Gas leakage inspection method and method for manufacturing columnar honeycomb structure filter
The gas leak inspection method using a mounting jig with O-rings addresses the issue of gaps in the particle deposition device, ensuring airtightness and improving the production efficiency of columnar honeycomb structure filters by identifying and rectifying issues before the film forming process.
Patent Information
- Application Number
- JP2023056771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
The production of columnar honeycomb structure filters is hindered by gaps that can form between the holder and chamber of the particle deposition device due to foreign matter or damage, leading to uneven ceramic particle adherence and reduced collection efficiency, resulting in defective products.
A gas leak inspection method using a mounting jig with embedded O-rings to ensure airtightness between the holder and chamber, involving a chuck mechanism, gas inlet and outlet, and flow rate measurement to detect leaks before the film forming process.
This method allows for the identification of potential gaps or leaks, ensuring that only leak-free structures undergo the film forming process, thereby improving the yield and reducing defective products.
Smart Images

Figure 2024143857000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for inspecting a columnar honeycomb structure for gas leakage prior to a film forming process, and also to a method for manufacturing a columnar honeycomb structure filter. [Background technology]
[0002] Exhaust gas emitted from internal combustion engines such as diesel engines and gasoline engines contains particulate matter (PM) such as soot. Soot is harmful to the human body, so its emission is regulated. Currently, in order to comply with exhaust gas regulations, filters such as DPF and GPF are widely used, which filter out soot and other PM by passing exhaust gas through a porous partition wall with small holes.
[0003] A known filter for capturing PM is a wall-flow type columnar honeycomb structure filter that includes a plurality of first cells extending in the height direction from the inlet side bottom surface to the outlet side bottom surface, having an open inlet side bottom surface and a plugged portion at the outlet side bottom surface, and a plurality of second cells that are arranged adjacent to the first cells with partition walls between them, extending in the height direction from the inlet side bottom surface to the outlet side bottom surface, having a plugged portion at the inlet side bottom surface and an open outlet side bottom surface.
[0004] In recent years, with the strengthening of exhaust gas regulations, stricter PM emission standards (PN regulations: Particle Matter number regulations) have been introduced, and filters are required to have high PM collection performance (high PN collection efficiency). Therefore, it has been proposed to form a layer for collecting PM on the surface of the cells (hereinafter also referred to as a "porous film" or "collection layer"). As a method for forming a porous film, a method is known in which an aerosol containing ceramic particles is supplied toward the bottom surface on the inlet side of a columnar honeycomb structure, and the particles are attached to the surface of the first cell, followed by heat treatment.
[0005] Patent Document 1 describes a particle attachment device for supplying an aerosol containing ceramic particles toward the inlet bottom surface of a columnar honeycomb structure. Specifically, the particle attachment device includes a holder for holding the columnar honeycomb structure, a blower for applying suction force to the outlet bottom surface of the columnar honeycomb structure, an aerosol generator for spraying an aerosol containing ceramic particles toward the inlet bottom surface from a direction perpendicular to the inlet bottom surface to attach the ceramic particles to the surface of the first cell, and a chamber provided between the nozzle of the aerosol generator and the inlet bottom surface for passing the aerosol through its interior and guiding it. According to Patent Document 1, the holder is connected to the downstream end of the side wall of the chamber. Patent Document 1 also describes that the holder has a chuck mechanism such as a balloon chuck for gripping the outer peripheral side wall of the columnar honeycomb structure.
[0006] According to Patent Document 1, the aerosol sprayed from the aerosol generator of the particle attachment device passes through the inside of a chamber by the suction force of a blower, and is then sucked into the first cells of the columnar honeycomb structure from the bottom surface of the inlet side of the columnar honeycomb structure held by a holder. The ceramic particles in the aerosol sucked into the first cells are attached to the surfaces of the first cells.
[0007] On the other hand, Patent Document 2, which is a technology related to a nuclear reactor, describes an opening and closing device for an access part to a reactor vessel, characterized in that a leak detection mechanism for detecting the occurrence of a leak between a ring member and a cover is provided on the cover. According to the leak detection mechanism, when air is supplied from a pump to a pipe while the cover is pressed against the ring member, the air is supplied through a detection port to a space between a large diameter O-ring and a small diameter O-ring attached to one end face of the ring member. Here, if the sealing effect of at least one of the end face large diameter O-ring and the end face small diameter O-ring is reduced due to the adhesion of foreign matter, a liquid level sensor detects the intrusion of water into the detection port, thereby making it possible to detect the occurrence of a leak between the cover and the ring member. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent Publication No. 2022-157612 [Patent Document 2] JP 2012-145479 A Summary of the Invention [Problem to be solved by the invention]
[0009] Considering the production efficiency of the columnar honeycomb structure filter and the maintainability of the particle attachment device, it is desirable that the holder is detachable from the chamber in the particle attachment device for supplying an aerosol containing ceramic particles. On the other hand, if the holder is detachable from the chamber, a gap may occur between the two due to foreign matter getting caught between them. Furthermore, a gap may occur between the two due to scratches or distortion of the holder or the chamber.
[0010] When a gap occurs between the holder and the chamber, the air that seeps in through the gap disrupts the flow of the aerosol. The air that seeps in through the gap also flows into the bottom surface of the inlet side of the columnar honeycomb structure. These phenomena cause uneven adhesion of the ceramic particles to the surface of the first cell, and the ceramic particles do not adhere sufficiently to the desired locations, adversely affecting the collection efficiency of the columnar honeycomb structure filter.
[0011] Since the collection efficiency of the columnar honeycomb structure filter can be inspected only after the columnar honeycomb structure filter is completed, if a large number of columnar honeycomb structure filters are manufactured without noticing the presence of gaps between the holder and the chamber, many defective products may be produced. Therefore, it is considered that the ability to inspect for the presence or absence of such gaps in advance will contribute to improving the yield.
[0012] In view of the above circumstances, an object of the present invention is to provide, in one embodiment, a gas leak inspection method before a film forming process is performed on a columnar honeycomb structure. Also, an object of the present invention is to provide, in another embodiment, a manufacturing method of a columnar honeycomb structure filter using the gas leak inspection method. [Means for solving the problem]
[0013] The inventors of the present invention have conducted extensive research to solve the above problems and have found that a method of testing for gas leaks by installing a specific mounting jig with two O-rings embedded between a chamber and a holder is useful. The present invention was completed based on this finding and is exemplified below.
