preferable.

[0043] It is preferable that the inorganic filler (C) contains silica. In particular, it is preferable that the inorganic filler (C) contains silica (c1) having a 50% particle size (i.e., median size D50) of a volume-based cumulative distribution of 10 μm or less and a 99% particle size (D99) of a volume-based cumulative distribution of 25 μm or less. In this case, it is easy to fill a narrow gap with the composition (X) when molding the composition (X), and when the cured product of the composition (X) is polished, the smoothness of the surface of the cured product after polishing can be improved. Therefore, defects (e.g., repelling and pinholes in the formation of a polyimide layer) when forming a rewiring layer on the encapsulant can be suppressed. Therefore, the composition (X) is more suitable for applications in which an encapsulant for a wafer level package is produced. The 50% particle size of the silica (c1) is more preferably 7 μm or less, and even more preferably 5 μm or less. The 50% particle size of the silica (c1) is, for example, 1 μm or more. The 99% particle size of silica (c1) is preferably 20 μm or less, more preferably 15 μm or less. The 99% particle size of silica is, for example, 3 μm or more. The volume-based cumulative distribution of the particle size of silica (c1) is obtained from the measurement results by a laser diffraction / scattering method.

[0044] The proportion of silica (c1) is preferably 75% by mass or more and 90% by mass or less with respect to the composition (X). The proportion is more preferably 78% by mass or more, and even more preferably 81% by mass or more. The proportion is more preferably 88% by mass or less, and even more preferably 87% by mass or less.

[0045] The composition (X) preferably contains a curing agent (D). The curing agent (D) is a component capable of reacting with the epoxy compound (A) to cure the composition (X). The curing agent (D) contains at least one selected from the group consisting of, for example, acid anhydrides, amines, phenolic resins, and thiols. The acid anhydride contains at least one selected from the group consisting of, for example, phthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, dodecylsuccinic anhydride, nadic anhydride, and trimellitic anhydride. The amine is a curing agent having at least two amino groups. Examples of the amino group include -NH2, monosubstituted NH2, disubstituted NH2, and trisubstituted NH2. The amine contains at least one selected from the group consisting of, for example, polyamines, modified polyamines, polyamide polyamines, and modified polyamide polyamines. The polyamine contains at least one selected from the group consisting of, for example, aliphatic polyamines (e.g., diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, m-xylenediamine, trimethylhexamethylenediamine, and 2-methylpentamethylenediamine, etc.), alicyclic polyamines (e.g., alicyclic-containing polyamines such as isophoronediamine, 1,3-bisaminomethylcyclohexane, bis(4-aminocyclohexyl)methane, norbornenediamine, and 1,2-diaminocyclohexane; and piperazine-type polyamines such as N-aminoethylpiperazine and 1,4-bis(2-amino-2-methylpropyl)piperazine), and aromatic polyamines (e.g., diaminodiphenylmethane, m-phenylenediamine, diaminodiphenylsulfone, diethyltoluenediamine, trimethylenebis(4-aminobenzoate), and polytetramethyleneoxide-di-p-aminobenzoate, etc.). The modified polyamine may be, for example, a product modified by epoxide addition, Michael addition, Mannich addition, thiourea addition, acrylonitrile addition, ketone blocking, etc. The polyamide polyamine may be, for example, a condensation product of a dimer acid and a polyamine.The modified polyamide polyamine may be, for example, an addition product of polyamide polyamine with an epoxy compound. The phenol resin contains at least one selected from the group consisting of, for example, phenol novolac resin, cresol novolac resin, naphthol novolac resin, bisphenol novolac resin, biphenyl novolac resin, dicyclopentadiene-phenol addition type resin, phenol aralkyl resin, naphthol aralkyl resin, triphenol methane type resin, tetraphenol ethane type resin, and amino triazine modified phenol resin. The thiol contains at least one selected from the group consisting of, for example, pentaerythritol tetrakis (3-mercaptopropionate), dipentaerythritol hexakis (3-mercaptopropionate), and trimethylolpropane tris (3-mercaptopropionate).

