Polyethylene sealant film suitable for polyethylene mono-material

A polyethylene sealant film with a tailored layer structure addresses the rigidity-strength and tearability issues in monomaterial packaging, enhancing recyclability and reducing resin use.

JP2024143816APending Publication Date: 2024-10-11JAPAN POLYETHYLENE CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023056715
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional polyethylene monomaterial packaging materials lack a good rigidity-strength balance and tearability, particularly when laminated with uniaxially stretched polyethylene films, limiting their recyclability and practical application.

Method used

A polyethylene sealant film with a specific layer structure comprising outer, intermediate, and inner layers of polyethylene, cyclic olefin resin, and linear low-density polyethylene, optimized for density, modulus, and tear strength, ensuring a balanced rigidity, strength, and tearability.

Benefits of technology

The film provides a polyethylene monomaterial packaging solution with improved rigidity-strength balance and tearability, enabling easy tearing and recyclability, while reducing resin usage and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143816000001
    Figure 2024143816000001
  • Figure 2024143816000002
    Figure 2024143816000002
  • Figure 2024143816000003
    Figure 2024143816000003
Patent Text Reader

Abstract

To provide a mono-material sealant film which is excellent in a rigidity strength balance and tearing properties.SOLUTION: A polyethylene sealant film of a polyethylene mono-material resin laminate having a polyethylene sealant film for a polyethylene mono-material resin laminate laminated on a polyethylene base material film has a layer structure of at least three or more layers, and is formed by laminating an outer layer (A) composed of polyethylene (a) having a density of 0.910 to 0.940 g / cm3, an intermediate layer (B) composed of 20 to 70 wt.% of a cyclic olefinic resin (b1) and 30 to 80 wt.% of linear low density polyethylene (b2) having a density of 0.870 to 0.935 g / cm3, and an inner layer (C) composed of polyethylene (c) having a density of 0.870 to 0.930 g / cm3 in this order.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a monomaterial sealant film that is used for resin laminates such as polyethylene monomaterial packaging materials and has an excellent balance of rigidity and strength and tear resistance, a polyethylene monomaterial resin laminate that contains the monomaterial sealant film, and a packaging material composed of the laminate. [Background technology]

[0002] Conventionally, one of the basic structures of packaging materials is a substrate film and a sealant film bonded together with an adhesive. Of these, a film made of a polyethylene resin composition, which has moderate flexibility, transparency, and excellent heat sealability, is widely used as the sealant film. On the other hand, a film made of a polyester resin composition or a polyamide resin composition, which is stretched, is used as the substrate film from the viewpoints of rigidity, impact resistance, and heat resistance (Patent Document 1).

[0003] In recent years, with the growing demand for the creation of a recycling-oriented society, there is a demand for packaging materials with high recyclability. However, conventional packaging materials are composed of different resin materials as described above, and since it is difficult to separate each resin material, they are not currently recycled.

[0004] One method for achieving high recyclability is to construct a packaging material made entirely of the same resin material (mono-material packaging material).Since polyethylene resin compositions are widely used as raw materials for packaging materials, polyethylene mono-material packaging materials, in which both the base film and the sealant film are made of polyethylene resin compositions, are expected to be highly recyclable packaging materials that will help realize a recycling-oriented society.

[0005] Polyethylene mono-material packaging materials are generally composed of a polyethylene base film and a polyethylene sealant film, but examples of polyethylene sealant films for polyethylene mono-material packaging materials include a polyethylene mono-material packaging material that uses a polyethylene sealant film that uses linear low-density polyethylene that is available on the market (Patent Document 2), and a polyethylene mono-material packaging material that uses a polyethylene resin composition with specific resin properties in the polyethylene sealant film to improve processability during sealing (Patent Document 3).Furthermore, a polyethylene mono-material packaging material in which a uniaxially oriented polyethylene film and a polyethylene sealant are laminated with an adhesive (Patent Document 4) has also been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2009-202519 A [Patent Document 2] JP 2019-166810 A [Patent Document 3] Special Publication No. 2020-526412 [Patent Document 4] Patent No. 7192238 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the polyethylene mono-material packaging material does not use a polyester base film, which has better rigidity than a polyethylene base film, or a polyamide base film, which has better strength, and therefore has a problem of inferior rigidity-strength balance compared to packaging materials of general configuration. Also, a laminate of a uniaxially oriented polyethylene film and a polyethylene sealant film has a problem that it can be torn in the stretching direction of the uniaxially oriented polyethylene film, but cannot be torn in a direction perpendicular to the stretching direction. For these reasons, there has been a demand for the development of a mono-material packaging material that has a good rigidity-strength balance in polyethylene mono-material packaging materials and has good tearability in the stretching direction and in the direction perpendicular to the stretching direction when laminated with a uniaxially oriented polyethylene film. An object of the present invention is to provide a polyethylene sealant film suitable as a polyethylene sealant film in a polyethylene monomaterial packaging material, and a resin laminate and a packaging material using the same. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that a monomaterial sealant film or a monomaterial resin laminate exhibiting properties capable of solving the above problems can be obtained by using, as a polyethylene sealant, a laminate in which a polyethylene resin composition satisfying specific conditions is laminated onto a specific layer, and have completed the present invention based on these findings.

[0009] That is, according to the present invention [1], there is provided a polyethylene sealant film for a polyethylene monomaterial resin laminate to be laminated on a polyethylene substrate film, the polyethylene sealant film having a layer structure of at least three layers and a density of 0.910 to 0.940 g / cm 3 The outer layer (A) is made of polyethylene (a), 20 to 70% by weight of a cyclic olefin resin (b1), and has a density of 0.870 to 0.935 g / cm 3 An intermediate layer (B) consisting of 30 to 80% by weight of a linear low-density polyethylene (b2) having a density of 0.870 to 0.930 g / cm 3and an inner layer (C) made of polyethylene (c) laminated in this order.