[0014] [Aspect 1] A gas leak inspection method before a film forming process is performed on a columnar honeycomb structure, comprising: The columnar honeycomb structure includes an outer peripheral side wall, a plurality of first cells arranged on the inner peripheral side wall, extending from the inlet side bottom surface to the outlet side bottom surface, having an open inlet side bottom surface and having plugging portions on the outlet side bottom surface, and a plurality of second cells arranged on the inner peripheral side of the outer peripheral side wall, extending from the inlet side bottom surface to the outlet side bottom surface, having plugging portions on the inlet side bottom surface and having an open outlet side bottom surface, the plurality of first cells and the plurality of second cells are arranged alternately adjacent to each other with a porous partition wall interposed therebetween, preparing a mounting jig that is installed at an upper end of a chamber and has a mounting surface having an opening, a first O-ring that is embedded in the mounting surface so as to protrude partially upward and that runs around the outer periphery of the opening, and a second O-ring that is embedded in the mounting surface so as to protrude partially upward and that runs around the outer periphery of the first O-ring at a distance; a step of preparing a holder having a through hole extending in the vertical direction and capable of gripping a columnar honeycomb structure inserted into the through hole from an outer peripheral side wall side, a gas inlet, a gas outlet provided on a lower surface, and a gas passage communicating the gas inlet and the gas outlet; a step of holding the columnar honeycomb structure by a chuck mechanism of the holder; a step of pressing a lower surface of a holder holding the columnar honeycomb structure against the first O-ring and the second O-ring of the mounting jig, on the condition that the gas outlet is located between the first O-ring and the second O-ring; supplying gas through a gas inlet of the holder while maintaining the pressing step, and measuring the flow rate of the gas with a flow meter; determining whether a flow rate measured by the flow meter exceeds a predetermined threshold; The method includes: [Aspect 2] The method according to embodiment 1, wherein the gas pressure at the gas inlet of the holder when gas is supplied from the gas inlet is 0.01 to 0.05 MPaG. [Aspect 3] The method according to aspect 1 or 2, wherein the predetermined threshold is set to any value within a range of 0 to 0.10 L / min when converted into a state of 1 atmospheric pressure and 20° C. [Aspect 4] The method according to any one of aspects 1 to 3, wherein the gas is air. [Aspect 5] The method according to any one of aspects 1 to 4, wherein the opening in the mounting surface and the through hole of the chuck mechanism are coaxial. [Aspect 6] The method according to any one of aspects 1 to 5, wherein the wire diameter of the first O-ring and the second O-ring is 5.57 to 5.83 mm. [Aspect 7] The method according to any one of Aspects 1 to 6, wherein the first O-ring and the second O-ring are embedded so as to protrude upward from the mounting surface by 1.27 to 1.58 mm. [Aspect 8] A method according to any one of Aspects 1 to 7, wherein in the pressing, the first O-ring and the second O-ring are pressed by 0.3 mm or more. [Aspect 9] The method according to any one of aspects 1 to 8, wherein the first O-ring and the second O-ring have a type A durometer hardness of 65 to 75 as measured in accordance with JIS K6253-3:2012. [Aspect 10] The method according to any one of Aspects 1 to 9, wherein the first O-ring and the second O-ring are made of nitrile rubber. [Aspect 11] The method according to any one of aspects 1 to 10, wherein the distance between the first O-ring and the second O-ring is 3 mm or more. [Aspect 12] In the method for manufacturing a columnar honeycomb structure filter according to any one of aspects 1 to 11, if a step of determining whether the flow rate measured by a flow meter exceeds a predetermined threshold is carried out and it is determined that the flow rate does not exceed the threshold, a film-forming step is included in which, while maintaining the pressing step, an aerosol containing ceramic particles is sprayed from a nozzle of an aerosol generator into the chamber in a direction perpendicular to the inlet bottom surface of the columnar honeycomb structure toward the inlet bottom surface, while applying a suction force to the outlet bottom surface, thereby sucking the sprayed aerosol from the inlet bottom surface and adhering the ceramic particles to the surface of the first cell. Effect of the Invention
[0015] According to the gas leak inspection method of the embodiment of the present invention, it is possible to determine in advance whether or not a film forming process should be performed on a columnar honeycomb structure. Therefore, by performing the film forming process on the columnar honeycomb structure only when the inspection is passed, it is expected that the yield of columnar honeycomb structure filters will be improved. In particular, the inspection method is useful when a particle attachment device for supplying an aerosol containing ceramic particles has a holder that can be attached and detached to a chamber. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a perspective view illustrating an example of a columnar honeycomb structure filter. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an example of a columnar honeycomb structure filter, observed from a cross section parallel to a cell extension direction. [Diagram 3] FIG. 2 is a schematic enlarged partial view of the columnar honeycomb structure filter when observed from a cross section perpendicular to the cell extension direction. [Figure 4]FIG. 1 is a diagram illustrating a structural example of an aerosol generator. [Diagram 5] FIG. 2 is a schematic diagram for explaining a configuration example of a particle adhering device. [Figure 6] FIG. [Figure 7] 4 is a schematic cross-sectional view for explaining the positional relationship and structure of a holder, a mounting jig, and a chamber. FIG. [Figure 8] FIG. 13 is a schematic diagram for explaining a method for replacing a workpiece (a columnar honeycomb structure) to be placed in a particle adhesion device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Next, an embodiment of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiment, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of a person skilled in the art without departing from the spirit of the present invention.
[0018] <1. Columnar honeycomb structure filter> A columnar honeycomb structure filter according to one embodiment of the present invention will be described. The columnar honeycomb structure filter can be used as a DPF (Diesel Particulate Filter) and a GPF (Gasoline Particulate Filter) that collect soot and are attached to an exhaust gas line from an engine of a combustion device, typically a vehicle. The columnar honeycomb structure filter according to the present invention can be installed in an exhaust pipe, for example.
[0019] 1 and 2 are schematic perspective views and cross-sectional views of a columnar honeycomb structure filter 100. The columnar honeycomb structure filter 100 includes an outer peripheral side wall 102, a plurality of first cells 108 arranged on the inner peripheral side of the outer peripheral side wall 102, extending in parallel from an inlet side bottom surface 104 to an outlet side bottom surface 106, opening at the inlet side bottom surface 104 and having plugging portions 109 at the outlet side bottom surface 106, and a plurality of second cells 110 arranged on the inner peripheral side of the outer peripheral side wall 102, extending in parallel from the inlet side bottom surface 104 to the outlet side bottom surface 106, having plugging portions 109 at the inlet side bottom surface 104, and opening at the outlet side bottom surface 106. In this columnar honeycomb structure filter 100, the first cells 108 and the second cells 110 are arranged alternately adjacent to each other with porous partition walls 112 in between, so that the inlet side bottom surface 104 and the outlet side bottom surface 106 each have a honeycomb shape.
[0020] When exhaust gas containing particulate matter (PM) such as soot is supplied to the inlet side bottom surface 104 on the upstream side of the columnar honeycomb structure filter 100, the exhaust gas is introduced into the first cells 108 and proceeds downstream inside the first cells 108. Since the first cells 108 have plugged portions 109 on the outlet side bottom surface 106 on the downstream side, the exhaust gas passes through the porous partition walls 112 that separate the first cells 108 and the second cells 110 and flows into the second cells 110. Since the particulate matter cannot pass through the partition walls 112, it is collected and accumulated inside the first cells 108. After the particulate matter is removed, the clean exhaust gas that has flowed into the second cells 110 proceeds downstream inside the second cells 110 and flows out from the outlet side bottom surface 106 on the downstream side.
