Light emitting device and method of manufacturing the same

The method of multiple bonding steps with a buffer sheet and element evaluation addresses bonding strength variations in light emitting devices, enhancing manufacturing efficiency and reliability.

JP2024143973APending Publication Date: 2024-10-11NICHIA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023116943
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-07-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing light emitting devices face variations in bonding strength between semiconductor elements and wiring boards, which affect manufacturing productivity and reliability.

Method used

A method involving multiple bonding steps with varying conditions, including the use of a buffer sheet to apply pressure and correct element positioning, followed by evaluating and replacing defective elements, to achieve uniform bonding strength.

Benefits of technology

Reduces variations in bonding strength, improves manufacturing efficiency, and enhances the reliability of the light emitting device by ensuring consistent and strong connections between elements and the wiring board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143973000001_ABST
    Figure 2024143973000001_ABST
Patent Text Reader

Abstract

To provide a light emitting device and a method of manufacturing the same, capable of bonding a plurality of elements to a wiring board with a uniform strength.SOLUTION: A method of manufacturing a light emitting device includes steps of: preparing a plurality of first elements including first bonding parts and a wiring board including a plurality of second bonding parts; placing the first elements on the wiring board by bonding the first bonding parts and the second bonding parts under first bonding conditions; and bonding the first bonding parts and the second bonding parts under second bonding conditions by placing a buffer sheet on the first elements and applying pressure on the first elements via the buffer sheet towards the wiring board. The step of bonding under the second bonding conditions is repeated multiple times.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a light emitting device and a method for manufacturing the same. [Background technology]

[0002] Patent Document 1 discloses a light-emitting device in which many semiconductor elements are arranged on one wiring board. When manufacturing such a light-emitting device, high productivity can be achieved by bonding many semiconductor elements to the wiring board all at once, but bonding all at once may cause variations in bonding strength between the semiconductor elements and the wiring board. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-074005 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of one embodiment of the present disclosure is to provide a light emitting device capable of reducing variation in bonding strength between a plurality of elements and a wiring substrate, and a manufacturing method thereof. [Means for solving the problem]

[0005] A method for manufacturing a light emitting device according to an embodiment of the present disclosure includes the steps of: preparing a plurality of first elements including first bonding portions and a wiring board including a plurality of second bonding portions, placing the plurality of first elements on the wiring board by bonding the first bonding portions and the second bonding portions under a first bonding condition, and placing a buffer sheet on the plurality of first elements and pressing the plurality of first elements toward the wiring board via the buffer sheet to bond the first bonding portions and the second bonding portions under a second bonding condition. The bonding step under the second bonding condition is repeated a plurality of times.

[0006] A light emitting device according to an embodiment of the present disclosure includes a wiring substrate having wiring, a plurality of first elements, and a plurality of bonding portions connecting the plurality of first elements to the wiring, wherein a ratio of a standard deviation to an average value of bonding strength of the plurality of first elements to the wiring substrate is 0.1 or less.

[0007] A light emitting device according to an embodiment of the present disclosure includes a wiring board having wiring, a plurality of first elements, and a plurality of bonding portions connecting the plurality of first elements to the wiring. In a plan view, the length of one side of each of the first elements is 500 μm or more and 1500 μm or less. The average bonding strength of the plurality of first elements to the wiring board is 10 kgf or more. Effect of the Invention

[0008] According to an embodiment of the present disclosure, it is possible to realize a light emitting device capable of reducing the variation in bonding strength between a plurality of elements and a wiring substrate, and a method for manufacturing the same. [Brief description of the drawings]

[0009] [Figure 1] 4 is a flowchart showing a method for manufacturing the light emitting device according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a first element in the first embodiment. [Diagram 3] FIG. 2 is a plan view showing a wiring board according to the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV shown in FIG. [Diagram 5] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 6] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 7] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 8] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 9] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 10] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 11] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 12] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 13] 2A to 2C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the first embodiment. [Figure 14] FIG. 1 is a plan view showing a light emitting device according to a first embodiment. [Figure 15] 15 is a cross-sectional view taken along line XV-XV shown in FIG. 14. [Figure 16] 5A to 5C are cross-sectional views illustrating a method for manufacturing the light emitting device according to the second embodiment. [Figure 17] FIG. 11 is a plan view showing a light-emitting module according to a third embodiment. [Figure 18] FIG. 11 is a partially enlarged plan view showing a first element and a wavelength conversion member in a third embodiment. [Figure 19] FIG. 13 is a diagram showing a measuring device for measuring bonding strength in a test example. [Figure 20A] FIG. 2 is a front view showing a jig of a measuring device used in a test example. [Figure 20B] FIG. 20B is a side view showing a jig of the measuring device of FIG. 20A. [Figure 20C] FIG. 20C is a partially enlarged side view showing an area XXC in FIG. 20B. [Figure 21] FIG. 4 is a cross-sectional view showing a method for measuring the bonding strength in a test example. [Figure 22] 1 is a graph showing the bonding strength of an example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments will be described with reference to the drawings. The drawings are schematic or conceptual, and the relationship between the thickness and width of each part, the ratio of the sizes between the parts, etc. are not necessarily the same as the actual ones. Even when the same part is shown, the dimensions and ratios of each part may be different depending on the drawing. Furthermore, in this specification and each drawing, elements similar to those described with reference to the previous drawings are given the same reference numerals, and detailed descriptions are omitted as appropriate. Also, an end view showing only the cut surface may be used as a cross-sectional view.

[0011] <First embodiment> A method for manufacturing the light emitting device according to the first embodiment will be described below. FIG. 1 is a flowchart showing a method for manufacturing a light emitting device according to this embodiment. FIG. 2 is a cross-sectional view showing a first element in this embodiment. FIG. 3 is a plan view showing the wiring board in this embodiment. FIG. 4 is a cross-sectional view taken along line IV-IV shown in FIG. 5 to 13 are cross-sectional views showing a method for manufacturing a light emitting device according to this embodiment.

[0012] (Step of Preparing the First Element and the Wiring Board) 1, a plurality of first elements 10 and a wiring board 20 are prepared, for example, as shown in FIGS. 2 and 3. The first elements include a first bonding portion 11. The wiring board 20 includes a plurality of second bonding portions 21. The order of the timing of preparing the first elements 10 and the timing of preparing the wiring board 20 is arbitrary. Furthermore, the first elements 10 and the wiring board 20 may be prepared by manufacturing, or may be prepared by purchasing them from a third party.

[0013] First, a description will be given of the first element 10. As shown in Fig. 2, the first element 10 is a light-emitting element having a pair of first bonding portions 11, a semiconductor member 12, and a wavelength conversion member 13, and is, for example, a light-emitting diode (LED).

[0014] In the semiconductor member 12, a p-type semiconductor layer, an active layer, and an n-type semiconductor layer are stacked. The semiconductor member 12 has a first surface 12a and a second surface 12b. The second surface 12b is the surface opposite to the first surface 12a. A pair of first bonding portions 11 are disposed on the first surface 12a of the semiconductor member 12.