[0046] The curing agent (D) preferably contains an acid anhydride, which can suppress an increase in the viscosity of the composition (X) or can lower the viscosity of the composition (X).

[0047] The amount of the curing agent (D) relative to 1 equivalent of the epoxy group of the epoxy resin (A) is, for example, 0.3 equivalents or more and 1.3 equivalents or less. When the curing agent (D) contains an acid anhydride, the amount of the acid anhydride is preferably 0.3 equivalents or more and 1.3 equivalents or less relative to 1 equivalent of the epoxy group of the epoxy resin (A).

[0048] It is preferable that the composition (X) contains a curing accelerator (E). In this case, the curability of the composition (X) can be improved. It is preferable that the curing accelerator (E) contains a microcapsule-type latent curing accelerator (e1). In this case, the curability and storage stability of the composition (X) can be compatible, and the composition (X) can be realized with good storage stability while maintaining good curability of the composition (X) by heating at a relatively low temperature.

[0049] The microcapsule-type latent curing accelerator (e1) has a core containing a compound having catalytic activity and a shell covering the core. The shell is made of at least one of an organic polymer and an inorganic compound, for example. The latent curing accelerator (e1) contains, for example, a microencapsulated imidazole containing an imidazole as a compound having catalytic activity.

[0050] The ratio of the latent curing accelerator (e1) is preferably 3% by mass or more and 20% by mass or less relative to the epoxy compound (A). In this case, the curability and storage stability of the composition (X) can be better realized. The ratio is more preferably 5% by mass or more, and even more preferably 8% by mass or more. The ratio is preferably 16% by mass or less, and more preferably 12% by mass or less.

[0051] The curing accelerator (E) preferably contains only the latent curing accelerator (e1), but may contain a curing accelerator (e2) other than the latent curing accelerator (e1). The curing accelerator (e2) contains, for example, at least one of a curing accelerator having no latency and a latent curing accelerator not of a microcapsule type. The curing accelerator having no latency contains, for example, at least one component selected from the group consisting of imidazoles, cycloamidines, tertiary amines, organic phosphines, tetra-substituted phosphonium / tetra-substituted borates, quaternary phosphonium salts having counter anions other than borate, and tetraphenyl boron salts. The latent curing accelerator not of a microcapsule type may contain, for example, at least one of a solid dispersion type latent curing accelerator other than the microcapsule type curing accelerator (e1) and a liquid latent curing accelerator. When the curing accelerator (E) contains a latent curing accelerator (e1) and a curing accelerator (e2), the percentage of the curing accelerator (e2) to the curing accelerator (E) is preferably 40 mass% or less, and more preferably 20 mass% or less.

[0052] Composition (X) may further contain various additives, for example, composition (X) may contain at least one selected from the group consisting of a coupling agent, a pigment such as carbon black, a thixotropic agent, a release agent, a flame retardant, a flame retardant assistant, an ion trapping agent, a colorant, a tackifier, and the like.

[0053] The composition (X) may contain a solvent, but it is preferable that it does not contain a solvent.

[0054] It is preferable that the composition (X) does not contain any elastomer other than the components shown above. In this case, the increase in viscosity of the composition (X) and deformation such as warping of the cured product can be further suppressed. When the composition (X) contains an elastomer, the proportion of the elastomer is preferably 1% by mass or less based on the composition (X).

[0055] Composition (X) can be produced, for example, by mixing the above-mentioned components using a stirring mixer, a three-roll mill or the like.

[0056] It is preferable that composition (X) is liquid at 25°C. In particular, it is preferable that composition (X) has a viscosity of 800 Pa·s or less at 25°C. In this case, the moldability when composition (X) is molded by coating or the like can be particularly good. It is more preferable that the viscosity is 600 Pa·s or less, and even more preferable that the viscosity is 400 Pa·s or less. In addition, the viscosity is, for example, 40 Pa·s or more. The method for measuring the viscosity is shown in the Examples.