[0021] 3 shows a schematic enlarged partial view of the columnar honeycomb structure filter 100 when observed at a cross section perpendicular to the extending direction of the cells 108 and 110. A porous film 114 is formed on the surface of each of the first cells 108 of the columnar honeycomb structure filter 100 (the same as the surface of the partition walls 112 that define the first cells 108).
[0022] The porous film can be made of ceramics. For example, the porous film can contain one or more ceramics selected from cordierite, silicon carbide (SiC), talc, mica, mullite, cerium oxide, aluminum titanate, alumina, silicon nitride, sialon, zirconium phosphate, zirconia, titania, and silica. The main component of the porous film is preferably silicon carbide, alumina, silica, cordierite, or mullite. Among them, the main component of the porous film is preferably silicon carbide, since the presence of the surface oxide film (SiO) allows the porous film to be firmly bonded to each other and difficult to peel off. The main component of the porous film refers to a component that occupies 50% or more by mass of the porous film. The porous film is preferably made of SiC that occupies 50% or more by mass, more preferably 70% or more by mass, and even more preferably 90% or more by mass. The shape of the ceramics that constitute the porous film is not particularly limited, and examples thereof include granular and fibrous shapes.
[0023] The material constituting the partition walls and the outer peripheral side walls of the columnar honeycomb structure filter according to the present embodiment is not limited, but may be porous ceramics. Examples of the ceramics include cordierite, mullite, zirconium phosphate, aluminum titanate, silicon carbide (SiC), silicon-silicon carbide composites (e.g., Si-bonded SiC), cordierite-silicon carbide composites, zirconia, spinel, indialite, sapphirine, corundum, titania, and silicon nitride. These ceramics may contain one type alone or two or more types.
[0024] The columnar honeycomb structure filter may support a PM combustion catalyst that assists in the combustion of PM such as soot, an oxidation catalyst (DOC), an SCR catalyst and an NSR catalyst for removing nitrogen oxides (NOx), and a three-way catalyst that can simultaneously remove hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NOx). The columnar honeycomb structure filter according to this embodiment may also support various catalysts.
[0025] The bottom shape of the columnar honeycomb structure filter is not limited, and may be, for example, a round shape such as a circle, an ellipse, a racetrack shape, or an oval shape, or a polygonal shape such as a triangle or a rectangle. The columnar honeycomb structure filter 100 in FIG. 1 has a circular bottom shape and is cylindrical as a whole.
[0026] The height of the columnar honeycomb structure filter (the length from the bottom surface on the inlet side to the bottom surface on the outlet side) is not particularly limited, and may be set appropriately depending on the application and required performance. There is also no particular limit to the relationship between the height of the columnar honeycomb structure filter and the maximum diameter of each bottom surface (the maximum length of the diameters passing through the center of gravity of each bottom surface of the columnar honeycomb structure filter). Therefore, the height of the columnar honeycomb structure filter may be longer than the maximum diameter of each bottom surface, or the height of the columnar honeycomb structure filter may be shorter than the maximum diameter of each bottom surface.
[0027] Although there is no limitation on the shape of the cells in a cross section perpendicular to the cell extension direction, a quadrangle, a hexagon, an octagon, or a combination thereof is preferable. Among these, a square and a hexagon are preferable. By using such a cell shape, it is possible to reduce the pressure loss when a fluid is passed through the columnar honeycomb structure filter.
[0028] The columnar honeycomb structure filter can be provided as an integrally molded product. The columnar honeycomb structure filter can also be provided as a segment joint body, which is formed by joining together the side surfaces of a plurality of columnar honeycomb structure filter segments, each of which has an outer peripheral side wall. By providing the columnar honeycomb structure filter as a segment joint body, the thermal shock resistance can be improved.
[0029] <2. Manufacturing method of columnar honeycomb structure filter> The manufacturing method of the columnar honeycomb structure filter is exemplified below. First, a raw material composition containing a ceramic raw material, a dispersion medium, a pore former, and a binder is kneaded to form a puddle, and then the puddle is extruded to form a desired columnar honeycomb molded body. Additives such as a dispersant can be mixed into the raw material composition as necessary. In the extrusion molding, a die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used.
[0030] After drying the columnar honeycomb formed body, plugging portions are formed at predetermined positions on both bottom surfaces of the columnar honeycomb formed body, and the plugging portions are then dried to obtain a columnar honeycomb formed body having plugging portions. The columnar honeycomb formed body is then degreased and fired to obtain a columnar honeycomb structure. A porous film is then formed on the surfaces of the first cells of the columnar honeycomb structure to obtain a columnar honeycomb structure filter.
[0031] The ceramic raw material remains after firing and is a raw material of a part that constitutes the skeleton of the honeycomb structure as ceramics. As the ceramic raw material, a raw material that can form the above-mentioned ceramics after firing can be used. The ceramic raw material can be provided in the form of, for example, powder. As the ceramic raw material, raw materials for obtaining ceramics such as cordierite, mullite, zircon, aluminum titanate, silicon carbide, silicon nitride, zirconia, spinel, indialite, sapphirine, corundum, and titania can be mentioned. Specific examples of the ceramic raw material include, but are not limited to, silica, talc, alumina, kaolin, serpentine, pyroferrite, brucite, boehmite, mullite, magnesite, and aluminum hydroxide. The ceramic raw material may be used alone or in combination of two or more types.
[0032] In the case of filter applications such as DPF and GPF, cordierite can be suitably used as the ceramic. In this case, a cordierite-forming raw material can be used as the ceramic raw material. The cordierite-forming raw material is a raw material that becomes cordierite by firing. The cordierite-forming raw material preferably has a chemical composition of 30 to 45 mass % alumina (Al2O3) (including aluminum hydroxide converted to alumina), 11 to 17 mass % magnesia (MgO), and 42 to 57 mass % silica (SiO2).
[0033] The dispersion medium may be water or a mixed solvent of water and an organic solvent such as alcohol, with water being particularly preferred.
[0034] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include wheat flour, starch, foamed resin, water-absorbent resin, porous silica, carbon (e.g., graphite), ceramic balloons, polyethylene, polystyrene, polypropylene, nylon, polyester, acrylic, and phenol. The pore-forming material may be used alone or in combination of two or more types. From the viewpoint of increasing the porosity of the fired body, the content of the pore-forming material is preferably 0.5 parts by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, relative to 100 parts by mass of the ceramic raw material. From the viewpoint of ensuring the strength of the fired body, the content of the pore-forming material is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 4 parts by mass or less, relative to 100 parts by mass of the ceramic raw material.
[0035] Examples of the binder include organic binders such as methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. In particular, it is preferable to use methyl cellulose and hydroxypropyl methyl cellulose in combination. In addition, the content of the binder is preferably 4 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 6 parts by mass or more, relative to 100 parts by mass of the ceramic raw material, from the viewpoint of increasing the strength of the honeycomb molded body. The content of the binder is preferably 9 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 7 parts by mass or less, relative to 100 parts by mass of the ceramic raw material, from the viewpoint of suppressing the occurrence of cracks due to abnormal heat generation in the firing process. The binder may be used alone or in combination of two or more types.