[0010] According to the present invention [2], the polyethylene sealant film according to the present invention [1] has a tensile modulus measured with reference to JIS K7127, in which the load at 1% deformation in the machine direction (MD) satisfies formula (1), and the dirt drop impact (DDI) value measured with reference to JIS K7124 satisfies formula (2). Formula (1): (MD 1% deformation load) = 0.0259 × (film thickness) × 5 / 4 + 0.6473 Formula (2): (DDI) = 4.73 x (film thickness) x 5 / 4 - 161.04

[0011] According to the present invention [3], the cyclic olefin resin (b1) is an ethylene-cyclic olefin copolymer, and the polyethylene sealant film according to the invention [1] is characterized in that the ethylene / cyclic olefin content is 15-40 / 85-60 by weight.

[0012] According to the present invention [4], the ethylene-cyclic olefin copolymer has a glass transition point of 60°C or higher and 150°C or lower, in the polyethylene sealant film according to the invention [1].

[0013] According to the present invention [5], the polyethylene sealant film according to the invention [1] is characterized in that the cyclic olefin resin (b1) is contained in an amount of 5 to 25% by weight based on the entire polyethylene sealant film.

[0014] According to the present invention [6], the polyethylene resin composition (a) and the polyethylene resin composition (c) are linear low-density polyethylene, and the polyethylene resin composition (a), the linear low-density polyethylene (b2) and the polyethylene resin composition (c) have a melt index at 190°C of 0.1 to 30 g / 10 min., according to the polyethylene sealant film according to the invention [1].

[0015] According to the present invention [7], the polyethylene sealant film described in invention [1] is characterized in that the Elmendorf tear strength measured in accordance with JIS K7128-2 is 50 N / mm or less in the direction perpendicular to the machine direction (TD).

[0016] According to the present invention [8], the polyethylene sealant film according to the invention [1] is characterized in that, in a heat seal strength measurement performed with reference to JIS Z1713, the heat seal strength at 160°C satisfies formula (3). Formula (3): (160°C heat seal strength) = 0.187 x (film thickness) x 5 / 4 + 7.160

[0017] According to the present invention [9], there is provided a resin laminate comprising a layer made of the polyethylene sealant film described in invention [1].

[0018] According to the present invention

[10] , there is provided a resin laminate as described in claim 9, which comprises a layer of the polyethylene sealant film described in invention [1] as a sealant and comprises a polyethylene base film.

[0019] According to the present invention

[11] , there is provided a resin laminate as described in invention [9], characterized in that all of the layers constituting the resin laminate are polyethylene monomaterial resin laminates composed of a polyethylene resin composition.

[0020] According to the present invention

[12] , there is provided a packaging material as described in invention [9], in which an unstretched polyethylene substrate film is used as the polyethylene substrate as described in invention [1]. Effect of the Invention

[0021] The polyethylene sealant film of the present invention can provide a sealant film suitable for polyethylene mono-material packaging materials. In addition, by using a polyethylene base film and laminating it with the polyethylene sealant film of the present invention, a highly recyclable packaging material, particularly a mono-material laminate and packaging material composed of a single material, can be provided. Furthermore, compared to existing polyethylene sealant films, downgauging is possible, and easy tearing properties can be imparted when laminated with a uniaxially oriented polyethylene film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] 1. Polyethylene resin composition The polyethylene resin composition in the present invention refers to a resin composition used as a raw material for a polyethylene sealant film, which is an ethylene homopolymer or a copolymer with an α-olefin having 3 to 18 carbon atoms, and has an ethylene ratio of at least 50 mol% or more. The α-olefin having 3 to 18 carbon atoms is preferably one having 3 to 12 carbon atoms, and specific examples thereof include propylene, 1-butene, 1-hexene, 1-octene, and 4-methyl-1-pentene. The content of these α-olefins is preferably selected in a range of usually 30 mol% or less, preferably 20 mol% or less in total. Within this range, the flexibility and heat resistance of the film, etc., are improved. The content of α-olefins is determined under the following conditions: 13 This is a value measured by the C-NMR method. Equipment: JEOL-GSX270 manufactured by JEOL Concentration: 300mg / 2mL Solvent: ortho-dichlorobenzene The polyethylene resin composition means either a polyethylene resin alone or a polyethylene resin mixture, to which necessary additives may be added. Furthermore, in the present invention, the polyethylene resin composition may be referred to as polyethylene resin composition (x) (x is any of the letters a to c), which is a convenient way to distinguish between a plurality of polyethylene resin compositions that satisfy the requirements of the present invention among the polyethylene resin compositions used as a raw material for the polyethylene sealant film, and means a certain part of the polyethylene resin composition.

[0023] ·Classification of polyethylene resin composition Polyethylene resin compositions can be classified according to density and polymer structure. In the present invention, high density polyethylene (HDPE) has a density of 0.950 to 0.970 g / cm 3 and medium density polyethylene (MDPE) has a density of 0.931 to 0.949 g / cm 3 and linear low density polyethylene (LLDPE) has a density of 0.911 to 0.930 g / cm 3 Ultra-low density polyethylene (ULDPE) has a density of 0.870 to 0.910 g / cm 3 The density of low-density polyethylene (LDPE) is in the same region as that of LLDPE, but whereas LLDPE has a mainly linear structure, LDPE is a polyethylene resin composition with a polymer structure that has many branches.

[0024] Resin Blend The polyethylene resin composition used in the present invention may be a single resin, or may be a mixture of two or more resins to produce a polyethylene resin composition that satisfies the requirements of the present invention and then used. The polyethylene resin to be mixed may be a virgin resin obtained by homopolymerizing ethylene or copolymerizing ethylene and an α-olefin, a recycled resin obtained by mechanically recycling a used product containing polyethylene as a main component, or an ethylene polymer produced by employing a mass balance method certified by ISCC PLUS certification or the like.

