Lead frame, conductive component and composite body
The implementation of a Ni-P plating layer on lead frames and conductive components addresses the issue of paste and resin spreading, enhancing the reliability and quality of these components by suppressing unwanted wetting and spreading.
Patent Information
- Application Number
- JP2023056742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The application of paste or resin on conductive components can lead to unwanted wetting and spreading due to capillary action, which can lower the reliability and quality of the conductive parts and increase the risk of defective products.
The use of a lead frame and conductive components with a plating layer containing a Ni-P layer, which has a dense crystal structure and smooth surface, effectively suppresses the spread of paste or resin.
The Ni-P layer prevents excessive wetting and spreading, ensuring the reliability of conductive parts and reducing the occurrence of defects.
Smart Images

Figure 2024143836000001_ABST
Abstract
Description
[Technical field]
[0001] This specification discloses technology relating to lead frames, conductive components and composites. [Background technology]
[0002] Lead frames and other conductive parts that are incorporated into electrical and electronic devices and through which current flows during use are often coated with paste or sealed with resin during the manufacture of the device.
[0003] For example, in the manufacture of semiconductor devices, during the so-called die bonding process, a paste containing a resin such as epoxy resin and metal powder (e.g., silver powder) is applied to the chip mounting portion of the lead frame. Then, with the semiconductor chip placed thereon, the paste is heated to sinter the metal powder. This fixes the semiconductor chip to the lead frame.
[0004] After the semiconductor chip is fixed to the lead frame, the semiconductor chip is sealed with silicone resin or the like, which results in the resin being bonded to a part of the lead frame. Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, when applying paste or bonding resin to the surface of a conductive part, the paste or resin may spread beyond the intended area due to capillary action on the surface, which may result in a decrease in reliability and other quality of the conductive part, or a decrease in yield due to the occurrence of defective products.
[0006] This specification provides a lead frame and a conductive part that can effectively suppress the wetting and spreading of a paste or resin on the surface, and a composite body in which the wetting and spreading is effectively suppressed. [Means for solving the problem]
[0007] The lead frame disclosed in this specification has a base material and a plating layer formed on the base material, the plating layer including a Ni-P layer containing Ni and P.
[0008] The conductive component disclosed in this specification has a substrate and a plating layer formed on the substrate, and the plating layer in at least a portion of a paste application area where a paste is applied and / or a resin bonding area where a resin is bonded includes a Ni-P layer containing Ni and P.
[0009] The composite disclosed in this specification is formed by joining a plurality of members together, and includes a first member and a second member included in the plurality of members, and a sintered portion interposed between the first member and the second member to join the first member and the second member, and a plating layer is formed on a base material of at least one of the first member and the second member, and at least a portion of the plating layer in a portion of the at least one member that contacts the sintered portion includes a Ni-P layer containing Ni and P. Effect of the Invention
[0010] The above-described lead frame and conductive part can effectively suppress the spreading of the paste or resin on the surface. The above-described composite is one in which the spreading of the paste or resin is effectively suppressed. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a partial cross-sectional view showing a substrate and a plating layer in one embodiment, taken along a direction perpendicular to the surface. [Diagram 2] FIG. 4 is a partial cross-sectional view taken along a direction perpendicular to the surface, illustrating a substrate and a plating layer in another embodiment. [Diagram 3] FIG. 11 is a partial cross-sectional view taken along a direction perpendicular to the surface, illustrating a substrate and a plating layer in yet another embodiment. [Figure 4]FIG. 11 is a partial cross-sectional view taken along a direction perpendicular to the surface, illustrating a substrate and a plating layer in yet another embodiment. [Diagram 5] 6 is a photograph showing the state of the silver powder paste in Samples A to E of Test Example 1 after hardening. [Figure 6] 13 is a photograph showing the appearance of Samples F to K of Test Example 2 after being sprayed with salt water. [Figure 7] 1 is an SEM image of Sample F in Test Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the above-mentioned lead frame, conductive part, and composite body will be described in detail. A lead frame, a conductive component, and a composite (hereinafter, sometimes referred to as a "lead frame, etc.") of one embodiment each have a base material 1 and a plating layer 2 formed on the base material 1, as exemplified in Fig. 1. The plating layer 2 includes a Ni-P layer 3 that contains Ni and P.