[0036] The dispersant may be ethylene glycol, dextrin, fatty acid soap, polyether polyol, etc. The dispersant may be used alone or in combination of two or more. The content of the dispersant is preferably 0 to 2 parts by mass per 100 parts by mass of the ceramic raw material.
[0037] The method for plugging the bottom surface of the columnar honeycomb formed body is not particularly limited, and a known method can be adopted. The material of the plugging portion is not particularly limited, but is preferably ceramics from the viewpoint of strength and heat resistance. The ceramic is preferably a ceramic material containing at least one selected from the group consisting of cordierite, mullite, zircon, aluminum titanate, silicon carbide, silicon nitride, zirconia, spinel, indialite, sapphirine, corundum, and titania. It is even more preferable that the plugging portion has the same material composition as the main body of the honeycomb formed body, since the expansion coefficient during firing can be made the same, which leads to improved durability.
[0038] After drying the honeycomb formed body, degreasing and firing are performed to manufacture a columnar honeycomb structure. The conditions for the drying, degreasing and firing processes may be known conditions according to the material composition of the honeycomb formed body, and no particular explanation is required, but examples of specific conditions are given below.
[0039] In the drying step, for example, a conventionally known drying method such as hot air drying, microwave drying, dielectric drying, reduced pressure drying, vacuum drying, freeze drying, etc. Among them, a drying method in which hot air drying is combined with microwave drying or dielectric drying is preferred in that the entire molded body can be dried quickly and uniformly.
[0040] When plugging portions are formed, it is preferable to form plugging portions on both bottom faces of the dried honeycomb formed body and then dry the plugging portions. The plugging portions are formed at predetermined positions so that a plurality of first cells extending from the inlet side bottom face to the outlet side bottom face, having an opening at the inlet side bottom face and a plugging portion at the outlet side bottom face, and a plurality of second cells extending from the inlet side bottom face to the outlet side bottom face, having a plugging portion at the inlet side bottom face and having an opening at the outlet side bottom face are alternately arranged adjacent to each other with the porous partition wall therebetween.
[0041] Next, the degreasing step will be described. The combustion temperature of the binder is about 200°C, and the combustion temperature of the pore-forming material is about 300 to 1000°C. Therefore, the degreasing step may be carried out by heating the honeycomb formed body to a temperature in the range of about 200 to 1000°C. The heating time is not particularly limited, but is usually about 10 to 100 hours. The honeycomb formed body after the degreasing step is called a calcined body.
[0042] The firing step depends on the material composition of the honeycomb formed body, but can be performed, for example, by heating the calcined body to 1350 to 1600°C and holding it for 3 to 10 hours. In this way, a columnar honeycomb structure is produced, which includes a plurality of first cells extending from the inlet side bottom face to the outlet side bottom face, having an open inlet side bottom face and having plugging portions at the outlet side bottom face, and a plurality of second cells extending from the inlet side bottom face to the outlet side bottom face, having plugging portions at the inlet side bottom face and having an open outlet side bottom face, and in which the first cells and the second cells are alternately arranged adjacent to each other with the porous partition walls therebetween.
[0043] Next, a porous film is formed on the surface of the first cell of the columnar honeycomb structure that has been subjected to the firing process. First, a film-forming process is performed in which an aerosol containing ceramic particles is sprayed in a direction perpendicular to the inlet-side bottom surface of the columnar honeycomb structure, preferably toward the center of the inlet-side bottom surface, while a suction force is applied to the outlet-side bottom surface to suck in the sprayed aerosol from the inlet-side bottom surface, thereby adhering the ceramic particles to the surface of the first cell. Illustratively, the distance between the aerosol spray nozzle and the inlet-side bottom surface can be 500 mm to 2000 mm, and the aerosol spray speed can be 2 to 80 m / s.
[0044] The ceramic particles in the aerosol preferably have a median diameter (D50) of 1.0 to 6.0 μm, more preferably 2.0 to 5.0 μm, in the volume-based cumulative particle size distribution measured by a laser diffraction / scattering method. By spraying extremely fine ceramic particles, it is possible to increase the porosity while miniaturizing the average pore diameter of the resulting porous film.
[0045] As the ceramic particles, the above-mentioned ceramic particles constituting the porous film are used. For example, ceramic particles containing one or more selected from cordierite, silicon carbide (SiC), talc, mica, mullite, cerium oxide, aluminum titanate, alumina, silicon nitride, sialon, zirconium phosphate, zirconia, titania and silica can be used. The main component of the ceramic particles is preferably silicon carbide, alumina, silica, cordierite or mullite. The main component of the ceramic particles refers to a component that occupies 50% by mass or more of the ceramic particles. The ceramic particles are preferably made up of SiC at 50% by mass or more, more preferably at 70% by mass or more, and even more preferably at 90% by mass or more.
[0046] In order to prevent aggregation of the ceramic particles, it is advantageous to use an aerosol generator that includes a drive gas flow path for flowing pressurized drive gas, a supply port provided in the middle of the drive gas flow path and capable of sucking ceramic particles from the outer periphery of the drive gas flow path toward the inside of the drive gas flow path, and a nozzle attached to the tip of the drive gas flow path and capable of spraying the aerosol, in order to prevent aggregation of the ceramic particles. In one embodiment, the supply port can be configured so that the ceramic particles are introduced into the drive gas flow path from a direction approximately perpendicular to the flow direction of the drive gas flowing through the drive gas flow path.
[0047] When ceramic particles are introduced into the drive gas flow passage, they may be agglomerated. In particular, fine ceramic particles tend to agglomerate easily. However, when ceramic particles are supplied from the outer periphery of the drive gas flow passage toward the inside of the drive gas flow passage, the ceramic particles are more effectively disintegrated by the drive gas. This is believed to enable ceramic particles with reduced agglomeration to be sprayed from the nozzle of the aerosol generator.
[0048] (aerosol generator) FIG. 4 shows a schematic example of the structure of an aerosol generator 420 suitable for spraying ceramic particles with reduced aggregation. The aerosol generator 400 is a drive gas flow passage 407 for flowing a pressurized drive gas; a supply port 407i provided in the middle of the driving gas flow channel 407 and capable of sucking the ceramic particles 402 from the outer periphery of the driving gas flow channel 407 toward the inside of the driving gas flow channel 407; A nozzle 401 that is attached to the tip of a driving gas flow path 407 and is capable of injecting an aerosol; A flow path 403 for sucking and transporting ceramic particles 402, the flow path 403 having an outlet 403e communicating with a supply port 407i; a container 409 for containing the ceramic particles 402 and supplying the ceramic particles 402 to a flow path 403 for suction and transport; has.
[0049] The container 409 may be, for example, a funnel. The ceramic particles 402 adjusted to a predetermined particle size distribution are contained in the container 409. The ceramic particles 402 contained in the container 409 are transported from an outlet 409e provided at the bottom of the container 409 through the flow path 403 to an outlet 403e by the suction force from the drive gas flow path 407, and then introduced into the drive gas flow path 407 from a supply port 407i. At this time, the surrounding gas (typically air) sucked from the inlet 409i of the container 409 is also introduced into the drive gas flow path 407 through the flow path 403 together with the ceramic particles 402. In this embodiment, the outlet 403e and the supply port 407i are common. In this embodiment, the ceramic particles 402 are introduced into the drive gas flow path 407 from a direction approximately perpendicular to the flow direction of the drive gas flowing through the drive gas flow path 407.