[0015] One of the pair of first joints 11 is connected to the p-type semiconductor layer of the semiconductor member 12, and the other is connected to the n-type semiconductor layer of the semiconductor member 12. As a result, the pair of first joints 11 function as an anode electrode or a cathode electrode of the first element 10. In this specification, "connection" refers to electrical connection. Also, "bonding" refers to a state in which electrical connection and mechanical connection are realized. The first joints 11 contain gold (Au). For example, at least the outermost surface of the first joints 11 is made of gold. The thickness of the first joints 11 is, for example, 0.01 μm or more and 1 μm or less.

[0016] The wavelength conversion member 13 is disposed on the second surface 12b of the semiconductor member 12. The wavelength conversion member 13 has, for example, a base material made of a translucent resin material or an inorganic material, and a phosphor disposed in the base material. The phosphor is, for example, YAG (Yttrium Aluminum Garnet). For example, as viewed from the second surface 12b side, the wavelength conversion member 13 is larger than the semiconductor member 12, and the outer edge of the wavelength conversion member 13 is located outside the outer edge of the semiconductor member 12. As viewed from the second surface 12b side, the shape of the wavelength conversion member 13 is, for example, a square, and the length of one side is, for example, 45 μm. In addition, the wavelength conversion member 13 may be disposed on the second surface 12b of the semiconductor member 12 via a translucent member such as sapphire.

[0017] The surface of the wavelength conversion member 13 opposite to the surface facing the semiconductor member 12 is a light emitting surface 13a. The light emitting surface 13a is parallel to the first surface 12a and the second surface 12b of the semiconductor member 12. In addition, the light emitting surface 13a is preferably a flat surface. However, there are cases where the shape of the first element 10 inevitably varies. For example, there are cases where the wavelength conversion member 13 is warped and the light emitting surface 13a is curved in a concave or convex shape.

[0018] Supplying electric power between the pair of first joints 11 causes, for example, the semiconductor member 12 to emit blue light. The wavelength conversion member 13 absorbs a portion of the light emitted from the semiconductor member 12 and emits yellow light. As a result, white light that is a mixture of blue light and yellow light is emitted from the first element 10.

[0019] Next, the wiring board 20 will be described. As shown in Fig. 3 and Fig. 4, the wiring board 20 includes one insulating base 22 and a plurality of second bonding portions 21. The plurality of second bonding portions 21 are disposed on the base 22. The second bonding portions 21 include gold. For example, at least the outermost surface of the second bonding portions 21 is made of gold.

[0020] The second bonding portions 21 are arranged, for example, in a matrix on the upper surface 22a of the base 22. However, the arrangement of the second bonding portions 21 is not limited to a matrix and may be any arrangement. Each of the second bonding portions 21 is arranged at a position where the first bonding portions 11 come into contact with the first bonding portion 11 when the first surface 12a of the semiconductor member 12 of the first element 10 is placed opposite the upper surface 22a of the base 22 of the wiring board 20.

[0021] 3 and 4, a plurality of wirings 23 are arranged inside the base 22. A plurality of openings 24 are formed in the base 22 on the upper surface 22a, and the wirings 23 are exposed in each opening 24. Areas of the surfaces of the wirings 23 that are not exposed in the openings 24 are covered by the base 22. The second bonding portions 21 are arranged on the upper surface 22a of the base 22 and within the openings 24. Each second bonding portion 21 is connected to each wiring 23 at the bottom of the opening 24.

[0022] (Step of placing the first element on the wiring board) Next, in step S2 of FIG. 1, a plurality of first elements 10 are placed on the wiring board 20 by bonding a first bonding portion 11 of the first element 10 to a second bonding portion 21 of the wiring board 20 under first bonding conditions, for example as shown in FIG. 5 or FIG. 6.

[0023] The first elements 10 may be placed one by one on the wiring board 20. Specifically, as shown in FIG. 5, the first elements 10 are placed one by one on the wiring board 20 using a suction nozzle 101. At this time, the first bonding portion 11 of the first element 10 and the second bonding portion 21 of the wiring board 20 are brought into contact with each other and bonded under a first bonding condition. Then, the process of moving the suction nozzle 101 to place the first elements 10 on the wiring board 20 is repeated, so that a plurality of first elements 10 are placed on one wiring board 20. The distance between adjacent first elements 10 is, for example, 5 μm.

[0024] Alternatively, a plurality of first elements 10 may be placed on the wiring board 20 all at once. Specifically, as shown in FIG. 6, a structure 110 is prepared in which a plurality of first elements 10 are arranged on a support substrate 111. Next, the structure 110 is placed opposite the wiring board 20, and the first bonding portion 11 of the first element 10 and the second bonding portion 21 of the wiring board 20 are brought into contact with each other, and then bonded under a first bonding condition. Next, the support substrate 111 is separated from the first element 10. In this manner, a plurality of first elements 10 are placed on one wiring board 20.

[0025] In the process shown in Figure 5 or Figure 6, the height of the light emitting surface 13a of the wavelength conversion member 13 of the first element 10, i.e., the distance from the upper surface 22a of the base 22 of the wiring board 20, is made uniform among the multiple first elements 10, and the light emitting surface 13a is made parallel to the upper surface 22a.

[0026] However, even in this process, variations inevitably occur, and the height of light emitting surface 13a may vary among the first elements 10. Also, light emitting surface 13a may be inclined with respect to upper surface 22a. Furthermore, light emitting surface 13a may be originally curved, and light emitting surface 13a may not be parallel to upper surface 22a.

[0027] In this step, under the first bonding condition, the first bonding portion 11 and the second bonding portion 21 are heated and a load is applied in a direction in which they approach each other. Under the first bonding condition, the temperature is preferably 80°C or more and 200°C or less, more preferably 100°C or more and 150°C or less, for example, 140°C. The load applied to the first bonding portion 11 and the second bonding portion 21 is preferably 10MPa or more and 100MPa or less, more preferably 10MPa or more and 40MPa or less. Moreover, under the first bonding condition, the time for which the load is applied to the first bonding portion 11 and the second bonding portion 21 is preferably 0.1 seconds or more and 10 seconds or less, more preferably 0.1 seconds or more and 1 second or less, for example, 0.5 seconds. Under the first bonding condition, it is preferable that ultrasonic waves are not applied.

[0028] In this process, the first bonding portion 11 and the second bonding portion 21 are bonded to each other at parts of their surfaces while the first bonding portion 11 and the second bonding portion 21 generally maintain their shapes before bonding. By bonding the first bonding portion 11 and the second bonding portion 21 under the first bonding conditions, the first bonding portion 11 and the second bonding portion 21 are connected, but the mechanical bonding strength is lower than the bonding strength under the second bonding conditions described below. Hereinafter, such a state achieved under the first bonding conditions is referred to as a "temporary bonded state." As a result, the multiple first elements 10 are placed on the wiring board 20.

[0029] (Step of Evaluating Electrical Characteristics of the First Element) Next, in step S3 of FIG. 1, the electrical characteristics of the multiple first elements 10 temporarily bonded to the wiring board 20 are evaluated, for example, as shown in FIG.