[0025] Polymerization catalyst and polymerization method for virgin resin The virgin resin for constituting the polyethylene resin composition is produced using at least one of ethylene derived from petroleum raw materials, ethylene derived from biomass raw materials, and ethylene obtained by chemical recycling, and using a conventionally known catalyst such as a polymerization catalyst such as a Ziegler-Natta catalyst, a Phillips catalyst, or a metallocene catalyst. A Ziegler-Natta catalyst or a metallocene catalyst is preferable. In general, these catalysts are in a state where a complex composed of an organometallic compound is supported on a carrier such as silica or an Mg compound. The polymerization method may be any of the high pressure method, solution method, slurry method, and gas phase method. The high pressure method uses a radical source such as oxygen or peroxide, or a catalyst made of a metal complex as an initiator, and polymerizes ethylene, comonomer, and initiator in a reaction vessel under high temperature and high pressure conditions. Depending on the shape of the reaction vessel, it can be further divided into the tubular method and the autoclave method. The solution process is a polymerization method in which the polymer is dissolved in a hydrocarbon solvent at a temperature above the melting point of the polymer. The slurry process is a polymerization method in which a hydrocarbon compound such as hexane or isobutane is used as the solvent, and the produced polyethylene exists in the solvent as a slurry. Depending on the shape of the reaction vessel, it is broadly divided into two types: the autoclave process and the loop pipe process. The gas phase method is a polymerization method in which ethylene, an α-olefin as a comonomer, and hydrogen as a chain transfer agent are fed in a gaseous state from the bottom of a vertical reaction vessel, and a polymerization catalyst is then added (from Polyethylene Technical Reader, edited by Matsuura Kazuo and Mikami Naotaka). The gas phase method is preferred as a method for producing the polyethylene resin composition of the present invention.

[0026] The polyethylene resin compositions obtainable by these production methods have a wide range of combinations of density, melt flow rate (MFR) and other resin physical properties in order to meet the various applications known so far, but the present invention is characterized in that a polyethylene resin composition that satisfies the requirements of the present invention is selected and used from among them.

[0027] Additives The polyethylene resin composition used in the present invention may contain additives generally used for resin compositions, such as antioxidants, heat stabilizers, neutralizing agents, antiblocking agents, tackifiers, antistatic agents, slip agents, nucleating agents, foaming agents, crosslinking agents, biomass resources, biodegradation accelerators, and the like, within the scope of not impairing the object of the present invention.

[0028] 2. Polyethylene base film The polyethylene monomaterial resin laminate of the present invention comprises at least a polyethylene substrate film and a polyethylene sealant film. As the polyethylene substrate film, an unstretched substrate film, a stretched substrate film, an electron beam crosslinked film, or the like can be used, but an unstretched substrate film or a stretched substrate film is preferably used. The term "unstretched substrate film" refers to a film obtained by subjecting a polyethylene resin composition to inflation molding or T-die molding. The term "stretched substrate film" refers to a film obtained by stretching a film obtained by subjecting a polyethylene resin composition to inflation molding or T-die molding.

[0029] Polyethylene resin composition used The polyethylene resin composition used for the polyethylene substrate film is not particularly limited, and may be a virgin resin obtained by homopolymerizing ethylene or copolymerizing ethylene and an α-olefin, a recycled resin obtained by mechanically recycling a product whose main component is used polyethylene, or an ethylene polymer produced by adopting a mass balance method certified by ISCC PLUS certification, etc. Classifications include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and the resin composition for polyethylene substrate film may be a mixture of these. Furthermore, additives generally used for resin compositions, such as antioxidants, heat stabilizers, neutralizing agents, antiblocking agents, tackifiers, antistatic agents, slip agents, nucleating agents, foaming agents, crosslinking agents, biomass resources, and biodegradation promoters, may be blended within the scope of the present invention.

[0030] ·Unstretched polyethylene base film Examples of methods for producing the unstretched polyethylene substrate film include inflation molding, T-die molding, and calendar molding, with inflation molding and T-die molding being preferred from the viewpoints of production speed, ease of production, etc. Furthermore, the film may be a single-layer film or a multi-layer film. The manufacturing conditions for the unstretched polyethylene substrate film are not particularly limited, but the thickness of the film is preferably 5 μm to 100 μm, more preferably 10 μm to 90 μm, and further preferably 15 μm to 80 μm.

[0031] ·Stretched polyethylene base film The stretched polyethylene substrate film is obtained by stretching a raw material. Examples of the method for producing the raw material include inflation molding, T-die molding, and calendar molding, with inflation molding and T-die molding being preferred from the viewpoints of production speed and ease of production. The film may be a single-layer film using a single polyethylene resin composition, or a multi-layer film using multiple polyethylene resin compositions. Although the manufacturing conditions of the raw roll are not particularly limited, the thickness of the raw roll film is preferably 20 μm to 200 μm, more preferably 30 μm to 200 μm, and further preferably 50 μm to 200 μm.

[0032] · Stretching method for oriented polyethylene base film The stretched polyethylene substrate film may be a uniaxially stretched film or a biaxially stretched film. The stretching method may be any of longitudinal uniaxial stretching, transverse uniaxial stretching, sequential biaxial stretching, and simultaneous biaxial stretching.

[0033] ·Longitudinal stretch ratio of stretched polyethylene base film The stretching ratio in the longitudinal direction, i.e., the machine direction (MD) of the stretched polyethylene substrate film is preferably 2 times or more and 15 times or less, and more preferably 5 times or more and 10 times or less. It is more preferably 7 times or more. By increasing the stretching ratio in the machine direction (MD) of the stretched substrate film, the strength and heat resistance of the laminate of the present invention can be improved. Furthermore, the printability of the substrate can be improved. In addition, since the transparency of the substrate can be improved, when an image is formed on the surface of the substrate on the polyethylene sealant film side, the visibility of the image can be improved. On the other hand, the upper limit of the stretching ratio in the machine direction (MD) of the stretched substrate film is not particularly limited, but from the viewpoint of the breaking limit, it is preferably 15 times or less, more preferably 10 times or less.