[0057] The composition (X) can be suitably used as a liquid encapsulant, particularly for preparing an encapsulant for wafer-level packaging. For example, the composition (X) can be molded by coating, etc., and then cured by heating, etc., to prepare an encapsulant made of a cured product of the composition (X).

[0058] The glass transition temperature of the cured product of the composition (X) is preferably 140°C or higher. In this case, the crack resistance of the cured product at high temperatures can be further improved. The glass transition temperature is more preferably 150°C or higher, and even more preferably 160°C or higher. The glass transition temperature is, for example, 190°C or lower. Such a high glass transition temperature can be achieved by appropriately adjusting the composition of the composition (X) within the range described above.

[0059] The fracture energy of the cured product of the composition (X) at 240°C is preferably 13 mJ or more. In this case, the crack resistance of the cured product at high temperatures can be further improved. The fracture energy is more preferably 14 mJ or more, and even more preferably 15 mJ or more. The fracture energy is, for example, 25 mJ or less. Such a high fracture energy can be achieved by appropriately adjusting the composition of the composition (X) within the range described above. The method for measuring the fracture energy is shown in the examples.

[0060] (Aspect) The curable resin composition according to the first embodiment contains an epoxy compound (A), an acrylic polymer (B), and an inorganic filler (C). The epoxy compound (A) contains a modified silicone-based epoxy compound (a1), an alicyclic epoxy compound (a2), and a compound (a3) ​​which is at least one of a novolac-type epoxy compound and a trisphenolmethane-type epoxy resin. The acrylic polymer (B) contains a liquid acrylic polymer (b1) which is liquid at 25°C.

[0061] According to this embodiment, the viscosity of the curable resin composition can be reduced, deformation of the cured product of the curable resin composition can be suppressed, and the crack resistance of the cured product can be improved.

[0062] In a second embodiment, the curable resin composition according to the first embodiment further contains a curing agent (D). The curing agent (D) contains an acid anhydride.

[0063] According to this embodiment, the reactivity of the curable resin composition can be increased, and the viscosity of the curable resin composition can be further reduced.

[0064] In a third embodiment, in the first or second embodiment, the ratio of the inorganic filler (C) to the curable resin composition is 75 mass % or more and 90 mass % or less.

[0065] According to this embodiment, deformation of the cured product can be further suppressed, and an increase in viscosity of the cured product can be suppressed.

[0066] In a fourth aspect, in any one of the first to third aspects, the liquid acrylic polymer (b1) has a weight average molecular weight of 5,000 or more and 40,000 or less.

[0067] According to this embodiment, deformation of the curable resin composition can be further suppressed, and an increase in viscosity of the curable resin composition can be further suppressed.

[0068] In a fifth aspect, in any one of the first to fourth aspects, the inorganic filler (C) contains silica (c1) having a 50% particle size of a volume-based cumulative distribution of 10 μm or less and a 99% particle size of a volume-based cumulative distribution of 25 μm or less.

[0069] According to this embodiment, it is easy to fill narrow gaps with the curable resin composition when molding the curable resin composition, and when a cured product of the curable resin composition is polished, the smoothness of the surface of the polished cured product can be increased.

[0070] In a sixth aspect, in any one of the first to fifth aspects, the curable resin composition further contains a curing accelerator (E). The curing accelerator (E) contains a microcapsule-type latent curing accelerator (e1).

[0071] According to this embodiment, the curability and storage stability of the curable resin composition can be improved.

[0072] In a seventh aspect, in any one of the first to sixth aspects, the ratio of the compound (a3) ​​to the epoxy compound (A) is 5% by mass or more and 30% by mass or less.