[0030] Specifically, power is supplied to the first elements 10 via the wiring board 20, and the electrical characteristics of the first elements 10 are evaluated. If the first elements 10 are light-emitting elements, the electrical characteristics to be evaluated are, for example, the luminance of light emitted from the light-emitting element when a predetermined voltage is applied. By evaluating such electrical characteristics, the first elements 10 bonded to the wiring board 20 are classified into good products and bad products.

[0031] For example, a first element 10 that emits light with a luminance equal to or greater than a reference value is determined as a good product, and a first element 10 that emits light with a luminance lower than the reference value or that does not emit light is determined as a defective product. Hereinafter, a first element 10 that is determined as defective is also referred to as a "first element 10x." In addition, the second bonding portion 21 to which a first element 10x that is determined as defective in the process of evaluating the electrical characteristics of the first element 10 is bonded is referred to as a "second bonding portion 21r."

[0032] (Step of removing the first element determined to be defective from the wiring substrate) 8 and 9, for example, the first bonding portion 11 of the first element 10x determined to be defective in the process shown in step S3 is separated from the second bonding portion 21r, thereby removing the first element 10x determined to be defective from the wiring substrate 20. Note that, if there is no first element 10x determined to be defective in step S3, this process is not performed.

[0033] In this embodiment, for example, the first element 10x is heated by irradiating the first element 10x with the laser light 104. As a result, thermal stress is applied to the interface between the first bonding portion 11 and the second bonding portion 21r, and the first bonding portion 11 of the first element 10x is separated from the second bonding portion 21r. When the first element 10x is a light-emitting element including a semiconductor member, the laser light 104 is focused on the upper surface of the semiconductor member. As a result, the semiconductor member on which the laser light 104 is focused thermally expands, generating thermal stress between the first bonding portion 11 and the second bonding portion 21r, and the first bonding portion 11 is separated from the second bonding portion 21r.

[0034] The method for removing the first element 10x from the wiring board 20 is not limited to the above-mentioned method using the laser light 104. For example, the first element 10x may be removed from the wiring board 20 by adhering an adhesive jig to the first element 10x and lifting it up. The first element 10x may also be removed by sucking it with a suction device or by blowing it off with air.

[0035] (Step of bringing the third bonding portion of the second element into contact with the second bonding portion) Next, in step S5 of Fig. 1, the second element 15 is prepared. The second element 15 has, for example, the same structure as the first element 10. The second element 15 includes a pair of third bonding portions 16 in addition to the semiconductor member 12 and the wavelength conversion member 13. The third bonding portions 16 contain gold. The position, configuration, composition and function of the third bonding portions 16 in the second element 15 are similar to the position, configuration, composition and function of the first bonding portions 11 in the first element 10. Note that if there are no first elements 10x determined to be defective in step S3, this step is not performed.

[0036] Next, as shown in FIG. 10, for example, the second element 15 is placed by the suction nozzle 101 in the area of ​​the wiring board 20 where the removed first element 10x was placed. This brings the third bonding portion 16 of the second element 15 into contact with the second bonding portion 21r. The third bonding portion 16 of the second element 15 may be temporarily bonded to the second bonding portion 21r of the wiring board 20 under the first bonding condition. In this case, too, the light emitting surface 13a of the wavelength conversion member 13 of the second element 15 may be curved, the light emitting surface 13a may be inclined with respect to the upper surface 22a, and the height of the light emitting surface 13a of the second element 15 may be different from the height of the light emitting surface 13a of the first element 10.

[0037] (Step of joining the first joining portion and the second joining portion under the second joining condition) Next, in step S6 of Fig. 1, a buffer sheet 103 is placed on the multiple first elements 10, for example, as shown in Fig. 11. If a second element 15 is present, a buffer sheet 103 is also placed on the second element 15. The buffer sheet 103 is a sheet that undergoes plastic deformation, for example, a carbon sheet. The thickness of the buffer sheet 103 is, for example, preferably 0.1 mm or more and 0.2 mm or less, more preferably 0.1 mm or more and 0.15 mm or less, for example, 0.13 mm.

[0038] Then, the press plate 102 presses the plurality of first elements 10 and second elements 15 toward the wiring board 20 via the buffer sheet 103. In this process, the bonding between the first bonding portion 11 and the second bonding portion 21, and the bonding between the third bonding portion 16 and the second bonding portion 21r are performed under second bonding conditions. The second bonding conditions are conditions that realize stronger bonding than the first bonding conditions.

[0039] As a result, the first bonding portion 11 and the second bonding portion 21 in a provisionally bonded state are bonded under the second bonding condition. Furthermore, if the second element 15 is present, the third bonding portion 16 of the newly placed second element 15 and the second bonding portion 21r to which the first bonding portion 11 of the removed first element 10x had been bonded are bonded under the second bonding condition.

[0040] Hereinafter, for ease of explanation, unless otherwise specified, regardless of whether or not the second element 15 is present, the first element 10 and the second element 15 will be collectively referred to as the "first element 10", the first joint 11 and the third joint 16 will be collectively referred to as the "first joint 11", and the second joint 21 and the second joint 21r will be collectively referred to as the "second joint 21".

[0041] The second bonding condition will be described below. The load under the second bonding condition may be higher than the load under the first bonding condition. For example, as described above, the load applied to the first bonding portion 11 and the second bonding portion 21 under the first bonding condition is preferably 10 MPa or more and 100 MPa or less, whereas the load applied to the first bonding portion 11 and the second bonding portion 21 under the second bonding condition is preferably 10 MPa or more and 440 MPa or less.

[0042] Alternatively, the time for which the load is applied under the second bonding condition may be longer than the time for which the load is applied under the first bonding condition. For example, as described above, the time for which the load is applied to the first bonding portion 11 and the second bonding portion 21 under the first bonding condition is preferably 0.1 seconds or more and 10 seconds or less, whereas the time for which the load is applied to the first bonding portion 11 and the second bonding portion 21 under the second bonding condition is preferably 1 minute or more and 10 minutes or less.

[0043] Alternatively, the temperature of the second bonding condition may be higher than that of the first bonding condition. For example, as described above, the temperature of the first bonding condition is preferably 80°C or more and 200°C or less, more preferably 140°C, whereas the temperature of the second bonding condition is preferably 100°C or more and 200°C or less, more preferably 150°C. Also, similar to the first bonding condition, it is preferable not to apply ultrasonic waves in the second bonding condition. The reason is that when multiple first elements 10 are bonded to the wiring board 20 at once, even if ultrasonic waves are applied to the multiple first elements 10, ultrasonic vibrations are difficult to stably apply to each first element 10, and there is a possibility that the bonding strength may vary.

[0044] In this embodiment, the bonding step under the second bonding conditions is repeated multiple times. At this time, in at least two bonding steps under the second bonding conditions, different buffer sheets 103 are used, or different parts of the same buffer sheet 103 are used. This makes it possible to bond the first bonding portion 11 and the second bonding portion 21 more firmly, and to reduce the variation in bonding strength between the wiring board 20 and the multiple first elements 10.