[0034] -Transverse stretch ratio of stretched polyethylene base film The stretching ratio in the transverse direction, ie, TD, of the stretched polyethylene substrate film is preferably 1.5 times or more, and more preferably 2 times or more. By setting the TD stretch ratio of the stretched substrate film to 1.5 times or more, the strength and heat resistance of the laminate of the present invention can be improved. Furthermore, the printability of the substrate can be improved. In addition, since the transparency of the substrate can be improved, when an image is formed on the polyethylene sealant side surface of the substrate, the visibility of the image can be improved. On the other hand, the upper limit of the TD stretch ratio of the polyethylene stretched substrate film is not particularly limited, but it is preferably 10 times or less from the viewpoint of the breaking limit.

[0035] Biaxial stretching ratio of oriented polyethylene base film When the stretched polyethylene substrate film is stretched in both MD and TD, the stretching is preferably at least 1.5 times, more preferably at least 2 times. By increasing the stretching ratios in the MD and TD of the stretched polyethylene substrate film, the strength and heat resistance of the laminate of the present invention can be improved. Furthermore, the printability of the substrate can be improved. In addition, the transparency of the substrate can be improved, so that when an image is formed on the surface of the substrate on the polyethylene sealant film side, the visibility of the image can be improved. On the other hand, the upper limits of the stretching ratios in the MD and TD of the stretched polyethylene substrate film are not particularly limited, but from the viewpoint of the breaking point limit of the stretched polyethylene substrate film, the lower limit of the stretching ratios in the MD and TD is preferably 1.5 times, preferably 2 times, and the product of the MD stretching ratio and the TD stretching ratio is preferably 50 or less.

[0036] Multilayer oriented film The stretched substrate film made of the polyethylene resin composition may be a multilayer stretched film in which a plurality of films are laminated. Examples of resins that can be used include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), and ultra low density polyethylene (ULDPE). As for the lamination method, a co-extrusion film obtained by co-extrusion molding may be further stretched, or films may be bonded together using an adhesive.

[0037] 3.Polyethylene sealant film The polyethylene sealant film is a film that contains at least one layer (heat seal layer) made of a polyethylene resin composition, and is characterized in that this layer can be fused to form a seal. The polyethylene sealant film of the present invention has a layer structure of at least three layers and a density of 0.910 to 0.940 g / cm 3 The outer layer (A) is made of the polyethylene resin composition (a), and the cyclic olefin resin (b1) is 20 to 70% by weight, and the density is 0.870 to 0.935 g / cm 3 an intermediate layer (B) consisting of 30 to 80% by weight of a linear low-density polyethylene resin composition (b2) having a density of 0.870 to 0.930 g / cm3 and an inner layer (C) made of the polyethylene resin composition (c) are laminated in this order.

[0038] -Production method and conditions for polyethylene sealant film The polyethylene sealant film can be produced by a known technique. Specific examples include inflation molding, T-die molding, and calendar molding, with inflation molding and T-die molding being preferred. The thickness of the polyethylene sealant film is not particularly limited, but is preferably 10 to 200 μm, more preferably 30 to 180 μm, for the entire film. The sealant film of the present invention is preferably laminated by co-extrusion molding using inflation molding or T-die molding.

[0039] An outer layer (A) made of a polyethylene resin composition (a) The polyethylene resin composition (a) used in the outer layer (A) in the polyethylene sealant film of the present invention has a density of 0.910 to 0.940 g / cm 3 It is essential that the density is 0.915 to 0.935 g / cm. 3 and more preferably 0.920 to 0.930 g / cm 3 The density is 0.910g / cm 3 If it is less than this, there will be problems with film blocking and moldability, and if it is less than 0.940 g / cm 3 If the thickness is more than this, there is a concern that the visibility of the contents may decrease due to deterioration in transparency, and that the film may curl, resulting in a decrease in the ease of handling. The melt flow rate (MFR) at 190° C. under a load of 2.16 kg is preferably from 0.1 to 30 g / 10 min, more preferably from 0.5 to 20 g / 10 min, and further preferably from 1 to 10 g / 10 min.

[0040] ·Middle layer (B) The polyethylene sealant film of the present invention comprises 20-70% by weight of a cyclic olefin resin (b1) and 30-80% by weight of a linear low-density polyethylene resin composition (b2) having a density of 0.870-0.935 g / cm3. If the cyclic olefin resin (b1) is less than 20% by weight, the rigidity-strength balance and tearability of the film deteriorate. If the cyclic olefin resin (b1) is more than 70% by weight, the rigidity of the film becomes too high, and moldability deteriorates.

[0041] Cyclic olefin resin (b1) Examples of the cyclic olefin resin (b1) used in the intermediate layer (B) of the polyethylene sealant film of the present invention include norbornene polymers, vinyl alicyclic hydrocarbon polymers, cyclic conjugated diene polymers, etc. Among these, norbornene polymers are preferred. Examples of norbornene polymers include ring-opening polymers (hereinafter also referred to as "COP") of norbornene monomers, and norbornene copolymers (hereinafter also referred to as "COC") obtained by copolymerizing norbornene monomers with α-olefins such as ethylene. Hydrogenated products of COP and COC can also be used. In the present invention, the cyclic olefin resin (b1) is preferably COC because of its dispersibility in polyethylene. The COC is preferably an ethylene-cyclic olefin copolymer in which the linear monomer is ethylene. Furthermore, the cyclic monomer is preferably norbornene or the like.