[0013] When a plating layer 2 including a Ni-P layer 3 containing Ni and P is formed on a substrate 1, the wetting and spreading of a paste or resin applied to or in contact with the surface is effectively suppressed. This is believed to be due to the fact that the Ni-P layer 3 has a dense crystal structure and a smooth surface. However, regardless of whether this reason is correct or not, as shown in the Examples section below, test results have been obtained that show that when a plating layer 2 including a Ni-P layer 3 is formed on a substrate 1, the wetting and spreading of a paste or resin is suppressed compared to the case of a Ni layer.
[0014] As shown in FIG. 2, the plating layer 12 may include a Ni-P layer 13 and an outermost layer 14 containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd, and Cu. As shown in FIG. 3, the plating layer 22 may include a Ni layer 25 containing Ni located between the substrate 21 and the Ni-P layer 23. As shown in FIG. 4, the plating layer 32 may include both an outermost layer 34 and a Ni layer 35 in addition to the Ni-P layer 33. Here, the details are mainly described using the embodiment shown in FIG. 1 as an example. Regarding each of the embodiments shown in FIGS. 2 to 4, only the configurations different from the embodiment shown in FIG. 1 will be described, but the other configurations may be the same as the embodiment shown in FIG. 1.
[0015] (base material) The material of the substrate 1 is not particularly limited and may be any metal or alloy. The material of the substrate 1 may be, for example, Cu (copper), Al (aluminum), or Fe (iron), or an alloy containing at least one of them. From the viewpoint of having high electrical conductivity and strength, the material of the substrate 1 is preferably Cu or a Cu alloy, more specifically, phosphor bronze, brass, Corson copper, oxygen-free copper, tough pitch copper, or the like. In particular, the material of the substrate 1 may be C11000, C10200, C19400, C70250, C26000, or C52100, or the like, which are standards set by the Copper Development Association (CDA). The dimensions and shape of the substrate 1 may be appropriately changed depending on the parts in which the lead frame or the like is used.
[0016] (Ni-P layer) The Ni--P layer 3 constituting at least a part of the plating layer 2 formed on the base material 1 contains Ni (nickel) and P (phosphorus).
[0017] The P content of the Ni-P layer 3 is preferably 8% by mass to 15% by mass. By setting the P content to 8% by mass or more, the Ni-P layer has an amorphous structure and becomes nonmagnetic, which reduces the transmission loss of the conductive member including the Ni-P layer. By setting the P content to 15% by mass or less, it is possible to suppress a decrease in the conductivity of the Ni-P layer due to the inclusion of P. More preferably, the P content is 10% by mass to 13% by mass. The remainder other than P is often substantially composed of Ni, but at least one selected from the group consisting of Cu, Pb and Zn may be contained as an impurity in a total amount of 15 ppm by mass or less.
[0018] The P content can be measured using an electron probe microanalyzer (EPMA, JXA-8500F manufactured by JEOL Ltd.). More specifically, the X-ray intensity at the P peak position (197.235 mm) of each of the standard specimen and the sample is measured using the electron probe microanalyzer, and the P content (at%) is calculated using the formula: P content (at%) = (average value of X-ray intensity of sample) ÷ (average value of X-ray intensity of standard specimen) × 50. The measurement conditions for the standard specimen are as follows: standard specimen: InP wafer (P content 50 at%), crystal used: PETH, X-ray used: Kα, acceleration voltage 15 kV, irradiation current 1 × 10-7 A, beam diameter 10 μm, and the X-ray intensity at the P peak position (197.235 mm) of the standard specimen is measured five times under these measurement conditions, and the average value is calculated. In the sample measurement, for a sample such as a lead frame having a Ni-P layer 3 formed on a substrate 1, the center of the sample is measured five times under the same measurement conditions as those for the standard sample, and the average value of the X-ray intensity at the P peak position (197.235 mm) is calculated.