[0045] These multiple bonding processes will be described in more detail below. 1, in this embodiment, the process of bonding under the second bonding condition (hereinafter, referred to as the "main bonding process") is repeated four times. The time for each main bonding process is, for example, four minutes. That is, the main bonding process is performed for a total of 16 minutes.

[0046] In the first main bonding process, which is step S6 in Fig. 1, for example as shown in Fig. 11, there is variation in the height, inclination or flatness of the light emitting surface 13a of each first element 10. However, the buffer sheet 103 plastically deforms to match the shape of the first element 10 and comes into contact with substantially the entire light emitting surface 13a. This makes it possible to correct the warping of the light emitting surface 13a without destroying the first element 10, and also correct the variation in the height of the light emitting surface 13a and the inclination of the light emitting surface 13a of each first element 10.

[0047] Note that "correction" is not limited to making the light emitting surface 13a completely flat, making the height of the light emitting surface 13a uniform among the multiple first elements 10, and making the light emitting surface 13a completely parallel to the upper surface 22a of the base 22, but only requires that the warping, height variation, and tilt of the light emitting surface 13a are improved compared to before the correction. For example, the warping, height variation, and tilt of the light emitting surface 13a after the first main bonding step are reduced compared to the previous temporary bonding state.

[0048] As described above, immediately before the first bonding process, there is variation in the height, inclination or flatness of the light emission surface 13a of each first element 10, and therefore stress is not applied uniformly from the buffer sheet 103 to the first elements 10.

[0049] For example, when the height of the light emitting surface 13a varies for each first element 10, the first element 10 whose light emitting surface 13a is located at a relatively low position receives a smaller stress from the buffer sheet 103 than the first element 10 whose light emitting surface 13a is located at a relatively high position. Also, when the light emitting surface 13a is inclined, the portion of the light emitting surface 13a close to the wiring board 20 receives a smaller stress from the buffer sheet 103 than the portion of the light emitting surface 13a far from the wiring board 20. Furthermore, when the light emitting surface 13a is curved concavely, the bottom of the curve receives a smaller stress from the buffer sheet 103 than the peripheral portion. When the light emitting surface 13a is curved convexly, the peripheral portion of the curve receives a smaller stress from the buffer sheet 103 than the top.

[0050] In the portion of the first element 10 where the stress applied from the buffer sheet 103 is small, the bonding strength between the first bonding portion 11 and the second bonding portion 21 is lower than in the portion where the stress is large. As a result, at the stage where the first main bonding step is completed, there is a large variation in the bonding strength between the first element 10 and the wiring board 20.

[0051] 12, the press plate 102 and the buffer sheet 103 are separated from the first element 10. The buffer sheet 103 is pressed by the first element 10 and plastically deformed, so that a recess 103a reflecting the shape of the first element 10 is formed on the lower surface of the buffer sheet 103.

[0052] Next, in step S7 of FIG. 1, a second main bonding process is performed, for example, as shown in FIG. 13. At this time, a new buffer sheet 103 is used, or an unused portion of the buffer sheet 103 used in the first main bonding process is used. Therefore, no recess 103a is formed in the portion of the buffer sheet 103 that contacts the first element 10. The bonding conditions in the second main bonding process are also the second bonding conditions. Note that the bonding conditions in the second main bonding process may be changed from the second bonding conditions in the first main bonding process.

[0053] Immediately before the second main bonding process, the variation in height, inclination, and curvature of the light emitting surface 13a have been corrected by the first main bonding process. In addition, no recesses 103a are formed in the buffer sheet 103 used. Therefore, in the second main bonding process, stress is applied more uniformly from the buffer sheet 103 to the first element 10 than in the first main bonding process.

[0054] As a result, after the second main bonding process, the variation in the bonding strength between the first element 10 and the wiring board 20 is smaller than that immediately after the first main bonding process. Furthermore, the variation in height, inclination, and curvature of the light emitting surface 13a that could not be completely corrected in the first main bonding process are also corrected in the second main bonding process.

[0055] Next, in step S8 of Fig. 1, a third main bonding process is performed. At this time, a new buffer sheet 103 is used, or an unused portion of the buffer sheet 103 used in the second main bonding process is used. The bonding conditions in the third main bonding process are the second bonding conditions. Note that the bonding conditions in the third main bonding process may be changed from the second bonding conditions in the first or second main bonding process.

[0056] This makes it possible to bond the first bonding portion 11 and the second bonding portion 21 more firmly. Also, the variation in bonding strength is reduced. Furthermore, even if there is any variation in height, inclination, or curvature of the light emitting surface 13a that could not be corrected in the first and second main bonding steps, these will be corrected in the third main bonding step.

[0057] Next, in step S9 of Fig. 1, a fourth main bonding process is performed. In this case, either a new buffer sheet 103 is used, or an unused portion of the buffer sheet 103 used in the third main bonding process is used. The bonding conditions in the fourth main bonding process are the second bonding conditions, but the bonding conditions in the fourth main bonding process may be changed from the second bonding conditions in the first, second or third main bonding processes. This allows the first bonding portion 11 and the second bonding portion 21 to be bonded more firmly, and the variation in bonding strength is further reduced.

[0058] The number of times of the main bonding step is not limited to four, but may be two or more, and may be five or more. In addition, in each main bonding step, it is preferable to use a different buffer sheet 103 each time, or to use different parts of the same buffer sheet 103, but this is not necessarily limited to this. However, it is preferable to use different buffer sheets 103 or different parts of the same buffer sheet 103 in at least two main bonding steps.

[0059] In this way, by carrying out the main bonding process multiple times, the corresponding first bonding portion 11 and second bonding portion 21 are integrated to form the fourth bonding portion 17. In the fourth bonding portion 17, most of the interface between the first bonding portion 11 and the second bonding portion 21 disappears. Also, if there is a gap at the interface, most of the gap disappears. As a result, the mechanical bonding strength between the first element 10 and the wiring board 20 becomes higher than in the temporary bonding state. This state is called the "main bonding state." In this way, the light emitting device 1 is manufactured.

[0060] (Light emitting device) Next, the structure of the manufactured light emitting device 1 will be described. FIG. 14 is a plan view showing the light emitting device according to this embodiment. FIG. 15 is a cross-sectional view taken along line XV-XV shown in FIG.

[0061] As shown in Figs. 14 and 15, the light emitting device 1 according to this embodiment has a wiring substrate 20, a plurality of first elements 10, and a plurality of fourth bonding portions 17. The first elements 10 also include the above-mentioned second elements 15. The number of the first elements 10 is, for example, 10 or more. The first elements 10 are light emitting elements, for example, light emitting diodes. In a plan view, the shape of the first elements 10 is rectangular, for example, square.

[0062] The first element 10 has a semiconductor member 12 and a wavelength conversion member 13 arranged on the semiconductor member 12. In the semiconductor member 12, a p-type semiconductor layer, an active layer, and an n-type semiconductor layer are laminated. In a plan view, the wavelength conversion member 13 is larger than the semiconductor member 12, and the outer edge of the wavelength conversion member 13 is located outside the outer edge of the semiconductor member 12. The wiring board 20 has an insulating base 22 and a plurality of conductive wirings 23 arranged in the base 22. The multiple first elements 10 are arranged, for example, in a matrix on the upper surface 22a of the wiring board 20.