[0042] Examples of COC include cyclic olefin copolymers obtained from linear monomers such as α-olefins, such as ethylene, propylene, butene-1, pentene-1, hexene-1, heptene-1, and octene-1, and cyclic monomers, such as tetracyclododecene and norbornene. More specifically, examples of COC include cyclic olefin copolymers obtained from the linear monomers and monocycloalkenes having 3 to 20 carbon atoms, bicyclo[2.2.1]-2-heptene (norbornene) and derivatives thereof, tricyclo[4.3.0.12,5]-3-decene and derivatives thereof, tetracyclo[4.4.0.1.2,5.17,10]-3-dodecene and derivatives thereof, pentacyclo[6.5.1.13,6.02,7.09,13]-4-pentadecene and derivatives thereof. pentacyclo[7.4.0.12,5.19,12.08,13]-3-pentadecene and its derivatives, pentacyclo[8.4.0.12,5.19,12.08,13]-3-hexadecene and its derivatives, pentacyclo[6.6.1.13,6.02,7.09,14]-4-hexadecene and its derivatives, hexacyclo[6.6.1.13,6.110,13.02,7.09,14]-4-hexadecene and its derivatives Putadecene and its derivatives, heptacyclo[8.7.0.12,9.14,7.111,17.03,8.012,16]-5-eicosene and its derivatives, heptacyclo[8.7.0.13,6.110,17.112,15.02,7.011,16]-4-eicosene and its derivatives, heptacyclo[8.8.0.12,9.14,7.111,18.03,8.012,17]-5-heneicosene Examples of the cyclic olefin copolymers include copolymers of cyclic olefins such as octacyclo[8.8.0.12,9.14,7.111,18.113,16.03,8.012,17]-5-docosene and its derivatives, nonacyclo[10.9.1.14,7.113,20.115,18.02,10.03,8.012,21.014,19]-5-pentacosene and its derivatives. The linear monomers and cyclic monomers can be used alone or in combination of two or more kinds. Such cyclic olefin copolymers can be used alone or in combination. The cyclic olefin resin (b) can also be used in combination with the COP and COC.In this case, it is possible to give different performance to the COP and COC.

[0043] In the present invention, the ethylene-cyclic olefin copolymer preferably has an ethylene / cyclic olefin content of 15-40 / 85-60 by weight. More preferably, it is 30-40 / 70-60. If the ethylene content is less than 15% by weight, the rigidity becomes too high, which is undesirable as it deteriorates the inflation moldability and the suitability for bag making. On the other hand, if the ethylene content is 40% by weight or more, it is undesirable as it is difficult to obtain sufficient tearability and rigidity. If the content is within this range, it is preferable as it improves the rigidity, tearability, processing stability, and impact strength of the film. Furthermore, the ethylene-cyclic olefin copolymer preferably has a glass transition temperature of 60 to 150°C. More preferably, it is 70°C to 140°C. If the glass transition temperature exceeds 150°C, the viscosity difference with polyethylene becomes too large, resulting in poor dispersibility and poor processing stability, and there is a possibility that sufficient tearability may not be obtained, which is not preferable. On the other hand, if the glass transition temperature is less than 60°C, sufficient rigidity may not be obtained, and there is a concern that the tearability may decrease. Furthermore, there is a possibility that sufficient tearability may not be obtained when exposed to a temperature above the glass transition temperature. The weight average molecular weight of the cyclic olefin resin (b1) is preferably from 5,000 to 500,000, and more preferably from 7,000 to 300,000. Commercially available products of such cyclic olefin resins (b1) include, for example, "ZEONOR" (COP) manufactured by Zeon Corporation, "APEL" (COC) manufactured by Mitsui Chemicals, Inc., and "TOPAS" (COC) manufactured by Polyplastics Co., Ltd. In the present invention, TOPAS grades 8007, 6013, and 6015 are preferred because the content ratio of norbornene monomer is within the above-mentioned range and because of processability and other reasons.

[0044] An inner layer (C) made of a polyethylene resin composition (c) The polyethylene resin composition (c) used in the outer layer (C) in the polyethylene sealant film of the present invention has a density of 0.870 to 0.930 g / cm 3 It is essential that the density is 0.880 to 0.927 g / cm. 3 and more preferably 0.890 to 0.925 g / cm 3 The density is 0.870g / cm 3 If it is less than this, there will be problems with film blocking and moldability, and if it is less than 0.930 g / cm 3 If this is the case, the sealing temperature will become high, and there is a possibility that the outer layer (A) or the base film arranged so as to be in contact with the outer layer (A) will be fused to the seal bar. The melt flow rate (MFR) at 190° C. under a load of 2.16 kg is not particularly limited, but is preferably 0.1 to 30 g / 10 min, more preferably 0.5 to 20 g / 10 min, and further preferably 1 to 10 g / 10 min.

[0045] Load at 1% deformation The polyethylene sealant film according to the present invention is characterized in that, in a tensile modulus measurement performed with reference to JIS K7127, the load at 1% deformation in the machine direction (MD) satisfies formula (1). Formula (1): (MD 1% deformation load (N)) = 0.0259 x (film thickness) x 5 / 4 + 0.6473 If the load at 1% MD deformation does not satisfy formula (1), it means that the rigidity of the film is low, which reduces the rigidity of the entire packaging material and reduces the amount of downgauge from the conventional packaging material.

[0046] Dirt Drop Impact (DDI) The polyethylene sealant film according to the present invention is characterized in that the DDI value measured with reference to JIS K7124 satisfies formula (2). Formula (2): (DDI(g)) = 4.73 x (film thickness) x 5 / 4 - 161.04 If the DDI value does not satisfy formula (2), it means that the impact resistance strength of the film is low, which reduces the impact resistance strength of the entire packaging material and reduces the amount of downgauge from the conventional packaging material.

[0047] Elmendorf tear strength The polyethylene sealant film of the present invention is characterized in that the Elmendorf tear strength measured in accordance with JIS K7128-2 is 50 N / mm or less in the direction perpendicular to the machine direction (TD). It is more preferably 40 N / mm or less, and even more preferably 30 N / mm or less. There is no particular restriction on the lower limit, but it is equal to or greater than the minimum value in the measurement of 0 N / mm. If the Elmendorf tear strength in the TD is 50 N / mm or more, the film cannot be torn well, which is undesirable.