[0073] According to this embodiment, the crack resistance of the cured product of the curable resin composition can be further improved, and an increase in viscosity of the curable resin composition can be suppressed.

[0074] In an eighth aspect, in any one of the first to seventh aspects, the viscosity of the curable resin composition at 25 is 800 Pa·s or less.

[0075] According to this embodiment, the curable resin composition can have good moldability. EXAMPLES

[0076] The present disclosure will be specifically described with reference to examples, but the present disclosure is not limited to only these examples.

[0077] 1. Preparation of the Composition A composition was prepared by mixing the raw materials shown in Table 1. Details of the raw materials shown in Table 1 are as follows. - Inorganic filler #1: Silica. Product name EUF-3V manufactured by Tatsumori Co., Ltd. D50: 4 μm. D99: 10 μm. - Inorganic filler #2: Silica. Product name SO25H manufactured by Admatechs. D50: 0.6 μm. D99: 2 μm. -Epoxy compound #1: Difunctional modified silicone epoxy compound. Momentive Performance Materials Japan, product name TSL9906. Epoxy equivalent 181. -Epoxy compound #2: Difunctional alicyclic epoxy compound. Manufactured by Daicel Corporation. Product name: Cel2021P. Epoxy equivalent: 135. -Epoxy compound #3: Phenol novolac type epoxy resin. Manufactured by Mitsubishi Chemical Corporation. Product name jER-154. Epoxy equivalent 178. -Epoxy compound #4: Trisphenolmethane type epoxy resin. Manufactured by Nippon Kayaku Co., Ltd. Product name: EPPN-502H. Epoxy equivalent: 168. -Epoxy compound #5: Difunctional dicyclopentadiene type epoxy resin. ADEKA, product name EP-4088S. Epoxy equivalent 170. -Epoxy compound #6: Bisphenol F type epoxy resin. Manufactured by Nippon Steel Chemical & Material Co., Ltd. Product name: YDF8170. Epoxy equivalent: 160. -Epoxy compound #7: Difunctional isocyanate-modified epoxy resin. Manufactured by Asahi Kasei Corporation. Product name: AER4004. Epoxy equivalent: 390. -Hardening agent #1: Acid anhydride. Manufactured by Shin-Nippon Rika Co., Ltd. Product name: Rikacid HNA100. Acid anhydride equivalent: 179. -Hardener #2: Acid anhydride. Manufactured by New Japan Chemical. Product name: Rikacid MH700. Acid anhydride equivalent: 163.5. -Curing accelerator: Microcapsule type latent curing accelerator. Manufactured by Asahi Kasei Corporation, product name HXA9322HP. -Coupling agent: Silane coupling agent. Manufactured by Toray Dow Corning. Product name: A187. - Low stress agent #3: Liquid acrylic polymer with acryloyl groups at both ends, as shown in formula (1). Manufactured by Kaneka Corporation. Product name: RC200C. Liquid at 25°C (viscosity 530 Pa·s). Weight average molecular weight: 15,300. -Low stress agent #4: Liquid acrylic polymer with an acryloyl group at one end. Made by Kaneka Corporation. Product name: MM110C. Liquid at 25°C (viscosity 45 Pa·s). Weight average molecular weight: 12390. -Low stress agent #1: Acrylic block copolymer. Manufactured by Kuraray. Product name: Clarity LA-2140. Solid at 25°C. Weight average molecular weight: 69050. -Low stress agent #2: Silicone rubber powder. Shin-Etsu Chemical Co., Ltd. Product name: KMP-597. -Pigment: Carbon black. Mitsubishi Chemical Corporation, product name MA100.

[0078] 2. Evaluation (1) Viscosity (25℃) The viscosity of the composition was measured using a B-type rotational viscometer (product name: TVB-10H, manufactured by Toki Sangyo Co., Ltd.) at 25° C. and 5 rpm.

