Cured product and resin composition

A phase-separated cured product with epoxy resin and branched polyphenylene ether, combined with unevenly distributed inorganic fillers, addresses the need for improved heat resistance and dielectric properties in miniaturized electronic devices, ensuring effective heat dissipation and insulation.

JP2024143935APending Publication Date: 2024-10-11TAIYO HOLDINGS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056893
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional heat dissipation materials fail to provide sufficient heat resistance and dielectric properties required for miniaturized electronic devices.

Method used

A cured product comprising a phase-separated structure with a first phase of cured epoxy resin and a second phase of branched polyphenylene ether, along with unevenly distributed inorganic fillers, such as boron nitride, to achieve balanced heat resistance, dielectric properties, and heat dissipation.

Benefits of technology

The solution provides a cured product with excellent heat resistance, dielectric properties, and sufficient heat dissipation, suitable for use in electronic components as a heat dissipation member.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143935000002
    Figure 2024143935000002
  • Figure 2024143935000003
    Figure 2024143935000003
  • Figure 2024143935000004
    Figure 2024143935000004
Patent Text Reader

Abstract

To provide a technique relating to a cured product that exhibits excellent heat resistance and dielectric properties while maintaining sufficient heat radiation capability.SOLUTION: A cured product according to an embodiment includes a first phase containing a cured product of an epoxy resin, a second phase containing polyphenylene ether with a branched-chain structure, and an inorganic filler. The first phase and the second phase form a phase separation structure, and the inorganic filler is unevenly distributed in the first phase.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cured product and a resin composition. [Background technology]

[0002] As electronic devices become smaller and more powerful, there is a demand for higher density and functionality in components such as semiconductors. This demands smaller and higher density circuit boards for mounting semiconductors. As a result, heat dissipation has become a major issue as components and circuit boards become smaller and denser. In order to solve such problems, development of a heat dissipating material made of a resin composition having excellent heat dissipation properties, in which an inorganic filler is filled in a resin, is underway (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] WO2016 / 125664 publication Summary of the Invention [Problem to be solved by the invention]

[0004] However, in recent years, the demand for miniaturization of electronic devices has been accelerating, and further improvement in the performance of heat dissipation materials is also required. As a result of intensive research, the present inventors have found a new problem that heat dissipation materials with excellent heat resistance and dielectric properties are particularly required, and that conventional heat dissipation materials cannot fully satisfy such required properties. The present invention has been made in consideration of these problems, and has an object to provide a cured product and a resin composition that are excellent in heat resistance and dielectric properties while maintaining sufficient heat dissipation properties. [Means for solving the problem]

[0005] One embodiment of the present invention is a cured product comprising a first phase (epoxy resin-rich phase) containing a cured epoxy resin, a second phase (branched polyphenylene ether-rich phase) containing a polyphenylene ether having a branched structure, and an inorganic filler, the first phase and the second phase forming a phase-separated structure, and the inorganic filler being unevenly distributed in the first phase. In the cured product of the above embodiment, the phase-separated structure may be selected from the group consisting of a co-continuous structure and a sea-island structure. Also, the inorganic filler may include boron nitride particles. Another aspect of the present invention is a resin composition comprising an epoxy resin, a curing agent for the epoxy resin, a polyphenylene ether having a branched structure, and an inorganic filler, and after curing, forms a phase-separated structure of a first phase (an epoxy resin-rich phase) containing a cured product of the epoxy resin and a second phase (a branched polyphenylene ether-rich phase) containing the polyphenylene ether having the branched structure, and the inorganic filler is unevenly distributed in the first phase. In the resin composition of the above aspect, an amine compound may be included as a curing agent for the epoxy resin. The phase-separated structure may be selected from the group consisting of a cocontinuous structure and a sea-island structure. Furthermore, the inorganic filler may include boron nitride particles. Effect of the Invention

[0006] According to the present invention, it is possible to provide a technique relating to a cured product and a resin composition that are excellent in heat resistance and dielectric properties while maintaining sufficient heat dissipation properties. [Brief description of the drawings]

[0007] [Figure 1] 1 is a cross-sectional SEM (scanning electron microscope) image of the cured product of Example 1. [Diagram 2] 1 is a cross-sectional SEM image of the cured product of Example 2. [Diagram 3] 1 is a cross-sectional SEM image of the cured product of Example 3. [Figure 4] 1 is a cross-sectional SEM image of the cured product of Example 4. [Diagram 5] 1 is a cross-sectional SEM image of the cured product of Example 5. [Figure 6] 1 is a cross-sectional SEM image of the cured product of Example 6. [Figure 7] 2 is a cross-sectional SEM image of the cured product of Comparative Example 1. [Figure 8] 2 is a cross-sectional SEM image of the cured product of Comparative Example 2. [Figure 9] 1 is a cross-sectional SEM image of the cured product of Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expression "a to b" in the explanation of a numerical range means that the range is from a to b, unless otherwise specified.