[0050] The ceramic particles 402 supplied into the drive gas flow passage 407 collide with the drive gas flowing through the drive gas flow passage 407, and are crushed and mixed to become an aerosol, which is then sprayed from the nozzle 401. The nozzle 401 is preferably installed at a position and with a direction such that the aerosol is sprayed in a direction perpendicular to the inlet side bottom surface of the columnar honeycomb structure. More preferably, the nozzle 401 is installed at a position and with a direction such that the aerosol is sprayed in a direction perpendicular to the inlet side bottom surface toward the center of the inlet side bottom surface.
[0051] The ceramic particles 402 are preferably supplied to the container 409 using, but not limited to, a powder quantitative feeder 411 such as a screw feeder or a belt conveyor. The ceramic particles 402 discharged from the powder quantitative feeder 411 can be allowed to fall into the container 409 by gravity.
[0052] In a preferred embodiment, the drive gas flow passage 407 has a venturi section 407v in the middle where the flow passage is narrowed, and the supply port 407i is provided downstream of the most narrowed part of the venturi section 407v. When the drive gas flow passage 407 has the venturi section 407v, the speed of the drive gas passing through the venturi section 407v increases, so that the drive gas can be collided at a higher speed against the ceramic particles 402 supplied downstream of the venturi section 407v, improving the crushing force. In order to increase the crushing force of the drive gas, it is more preferable that the supply port 407i is provided downstream of the most narrowed part of the venturi section 407v and adjacent to the part. This configuration can be realized, for example, by connecting the drive gas flow passage 407 and the flow passage 403 for suction and transport using a venturi ejector 410.
[0053] From the viewpoint of increasing the disintegration force of ceramic particles, the lower limit of the flow velocity of the driving gas immediately before passing through the venturi portion 407v is preferably 13 m / s or more, more preferably 20 m / s or more, and even more preferably 26 m / s or more. The upper limit of the flow velocity of the driving gas immediately before passing through the venturi portion 407v is not particularly set, but is usually 50 m / s or less, typically 40 m / s or less.
[0054] The lower limit of the ratio of the flow passage cross-sectional area immediately before the venturi portion to the flow passage cross-sectional area of the venturi portion is preferably 8 or more, more preferably 16 or more, from the viewpoint of increasing the disintegration force. The upper limit of the ratio of the flow passage cross-sectional area immediately before the venturi portion to the flow passage cross-sectional area of the venturi portion is not particularly limited, but if it is too large, the pressure loss in the venturi portion increases, so it is preferably 64 or less, more preferably 32 or less. Here, the flow passage cross-sectional area of the venturi portion means the flow passage cross-sectional area at the narrowest point in the venturi portion. In addition, the flow passage cross-sectional area immediately before the venturi portion means the flow passage cross-sectional area immediately before the flow passage narrows on the upstream side of the venturi portion.
[0055] By using the Venturi ejector 410, for example, when the driving gas is flowed through the driving gas flow path 407, a large suction force can be applied to the flow path 403 for suction and transport, and the flow path 403 for suction and transport can be prevented from being clogged with the ceramic particles 402. The Venturi ejector 410 is also effective as a means for removing the ceramic particles 402 when the flow path 403 for suction and transport is clogged with the ceramic particles 402.
[0056] The flow rate of the aerosol sprayed from the nozzle 401 can be controlled by using a compressed gas such as pressure-adjusted compressed air as the driving gas. It is preferable to use dry air (e.g., with a dew point of 10°C or less) as the driving gas in order to suppress the aggregation of ceramic particles. In this specification, the "dew point" refers to a value measured by a polymer-type capacitance dew point meter conforming to JIS Z8806:2001.
[0057] Fine ceramic particles have a tendency to aggregate easily. However, by using the aerosol generator 400 according to this embodiment, it is possible to spray ceramic particles with a desired particle size distribution in which aggregation is suppressed.
[0058] (Particle Adhesion Device) FIG. 5 shows a schematic configuration example of a particle attachment device 510 suitable for carrying out a film forming process in which ceramic particles are attached to the surfaces of the first cells of a pillar-shaped honeycomb structure. The particle attachment device 510 includes: a holder 514 for holding the columnar honeycomb structure 500; A blower 512 for applying suction force to the outlet side bottom surface 506 of the columnar honeycomb structure 500; an aerosol generator 511 for spraying an aerosol containing ceramic particles toward the inlet side bottom surface 504 in a direction perpendicular to the inlet side bottom surface 504 to cause the ceramic particles to adhere to the surface of the first cell; A chamber 513 is provided between the nozzle 511a of the aerosol generator 511 and the inlet side bottom surface 504, for passing the aerosol through its interior and guiding it; Equipped with.
[0059] The holder 514 is configured so as to be able to hold the columnar honeycomb structure 500 at a position facing the nozzle 511a of the aerosol generator 511 with the inlet side bottom surface 504 exposed. For example, the holder 514 has a main body portion 514a. The main body portion 514a has a through hole 514c extending in the vertical direction, and can have a chuck mechanism 514b for holding the columnar honeycomb structure 500 inserted into the through hole 514c from the outer peripheral side wall 502 side. The chuck mechanism 514b is not particularly limited, but a balloon chuck is exemplified. The material of the main body portion 514a of the holder 514 is not particularly limited, but can be made of plastic such as nylon, for example.
[0060] The holder 514 holding the columnar honeycomb structure 500 is preferably surrounded by a housing 520 in order to straighten the aerosol that has passed through the columnar honeycomb structure 500 in one direction without diffusing when performing a film forming process. The housing 520 may be attached and detached manually, but it is also possible to automate the up and down movement of the housing by connecting the housing 520 to an electric cylinder 570 such as a ROBO Cylinder, a single-axis actuator, or a single-axis robot. It is also possible to press the lower surface 514f of the holder 514 holding the columnar honeycomb structure 500 against a first O-ring 533 and a second O-ring 534 of a mounting jig 530 described later through the housing 520 by the pressing force from the electric cylinder 570.
[0061] Side wall 513d of chamber 513 can be formed in a tubular shape such as a cylindrical shape or a square tube. Chamber 513 has surface 513a facing inlet side bottom surface 504. Surface 513a facing inlet side bottom surface 504 has insertion port 513b for nozzle 511a of aerosol generator 511. With this configuration, aerosol sprayed from aerosol generator 511 can be directly introduced into chamber 513.
[0062] The opposing surface 513a is provided at a lower end 513f of the chamber 513 (typically, at an upstream end of the side wall 513d). The side wall 513d and / or the surface 513a facing the inlet bottom surface 504 may be provided with an opening 513c for taking in ambient gas. This allows the flow rate of gas flowing into the chamber 513 to be adjusted according to the suction force from the blower 512. However, as shown in FIG. 5, it is preferable that the side wall 513d of the chamber 513 does not have an opening 513c for taking in ambient gas, and the ambient gas flowing into the chamber 513 is taken in only from the opening 513c provided in the surface 513a facing the inlet bottom surface 504.