[0019] The thickness of the Ni-P layer 3 is preferably 1 μm to 6 μm. If the thickness of the Ni-P layer 3 is less than 1 μm, pits and pinholes are likely to occur, and corrosion resistance may decrease. On the other hand, if the thickness of the Ni-P layer 3 exceeds 6 μm, there is a concern that cracks may occur when a lead frame or the like is bent due to the hardness of Ni-P. The thickness of the Ni-P layer 3 can be measured by a fluorescent X-ray film thickness meter. The thicknesses of layers other than the Ni-P layer 3 in the plating layer 2 can also be measured in the same manner.
[0020] To form the Ni-P layer 3 on the substrate 1, for example, a plating bath is a Ni sulfate bath, and Ni(II) sulfate hexahydrate or the like is added to the substrate 1 to set the Ni sulfate concentration to 205 g / L to 295 g / L, the phosphorous acid concentration to 68 g / L to 95 g / L, and the current density to 7 A / dm 2 ~13A / dm 2 The Ni-P layer 3 can be formed by setting the solution temperature at 55° C. to 65° C. The P concentration in the Ni-P layer 3 can be controlled by the current density. Specifically, the P concentration in the Ni-P layer 3 can be increased by lowering the current density. In other embodiments, the Ni-P layer 3 may be formed by electroless plating instead of electrolytic plating.
[0021] (top layer) As in the embodiment shown in Figures 2 and 4, the plating layers 12, 32 of the lead frame or the like preferably include an outermost layer 14, 34 containing at least one metal selected from the group consisting of Au (gold), Ag (silver), Sn (tin), Pd (palladium) and Cu (copper). In the illustrated example, the outermost layer 14, 34 is formed on the Ni-P layer 13, 33 on the outermost surface side (upper side in Figures 2 and 4).
[0022] The plating layers 12, 32 include the outermost layers 14, 34, thereby ensuring appropriate wettability of the paste to the outermost layers 14, 34. On the other hand, if the outermost layer contains a large amount of Ni, such as Ni-P, the surface oxidizes and becomes difficult to wet with the paste.
[0023] The thickness of the outermost layers 14, 34 may be 0.005 μm to 5 μm. If the thickness of the outermost layers 14, 34 is too thin, the wettability of the paste may decrease, whereas if the thickness is too thick, there is a concern that the paste and resin may easily wet and spread beyond the target range, and manufacturing costs may increase.
[0024] For example, when the outermost layer 14, 34 is formed by Au-Co plating (hard plating), the Au content of the outermost layer 14, 34 may be about 99.7% by mass. When the outermost layer 14, 34 is formed by pure Au plating (soft plating), the Au content of the outermost layer 14, 34 may be almost 100% by mass. When the outermost layer 14, 34 contains other metals (Ag (silver), Sn (tin), Pd (palladium) or Cu (copper)), the content of the metal may be almost 100% by mass. The metal content of the outermost layer 14, 34 can be measured by using an electron probe microanalyzer (EPMA, JXA-8500F manufactured by JEOL Ltd.). For example, the outermost layer 14, 34 may further contain Co, such as Au-Co. It is also possible to form two or more outermost layers 14, 34 of different materials.
[0025] To form the outermost layer 14, 34, the substrate 11, 31 on which the Ni-P layer 13, 33 has been formed can be plated using a plating solution appropriate for the material of the outermost layer 14, 34. For example, the plating solution may be EEJA Silbrex Bright HS for the outermost layer 14, 34 containing Ag, or a hard Au plating solution for the outermost layer 14, 34 containing Au. For example, in Ag plating, a current density of 5 A / dm 2 ~25A / dm 2 The solution temperature may be set to 30°C to 60°C. For example, in Au plating, the current density is set to 5 A / dm 2 ~60A / dm 2 The liquid temperature may be set to 50℃ to 60℃.
[0026] (Ni layer) As in the embodiment shown in Figs. 3 and 4, the plating layers 22, 32 preferably include Ni layers 25, 35 located between the substrates 21, 31 and the above-mentioned Ni-P layers 23, 33 from the viewpoint of improving corrosion resistance.