[0009] Hereinafter, the resin composition of the present disclosure will be described, and then the cured product obtained using the resin composition will be described.

[0010] (Resin composition) The resin composition of the present disclosure contains a polyphenylene ether having a branched structure (hereinafter, sometimes referred to as branched PPE), an epoxy resin, a curing agent for the epoxy resin, and an inorganic filler. After curing, the resin composition forms a phase-separated structure of a first phase containing a cured product of the epoxy resin and a second phase containing the branched PPE. Each component of the resin composition will be described in detail below.

[0011] <Branched PPE> A branched PPE is a polyphenylene ether produced from a raw material phenol containing a phenol having hydrogen atoms at the ortho and para positions. Since such phenols also have hydrogen atoms at the ortho positions, when oxidatively polymerized with phenols, ether bonds can be formed not only at the ipso and para positions but also at the ortho positions, so that the polyphenylene ether obtained by using such phenols as raw material phenols can form a branched chain structure.

[0012] Such branched PPE has excellent solubility in solvents, as well as excellent compatibility and reactivity with each component in the resin composition.

[0013] The branched PPE may be a conventionally known PPE containing a functional group having an unsaturated carbon bond, such as an allyl group or a vinyl group, or may contain a hydrocarbon group having an unsaturated carbon bond.

[0014] Examples of branched PPEs containing a functional group having an unsaturated carbon bond (hereinafter also simply referred to as unsaturated carbon bond-containing polyphenylene ethers) include the polyphenylene ethers disclosed in WO 2020 / 017570.

[0015] The equivalent weight of the functional group having an unsaturated carbon bond in the unsaturated carbon bond-containing polyphenylene ether can be appropriately changed depending on the curability and application of the resin composition.

[0016] The polyphenylene ether containing an unsaturated carbon bond may be obtained by either of the following methods: (Method 1) a method of synthesizing a polyphenylene ether using a phenol containing a functional group having an unsaturated carbon bond as a raw material phenol, or (Method 2) a method of synthesizing a polyphenylene ether using a phenol not containing a functional group having an unsaturated carbon bond as a raw material phenol, and modifying the obtained polyphenylene ether to introduce a functional group having an unsaturated carbon bond into the polyphenylene ether. The polyphenylene ether obtained by (Method 1) may also be further modified to introduce a functional group having an unsaturated carbon bond.

[0017] The unsaturated carbon bond-containing polyphenylene ether may be a mixture of two or more types of polyphenylene ethers made from different types of raw material phenols.

[0018] The weight average molecular weight of the polyphenylene ether is preferably from 1,000 to 150,000, more preferably from 3,000 to 130,000, and even more preferably from 5,000 to 100,000. The weight average molecular weight is a standard polystyrene-equivalent value obtained by GPC (gel permeation chromatography).

[0019] The polyphenylene ether preferably has a polydispersity index (PDI: weight average molecular weight / number average molecular weight) of 1.5-20.

[0020] The ratio of the branched PPE to 100 parts by mass of the solid content of the epoxy resin in the resin composition according to the present disclosure can be, for example, 1 to 100 parts by mass, preferably 15 to 95 parts by mass, and more preferably 25 to 95 parts by mass. In particular, by appropriately adjusting the compounding ratio of the epoxy resin and the branched PPE according to the type of the curing agent for the epoxy resin, a suitable phase-separated structure can be formed. For example, when an amine compound is used as the curing agent for the epoxy resin, the cured product of the resin composition can form a phase-separated structure by setting the ratio of the branched PPE to 100 parts by mass of the solid content of the epoxy resin in the resin composition to 15 parts by mass or more, and by setting the ratio to 15 to 95 parts by mass, a co-continuous structure or a sea-island structure in which the phase containing the cured product of the epoxy resin is the sea phase can be formed.

[0021] <Epoxy resin> The epoxy resin is not particularly limited, and may be bifunctional or trifunctional or higher.