[0063] The first element 10 is connected to the wiring 23 of the wiring board 20 via the fourth bonding portion 17 and is mechanically coupled thereto. As described above, the fourth bonding portion 17 is formed by integrating the first bonding portion 11 and the second bonding portion 21. Therefore, the fourth bonding portion 17 contains gold. For example, the fourth bonding portion 17 is entirely made of gold. In this embodiment, two fourth bonding portions 17 are bonded to each first element 10. One fourth bonding portion 17 is connected to the p-type semiconductor layer of the first element 10, and the other fourth bonding portion 17 is connected to the n-type semiconductor layer of the first element 10.

[0064] In the light emitting device 1, the variation in the bonding strength between the multiple first elements 10 and the wiring board 20 is reduced. Furthermore, the height of the light emitting surface 13a of the wavelength conversion member 13 from the wiring board 20 is substantially uniform, and the light emitting surface 13a is parallel to the upper surface 22a of the base 22 of the wiring board 20. In this specification, it is considered that an angle deviation of ±5° from the parallel state is allowed. Furthermore, the light emitting surface 13a is substantially flat.

[0065] The ratio (σ / A) of the standard deviation (σ) to the average value (A) of the bonding strength of each first element 10 to the wiring board 20 is preferably 0.1 or less, and more preferably 0.03 or less. The bonding strength is the magnitude of a force that is applied to one first element 10 in a direction parallel to the upper surface 22a of the base 22 of the wiring board 20 when the first element 10 is separated from the wiring board 20. The average value and standard deviation of the bonding strength are preferably determined by measuring the bonding strength of all the first elements 10 included in the light emitting device 1, but when the light emitting device 1 includes 10 or more first elements 10, it is sufficient to measure the bonding strength of at least 10 first elements 10.

[0066] An example of the size and strength of the light emitting device 1 will now be described. In the first example, the length of one side of the first elements 10, i.e., the length of one side of the wavelength conversion member 13, is 40 μm or more and 50 μm or less, for example, 45 μm, in a plan view. The distance between the first elements 10 is 5 μm.

[0067] In the second example, in plan view, the length of one side of the first elements 10, i.e., the length of one side of the wavelength conversion member 13, is 500 μm or more and 1500 μm or less, for example, 1000 μm. The distance between the first elements 10 is 50 μm or more and 150 μm or less, for example, 100 μm. In this case, the thickness of the fourth bonding portion 17 is about 1 μm. Also, the average bonding strength of the multiple first elements 10 to the wiring board 20 is 10 kgf or more.

[0068] (effect) The effects of this embodiment will be described. According to this embodiment, as shown in steps S6 to S9 in Fig. 1, by performing this bonding process multiple times, even if the light emitting surface 13a of the first element 10 varies in height, is inclined, or is curved with respect to the upper surface 22a of the wiring board 20, it is possible to apply a load to the first connection portion 11 and the second connection portion 12 while correcting the variation in height, inclination, and curvature. Therefore, it is possible to apply a load uniformly to the first connection portion 11 and the second connection portion 12, and it is possible to bond a plurality of first elements 10 to the wiring board 20 with uniform strength. That is, as described above, the value (σ / A) of the ratio of the standard deviation (σ) to the average value (A) of the bonding strength of each first element 10 to the wiring board 20 can be set to 0.1 or less, for example, 0.03 or less.

[0069] In this embodiment, in a process shown in step S2 of Fig. 1, the first bonding portions 11 of the multiple first elements 10 are temporarily bonded to the second bonding portions 21 of the wiring board 20 under a first bonding condition, and then in a process shown in step S3 of Fig. 1, a process of evaluating the electrical characteristics of each first element 10 is performed, and the first elements 10x determined to be defective are removed in a process shown in step S4. Next, in a process shown in step S5, a second element 15 is placed in the area of ​​the wiring board 20 after the first elements 10x have been removed, and in multiple main bonding processes shown in steps S6 to S9, the first bonding portions 11 of the first elements 10 determined to be non-defective are bonded to the second bonding portions 21r, and the newly placed second element 15 is bonded to the second bonding portions 21r to which the first elements 10x determined to be defective were bonded.

[0070] This allows multiple first elements 10 to be temporarily bonded to the wiring board 20 all at once, and allows the electrical characteristics of the multiple first elements 10 to be evaluated via the wiring board 20. Furthermore, it allows efficient replacement of defective first elements 10x with non-defective second elements 15. As a result, the productivity of the light emitting device 1 is improved.

[0071] Furthermore, in this embodiment, the provisional bonding step is performed under the first bonding condition, and the main bonding step is performed under the second bonding condition. The second bonding condition is a condition that the bonding strength is higher than that of the first bonding condition. As a result, in the provisional bonding step under the first bonding condition, the first bonding portion 11 is connected to the second bonding portion 21, but the mechanical bonding strength is in a provisional bonding state that is lower than that of the main bonding state. As a result, it becomes easy to remove the first element 10x that is determined to be defective while evaluating the electrical characteristics of the first element 10. On the other hand, in the main bonding step under the second bonding condition, the bonding strength between the first bonding portion 11 and the second bonding portion 21 is higher than that in the provisional bonding state. As a result, the bonding strength between the first element 10 and the wiring board 20 can be increased, and the reliability of the light emitting device 1 is improved.

[0072] Furthermore, in this embodiment, the first element 10x determined to be defective is irradiated with laser light 104 to heat the first element 10x, thereby generating thermal stress between the first bonding portion 11 of the first element 10x and the second bonding portion 21r of the wiring board 20. This makes it possible to release the bonding between the first bonding portion 11 and the second bonding portion 21r while suppressing damage to the wiring board 20. Furthermore, by irradiating only the first element 10x with laser light 104, it is possible to accurately heat only the first element 10x determined to be defective among the multiple first elements 10.

[0073] Furthermore, in this embodiment, the first bonding portion 11, the second bonding portion 21, and the third bonding portion 16 contain gold. In a temporary bonding step, a portion of the first bonding portion 11 containing gold and a portion of the second bonding portion 21 containing gold are bonded together. For example, the outermost surface of the first bonding portion 11 made of gold and the outermost surface of the second bonding portion 21 made of gold are bonded together. Thereafter, thermal stress is generated at the bonding interface between the first bonding portion 11 and the second bonding portion 21 to remove the first elements 10x determined to be defective.

[0074] In response to this, for example, it is conceivable to temporarily bond the first bonding portion 11 and the second bonding portion 21 using a bonding material containing tin (Sn). However, since the bonding material containing tin is difficult to remove after bonding, there is a possibility that residue of the bonding material will remain on the surface of the second bonding portion 21r after the first element 10x is removed. Therefore, there is a possibility that the bonding strength between the third bonding portion 16 of the second element 15 and the second bonding portion 21r will be reduced due to the residue of the bonding material.