[0027] By interposing the Ni layers 25, 35 between the substrates 21, 31 and the Ni-P layers 23, 33, even if pinholes occur in the Ni-P layers 23, 33, the corrosive substances are blocked by the Ni layers 25, 35 below, and the corrosive substances are prevented from reaching the substrates 21, 31. As a result, corrosion resistance is improved. Note that the Ni-P layers 23, 33 are more susceptible to hydrogen gas generation than the Ni layers 25, 35, and therefore pinholes are more likely to form on the surface.
[0028] When the Ni layers 25, 35 are formed, the thickness of the Ni layers 25, 35 is preferably 1 μm to 6 μm. If the Ni layers 25, 35 are too thin, there is a concern that the blocking effect against corrosive substances will be insufficient, whereas if they are too thick, the surface smoothness of the outermost layer will decrease, and the paste or resin may easily wet and spread beyond the target range.
[0029] The Ni content of the Ni layers 25, 35 can be nearly 100 mass %. The Ni content of the Ni layers 25, 35 can be measured by using an electron probe microanalyzer (EPMA, JXA-8500F manufactured by JEOL Ltd.).
[0030] The Ni layers 25, 35 can be formed by, but not limited to, applying non-glossy, semi-glossy, roughened Ni plating to the substrates 21, 31. For example, a nickel sulfamate plating solution may be used as the plating solution, and the current density may be set to 3 A / dm 2 ~20A / dm 2 The liquid temperature may be set to 40°C to 60°C.
[0031] In the embodiment of Fig. 3, a Ni layer 25 and a Ni-P layer 23 are formed in this order on a substrate 21. In the embodiment of Fig. 4, an outermost layer 34 is further formed thereon, and the Ni layer 35, Ni-P layer 33, and outermost layer 34 are formed in this order from the substrate 31 side toward the surface side.
[0032] (Surface roughness) The arithmetic mean height Sa of the three-dimensional surface property (surface roughness) of the surface (surface exposed to the outside) of the lead frame or the like is preferably 0.2 μm or less. This makes it possible to effectively suppress the wetting and spreading due to the capillary phenomenon. The above surface means the surfaces of the Ni-P layers 3, 23 in Figures 1 and 3, and the surfaces of the outermost layers 14, 34 in Figures 2 and 4.
[0033] The arithmetic mean height Sa of the surface is in accordance with ISO25178 and means the average value of the absolute height from the mean plane of the surface, and can be measured using a laser microscope. More specifically, the surface is measured using a VK-X150 manufactured by Keyence Corporation at an observation magnification of 2000 times, a measurement area of 100 μm × 140 μm, and a spot diameter of φ0.8 mm, and the measurement data is the value obtained by setting the reference plane so that the reference plane is flat. The measurement point within a sample such as a lead frame can be one point at its center. When setting the sample in the laser microscope, the measurement is performed so that the inclination and warp are less than 1 degree.
[0034] (Lead frames, conductive parts, composites) The plating layer 2 as described above can be provided on a substrate 1 such as a lead frame or other conductive part or composite.
[0035] A lead frame is a conductive part that supports a semiconductor chip mounted on a semiconductor device and connects to external wiring, and may be composed of a die pad on which the semiconductor chip is placed and leads such as inner leads and outer leads around the die pad. Other conductive parts to which paste is applied or which are joined with resin include, for example, connectors. Such conductive parts are used in, for example, motors, secondary batteries, power control units (PCUs), electronic control units (ECUs), etc.
[0036] Conductive components such as lead frames may have a paste application region where a paste is applied and / or a resin bonding region where a resin is bonded on the surface. The paste may contain a metal powder such as silver powder. When paste is applied to such a paste application region or resin bonding region, or when molten resin flows into and contacts the paste application region or resin bonding region during insert molding, the paste or resin may wet and spread beyond the intended range due to capillary action, which may result in a decrease in reliability of the conductive component or the occurrence of defects.
[0037] In contrast, in this embodiment, the plating layer on the front surface of the conductive component includes a Ni-P layer, which effectively suppresses the spreading of the paste or resin, as described above, thereby ensuring the reliability of the conductive component and suppressing the occurrence of defective products.
[0038] The composite object here is a composite formed by joining a plurality of parts together, and has a first member and a second member as at least a part of the plurality of parts, and a sintered portion interposed between the first member and the second member to join the first member and the second member. At least one of the first member and the second member may be configured to include a base material and a plating layer formed on the base material.