[0079] (2) Fracture energy (240℃) The composition was molded, heated at 120°C for 10 minutes, and then heated at 150°C for 60 minutes to prepare a test piece with a length of 40 mm, a width of 10 mm, and a thickness of 1 mm. A bending test was performed on this test piece using a bending tester (Instron 68TM-5 universal testing machine) under conditions of an ambient temperature of 240°C, a support distance of 30 mm, and a test speed of 100 μm / sec, to obtain a stress-strain curve until the test piece broke. The area under the curve of this stress-strain curve was calculated as the fracture energy of the test piece.

[0080] From the viewpoint of improving crack resistance at high temperatures, it can be evaluated that the fracture energy is preferably 13 mJ or more, more preferably 14 mJ or more, and even more preferably 15 mJ or more.

[0081] (3) Warping Using a TOWA molding machine (model number CPM-1080), the composition was compression molded on one side of a silicon wafer with a diameter of 12 inches (304.8 mm) and a thickness of 775 μm under conditions of a heating temperature of 130°C, a heating time of 10 minutes, and a compression pressure of 5 MPa, and then heated at a heating temperature of 150°C for a heating time of 60 minutes to produce a cured product (sealing material) with a thickness of 500 μm.

[0082] The warpage of the silicon wafer was evaluated by the following method. The silicon wafer was placed on a flat surface with the encapsulant facing upward. In this state, the center of the upper surface of the encapsulant was set as the reference point. Four measurement points were set at the ends of the upper surface of the encapsulant. These measurement points were set at the intersections of two imaginary lines that cross at the center of the encapsulant and the ends of the upper surface of the encapsulant. The Z-axis dimension (height dimension) between the flat surface and the reference point, as well as the Z-axis dimension (height dimension) between the flat surface and each measurement point were measured. A differential interference microscope (MM-40) manufactured by Nikon Corporation was used to measure the Z-axis dimension. The value obtained by subtracting the value of the Z-axis dimension of the reference point from the average value of the Z-axis dimensions of the four measurement points was taken as the warpage value.

[0083] It can be evaluated that the value of this warpage is preferably 11 mm or less, more preferably 10 mm or less, and even more preferably 9 mm or less.

[0084]

Table 1

[0085]

Table 2

Claims

1. An epoxy compound (A), An acrylic polymer (B), Contains an inorganic filler (C), The epoxy compound (A) contains a modified silicone-based epoxy compound (a1), an alicyclic epoxy compound (a2), and a compound (a3) ​​which is at least one of a novolac-type epoxy compound and a trisphenolmethane-type epoxy resin, The acrylic polymer (B) contains a liquid acrylic polymer (b1) that is liquid at 25°C. Curable resin composition.

2. Further containing a curing agent (D), The curing agent (D) contains an acid anhydride. The curable resin composition according to claim 1.

3. The ratio of the inorganic filler (C) to the curable resin composition is 75% by mass or more and 90% by mass or less. The curable resin composition according to claim 1 or 2.

4. The weight average molecular weight of the liquid acrylic polymer (b1) is 5,000 or more and 40,000 or less. The curable resin composition according to claim 1 or 2.

5. The inorganic filler (C) contains silica (c1) having a 50% particle size of a volume-based cumulative distribution of 10 μm or less and a 99% particle size of a volume-based cumulative distribution of 25 μm or less. The curable resin composition according to claim 1 or 2.

6. Further containing a curing accelerator (E), The curing accelerator (E) contains a microcapsule-type latent curing accelerator (e1); The curable resin composition according to claim 1 or 2.

7. The ratio of the compound (a3) ​​to the epoxy compound (A) is 5% by mass or more and 30% by mass or less. The curable resin composition according to claim 1 or 2.

8. The viscosity at 25 is 800 Pa s or less. The curable resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Semiconductor device

    JP1994069380A

  • Epoxy resin composition

    JP2017226824A

  • Resin composition

    JP2020138994A

  • Resin composition

    JP2018024774A