[0022] Examples of epoxy resins include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol E type epoxy resin, bisphenol M type epoxy resin, bisphenol P type epoxy resin, and bisphenol Z type epoxy resin; novolac type epoxy resins such as bisphenol A novolac type epoxy resin, phenol novolac type epoxy resin, and cresol novolac epoxy resin; biphenyl type epoxy resin, biphenyl aralkyl type epoxy resin, aryl alkylene type epoxy resin, tetraphenylol ethane type epoxy resin, naphthalene type epoxy resin, anthracene type epoxy resin, phenoxy type epoxy resin, dicyclopentadiene type epoxy resin, norbornene type epoxy resin, trihydroxyphenylmethane type epoxy resin, hydantoin ... Examples of the epoxy resins include laphenylolethane type epoxy resins, brominated epoxy resins, hydrogenated (bisphenol) type resins, glycidylamine type epoxy resins, alicyclic epoxy resins, diglycidyl phthalate resins, tetraglycidyl xylenoylethane resins, glycidyl methacrylate copolymer epoxy resins, cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resins, epoxy-modified polybutadiene rubber derivatives, CTBN-modified epoxy resins, trimethylolpropane polyglycidyl ether, phenyl-1,3-diglycidyl ether, 1,6-hexanediol diglycidyl ether, ethylene glycol or propylene glycol diglycidyl ether, sorbitol polyglycidyl ether, tris(2,3-epoxypropyl)isocyanurate, and triglycidyl tris(2-hydroxyethyl)isocyanurate. These epoxy resins can be used alone or in combination of two or more.

[0023] Of these, it is preferable to use biphenyl-type epoxy resins or naphthalene-type epoxy resins from the viewpoint of thermal dimensional stability of the resulting cured product, dicyclopentadiene-type epoxy resins from the viewpoint of low dielectric properties, and novolac-type epoxy resins from the viewpoint of heat resistance.

[0024] These epoxy resins can be used alone or in combination of two or more.

[0025] <Epoxy resin hardener> The epoxy resin curing agent is not particularly limited, and conventionally known curing agents can be used, such as phenolic resins, polycarboxylic acids and their acid anhydrides, cyanate ester resins, active ester resins, melamine compounds, amine compounds, dicyandiamide, and imidazole compounds. By including an epoxy resin curing agent, the molecular weight of the epoxy resin changes significantly when the resin composition is cured, as described below, and a phase separation structure is formed when the resin composition is cured. Among these, amine compounds are preferred, and diamine compounds are particularly preferred, because they have a good balance of reaction speed with the epoxy resin and are easy to form a phase separation structure. <Amine compounds> Examples of the amine compound include a diamine compound having two amino groups and a polyamine compound having three or more amino groups. Specifically, examples of the diamine compound include aliphatic diamines, aromatic diamines, diaminosiloxanes, aliphatic polyamines, and mixtures thereof. In this embodiment, the term "aromatic diamine" refers to a diamine in which an amino group is directly bonded to an aromatic ring, and may include an aliphatic group or other substituents in a part of the structure. The aromatic ring may be a single ring or a condensed ring, and examples include a benzene ring, a naphthalene ring, an anthracene ring, and a fluorene ring, but are not limited to these. Among these, the benzene ring is preferable. The term "aliphatic diamine (aliphatic polyamine)" refers to an amine in which an amino group is directly bonded to an aliphatic group, and may include an aromatic ring or other substituents in a part of the structure. Furthermore, the term "diaminosiloxane" refers to a compound having an amino group at the end of a siloxane skeleton, and may include a part of the structure substituted by a hydrocarbon group.

[0026] Examples of the aliphatic diamine include acyclic aliphatic diamines such as hexamethylenediamine, and cyclic aliphatic diamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, norbornanediamine, and 4,4'-diaminodicyclohexylmethane. These can be used alone or in combination of two or more.

[0027] Examples of aromatic diamines include aromatic diamines having one aromatic ring, such as p-phenylenediamine, m-phenylenediamine, 2,4-toluenediamine, m-xylylenediamine, p-xylylenediamine, 1,5-diaminonaphthalene, and 2,6-diaminonaphthalene, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, and 3,3'-diaminodiphenyl sulfone (sometimes abbreviated as 3,3'DDS), 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene (sometimes abbreviated as TPE-R), and 1,3-bis(3-aminophenoxy)benzene. Examples of aromatic diamines having two or more aromatic rings include aromatic diamines having two or more aromatic rings, such as 9,9-bis(4-aminophenyl)fluorene, 9,9-bis(4-amino-3-methylphenyl)fluorene, 9,9-bis(4-amino-3-chlorophenyl)fluorene, and 9,9-bis(4-amino-3-fluorophenyl)fluorene. These can be used alone or in combination of two or more.