[0075] In the present embodiment, in the step of removing the first element 10x, the bond is released at the interface between the gold-containing portion of the first bonding portion 11 and the gold-containing portion of the second bonding portion 21, so that residue is less likely to remain on the surface of the second bonding portion 21r. Therefore, the third bonding portion 16 of the second element 15 can be bonded to the second bonding portion 21r with high strength.

[0076] In this embodiment, the third bonding portion 16 of the second element 15 may be brought into contact with the second bonding portion 21r of the wiring board 20, and then the electrical characteristics of the second element 15 may be evaluated via the wiring board 20. If the second element 15 is determined to be defective by this process, the second element 15 may be removed by a method similar to that for the first element 10x. At this time, before evaluating the electrical characteristics, the third bonding portion 16 may be bonded under the first bonding conditions, and the bonded state between the third bonding portion 16 and the second bonding portion 21r may be a temporary bonded state.

[0077] In addition, in the present embodiment, an example has been shown in which the first element 10 has the wavelength conversion member 13, but the first element 10 does not have to have a wavelength conversion member. Furthermore, in the present embodiment, an example has been shown in which the first element 10 is a light-emitting element, but the present invention is not limited thereto, and the first element 10 may be, for example, a calculation element, a memory element for storing data, or a switching element for power control.

[0078] <Second embodiment> FIG. 16 is a cross-sectional view showing a method for manufacturing a light emitting device according to this embodiment. FIG. 16 corresponds to FIG. 12 of the first embodiment, and shows a state between the first and second main bonding steps.

[0079] 16, this embodiment differs from the first embodiment in that an elastically deforming buffer sheet 105 is used instead of the plastically deforming buffer sheet 103, and that the same portion of the same buffer sheet 105 is used in at least two main joining steps. The elastically deforming buffer sheet 105 is, for example, a sheet made of silicone rubber, and has a thickness of, for example, 0.1 mm or more and 0.2 mm or less, for example, 0.1 mm.

[0080] In this embodiment, an elastically deformable sheet is used as the buffer sheet 105, so that after the main bonding step, no depression reflecting the shape of the first element 10 is formed in the buffer sheet 105. Therefore, even if the same portion of the same buffer sheet 105 is used in the next main bonding step, a load can be applied uniformly to the multiple first elements 10. Other methods, configurations, and effects of this embodiment are similar to those of the first embodiment. Note that in this embodiment, as in the first embodiment, different buffer sheets 105 or different portions of the same buffer sheet 105 may be used in at least two main bonding steps.

[0081] <Third embodiment> The third embodiment is an example of manufacturing a light emitting module using the manufacturing method for the light emitting device according to the above-described first embodiment.

[0082] First, the configuration of the light emitting module according to this embodiment will be described. FIG. 17 is a plan view showing the light emitting module according to the present embodiment. FIG. 18 is a partially enlarged plan view showing the first element and the wavelength conversion member in this embodiment.

[0083] 17 and 18, a light emitting module 201 according to this embodiment includes a wiring board 211. The shape of the wiring board 211 in a plan view is, for example, a rectangle. A plurality of first elements 212 are arranged on the upper surface of the wiring board 211. Two bonding portions 213 are arranged on each of the first elements 212, and the first elements 212 are placed on the wiring board 211 via the bonding portions 213. The bonding portions 213 contain gold.

[0084] In this embodiment, for convenience of explanation, an XYZ orthogonal coordinate system is adopted. The longitudinal direction of wiring board 211 is defined as the "X direction", the lateral direction as the "Y direction", and the thickness direction as the "Z direction". Within the Z direction, the direction from wiring board 211 toward first element 212 is also referred to as "up" and the opposite direction as "down", but these expressions are also for convenience and are unrelated to the direction of gravity.

[0085] On the upper surface of the wiring board 211, the first elements 212 are arranged, for example, in two rows. Each row extends in the longitudinal direction of the wiring board 211, i.e., in the X direction. In the first row 221, for example, 20 first elements 212 are arranged, and in the second row 222, for example, 22 first elements 212 are arranged. Therefore, a total of 42 first elements 212 are arranged in the light-emitting module 201. In one example, the shape of each first element 212 in a plan view is a square, and the length of one side is 500 μm or more and 1000 μm or less.

[0086] A wavelength conversion member 214 is disposed on each of the first elements 212. The wavelength conversion member 214 is, for example, a plate-like member containing YAG as a phosphor. In one example, the shape of each wavelength conversion member 214 in a plan view is a square, and the length of one side is 550 μm to 1100 μm. In one example, the distance between adjacent wavelength conversion members 214 in each row is 30 μm to 70 μm. The number of wavelength conversion members 214 is the same as the number of first elements 212.

[0087] Resin member 215 is disposed on wiring board 211. Resin member 215 covers a central portion of the upper surface of wiring board 211. Resin member 215 covers the side surfaces of first element 212 and wavelength conversion member 214, but does not cover the upper surface of wavelength conversion member 214. Therefore, the upper surface of wavelength conversion member 214 is exposed from resin member 215. In resin member 215, for example, a light-transmitting resin contains a light-reflecting substance. The resin is, for example, a silicone resin. The light-reflecting substance is, for example, titanium oxide.

[0088] Pads 216 are arranged on both sides in the Y direction of the area covered by resin member 215 on the upper surface of wiring board 211. Pads 216 are arranged in two rows along an edge extending in the X direction of wiring board 211. Third row 223 of pads 216 is arranged on the first row 221 side of first elements 212. Fourth row 224 of pads 216 is arranged on the second row 222 side of first elements 212.

[0089] The number of pads 216 belonging to each row is one more than the number of first elements 212 belonging to the corresponding row. That is, 21 pads 216 are arranged in the third row 223, and 23 pads 216 are arranged in the fourth row 224. The 21 pads 216 belonging to the third row and the 20 first elements 212 belonging to the first row are alternately connected in series. Similarly, the 23 pads 216 belonging to the fourth row and the 22 first elements 212 belonging to the second row are alternately connected in series.

[0090] Next, a method for manufacturing the light emitting module according to this embodiment will be described. As shown in Fig. 17, wiring board 211 is prepared. Pads 216 are arranged on the upper surface of wiring board 211. Wiring board 211 of the present embodiment corresponds to wiring board 20 of the first embodiment. Next, a plurality of first elements 212 are placed on wiring board 211. First elements 212 of the present embodiment correspond to a configuration of first element 10 of the first embodiment excluding wavelength conversion member 13.

[0091] At this time, as described in the first embodiment, the first element 212 is bonded to the wiring board 211 in a provisionally bonded state, and the electrical characteristics, for example, luminance, of the first element 212 are evaluated, and the first element 212 determined to be defective is removed. Then, a new first element 212 is placed in the area after the first element 212 determined to be defective is removed, and all the first elements 212 are bonded together in a permanently bonded state. The new first element 212 in this embodiment corresponds to the second element 15 in the first embodiment. As a result, the defective first element 212 is replaced with a good one. In addition, a bonding portion 213 is formed between the wiring board 211 and the first element 212. The bonding portion 213 corresponds to the fourth bonding portion 17 in the first embodiment.

