Decorative sheet and decorative member
The decorative sheet design addresses the issue of high glossiness in large particle-sized beads by using a lower gloss protective layer and strategic layer ratios, achieving a strong tactile and authentic appearance.
Patent Information
- Application Number
- JP2023148259
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-09-13
- Publication Date
- 2024-10-11
AI Technical Summary
Decorative sheets with large particle-sized beads in the raised parts achieve a strong tactile sensation but result in high glossiness, leading to an unnatural and less authentic appearance.
A decorative sheet design with a protective layer having a lower gloss value than the raised layer, a ratio of the raised layer area to the protective layer area of 10% or more, and an average distance of 1.6 mm or more between adjacent raised parts, along with specific particle compositions and thickness ratios.
The design provides a strong tactile feel with a realistic and authentic appearance by reducing glossiness while maintaining durability and design synergy.
Smart Images

Figure 2024144010000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a decorative sheet and a decorative member. [Background technology]
[0002] For example, decorative members having a base and a decorative sheet are used to impart design features to the surfaces of building materials, furniture, and the like.
[0003] A decorative sheet has, for example, a design layer and a surface protection layer on a base layer. Furthermore, it has been proposed to provide a raised portion on the surface of the decorative sheet in order to obtain a tactile feel (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-87158 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a demand for decorative sheets with a strong, rough feel. It has been thought that a strong feel can be imparted by including beads with a large particle size in the raised portion. However, including beads with a large particle size in the raised portion can make the raised portion highly glossy, resulting in an unnatural design that lacks a sense of realism. For this reason, there is a demand for decorative sheets that have a sense of realism while enhancing the feel of the raised portion.
[0006] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide a decorative sheet that has a strong tactile sensation and a feeling of the real thing. [Means for solving the problem]
[0007] The present disclosure provides a decorative sheet having, in that order in the thickness direction, a base layer, a design layer, a protective layer, and a raised layer having a patterned raised portion, wherein the 60° gloss value of the protective layer is smaller than the 60° gloss value of the raised layer, the 60° gloss value of the raised layer is 20 or less, the ratio of the area of the raised layer to the area of the protective layer in the thickness direction is 10% or more, and the average spacing between adjacent raised portions is 1.6 mm or more.
[0008] The present disclosure provides a decorative member having a substrate and the decorative sheet described above. Effect of the Invention
[0009] The present disclosure has the effect of providing a decorative sheet that has a strong feel and a sense of realism. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. [Diagram 2] FIG. 2 is a schematic top view illustrating a decorative sheet according to the present disclosure. [Diagram 3] 3 is a schematic enlarged top view of a protruding portion 4a within a dotted frame P of the decorative sheet shown in FIG. 2. FIG. [Figure 4] 1 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. [Diagram 5] 1 is a schematic cross-sectional view illustrating a decorative member according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following describes the embodiments with reference to the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the description of the embodiments exemplified below. In addition, in order to clarify the description, the drawings may show the width, thickness, and shape of each part in a schematic manner compared to the actual form, but this is merely an example and should not be interpreted as being limiting.
[0012] In this specification, when describing a mode in which another component is disposed on a certain component, the term "above" or "below" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified. In addition, in this specification, when describing a mode in which another component is disposed on the surface of a certain component, the term "on the surface" includes both cases in which another component is disposed directly above or below the certain component so as to be in contact with the component, and cases in which another component is disposed above or below the certain component with another component interposed therebetween, unless otherwise specified.
[0013] As described above, by including beads having a large particle size in the raised portion, a strong tactile feel can be obtained, but the raised portion has a high gloss, making it difficult to reproduce the appearance of a natural material such as natural wood.
[0014] A. Decorative sheet The decorative sheet according to the present disclosure will be described in detail below. Fig. 1 is a schematic cross-sectional view illustrating a decorative sheet according to the present disclosure. The decorative sheet 10 shown in Fig. 1 is made up of a base layer 1, a design layer 2, a protective layer 3, and a raised layer 4 having a patterned raised portion 4a, which are arranged in a thickness direction D. T In the present disclosure, the 60° gloss value of the protective layer 3 is smaller than the 60° gloss value of the protruding layer 4, and the 60° gloss value of the protruding layer 4 is 20 or less, and T In this case, the ratio of the area of the protruding layer 4 to the area of the protective layer 3 is 10% or more, and the average distance between adjacent protruding portions 4a is 1.6 mm or more.
[0015] According to the present disclosure, a strong uneven feel can be obtained by having the average spacing between adjacent raised portions 4a be equal to or greater than a predetermined value and by having the ratio of the area of raised layer 4 to the area of protective layer 3 be equal to or greater than a predetermined value. Furthermore, by having the 60° gloss value of protective layer 3 be smaller than the 60° gloss value of raised layer 4 and having the 60° gloss value of raised layer 4 be equal to or less than a predetermined value, it is possible to reduce the glossiness of the raised layer while maintaining a matte gloss feel, and a natural, authentic design can be achieved with a reduced layer configuration.