[0048] Heat seal strength The polyethylene sealant film of the present invention is characterized in that, in a heat seal strength measurement performed with reference to JIS Z1713, the heat seal strength at 160° C. satisfies formula (3). Formula (3): (160°C heat seal strength (N / 15mm)) = 0.187 x (film thickness) x 5 / 4 + 7.160 If the heat seal strength at 160°C does not satisfy formula (3), when a polyethylene sealant film down-gauge is used to make a packaging material from a conventional packaging, there is a high possibility that the bag will break at the seal, which is not preferable.

[0049] 4.Other The polyethylene monomaterial resin laminate of the present invention refers to a resin laminate in which all or the main layers of the resin laminate are composed of a polyethylene resin composition. This resin laminate can be treated as a polyethylene monomaterial resin laminate composed only of a polyethylene resin composition. The proportion of the polyethylene resin composition, which is the main component, among the resin components in the polyethylene monomaterial resin laminate is not particularly limited, but is preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.

[0050] Surface treatment The base film and the sealant film are preferably subjected to a surface treatment, which can improve the adhesion between the adjacent layers. The method of surface treatment is not particularly limited, and examples thereof include physical treatments such as corona discharge treatment, ozone treatment, low-temperature plasma treatment using oxygen gas and / or nitrogen gas, and glow discharge treatment, as well as chemical treatments such as oxidation treatment using chemicals. Furthermore, an anchor coat layer may be formed on the surface of the substrate using a conventionally known anchor coat agent.

[0051] ·printing At least one surface of the base film or the sealant may have an image such as a letter, a pattern, a symbol, etc. It is preferable that the image is formed on the surface where the base film and the sealant film face each other, since this can prevent deterioration of the image over time. The method for forming the image is not particularly limited, and examples of the method include conventionally known printing methods such as gravure printing, offset printing, flexographic printing, etc. Among these, flexographic printing is preferred from the viewpoint of environmental load.

[0052] Vapor deposition film At least one surface of the base film or the sealant film may be provided with a vapor-deposited film, which may be a vapor-deposited film made of a metal such as aluminum, or an inorganic oxide such as aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, or barium oxide.

[0053] The thickness of the evaporated film is preferably 1 nm or more and 150 nm or less, more preferably 5 nm or more and 60 nm or less, and even more preferably 10 nm or more and 40 nm or less. By making the thickness of the vapor-deposited film 1 nm or more, the oxygen barrier property and water vapor barrier property of the laminate of the present invention can be further improved, and by making the thickness of the vapor-deposited film 150 nm or less, the occurrence of cracks in the vapor-deposited film can be prevented and the recyclability of the laminate of the present invention can be improved.

[0054] When the vapor-deposited film is an aluminum vapor-deposited film, the OD value is preferably 2 or more and 3.5 or less. This makes it possible to improve the oxygen barrier property and water vapor barrier property while maintaining the productivity of the laminate of the present invention. In the present invention, the OD value can be measured in accordance with JIS-K-7361.

[0055] The vapor deposition film can be formed by using a conventional method, for example, physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.

[0056] Also, for example, a composite film consisting of two or more layers of vapor-deposited films of different inorganic oxides can be formed and used by combining both physical vapor deposition and chemical vapor deposition. The degree of vacuum in the vapor deposition chamber is 10 -2 ~10 -8 After oxygen is introduced, the pressure is preferably about 10 -1 ~10 -6 The pressure is preferably about mbar. The amount of oxygen introduced varies depending on the size of the deposition machine. For the oxygen to be introduced, an inert gas such as argon gas, helium gas, or nitrogen gas may be used as a carrier gas to the extent that no problems occur. The film transport speed can be about 10 to 800 m / min.

[0057] The surface of the deposited film is preferably subjected to the above-mentioned surface treatment, which can improve adhesion to adjacent layers.

[0058] Coat At least one surface of the base film or sealant film may be provided with a heat-resistant coating layer or a barrier coating layer, which contains at least one resin material. Examples of the resin material for the coating layer include polyester, polyolefin, cellulose resin, (meth)acrylic resin, urethane resin, and vinyl resin.

[0059] The proportion of the resin material contained in the coating layer to the total weight of the laminate is preferably 3 mass % or less, and more preferably 1 mass % or less, which can improve the heat resistance and barrier property while maintaining the recyclability of the laminate of the present invention.

[0060] The thickness of the coating layer is preferably 0.1 μm or more and 5 μm or less, and more preferably 0.5 μm or more and 3 μm or less, which can improve the heat resistance and barrier property while maintaining the recyclability of the laminate obtained by using the stretched base film of the present invention.

[0061] ·glue An adhesive can be used to laminate the resin laminate. The adhesive used contains at least one resin composition, but is not particularly limited. Examples of adhesives that can be used include epoxy, acrylic, and urethane adhesives. The adhesive containing any of the above resin compositions is not particularly limited, but may be of one-component type, two-component type, or hot melt type, as required. In addition, the use of an adhesive with barrier properties, such as PASLIM (trade name) manufactured by DIC Corporation or Maxive (trade name) manufactured by Mitsubishi Gas Chemical Company, Inc., is preferable because it reduces the amount of other materials with barrier properties used and increases the proportion of polyethylene in the resin laminate.

[0062] 5. Packaging material The laminate of the present invention can be particularly suitably used for packaging material applications. The shape of the packaging material is not particularly limited and may be a packaging bag or a stand-up pouch. In the stand-up pouch, only the body part may be formed of the resin laminate, only the bottom part may be formed of the resin laminate, or both the body part and the bottom part may be formed of the resin laminate.