[0039] To manufacture such a composite, a paste containing metal powder may be applied to a predetermined area (paste application area) on the surface of at least one of the first and second members, and the paste may be sandwiched between the first and second members and heated. This causes the metal powder in the paste to sinter into a sintered portion, which functions as an adhesive to bond the first and second members together.
[0040] In this embodiment, in such a composite, at least a part of the plating layer in the portion in contact with the sintered portion of at least one of the members having a plating layer formed on the base material includes a Ni-P layer. As a result, when a paste containing metal powder is applied to the paste application area on the surface of the portion in contact with the sintered portion, the composite is one in which the wetting and spreading of the paste is effectively suppressed. As a result, the composite has a sintered portion in a desired range and has excellent quality. EXAMPLES
[0041] Next, tests were carried out to verify the effects of the lead frame, conductive parts, and composite body described above, which will be described below. However, the description here is merely for illustrative purposes and is not intended to be limiting.
[0042] (Test Example 1) Two plate-shaped samples A to E were prepared, each having a pure copper substrate on which a plating layer including a Ni-P layer or Ni layer, an optional Pd layer, and an Au layer was formed in this order from the substrate side to the surface side, as shown in Table 1. The P concentration of the Ni-P layers was all 11 wt%.
[0043] [Table 1]
[0044] For each of the above samples A to E, silver powder paste (QMI519 manufactured by Henkel Ablestick) was applied to the surface, and after leaving it at room temperature for 1 hour, it was heated in an oven (DO-450A manufactured by AS ONE) at 175 ° C. for 1 hour to harden the silver powder paste. After that, using a stereo microscope (M125C manufactured by LEICA MICROSYSTEMS), the range of the wetted and spread part around the silver powder paste ((wetted and spread diameter - silver powder paste diameter) ÷ 2) was confirmed. The results are shown in Table 2. In addition, the state of the silver powder paste of samples A to E after hardening is shown in FIG. 5 by a photograph. Note that, as shown in FIG. 5, the diameter of the most wetted and spread diameter was measured by visual observation in the area where the paste shape after wetted and spread was not a perfect circle. In addition, in the area where the shape of the silver powder paste that was not wetted and spread was not a perfect circle, the distance between the two points where the straight line corresponding to the above-mentioned most wetted and spread diameter intersects with the outline of the silver powder paste that was not wetted and spread was measured as the silver powder paste diameter.
[0045] [Table 2]
[0046] As shown in Table 2, it can be seen that the area of the silver powder paste wetted and spread is smaller in samples A and B with Ni-P layers than in samples C to E with Ni layers. Since there is a correlation between the wettability of silver powder paste and the wettability of resin (e.g., epoxy resin used as sealing resin), it can be inferred that the wettability of resin will follow a similar trend.
[0047] Therefore, the above test showed that the formation of a Ni-P layer can effectively suppress the spreading of paste or resin.
[0048] The arithmetic mean height Sa of the three-dimensional surface properties (surface roughness) of samples A to E was measured by the method described above, and the results shown in Table 3 were obtained. Here, measurements were taken at one point in the center of each of two sheets of each of samples A to E, and the average value was taken as the arithmetic mean height Sa.
[0049] [Table 3]
[0050] From Table 3, it can be seen that there is not much difference in the arithmetic mean heights Sa of samples A to E. In addition, the outermost layers of samples A to E are all Au layers. Nevertheless, as described above, the results showed that the wetting and spreading was more suppressed in samples A and B than in samples C to E. From this, it is considered that the wetting and spreading can be suppressed by forming a Ni-P layer regardless of the surface roughness, although the reason is unclear.