[0063] By taking in the ambient gas only from the surface 513a facing the inlet bottom surface 504, the ambient gas flows in in the same direction as the flow direction of the sprayed aerosol, which is advantageous in that there is no disturbance to the aerosol and the aerosol is stable. Conversely, if the side wall 513d of the chamber 513 has an opening 513c, the ambient gas flowing in from there is likely to cause disturbance, which is disadvantageous in that the flow of the aerosol becomes unstable. Therefore, in a preferred embodiment, the surface 513a facing the inlet bottom surface 504 has one or more openings 513c for taking in the ambient gas into the chamber 513, and has no openings for taking in the ambient gas into the chamber 513 other than the facing surface 513a.
[0064] In one embodiment, the opposing surface 513a may be made of a punched plate and / or a nonwoven fabric. Furthermore, since the opening 513c may be entangled with agglomerated powder, honeycomb fragments, and dust, a filter 513g may be installed.
[0065] A mounting jig 530 is installed at an upper end 513e of the chamber 513 (typically, a downstream end of the side wall 513d). The mounting jig 530 may be configured to be able to fit into the inner peripheral surface of the side wall 513d of the chamber 513. The mounting jig 530 may also have a flange portion 535 that can come into contact with the upper end 513e of the chamber 513. FIG. 6 shows a schematic plan view of the mounting jig 530. Referring to FIG. 6, the mounting jig 530 is installed on the inner peripheral side of the side wall 513d of the chamber 513, and has a mounting surface 532 having an opening 531, a first O-ring 533 embedded in the mounting surface 532 so as to protrude upward in part and surrounding the outer peripheral side of the opening 531, and a second O-ring 534 embedded in the mounting surface 532 so as to protrude upward in part and surrounding the first O-ring 533 at a distance S on the outer peripheral side. The material of the mounting jig 530 is not particularly limited, but it may be made of a plastic material such as nylon.
[0066] It is preferable that the opening 531 of the mounting surface 532 and the through hole 514c of the chuck mechanism 514b are coaxial, since this allows the aerosol to flow in a well-balanced manner into the inlet side bottom surface 504 of the columnar honeycomb structure 500. For example, when the outer shape of the columnar honeycomb structure 500 is cylindrical, it is preferable that the opening 531 of the mounting surface 532 and the through hole 514c of the holder 514 are concentrically arranged.
[0067] The shape and size of the opening 531 of the mounting surface 532 preferably correspond to the shape and size of the bottom surface of the columnar honeycomb structure 500. This makes it possible to stabilize the flow of the aerosol flowing into the inlet side bottom surface 504 of the columnar honeycomb structure 500.
[0068] 7, the holder 514 has a gas inlet 514d, a gas outlet 514e provided on a lower surface 514f, and a gas passage 514g connecting the gas inlet 514d and the gas outlet 514e. The gas passage 514g can be provided, for example, inside the main body portion 514a of the holder 514. A gas pipe 561 can be connected to the gas inlet 514d of the holder 514 so as to supply a gas for testing. A flowmeter 562 can be installed midway along the gas pipe 561 to measure the flow rate of the gas.
[0069] There is no particular limitation on the location where gas inlet 514d is installed, and as long as gas piping 561 can be connected, it may be on any of the outer peripheral side surface, inner peripheral side surface, upper surface, or lower surface of holder 514. In the embodiment shown in Fig. 7, gas inlet 514d is installed on the outer peripheral side surface of holder 514. Installing gas inlet 514d on the outer peripheral side surface of holder 514 is preferable because gas piping 561 can be easily connected.
[0070] Gas outlet 514e provided on lower surface 514f of holder 514 is located between first O-ring 533 and second O-ring 534. With this configuration, when an inspection method described later is performed, it can be determined whether or not a predetermined airtightness is present in the space between first O-ring 533 and second O-ring 534, which is sandwiched between lower surface 514f of holder 514 and mounting surface 532 of mounting jig 530.
[0071] If the first O-ring 533 and the second O-ring 534 are embedded so that a portion of them protrudes upward from the mounting surface 532, when the step of pressing the lower surface 514f of the holder 514 against the mounting surface 532 of the mounting jig 530 is performed, the lower surface 514f of the holder 514 comes into contact with the first O-ring 533 and the second O-ring 534. At this time, the first O-ring 533 and the second O-ring 534 are crushed by the pressing pressure, and therefore a certain amount of airtight space is created between the first O-ring 533 and the second O-ring 534 unless there is a defect.
[0072] For example, the first O-ring 533 and the second O-ring 534 can be embedded so as to protrude 1.27 to 1.58 mm upward from the mounting surface 532. In the pressing step, from the viewpoint of increasing airtightness, the first O-ring 533 and the second O-ring 534 are preferably pressed by 0.3 mm or more, more preferably pressed by 0.5 mm or more, and even more preferably pressed by 0.7 mm or more. The pressing step can adopt the same conditions when performing the film forming step and when performing the gas leak inspection described later. Therefore, it is possible to perform the film forming step successively while maintaining the pressing conditions when performing the gas leak inspection method.
[0073] The specifications of the first O-ring 533 and the second O-ring 534 are not particularly limited and may be appropriately selected in consideration of the purpose of the inspection. However, it is desirable that the specifications of the first O-ring 533 and the second O-ring 534 are the same except for the difference in the opening area (diameter), such as the wire diameter (meaning the circle equivalent diameter of the cross section perpendicular to the circumferential direction), the height protruding upward from the mounting surface 532, and the material, in order to improve the airtightness of the space between the first O-ring 533 and the second O-ring 534. For example, the wire diameter of the first O-ring 533 and the second O-ring 534 may be 5.57 to 5.83 mm. In addition, the type A durometer hardness of the first O-ring 533 and the second O-ring 534 measured in accordance with JIS K6253-3:2012 may be 65 to 75. The material of the first O-ring 533 and the second O-ring 534 may be rubber such as nitrile rubber.
[0074] The interval S between the first O-ring 533 and the second O-ring 534 is not particularly limited, and it is sufficient if the interval S is sufficient to carry out the gas leak inspection method, taking into consideration the dimensions of the gas outlet 514e (e.g., 2 to 4 mm in circle equivalent diameter). However, if the interval S is too large, the time required for the gas leak inspection will be long. Therefore, the interval S can be, for example, 3 mm or more, typically 3 to 10 mm, and more typically 4.5 to 8.5 mm. The interval S refers to the length of a line segment extending from a point on the outer periphery of the first O-ring 533 to a point on the inner periphery of the second O-ring 534, the line segment being perpendicular to the tangent line that has the point as a tangent point, when the line segment is extended toward the inner periphery of the second O-ring 534. And, the interval S being between X and Y means that the interval S is within the range of X to Y, regardless of which point on the outer periphery of the first O-ring 533 is used as a reference point to measure the interval S.