[0028] The aromatic diamine is preferably 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone (3,3'DDS), 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene, These are 4,4'-bis(4-aminophenoxy)biphenyl (APB-N), bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl (TFMB), and 4,4'-bis(4-aminophenoxy)biphenyl. These can be used alone or in combination of two or more.

[0029] Examples of diaminosiloxanes include 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(4-aminobutyl)tetramethyldisiloxane, α,ω-bis(2-aminoethyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydimethylsiloxane, α,ω-bis(5-aminopentyl)polydimethylsiloxane, α,ω-bis[3-(2-aminophenyl)propyl]polydimethylsiloxane, and α,ω-bis[3-(4-aminophenyl)propyl]polydimethylsiloxane. These can be used alone or in combination of two or more.

[0030] Examples of the aliphatic polyamine include polyalkylene polyamines having 2 to 6 carbon atoms, such as diethylenetriamine and triethylenetriamine, etc. These can be used alone or in combination of two or more kinds.

[0031] The ratio of the epoxy resin curing agent in the resin composition, epoxy equivalent of the epoxy resin:active hydrogen equivalent of the epoxy resin curing agent, is preferably 1.0:0.5 to 1.0:1.5, and more preferably 1.0:0.7 to 1.0:1.3.

[0032] <Inorganic filler> The inorganic filler is not particularly limited, and examples thereof include metal oxides such as silica (amorphous silica, crystalline silica, fused silica, spherical silica, etc.), alumina, and titanium oxide; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; clay minerals such as talc and mica; fillers having a perovskite crystal structure such as barium titanate and strontium titanate; silicon nitride, boron nitride, aluminum nitride, aluminum borate, barium sulfate, calcium carbonate, and magnesium carbonate. These can be used alone or in combination. By including an inorganic filler, the volumetric shrinkage during curing can be reduced, and the known properties of various inorganic fillers can be imparted to the cured product. Of these inorganic fillers, from the viewpoint of improving the thermal conductivity of the cured product obtained by curing the resin composition, it is preferable to use boron nitride, aluminum nitride, alumina, silicon nitride, and aluminum hydroxide, and it is particularly preferable to use boron nitride.

[0033] The ratio of the volume of the inorganic filler to the total solid volume of the resin composition is preferably from 1 to 90% by volume, more preferably from 5 to 80% by volume, and further preferably from 10 to 70% by volume.

[0034] The average particle size of the inorganic filler is preferably 10 to 700 nm, more preferably 20 to 600 nm, and further preferably 30 to 550 nm. When the inorganic filler has anisotropic shape, such as a scale shape or an elliptical shape, the long side of the inorganic filler is taken as the particle size. By setting the average particle size of the inorganic filler within this range, when the resin composition forms a phase-separated structure, the balance between the size of the phase-separated structure and the size of the inorganic filler is maintained, so that the inorganic filler is likely to be unevenly distributed in the first phase while maintaining the phase-separated structure.

[0035] (Organic solvent) The resin composition of the present disclosure may further contain an organic solvent. There is no particular limitation on the organic solvent as long as it has good solubility for each component and does not inhibit the formation of a phase-separated structure described later when a cured product is formed. Examples of the organic solvent include aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene, halogenated aromatic hydrocarbons such as chloroform, methylene chloride, chlorobenzene, dichlorobenzene, and trichlorobenzene, nitro compounds such as nitrobenzene, methyl ethyl ketone (MEK), cyclohexanone, tetrahydrofuran, ethyl acetate, N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), propylene glycol monomethyl ether acetate (PMA), and diethylene glycol monoethyl ether acetate (CA). Only one type of solvent may be used, or two or more types may be used. Of these, it is preferable to use cyclohexanone since it has good solubility for each component in the resin composition.

[0036] (Other Ingredients) The resin composition of the present disclosure may contain other components as long as the effects of the present disclosure are not impaired.

[0037] In addition, in the resin composition of the present disclosure, only the epoxy resin is cured during curing as described below, and the compatibility between the epoxy resin and the branched PPE changes significantly, so that the cured product forms a phase-separated structure. Therefore, when the branched PPE has an unsaturated carbon bond, it is preferable that the resin composition does not substantially contain a component that advances the crosslinking reaction of the unsaturated carbon bond during curing, specifically, a thermal radical generator. In addition, the term "substantially free" is not particularly limited as long as the crosslinking reaction of the branched PPE does not advance, but for example, it is less than 0.1 parts by mass when the solid content of the branched PPE is 100 parts by mass.

[0038] The phase-separated structure formed when the resin composition of the present disclosure is cured will be described later.