[0092] As in the first embodiment, the main bonding step is repeated multiple times. In the main bonding step, a plastically deformable buffer sheet 103 is used, and a different buffer sheet 103 is used at least twice, or preferably each time, or different parts of the same buffer sheet 103 are used. As in the second embodiment, an elastically deformable buffer sheet 105 may be used, and the same parts of the same buffer sheet 105 may be used in multiple main bonding steps.

[0093] Next, wavelength conversion members 214 are placed on each of the first elements 212. The wavelength conversion members 214 in this embodiment correspond to the wavelength conversion members 13 in the first embodiment. Next, a resin member 215 is formed so as to cover the upper surface of the wiring board 211, the side surfaces of the first elements 212, and the side surfaces of the wavelength conversion members 214. In this manner, the light emitting module 201 according to this embodiment is manufactured.

[0094] The ratio of the standard deviation to the average value of the bonding strength of each first element 212 to wiring board 211 is preferably 0.1 or less, and more preferably 0.03 or less. The average value of the bonding strength is preferably 10 kgf or more.

[0095] The above-described embodiments are examples of the present invention, and the present invention is not limited to these embodiments. For example, the present invention also includes the addition, deletion, or modification of some components or steps in the above-described embodiments.

[0096] <Test Example> Next, a test example showing the effect of the first embodiment will be described. FIG. 19 is a diagram showing a measuring device for measuring the bonding strength in this test example. FIG. 20A is a front view showing a jig of a measuring device used in this test example, FIG. 20B is a side view thereof, and FIG. 20C is a partially enlarged side view showing an area XXC in FIG. 20B. FIG. 21 is a cross-sectional view showing a method for measuring the bonding strength in this test example. 22 is a graph showing the bonding strength of the example and the comparative example. Note that this graph shows the effect of repeating this bonding process multiple times, with the horizontal axis representing the type of sample and the vertical axis representing the bonding strength between the first element and the wiring board.

[0097] As shown in FIG. 19, a bonding strength measuring device 300 is provided with a load sensor 301 and a jig 302 attached to the load sensor 301 . As shown in Figures 20A to 20C, in jig 302, main body 303 and tip 304 are integrally formed. Jig 302 is made of cemented carbide. Main body 303 is approximately cylindrical in shape. The thickness of the upper part of main body 303 is uniform, and the lower part becomes thinner toward the lower end. Tip 304 extends from the lower end of main body 303. Tip 304 is plate-shaped. Tip 304 has a width a of approximately 1 mm, a thickness b of approximately 0.2 mm, and a height c of approximately 0.2 mm.

[0098] In this test example, a sample was prepared as an example, in which the main bonding was performed by the method described in the first embodiment. The number of bonding operations was four, and the bonding time was four minutes per operation. In other words, the total bonding time was 16 minutes. A carbon sheet with a thickness of 0.13 mm was used as the buffer sheet 103. Meanwhile, a sample was prepared as a comparative example, in which the main bonding was performed only once. The bonding time was 15 minutes. The temperature in the example and comparative example was 200°C, and the load was 44 MPa.

[0099] As shown in FIG. 21 , tip 304 of jig 302 of measuring device 300 was inserted between first elements 10 and faced the side surface of wavelength conversion member 13 of one of the first elements 10. At this time, clearance d between wiring board 20 and jig 302 was set to 30 μm. Then, measuring device 300 was moved along a direction parallel to upper surface 22a of wiring board 20. Moving speed v was set to 100 μm / s. By moving measuring device 300, tip 304 of jig 302 came into contact with the side surface of wavelength conversion member 13 of one of the first elements 10, and a force was applied to this first element 10. Then, load sensor 301 measured the load when this first element 10 was detached from wiring board 20, and this was taken as the bonding strength.

[0100] For the examples, the bonding strength was measured for 12 first elements 10. For the comparative examples, the bonding strength was measured for 24 first elements 10. The measurement results are shown in Fig. 22. Table 1 shows the average (A), maximum (Max), minimum (Min) and standard deviation (σ) of the bonding strength in the examples and comparative examples, as well as the ratio of the standard deviation to the average (σ / A).

[0101] [Table 1]

[0102] 22, the average bonding strength of the samples according to the comparative example was 6.01 kgf, while the average bonding strength of the samples according to the embodiment was 12.43 kgf, which was higher than the average bonding strength of the samples according to the comparative example. In addition, the ratio (σ / A) of the standard deviation to the average value of the samples according to the comparative example was 0.22, while the ratio (σ / A) of the samples according to the embodiment was 0.02, which was smaller in variation.

[0103] The present invention includes the following aspects.

[0104] (Appendix 1) preparing a wiring substrate including a plurality of first elements including a first bonding portion and a plurality of second bonding portions; a step of mounting the first elements on the wiring substrate by bonding the first bonding portion and the second bonding portion under a first bonding condition; a step of placing a buffer sheet on the plurality of first elements and pressing the plurality of first elements toward the wiring board via the buffer sheet, thereby bonding the first bonding portion and the second bonding portion under a second bonding condition; Equipped with A method for manufacturing a light emitting device, comprising repeating the bonding step under the second bonding condition a plurality of times.

[0105] (Appendix 2) After the step of placing the substrate on the wiring board and before the step of bonding under the second bonding condition, evaluating electrical characteristics of the plurality of first elements; removing the first element determined to be defective in the evaluating step from the wiring substrate by separating the first bonding portion of the first element from the second bonding portion; placing a second element including a third bonding portion in a region of the wiring board where the removed first element was placed, thereby bringing the third bonding portion into contact with the second bonding portion to which the first bonding portion of the removed first element was bonded; Further equipped with A method for manufacturing a light emitting device as described in Appendix 1, wherein in the bonding step under the second bonding conditions, the third bonding portion is bonded to a second bonding portion to which the first bonding portion of the removed first element was bonded.

[0106] (Appendix 3) The buffer sheet is a sheet that undergoes plastic deformation, The method for manufacturing a light emitting device according to claim 1 or 2, wherein in the step of bonding under the second bonding condition at least twice, different buffer sheets are used, or different parts of the same buffer sheet are used.

[0107] (Appendix 4) The buffer sheet is an elastically deformable sheet, The method for manufacturing a light emitting device according to claim 1 or 2, wherein the same buffer sheet is used in at least two bonding steps under the second bonding condition.

[0108] (Appendix 5) 5. The method for manufacturing a light emitting device according to claim 1, wherein the load under the second bonding condition is higher than the load under the first bonding condition.

[0109] (Appendix 6) A method for manufacturing a light emitting device described in any one of Appendices 1 to 5, wherein a load applied to the first bonding portion and the second bonding portion under the first bonding condition is 10 MPa or more and less than 100 MPa, and a load applied to the first bonding portion and the second bonding portion under the second bonding condition is 10 MPa or more and 440 MPa or less.

[0110] (Appendix 7) A method for manufacturing a light emitting device described in any one of Appendices 1 to 6, wherein the time for which a load is applied to the first bonding portion and the second bonding portion under the second bonding condition is longer than the time for which a load is applied to the first bonding portion and the second bonding portion under the first bonding condition.