[0075] When the cross-sectional area of the flow path of the aerosol flowing through the chamber 513 is larger than the size of the inlet side bottom surface 504, a tapered portion 513h may be provided on the side wall 513d so that the cross-sectional area of the flow path gradually decreases toward the inlet side bottom surface 504. It is preferable that the contour of the flow path cross section formed by the tapered portion 513h at the downstream end of the side wall 513d matches the outer circumferential contour of the inlet side bottom surface 504. By providing the tapered portion 513h, the ceramic particles are easily sucked into the inlet side bottom surface 504.
[0076] It is preferable that the distance L from the outlet of the nozzle 511a to the inlet side bottom surface 504 of the columnar honeycomb structure 500 is designed according to the area A of the inlet side bottom surface 504 of the columnar honeycomb structure 500. Specifically, the area A (mm 2 ) is larger, it is preferable to increase the distance L (mm) because this makes it easier for the aerosol to spread uniformly in the direction perpendicular to the aerosol flow direction.
[0077] The aerosol sprayed from the aerosol generator 511 passes through the inside of a chamber 513 by the suction force of a blower 512, and is then sucked into the first cells of the columnar honeycomb structure 500 from the inlet side bottom surface 504 of the columnar honeycomb structure 500 held by a holder 514. The ceramic particles in the aerosol sucked into the first cells adhere to the surfaces of the first cells.
[0078] The housing 520 has an exhaust port 520e downstream of the outlet side bottom surface 506 of the columnar honeycomb structure 500. The exhaust port 520e is connected to an exhaust pipe 515, and a blower 512 is provided downstream of the exhaust port 520e. Therefore, when the aerosol from which the ceramic particles have been removed is discharged from the outlet side bottom surface 506 of the columnar honeycomb structure 500, it passes through the exhaust pipe 515 and is then exhausted through the blower 512. A flow meter 516 is provided in the exhaust pipe 515, so that the gas flow rate measured by the flow meter 516 can be monitored, and the strength of the blower 512 can be controlled according to the gas flow rate.
[0079] When the film-forming process of adhering ceramic particles to the surface of the first cell continues, the pressure loss between the inlet side bottom surface and the outlet side bottom surface of the columnar honeycomb structure increases with an increase in the amount of adhering ceramic particles. Therefore, by determining the relationship between the amount of adhering ceramic particles and the pressure loss in advance, the end point of the film-forming process of adhering ceramic particles to the surface of the first cell can be determined based on the pressure loss. Therefore, the particle adhering device 510 can be provided with a differential pressure gauge 550 to measure the pressure loss between the inlet side bottom surface 504 and the outlet side bottom surface 506 of the columnar honeycomb structure 500, and the end point of the process can be determined based on the value of the differential pressure gauge.
[0080] 8 is a schematic diagram for explaining a method for replacing a work (columnar honeycomb structure 500) to be placed in the particle attachment device. First, a first work 1 is placed in the particle attachment device, and a film forming process is carried out on the work 1 by the method described above (step 1). Step 1 can be performed in a state where the holder 514 holding the work 1 is pressed against the first O-ring and the second O-ring of the mounting jig 530 via the housing 520 by the pressing force from the electric cylinder 570.
[0081] When the film forming process is completed, the housing 520 is lifted by the electric cylinder 570 (step 2). This allows access to the holder 514 holding the workpiece 1, and since the pressing force is released, the holder 514 holding the workpiece 1 can be easily removed from the mounting jig 530.
[0082] Next, the work 1 is removed from the particle attachment device together with the holder 514, and the holder 514 holding the second work 2 is placed in the particle attachment device (step 3). By having the work 2 held by the holder 514 in advance, it is possible to shorten the work replacement operation. Thereafter, similar to step 1, a film forming process is performed on the work 2 by the method described above (step 4). By repeating this operation, it is possible to efficiently perform the film forming process on a large number of columnar honeycomb structures 500.
[0083] After removing the columnar honeycomb structure with the ceramic particles attached to the surface of the first cell from the holder 514, the columnar honeycomb structure filter is completed by heat treatment under conditions of keeping the maximum temperature at 1000°C or more for 1 hour or more, for example, 1 hour to 6 hours, typically keeping the maximum temperature at 1100°C to 1400°C for 1 hour to 6 hours. The heat treatment can be performed, for example, by placing the columnar honeycomb structure in an electric furnace or a gas furnace. The heat treatment bonds the ceramic particles together and burns them to the partition walls in the first cells, forming a porous film on the surface of the first cells. When the heat treatment is performed under oxygen-containing conditions such as air, a surface oxide film is generated on the surface of the ceramic particles, promoting the bonding between the ceramic particles. As a result, a porous film that is difficult to peel off is obtained.
[0084] <3. Gas leak inspection method> Before carrying out the film-forming process on the columnar honeycomb structure, a gas leak inspection method according to one embodiment of the present invention can be carried out. According to this gas leak inspection method, it is possible to determine in advance whether or not the film-forming process should be carried out on the columnar honeycomb structure. Therefore, by carrying out the film-forming process on the columnar honeycomb structure only if it passes the inspection, it is expected that the yield of the columnar honeycomb structure filter will be improved. Furthermore, if it does not pass the inspection, this means that there is some abnormality in the particle attachment device, and it becomes possible to immediately carry out the necessary repairs.
[0085] In one embodiment, the gas leak inspection method includes: a step of preparing a mounting jig 530 which is installed at an upper end 513e of the chamber 513 and has a mounting surface 532 having an opening 531, a first O-ring 533 which is embedded in the mounting surface 532 so as to protrude partially upward and which runs around the outer periphery of the opening 531, and a second O-ring 534 which is embedded in the mounting surface 532 so as to protrude partially upward and which runs around the outer periphery of the first O-ring 533 at a distance; a step of preparing a holder 514 having a through hole 514c extending in the vertical direction and a chuck mechanism 514b capable of holding a columnar honeycomb structure 500 inserted into the through hole 514c from the outer peripheral side wall 502 side, a gas inlet 514d, a gas outlet 514e provided on a lower surface 514f, and a gas passage 514g communicating the gas inlet 514d and the gas outlet 514e; a step of holding the columnar honeycomb structure 500 by a chuck mechanism 514b of a holder 514; a step of pressing a lower surface 514f of a holder 514 holding the columnar honeycomb structure 500 against the first O-ring 533 and the second O-ring 534 of a mounting jig 530, on the condition that a gas outlet 514e is positioned between the first O-ring 533 and the second O-ring 534; a step of supplying gas from a gas inlet 514d of the holder 514 while maintaining the pressing step, and measuring the flow rate of the gas with a flow meter 562; determining whether the flow rate measured by the flow meter 562 exceeds a predetermined threshold; Includes.
[0086] There is no particular limit to the type of gas used in the inspection, and for example, air, nitrogen, argon, etc. can be used, but air is preferred from the viewpoints of simplicity, cost, and safety. In addition, if the gas pressure at the gas inlet 514d when supplying gas from the gas inlet 514d of the holder 514 is too high, gas leakage occurs even when the desired airtightness is obtained, making it difficult to set the threshold. In addition, if the gas pressure is too low, gas leakage does not occur even when the airtightness is poor, so the inspection accuracy decreases. Therefore, it is preferable to set the gas pressure so that gas leakage is hardly detected when the desired airtightness is obtained. From this viewpoint, the gas pressure is preferably, for example, 0.01 to 0.05 MPaG, and more preferably 0.03 to 0.05 MPaG.