[0051] (Test Example 2) On a flat plate (base material) made of pure copper, each plating was applied in sequence from left to right as shown below to form each plating layer, thereby producing metal materials of samples F to K. Sample F: Ni-P(P11wt%)1μm / Au-Co0.01μm Sample G: Ni-P(P11wt%)1μm / Pd0.015μm / Au-Co0.01μm Sample H: Matte Ni 1μm / Au-Co 0.01μm Sample I: Matte Ni 1 μm / Pd 0.015 μm / Au-Co 0.01 μm Sample J: Matte Ni 0.5μm / Ni-P (P11wt%) 0.5μm / Au-Co 0.01μm Sample K: Matte Ni 0.25μm / Ni-P (P11wt%) 0.75μm / Au-Co 0.01μm
[0052] Each of Samples F to K was subjected to salt spray for 24 hours under the following conditions, and then the appearance was observed. The appearance of each of Samples F to K is shown in FIG. Equipment: Suga Testing Machine ST-ISO-3 Concentration: Sodium chloride 50±5g / L pH: 6.5~7.2 Temperature: 35±2℃ Compressed air pressure: 98±10kPa Spray liquid collection amount: 1.5±0.5mL / h Horizontal sampling area: 80cm 2
[0053] As shown in Figure 6, samples F and G, which have a Ni-P layer as the base, have more severely corroded base materials than samples H and I, which have a Ni layer as the base, and there were some areas where the Cu of the base material was exposed and some green areas that were thought to be copper chloride.
[0054] Figure 7 shows an SEM image of sample F after salt spraying. It can be seen that there are numerous pinholes on the surface along the rolling marks. It is believed that these pinholes have deteriorated the corrosion resistance.
[0055] In contrast, in samples J and K, which had a Ni layer formed under the Ni-P layer, corrosion of the substrate was suppressed, as shown in Figure 6. This is thought to be because even if pinholes were to occur on the surface side of the Ni-P layer, the Ni layer would have prevented corrosive substances from reaching the substrate. For this reason, it can be said that by forming a Ni layer between the substrate and the Ni-P layer, it is possible to improve the corrosion resistance of lead frames and the like. [Explanation of symbols]
[0056] 1, 11, 21, 31 Base material 2, 12, 22, 32 plating layers 3, 13, 23, 33 Ni-P layer 14, 34 Top layer 25, 35 Ni layers
Claims
1. A lead frame having a base material and a plating layer formed on the base material, The plating layer includes a Ni--P layer containing Ni and P.
2. 2. The lead frame according to claim 1, wherein the P content of the Ni--P layer is 8% by mass to 15% by mass.
3. 3. The lead frame according to claim 1, wherein the Ni--P layer has a thickness of 1 μm to 6 μm.
4. 3. The lead frame according to claim 1, wherein the plating layer includes an outermost layer containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd and Cu.
5. 3. The lead frame according to claim 1, wherein the plating layer includes a Ni layer that contains Ni and is located between the base material and the Ni--P layer.
6. A conductive component having a substrate and a plating layer formed on the substrate, A conductive component, wherein the plating layer in at least a portion of a paste application region where a paste is applied and / or a resin joining region where a resin is joined includes a Ni-P layer containing Ni and P.
7. The conductive part according to claim 6, wherein the P content of the Ni--P layer is 8 mass % to 15 mass %.
8. 8. The conductive part according to claim 6, wherein the Ni--P layer has a thickness of 1 μm to 6 μm.
9. 8. The conductive part according to claim 6, wherein the plating layer includes an outermost layer containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd, and Cu.
10. 8. The conductive component according to claim 6, wherein the plating layer includes a Ni layer that contains Ni and is located between the substrate and the Ni--P layer.
11. A composite body formed by bonding a plurality of members to each other, The plurality of members include a first member and a second member, and a sintered portion is interposed between the first member and the second member to bond the first member and the second member, a plating layer is formed on a base material of at least one of the first member and the second member, A composite, wherein at least a portion of the plating layer in the portion of at least one of the members that contacts the sintered portion includes a Ni-P layer that contains Ni and P.
12. The composite according to claim 11, wherein the P content of the Ni-P layer is 8% by mass to 15% by mass.
13. The composite according to claim 11 or 12, wherein the Ni-P layer has a thickness of 1 μm to 6 μm.
14. The composite according to claim 11 or 12, wherein the plating layer includes an outermost layer containing at least one metal selected from the group consisting of Au, Ag, Sn, Pd, and Cu.
15. 13. The composite according to claim 11, wherein the plating layer includes a Ni layer containing Ni located between the substrate and the Ni--P layer.