[0111] (Appendix 8) A method for manufacturing a light emitting device described in any one of Appendices 1 to 7, wherein the time for which a load is applied to the first bonding portion and the second bonding portion under the first bonding condition is 0.1 seconds or more and 10 seconds or less, and the time for which a load is applied to the first bonding portion and the second bonding portion under the second bonding condition is 1 minute or more and 10 minutes or less.

[0112] (Appendix 9) 9. The method for producing a light emitting device according to any one of claims 1 to 8, wherein the temperature of the second bonding condition is 100° C. or higher and 200° C. or lower.

[0113] (Appendix 10) A method for manufacturing a light emitting device according to any one of claims 1 to 9, wherein the first element includes a semiconductor member, the first bonding portion arranged on a first surface of the semiconductor member, and a wavelength conversion member arranged on a second surface of the semiconductor member opposite the first surface.

[0114] (Appendix 11) 11. The method for producing a light emitting device according to any one of claims 1 to 10, wherein the first bonding portion and the second bonding portion contain gold.

[0115] (Appendix 12) A wiring board having wiring; A plurality of first elements; a plurality of junctions connecting the plurality of first elements to the wiring; Equipped with A light emitting device, wherein a ratio of a standard deviation to an average value of bonding strength of the plurality of first elements to the wiring board is 0.1 or less.

[0116] (Appendix 13) 13. The light emitting device of claim 12, wherein the value of the ratio is 0.03 or less.

[0117] (Appendix 14) A wiring board having wiring; A plurality of first elements; a plurality of junctions connecting the plurality of first elements to the wiring; Equipped with In a plan view, the length of one side of each of the first elements is 500 μm or more and 1500 μm or less, The light emitting device, wherein the average bonding strength of the plurality of first elements to the wiring board is 10 kgf or more.

[0118] (Appendix 15) 15. The light emitting device according to claim 14, wherein a ratio of a standard deviation to an average value of bonding strengths of the plurality of first elements to the wiring substrate is 0.1 or less. [Industrial Applicability]

[0119] The embodiment of the present invention can be used, for example, as a headlamp for a vehicle and a light source for a display device. [Explanation of symbols]

[0120] 1 Light emitting device 10 First element 11 1st joint 12 Semiconductor materials 12a 1st page 12b Side 2 13 Wavelength conversion materials 13a Light exit surface 15 Second element 16 Third joint 17 4th joint 20 Wiring board 21 Second joint 22 Base 22a Top side 23 Wiring 24 Opening 101 Suction nozzle 102 Press plate 103 Cushioning sheet 103a Dent 104 Laser light 105 Cushioning Sheet 110 Structure 111 Support substrate 201 Light Emitting Module 211 Wiring board 212 1st element 213 Joint 214 Wavelength conversion material 215 Resin parts 216 Pad 221 1st row 222 2nd row 223 3rd row 224 4th column 300 Measuring Equipment 301 Load Sensor 302 Jig 303 Main body 304 Tip a Width of the tip 304 b Thickness of tip portion 304 c Height of tip 304 d Clearance between the wiring board 20 and the jig 302 v. Moving speed of the measuring device 300

Claims

1. preparing a wiring substrate including a plurality of first elements including a first bonding portion and a plurality of second bonding portions; a step of mounting the first elements on the wiring substrate by bonding the first bonding portion and the second bonding portion under a first bonding condition; a step of placing a buffer sheet on the plurality of first elements and pressing the plurality of first elements toward the wiring board via the buffer sheet, thereby bonding the first bonding portion and the second bonding portion under a second bonding condition; Equipped with The method for manufacturing a light emitting device includes repeating the bonding step under the second bonding condition a plurality of times.

2. After the step of placing the substrate on the wiring board and before the step of bonding under the second bonding condition, evaluating electrical characteristics of the plurality of first elements; removing the first element determined to be defective by the evaluating step from the wiring substrate by separating the first bonding portion of the first element from the second bonding portion; placing a second element including a third bonding portion in a region of the wiring board where the removed first element was placed, thereby bringing the third bonding portion into contact with the second bonding portion to which the first bonding portion of the removed first element was bonded; Further equipped with The method for manufacturing a light emitting device according to claim 1 , wherein in the step of bonding under the second bonding condition, the third bonding portion is bonded to a second bonding portion to which the first bonding portion of the removed first element was bonded.

3. The buffer sheet is a sheet that undergoes plastic deformation, The method for manufacturing a light emitting device according to claim 1 , wherein different buffer sheets or different portions of the same buffer sheet are used in at least two bonding steps under the second bonding condition.

4. The buffer sheet is an elastically deformable sheet, The method for manufacturing a light emitting device according to claim 1 , wherein the same buffer sheet is used in at least two bonding steps under the second bonding condition.

5. The method for manufacturing a light emitting device according to claim 1 , wherein the load under the second bonding condition is higher than the load under the first bonding condition.

6. 2. The method for manufacturing a light emitting device according to claim 1, wherein the load applied to the first bonding portion and the second bonding portion under the first bonding condition is 10 MPa or more and less than 100 MPa, and the load applied to the first bonding portion and the second bonding portion under the second bonding condition is 10 MPa or more and 440 MPa or less.

7. The method for manufacturing a light emitting device according to claim 1 , wherein the time for which a load is applied to the first bonding portion and the second bonding portion under the second bonding condition is longer than the time for which a load is applied to the first bonding portion and the second bonding portion under the first bonding condition.

8. 2. The method for manufacturing a light-emitting device according to claim 1, wherein the time for which a load is applied to the first bonding portion and the second bonding portion under the first bonding condition is 0.1 seconds or more and 10 seconds or less, and the time for which a load is applied to the first bonding portion and the second bonding portion under the second bonding condition is 1 minute or more and 10 minutes or less.

9. The method for manufacturing a light emitting device according to claim 1 , wherein the temperature of the second bonding condition is 100° C. or higher and 200° C. or lower.

10. The method for manufacturing a light emitting device according to claim 1, wherein the first element includes a semiconductor member, the first bonding portion arranged on a first surface of the semiconductor member, and a wavelength conversion member arranged on a second surface of the semiconductor member opposite the first surface.

11. The method for manufacturing a light emitting device according to claim 1 , wherein the first bonding portion and the second bonding portion contain gold.

12. A wiring board having wiring; A plurality of first elements; a plurality of junctions connecting the plurality of first elements to the wiring; Equipped with A light emitting device, wherein a ratio of a standard deviation to an average value of bonding strength of the plurality of first elements to the wiring substrate is 0.1 or less.

13. 13. The light emitting device of claim 12, wherein the value of said ratio is 0.03 or less.

14. A wiring board having wiring; A plurality of first elements; a plurality of junctions connecting the plurality of first elements to the wiring; Equipped with In a plan view, the length of one side of each of the first elements is 500 μm or more and 1500 μm or less, A light emitting device, wherein an average bonding strength of the plurality of first elements to the wiring board is 10 kgf or more.

15. The light emitting device according to claim 14 , wherein a ratio of a standard deviation to an average value of bonding strengths of the plurality of first elements to the wiring board is 0.1 or less.

Citation Information

Patent Citations

  • Image forming element and manufacturing method

    JP2020074005A