[0087] Even if the airtightness of the space between the first O-ring 533 and the second O-ring 534, sandwiched between the lower surface 514f of the holder 514 and the mounting surface 532 of the mounting jig 530, is the same, the threshold value to be set varies depending on the pressure of the gas to be supplied. Therefore, the threshold value that is the criterion for judging the presence or absence of gas leakage can be set arbitrarily as long as it is possible to judge whether or not there is airtightness that does not affect the flow of the aerosol when performing the film forming process. For example, it can be set to any value in the range of 0 to 0.10 L / min converted to a state of 1 atm and 20°C. In particular, when the gas pressure at the gas inlet 514d is set to 0.01 to 0.05 MPaG, it is preferable to set the threshold value to any value in that range.
[0088] As a result of carrying out a step of judging whether the flow rate measured by the flow meter 562 exceeds a predetermined threshold value or not, if it is judged that the flow rate does not exceed the threshold value, the film forming step can be carried out while maintaining the pressing step. This makes it possible to carry out the film forming step while maintaining a state in which a predetermined airtightness is ensured, thereby reducing the rate of defective products and improving the yield. [Explanation of symbols]
[0089] 100: Pillar honeycomb structure filter 102: Outer wall 104: Bottom of inlet 106: Outlet side bottom surface 108: First cell 109: Plugging part 110: Second cell 112: Bulkhead 114: Porous membrane 400: Aerosol generator 401: Nozzle 402: Ceramic particles 403: Flow path 403e :Exit 407: Drive gas flow path 407i: Supply port 407v: Venturi section 409: Storage unit 409e :Exit 409i :Entrance 410: Venturi ejector 411: Powder quantitative feeder 420: Aerosol generator 500: Pillar honeycomb structure 502: Outer wall 504: Bottom of inlet 506: Outlet side bottom surface 510: Particle attachment device 511: Aerosol generator 511a: Nozzle 512: Blower 513: Chamber 513a: Opposing surface 513b: Insertion port 513c :Aperture 513d: Side wall 513e :Top edge 513f: Bottom end 513g: Filter 513h: Tapered section 514: Holder 514a: Main body part 514b: Chuck mechanism 514c:Through hole 514d: Gas inlet 514e: Gas outlet 514f: Bottom surface 514g: Gas passage 515: Exhaust pipe 516:Flowmeter 520: Housing 520e: Exhaust port 530: Mounting fixture 531 :Aperture 532: Placement surface 533: First O-ring 534: Second O-ring 535: Flange part 550: Differential pressure gauge 561: Gas piping 562:Flowmeter 570: Electric cylinder
Claims
1. A gas leak inspection method before a film forming process is performed on a columnar honeycomb structure, comprising: The columnar honeycomb structure includes an outer peripheral side wall, a plurality of first cells arranged on the inner peripheral side wall, extending from an inlet side bottom surface to an outlet side bottom surface, having an open inlet side bottom surface and having plugging portions on the outlet side bottom surface, and a plurality of second cells arranged on the inner peripheral side of the outer peripheral side wall, extending from the inlet side bottom surface to the outlet side bottom surface, having plugging portions on the inlet side bottom surface and having an open outlet side bottom surface, the plurality of first cells and the plurality of second cells being arranged alternately adjacent to each other with a porous partition wall therebetween, preparing a mounting jig that is installed at an upper end of a chamber and has a mounting surface having an opening, a first O-ring that is embedded in the mounting surface so as to protrude partially upward and that runs around the outer periphery of the opening, and a second O-ring that is embedded in the mounting surface so as to protrude partially upward and that runs around the outer periphery of the first O-ring at a distance; a step of preparing a holder having a through hole extending in the vertical direction and capable of gripping a columnar honeycomb structure inserted into the through hole from an outer peripheral side wall side, a gas inlet, a gas outlet provided on a lower surface, and a gas passage communicating the gas inlet and the gas outlet; a step of holding the columnar honeycomb structure by a chuck mechanism of the holder; a step of pressing a lower surface of a holder holding the columnar honeycomb structure against the first O-ring and the second O-ring of the mounting jig, on the condition that the gas outlet is located between the first O-ring and the second O-ring; supplying gas through a gas inlet of the holder while maintaining the pressing step, and measuring the flow rate of the gas with a flow meter; determining whether a flow rate measured by the flow meter exceeds a predetermined threshold; The method includes:
2. 2. The method according to claim 1, wherein the gas pressure at the gas inlet of the holder when gas is supplied from the gas inlet is 0.01 to 0.05 MPaG.
3. 3. The method according to claim 1, wherein the predetermined threshold value is set to any value within a range of 0 to 0.10 L / min when converted to a state of 1 atmospheric pressure and 20° C.
4. 3. The method of claim 1 or 2, wherein the gas is air.
5. The method according to claim 1 or 2, wherein the opening in the mounting surface and the through hole in the chuck mechanism are coaxial.
6. The method according to claim 1 or 2, wherein the wire diameter of the first O-ring and the second O-ring is 5.57 to 5.83 mm.
7. 3. The method according to claim 1, wherein the first O-ring and the second O-ring are embedded so as to protrude 1.27 to 1.58 mm above the mounting surface.
8. The method according to claim 1 or 2, wherein in the pressing step, the first O-ring and the second O-ring are pressed by 0.3 mm or more.
9. The method according to claim 1 or 2, wherein the first O-ring and the second O-ring have a type A durometer hardness of 65 to 75 as measured in accordance with JIS K6253-3:2012.
10. 3. The method according to claim 1, wherein the first O-ring and the second O-ring are made of nitrile rubber.
11. 3. The method according to claim 1 or 2, wherein the distance between the first O-ring and the second O-ring is 3 mm or more.
12. A method for manufacturing a columnar honeycomb structure filter according to claim 1 or 2, comprising, as a result of carrying out a step of determining whether the flow rate measured by a flow meter exceeds a predetermined threshold value, if it is determined that the flow rate does not exceed the threshold value, a film-forming step of spraying an aerosol containing ceramic particles from a nozzle of an aerosol generator into the chamber in a direction perpendicular to the inlet bottom surface of the columnar honeycomb structure toward the inlet bottom surface while applying a suction force to the outlet bottom surface, thereby sucking the sprayed aerosol from the inlet bottom surface and adhering the ceramic particles to the surface of the first cell, while maintaining the pressing step.
Citation Information
Patent Citations
Sealing material, method for producing the same and treating agent
JP2006036884A
Vacuum processing apparatus
JP2011032527A
Opening and closing device of access area of nuclear reactor vessel, and maintenance method of seal member in access area of nuclear reactor vessel
JP2012145479A
Honeycomb filter manufacturing method, and honeycomb filter manufacturing system
JP2013234952A
Defect inspection method of porous structure, and manufacturing method of separation membrane structure
JP2017087192A