[0039] (cured product) The cured product of the present disclosure includes a first phase including a cured product of an epoxy resin, a second phase including a polyphenylene ether having a branched structure, and an inorganic filler. The first phase and the second phase form a phase-separated structure. The inorganic filler is unevenly distributed in the first phase.

[0040] The cured epoxy resin of the cured product of the present disclosure is a cured product obtained by a curing reaction between the epoxy resin in the resin composition and a curing agent for the epoxy resin, and details of the branched PPE and inorganic filler are the same as those of the resin composition described above.

[0041] In the technology disclosed herein, the resin composition is a homogeneous resin composition in which each component is compatible with each other, but a phase-separated structure is formed in the cured product. The mechanism by which the phase-separated structure is formed in the cured product is not necessarily clear, but it is presumed that reaction-induced phase separation occurs during the curing reaction. That is, the epoxy resin contained in the resin composition hardens during curing and the molecular weight changes significantly, so that the compatibility between the epoxy resin and the branched PPE changes during the curing process, forming a phase-separated structure.

[0042] The first phase is the so-called epoxy resin rich phase. The second phase is a so-called branched PPE-rich phase. Whether each phase is an epoxy resin-rich phase or a branched PPE-rich phase can be distinguished by immersing the cured product in an organic solvent, as described below.

[0043] The phase-separated structure formed by the first phase and the second phase is selected from the group consisting of a bicontinuous structure and an islands-in-a-sea structure (also called a BCC structure).

[0044] When a sea-island structure is formed by the first phase and the second phase, it is preferable that the "sea" portion of the sea-island structure is the first phase, and the "island" portion of the sea-island structure is the second phase, which makes it easier for the inorganic filler contained in the first phase to form a thermal conduction path.

[0045] The fact that the cured product of the present disclosure forms a phase-separated structure and that the inorganic filler is unevenly distributed in the first phase can be confirmed, for example, by imaging a cross section perpendicular to the main surface of the cured product of the present disclosure (hereinafter referred to as a thickness direction cross section) with a scanning electron microscope (SEM). Specifically, when the cross section of the cured product of the present disclosure in the thickness direction is observed with an SEM, the inorganic filler is visually recognized as a relatively whiter region compared to other parts such as the first phase and the second phase. Therefore, when the inorganic filler is unevenly distributed in either phase, it can be confirmed that the relatively white region and the other regions form a co-continuous structure or a sea-island structure. In addition, the first phase is insoluble in organic solvents because it has cured, but the second phase is soluble in organic solvents because it has not cured. Therefore, when the cured product is immersed in an organic solvent (e.g., dichloromethane), only the second phase dissolves, and the first phase remains undissolved. Therefore, if the inorganic filler is unevenly distributed in the first phase, it can be confirmed that the inorganic filler is dispersed in the first phase that remains undissolved by immersing a cross-sectional sample of the cured product in an organic solvent and then observing the cross-section in the thickness direction with an SEM. From another perspective, when a cross-sectional sample of the cured product is immersed in an organic solvent, the insoluble region can be confirmed as the first phase (epoxy resin-rich phase), and when a cross-sectional sample of the cured product is immersed in an organic solvent, the soluble region can be confirmed as the second phase (branched PPE-rich phase).

[0046] The inorganic filler is unevenly distributed in the first phase because the affinity or compatibility between the inorganic filler and the epoxy resin is higher than the affinity or compatibility between the inorganic filler and the branched PPE. In order to increase the affinity between the inorganic filler and the epoxy resin, the surface of the inorganic filler may be subjected to a surface treatment using a silane coupling agent, a titanate coupling agent, or an aluminate coupling agent.

[0047] The mechanism by which such a configuration provides the effects of the disclosed technology is not entirely clear, but is speculated as follows. The present inventors have found that when an inorganic filler is blended into a resin composition using only branched PPE, the dispersibility of the inorganic filler is poor and sufficient heat dissipation properties may not be obtained. On the other hand, when only epoxy resin is used, although the dispersibility of the filler is excellent, the heat resistance and dielectric properties are insufficient. In this respect, in the resin composition of the present disclosure, after curing, the inorganic filler is unevenly distributed in the first phase, i.e., the phase containing the cured product of the epoxy resin, so that the good inorganic filler dispersion inherent to the epoxy resin is maintained without being lost even when blended with the branched PPE. On the other hand, since a phase containing the branched PPE is also simultaneously present as the second phase, the heat resistance and dielectric properties inherent to the branched PPE are maintained without being lost even when blended with the epoxy resin. It is presumed that the synergistic effect of these two factors results in an excellent balance between heat resistance and dielectric properties while exhibiting sufficient heat dissipation properties.