[0063] ·Packaging bag The bag-shaped packaging material can be produced by folding the laminate in half, overlapping it so that the heat seal layer of the laminate is on the inside, and heat sealing the ends. Alternatively, a bag-shaped packaging material can be produced by overlapping two laminates with their heat seal layers facing each other, and then heat sealing the ends.

[0064] ·Stand up pouch A packaging material in the form of a stand-up pouch can be produced by heat-sealing the laminate into a cylindrical shape with the heat-sealed layer on the inside to form a body, folding the laminate into a V-shape with the heat-sealed layer on the inside, sandwiching one end of the body, and heat-sealing to form a bottom.

[0065] The heat sealing method is not particularly limited, and can be performed by a known method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, etc.

[0066] The contents filled in the packaging material are not particularly limited, and may be liquid, powder, or gel. The contents may be food or non-food. After filling with the contents, the opening is heat-sealed to form a package. EXAMPLES

[0067] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In film molding, the machine direction in which the film flows is called MD, and the direction perpendicular to MD is called TD. The raw materials and evaluations used in the examples and comparative examples are as follows.

[0068] <Evaluation method> (1) MD 1% deformation load Measurements were made with reference to JIS K7127. Test pieces measuring 200 mm in length and 10 mm in width were cut in the MD. Using an ORIENTEC universal tensile testing machine (RTC-1210A), measurements were made by pulling 5 mm at a tensile speed of 2 mm / min and a chuck distance of 100 mm. The measurement data was automatically imported into A&D Corporation's analysis software (TACT), and the load at 1% deformation in the MD was calculated by processing the data on the software.

[0069] (2)DDI Measurements were made with reference to JIS K7124-1. The test machine used was the IM-302 Dart Impact Tester manufactured by Tester Sangyo Co., Ltd. The sample film was clamped in the clamp, and a weight holder was attached to the support at a height of 66 cm from the film surface. A weight (dart) consisting of an aluminum semicircular sphere with a diameter of 38 mm and a shaft with a length of 150 mm was set to an arbitrary weight and attached to the weight holder. In this state, the weight was allowed to fall freely, and it was judged visually whether the film surface was broken. The weight of each dart was measured five times, and if the film did not break all five times, the dart was made heavier by a certain percentage and measured again. If the film broke all five times, the dart was made lighter by a certain percentage and measured again. In this way, the weight was changed and measurements were completed when the weight of the dart that did not break all five times and the weight of the dart that broke all five times were determined. Finally, the 50% breaking mass (M50) and 50% breaking energy (E50) of the film sample were calculated using the following formulas [1] [2]. [1] M50=WS(T / 100-1 / 2) [2] E50 = M50 x g x H W: Minimum mass at which all tests break (g) S: Mass interval during repeated testing (g) T: Sum of the destruction rates of the five film samples for each test mass (%) H: Distance from the film sample surface to the tip of the dart (m) g:Gravity acceleration (9.81m / s 2 )

[0070] (3) TD Elmendorf tear strength With reference to JIS K7128-2, the TD Elmendorf tear strength was evaluated using a Digital Elmendorf tear tester (model SA) manufactured by Toyo Seiki Seisakusho Co., Ltd.

[0071] (4) Heat seal strength - Making heat seal samples Measurements were made with reference to JIS Z1713. A sample measuring MD×TD=200×150 (mm) was prepared, and this sample was folded in half in the TD so that the outer layer (A) was on the outside. This was then covered with a 12μm PET film and heat sealed parallel to the TD. The sealing conditions were a pressure of 0.2MPa, a sealing time of 1.0s, and a sealing temperature of 160℃.

[0072] Heat seal strength test The heat seal samples prepared above were cut into 15mm widths in the MD and used as test pieces to measure the strength using a universal tensile tester manufactured by ORIENTEC. The measurement conditions were a chuck distance of 50mm and a tensile speed of 500mm / min. Five measurements were taken, and the weighted average of the five measurements was used as the heat seal strength.

[0073] <Raw materials used> (1-1) Polyethylene (a) (c) "Novatec UF320" manufactured by Japan Polyethylene Corporation, MFR 0.9g / 10min, density 0.922g / cm 3 - Japan Polyethylene Corporation "Harmolex NF366A", MFR 1.5g / 10min, density 0.919g / cm 3 "Novatec UF943" manufactured by Japan Polyethylene Corporation, MFR 2.1g / 10min, density 0.938g / cm 3 - Japan Polyethylene Corporation "Harmolex NF324A", MFR 1.0g / 10min, density 0.906g / cm 3

[0074] (1-2) Cyclic olefin resin (b1) Polyplastics Co., Ltd. "TOPAS8007F-600"

[0075] (1-3) Linear low-density polyethylene (b2) · Linear low density polyolefin LL (b2-1) Linear low density polyethylene LL (b-2-2) "Novatec UF320" manufactured by Japan Polyethylene Corporation, MFR 0.9g / 10min, density 0.922g / cm 3 "Novatec UF943" manufactured by Japan Polyethylene Corporation, MFR 2.1g / 10min, density 0.938g / cm 3 - Japan Polyethylene Corporation "Harmolex NF324A", MFR 1.0g / 10min, density 0.906g / cm 3

[0076] [Example 1] Using an inflation molding machine, a three-layer co-extruded film was molded with the film configuration shown in Table 1. The physical properties of the film are shown in Table 1. [Example 2] Except for the film thickness being 100 μm, the results were the same as in Example 1. The physical properties of the film are shown in Table 1. [Example 3] Except for the film layer ratio being 1 / 2 / 1, the results were the same as in Example 1. The physical properties of the film are shown in Table 1. [Example 4] Except for the film thickness being 100 μm, the results were the same as in Example 3. The physical properties of the film are shown in Table 1. [Example 5] Using an inflation molding machine, a three-layer co-extruded film was molded with the film configuration shown in Table 1. The physical properties of the film are shown in Table 1. [Example 6] Except for changing the film thickness to 100 μm, the results were the same as in Example 5. The physical properties of the film are shown in Table 1. [Example 7] Except for the film thickness being 140 μm, the results were the same as in Example 5. The physical properties of the film are shown in Table 2. [Example 8] Using an inflation molding machine, a three-layer co-extruded film was molded with the film configuration shown in Table 1. The physical properties of the film are shown in Table 2. [Example 9] Except for changing the film thickness to 100 μm, the results were the same as in Example 8. The physical properties of the film are shown in Table 2. [Example 10] Except for the film thickness being 140 μm, the results were the same as in Example 8. The physical properties of the film are shown in Table 2. [Example 11] The film was produced in the same manner as in Example 8, except that the film layer ratio was 2 / 3 / 2. The physical properties of the film are shown in Table 2. [Example 12] The film was produced in the same manner as in Example 8, except that the film layer ratio was 1 / 2 / 1. The physical properties of the film are shown in Table 2.