[0048] (Method of producing the cured product) The cured product of the present disclosure can be obtained by curing the above-mentioned resin composition. An example of a method for producing the cured product of the present disclosure is described below.

[0049] First, the above-mentioned predetermined amounts of each component are mixed and stirred to obtain a resin composition. As long as a resin composition in which each component is sufficiently mixed is obtained, the method for producing the resin composition is not particularly limited. An example of the method for producing the resin composition is shown below. First, the above-mentioned organic solvent and the branched PPE are mixed and stirred to obtain a preparation solution A. The stirring conditions at this time are not particularly limited as long as the branched PPE is sufficiently dissolved in the organic solvent. Next, the above-mentioned epoxy resin is added to the adjusted solution A and stirred to obtain an adjusted solution B. The stirring conditions at this time are not particularly limited as long as each component in the adjusted solution B is sufficiently mixed. Next, the inorganic filler described above is added to the adjusted solution B, and the mixture is stirred to obtain an adjusted solution C. The stirring conditions at this time are not particularly limited, and it is sufficient that each component in the adjusted solution C is sufficiently mixed. When an inorganic filler is added, it is preferable to add the inorganic filler as a slurry in which the inorganic filler is dispersed in the same organic solvent as that used in the adjustment liquid A. This can enhance the dispersibility of the inorganic filler in the adjustment liquid C. Next, the above-mentioned epoxy resin curing agent is added to the adjusted liquid C, and the mixture is stirred to obtain a resin composition. The stirring conditions are not particularly limited as long as each component in the resin composition is sufficiently mixed.

[0050] Next, the obtained resin composition is used to form a coating film (resin layer) having a desired thickness. The method for forming the coating film is not particularly limited. One example of the coating film formation method is the formation of a coating film using a spin coating method. In this case, a predetermined amount of the obtained resin composition is applied onto a substrate such as a Si substrate using a spin coating method. The conditions such as the rotation speed and time during spin coating are not particularly limited, and it is sufficient that a coating film of the resin composition having a desired thickness is formed on the substrate. Another example of the coating film forming method is the formation of a coating film using an applicator. In this case, a predetermined amount of the obtained resin composition is applied onto a metal foil such as a copper foil using an applicator. The conditions during application are not particularly limited, and it is sufficient that a coating film of the resin composition having a desired thickness is formed on the substrate.

[0051] Next, the resulting coating is heated and cured. The heating conditions can be appropriately adjusted depending on the content of each component and the thickness of the coating. An example of the heating conditions is a procedure in which a soft bake step at 80 to 100°C for 1 to 10 minutes is followed by a heating step at 160 to 200°C for 1 to 3 hours, and then a heating step at 180 to 220°C for 3 to 5 hours.

[0052] According to the cured product of the present disclosure as described above, it is possible to obtain a good balance of heat resistance and dielectric properties while maintaining sufficient heat dissipation properties.

[0053] (Electronic Components) The cured product of the present disclosure has insulating properties and excellent thermal conductivity, and can therefore be used as a heat dissipation member in electronic components. Specifically, the cured product of the present disclosure can be used as an encapsulant that covers at least a portion of a semiconductor chip.

[0054] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES

[0055] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these.

[0056] (raw materials) The details of the raw materials shown in Table 1 are as follows: Epoxy resin: bisphenol A diglycidyl ether (DGEBA), epoxy equivalent: 189g / eq, Mitsubishi Chemical Corporation, jER828 Epoxy resin hardener (diamine compound): 4,4'-diaminodiphenylmethane (DDM), manufactured by Tokyo Chemical Industry Co., Ltd. Branched PPE: Branched PPE obtained by Synthesis Example 1 below (Synthesis Example 1) In a 500mL separable flask, 19.8g (0.162mol%) of 2,6-dimethylphenol and 2.42g (0.018mol%) of 2-allylphenol were dissolved in 261g of toluene as raw material phenols to prepare a raw material solution. Furthermore, di-μ-hydroxo-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride (Cu / TMEDA) was adjusted to 0.18wt% and tetramethylethylenediamine (TMEDA) to 0.16wt%, and the reaction was carried out at 40℃ for 8 hours while blowing dry air into the reaction solution at a flow rate of 75mL / min, stirring at a stirring speed of 200rpm. After stopping heating the reaction solution and blowing in dry air, di-μ-hydroxo-bis[(N,N,N',N'-tetramethylethylenediamine)copper(II)] chloride (Cu / TMEDA) was removed by filtration, and the precipitate was reprecipitated in a mixture of 1,200 mL of methanol, 4.0 mL of concentrated hydrochloric acid, and 7.0 mL of H2O2, filtered under reduced pressure, washed with methanol, and dried at 80°C for 24 hours to obtain PPE-1. PPE-1 had a number-average molecular weight of 14,200 and a weight-average molecular weight of 54,400. Boron nitride: Nano boron nitride (average particle size = 509 nm) slurry, manufactured by Tokushiki Co., Ltd., LDBN-0001C

[0057] (Preparation of resin composition) Example 1 A preparation A was prepared by blending the branched PPE and organic solvent shown in Table 1. The obtained preparation A was stirred at 2000 rpm for 5 minutes using a stirrer (Thinky Corporation, Awatori Rentaro ARV-310P, hereinafter simply referred to as the stirrer). Next, an epoxy resin was added to the stirred adjusted solution A to prepare adjusted solution B. The obtained adjusted solution B was stirred at 2000 rpm for 5 minutes using a stirrer. Next, a slurry (a cyclohexane solution containing 40% by mass of inorganic filler) was added to the stirred adjusted liquid B to prepare adjusted liquid C. The obtained adjusted liquid C was stirred at 2000 rpm for 5 minutes using a stirrer. Next, a diamine compound was added to the stirred Adjusted Liquid C, and the mixture was stirred at 2000 rpm for 5 minutes using a stirrer to prepare a resin composition.

[0058] (Examples 2 to 6, Comparative Example 3) A resin composition was obtained in the same manner as in Example 1, except that the components of the resin composition were mixed in the amounts shown in Table 1.

[0059] Comparative Example 1 A resin composition was obtained in the same manner as in Example 1, except that an epoxy resin was used in the preparation of preparation A, and preparation C was prepared by adding a slurry to preparation A.

[0060] Comparative Example 2 A resin composition was obtained in the same manner as in Example 1, except that a slurry was added to the above-mentioned preparation liquid A to prepare preparation liquid C, and that no diamine compound was added.

[0061] (Preparation of spin-coated film) Each of the prepared resin compositions was dropped onto a Si wafer, and then spin-coated using a spin coater at 500 rpm for 20 seconds to form a laminate in which a resin layer made of the resin composition was laminated on the Si wafer. Next, the obtained laminate was subjected to a soft bake (SB) at 90° C. for 5 minutes. Next, the laminate after SB was subjected to a curing step A at 180° C. for 2 hours, and then a curing step B at 200° C. for 4 hours to obtain a cured product (spin-coated film).

[0062] (Preparation of single membrane) Each resin composition was applied to the shiny surface of a 18 μm-thick copper foil with an applicator so that the film thickness after drying was 25 μm, and then dried in a hot air circulation drying oven at 90° C. for 5 minutes. Next, the curing step A and the curing step B were carried out in the same manner as above in the hot air circulation drying oven, and the copper foil was etched to obtain a cured product (single film) made of each resin composition.

[0063] (Cross-sectional SEM observation) Cross-sectional samples were prepared by subjecting each of the spin-coated films of the Examples and Comparative Examples to ion milling. As a result of observing the cross-sections of the cross-sectional samples with an SEM, it was confirmed that in the cured products of each Example, a co-continuous structure or a sea-island structure was formed in which the first phase rich in epoxy resin constituted the "sea" and the second phase rich in branched PPE constituted the "islands," as shown in Figures 1 to 6. In addition, by immersing each of the cured products in dichloromethane and then observing the cross-section with an SEM, it was confirmed that boron nitride was unevenly distributed in the first phase. On the other hand, in the cured products of each Comparative Example, no phase separation structure was observed as shown in Figures 7 to 9. Although the inorganic filler was unevenly distributed in the cured product of Comparative Example 2, it was found that the inorganic filler was not unevenly distributed due to the phase separation structure, but due to the aggregation of the inorganic filler, because the cured product was made using only branched PPE. Therefore, it was determined that the cured product of Comparative Example 2 did not form a phase separation structure.