[0077] [Comparative Example 1] Using an inflation molding machine, a three-layer co-extruded film was molded with the film configuration shown in Table 1. The physical properties of the film are shown in Table 3. [Comparative Example 2] Except for the film thickness being 100 μm, the results were the same as in Comparative Example 1. The physical properties of the film are shown in Table 3. [Comparative Example 3] Except for the film thickness being 140 μm, the results were the same as in Comparative Example 1. The physical properties of the film are shown in Table 3. [Comparative Example 4] Using an inflation molding machine, a three-layer co-extruded film was molded with the film configuration shown in Table 1. The physical properties of the film are shown in Table 3. [Comparative Example 5] Except for the film thickness being 100 μm, the results were the same as in Comparative Example 4. The physical properties of the film are shown in Table 3.

[0078] <Evaluation> As seen in Tables 1 to 3, the polyethylene sealant film of the present invention has an excellent balance of rigidity and strength, and has a higher heat seal strength at 160° C. than the comparative example of the same thickness. Furthermore, since it has easy tearability, it has excellent cuttability when laminated with a base film.

[0079] [Table 1]

[0080] [Table 2]

[0081] [Table 3]

[0082] According to the present invention, a polyethylene sealant film having excellent properties as a polyethylene monomaterial resin laminate can be provided. It is extremely useful as a sealant film to be used in applications of polyethylene monomaterial resin laminates in which both the substrate and the sealant film are composed of a polyethylene resin composition, and by downgauging the sealant film of a conventional polyethylene monomaterial resin laminate, the amount of resin used can be reduced, thereby contributing further to reducing the environmental burden.

Claims

1. A polyethylene sealant film for a polyethylene monomaterial resin laminate to be laminated on a polyethylene substrate film, the film having a layer structure of at least three layers and a density of 0.910 to 0.940 g / cm 3 An outer layer (A) made of polyethylene (a), a cyclic olefin resin (b1) of 20 to 70% by weight, and a density of 0.870 to 0.935 g / cm 3 and an intermediate layer (B) consisting of 30 to 80% by weight of a linear low-density polyethylene (b2) having a density of 0.870 to 0.930 g / cm 3 and an inner layer (C) made of a polyethylene resin composition (c) of the above-mentioned formula (1), which are laminated in this order.

2. 2. The polyethylene sealant film according to claim 1, wherein in a tensile modulus measurement performed with reference to JIS K7127, the load at 1% deformation in the machine direction (MD) satisfies formula (1), and further, the dart drop impact (DDI) value measured with reference to JIS K7124 satisfies formula (2). Formula (1): (Load at 1% deformation in MD) = 0.0259 × (film thickness) × 5 / 4 + 0.6473 Formula (2): (DDI) = 4.73 × (film thickness) × 5 / 4 - 161.04

3. The polyethylene sealant film according to claim 1, characterized in that the cyclic olefin resin (b1) is an ethylene-cyclic olefin copolymer, and the ethylene / cyclic olefin content is 15 to 40 / 85 to 60 by weight ratio.

4. The polyethylene sealant film according to claim 1, wherein the ethylene-cyclic olefin copolymer has a glass transition point of 60°C or higher and 150°C or lower.

5. The polyethylene sealant film according to claim 1, wherein the cyclic olefin resin (b1) is contained in an amount of 5 to 25% by weight based on the entire polyethylene sealant film.

6. The polyethylene sealant film according to claim 1, characterized in that the polyethylene (a) and the polyethylene resin composition (c) are linear low-density polyethylenes, and the polyethylene (a), the linear low-density polyethylene (b2), and the polyethylene resin composition (c) have melt indexes at 190°C of 0.1 to 30 g / 10 min.

7. The polyethylene sealant film according to claim 1, characterized in that the Elmendorf tear strength measured in accordance with JIS K7128-2 is 50 N / mm or less in a direction perpendicular to the machine direction (TD).

8. 2. The polyethylene sealant film according to claim 1, wherein the heat seal strength at 160° C. satisfies formula (3) in a heat seal strength measurement performed with reference to JIS Z1713. Formula (3): (160° C. heat seal strength)=0.187×(film thickness)×5 / 4+7.160

9. A resin laminate comprising a layer made of the polyethylene sealant film according to claim 1.

10. The resin laminate according to claim 9, comprising a layer of the polyethylene sealant film according to claim 1 as a sealant and a polyethylene substrate film.

11. 10. The resin laminate according to claim 9, wherein all layers constituting the resin laminate are a polyethylene monomaterial resin laminate constituted by the polyethylene resin composition.

12. The packaging material according to claim 9, wherein an unstretched substrate film is used as the polyethylene substrate film according to claim 1.

Citation Information

Patent Citations

  • Gas barrier film, packaging material, package

    JP2009202519A

  • Polyethylene laminate for packaging material and packaging material composed of laminate

    JP2019166810A

  • Multilayer polyethylene laminates and films for use in flexible packaging materials

    JP2020526412A

  • Polyethylene laminate for packaging material and packaging material made of said laminate

    JP7192238B2