[0064] (density) The density was calculated based on the components and contents of each cured product. The results are shown in Table 1. The density of each component used in the calculation is as follows. Epoxy resin: 1.17g / cm 3 Diamine compound: 1.15 g / cm 3 Branched PPE: 1.00g / cm 3 Boron nitride: 2.1g / cm 3 Cyclohexanone: 0.948g / cm 3

[0065] (DSC measurement) For each of the examples and comparative examples, a single film was rapidly cooled to -20°C, then heated to 330°C (heating rate: 10°C / min), cooled to -20°C (heating rate: 10°C / min), and then the onset Tg (°C) of each cured product was measured during the second heating (heating rate: 10°C / min) using a differential scanning calorimeter (DSC, Hitachi High-Tech Science Corporation, DSC600). The results are shown in Table 1. The obtained glass transition temperatures (onset Tg) were evaluated according to the following glass transition temperature evaluation criteria. <Glass transition temperature evaluation criteria> A: 200℃ or higher B: 150℃ or higher but less than 200℃ C: Less than 150℃ (A and B are pass, C is fail) In addition, the constant pressure specific heat capacity Cp was measured using modulated DSC (frequency: 0.016 Hz, heating rate: 3° C. / min). The results are shown in Table 1.

[0066] (TGA measurement) For each of the examples and comparative examples, a thermogravimetric analyzer (TGA, TGA5500, manufactured by TA Instruments Japan) was used to measure the temperature T d5 The results are shown in Table 1. d5 Regarding the following T d5 The evaluation was based on the evaluation criteria. <T d5 Evaluation criteria> A: 400℃ or higher B: 300℃ or higher and less than 400℃ C: Less than 300℃ (A and B are pass, C is fail)

[0067] (Thermal diffusivity and thermal conductivity measurements) The thermal diffusivity α in the thickness direction at room temperature for each of the single films of the Examples and Comparative Examples was measured using an ultra-high sensitivity thermal diffusivity measuring device for thin films (ai-phase Mobile M3 Type 1, manufactured by ai-phase Corporation). The results are shown in Table 1. The thermal conductivity λ of each cured product in the thickness direction was calculated using the following formula. λ=αρCp α: thermal diffusivity, ρ: density, Cp: specific heat capacity at constant pressure (measured by modulated DSC as described above) The obtained results are shown in Table 1. The calculated thermal conductivity was evaluated according to the following thermal conductivity evaluation criteria. <Thermal conductivity evaluation criteria> A: 0.450W / (m·K) or more B: 0.350W / (m K) or more and less than 0.450W / (m K) C: 0.300W / (m K) or more and less than 0.350W / (m K) D: Less than 0.300W / (m K) (A, B, C are pass, D is fail)

[0068] (Dielectric constant measurement) The single films of each example and comparative example, cut into a length of 80 mm and a width of 35 mm, were used as test pieces, and the dielectric loss tangent Df was measured by the SPDR (Split Post Dielectric Resonator) resonator method. As the measuring instrument, a vector network analyzer E5071C manufactured by Keysight Technologies Co., Ltd. and an SPDR resonator were used, and a calculation program manufactured by QWED Co., Ltd. was used. The conditions were a frequency of 19.8 GHz and a measurement temperature of 25°C. The obtained dielectric loss tangent Df was evaluated according to the following evaluation criteria respectively. <Df Evaluation Criteria> A: Less than 0.0130 B: 0.0130 or more and less than 0.0150 C: 0.0150 or more (A and B are considered qualified, and C is considered unqualified)

[0069]

Table 1

[0070] As shown in Table 1, it was confirmed that the cured products of Examples 1 to 6 exhibited good balance in heat resistance and dielectric properties while maintaining sufficient heat dissipation.

Claims

1. a first phase including a cured epoxy resin; a second phase comprising a polyphenylene ether having a branched structure; An inorganic filler; Including, A cured product, wherein the first phase and the second phase form a phase-separated structure, and the inorganic filler is unevenly distributed in the first phase.

2. The cured product according to claim 1 , wherein the phase-separated structure is selected from the group consisting of a co-continuous structure and a sea-island structure.

3. The cured product according to claim 1 or 2, comprising boron nitride particles as the inorganic filler.

4. Epoxy resin, A hardener for the epoxy resin; A polyphenylene ether having a branched structure; An inorganic filler; Including, A resin composition which, after curing, forms a phase-separated structure having a first phase containing a cured product of the epoxy resin and a second phase containing the polyphenylene ether having a branched structure, and the inorganic filler is unevenly distributed in the first phase.

5. The resin composition according to claim 4, further comprising an amine compound as a curing agent for the epoxy resin.

6. The resin composition according to claim 4 or 5, wherein the phase-separated structure is selected from the group consisting of a co-continuous structure and a sea-island structure.

7. The resin composition according to claim 4 or 5, comprising boron nitride particles as the inorganic filler.

Citation Information

Patent Citations

  • Resin composition

    WO2016125664A1