[0016] 1.Morijo layer 1, the protruding layer 4 in the present disclosure is disposed on the surface of the protective layer 3 opposite the design layer 2, and has a patterned protruding portion 4a. The protruding layer 4 is formed from a large number of protruding portions 4a provided on the protective layer 3, thereby enhancing the design of the decorative sheet.
[0017] (1) 60° gloss The 60° gloss value of the protruding layer is greater than the 60° gloss value of the protective layer and is not greater than 20. The 60° gloss value of the protruding layer is preferably not greater than 15, and more preferably not greater than 10. When the 60° gloss value is within the above range, the glossiness of the protruding layer can be reduced, and a design that is natural and feels real can be obtained. On the other hand, the 60° gloss value may be, for example, not less than 4, and may be not less than 6. When the 60° gloss value is within the above range, it is possible to prevent the protruding layer from becoming too low in gloss, and it is possible to maintain an excellent gloss matte feel between the protruding layer and the protective layer.
[0018] In the present disclosure, the 60° gloss value of the protruding layer is a value measured by the following method. The decorative sheet is placed with the raised layer side facing up, and the 60° specular gloss of the raised layer is measured from the raised layer side using a gloss meter in accordance with method 3 of JIS Z 8741:1997. The 60° gloss value of the raised layer is the average value of the measurements at any 10 points on the raised part. At each measurement point, the raised part is at the center of the measurement part of the gloss meter, and the measurement is performed so that 50% or more of the area of the measurement part overlaps with the raised part. The center of the measurement part of the gloss meter refers to the center of the incident area where light from the light source of the gloss meter enters.
[0019] The 60° gloss value of the raised layer can be adjusted by the type, average particle size, content, etc. of the filler described below. For example, the gloss value tends to decrease when inorganic particles are used as the filler. The gloss value tends to decrease when the average particle size of the inorganic particles is increased. The gloss value tends to decrease when the content of the inorganic particles is increased. Although organic particles have a weaker matting effect than inorganic particles, the gloss value tends to decrease when the content of the organic particles is increased. In addition, organic particles generally have a larger average particle size than inorganic particles, but the 60° gloss value tends to decrease when the average particle size is reduced.
[0020] (2) Mound part The raised layer has a patterned raised portion 4a. The raised portion 4a is preferably arranged to harmonize with the design of the design layer 2. "Harmony" means that the shapes and positions of the two target patterns generally match. Specifically, it means that the shapes and positions of the raised portion 4a and at least a part of the pattern constituting the design of the design layer 2 match to an extent that does not impair realism and a sense of luxury.
[0021] In FIG. 1, the design layer 2 has a pattern layer 2y, and the raised portion 4a is in harmony with the pattern layer 2y. By arranging the raised portion 4a so as to be in harmony with the pattern of the design layer, the design of the decorative sheet can be improved by the synergistic effect of the raised portion 4a and the pattern of the design layer. For example, in the case of a wood grain pattern, the texture is improved by harmonizing the pattern of the raised portion 4a with a dark pattern such as a vessel. For example, when the decorative sheet is viewed in a plane, when the total area of the pattern layer is 100, the area of the raised portion 4a in harmony with the pattern layer is preferably 90 or more, more preferably 95 or more, even more preferably 97 or more, and even more preferably 99 or more. On the other hand, the raised portion 4a does not have to be arranged in harmony with the pattern of the design layer.
[0022] In the present disclosure, the average distance between adjacent raised portions 4a is usually 1.6 mm or more, preferably 2.0 mm or more, and more preferably 2.3 mm or more. If the average distance between adjacent raised portions 4a is smaller than the above range, a strong tactile sensation cannot be obtained. On the other hand, the average distance between adjacent raised portions 4a may be, for example, 4.0 mm or less, and may be 3.0 mm or less.
[0023] In the present disclosure, the average spacing between adjacent raised portions 4a refers to the average spacing W4 between the upper ends of adjacent raised portions 4a measured at 100 points on a cross-sectional image of the decorative sheet, excluding the minimum to 10th smallest value and the maximum to 10th largest value, and excluding the minimum to 10th largest value. For example, in Fig. 1 and Fig. 2, the average spacing between adjacent raised portions 4a corresponds to the average spacing between adjacent raised portions 4a in a direction D2 perpendicular to the longitudinal direction D1 of the raised portions 4a. In particular, when the pattern of the decorative layer is a wood grain pattern, the direction in which the conduits of the wood grain extend coincides with the longitudinal direction of the raised portions 4a. In addition, when the pattern of the decorative layer is a stone grain pattern, for example, and the raised portions 4a do not have a specific longitudinal direction, the average spacing corresponds to the average spacing between adjacent raised portions 4a in any multiple directions not limited to a specific direction.
[0024] The cross-sectional shape of the mound in the direction D2 is not particularly limited, and examples thereof include a substantially rectangular shape, a substantially polygonal shape, a substantially circular shape, etc. In Fig. 4, the cross-sectional shape of the mound 4a is a substantially rectangular shape (trapezoidal shape).
[0025] FIG. 3 is a schematic top view of the raised portion 4a in the dotted frame P of the decorative sheet shown in FIG. 2 in an enlarged manner. As shown in FIG. 3, one raised portion 4a may include an irregular uneven surface 45. Examples of such uneven surfaces include the uneven surface of the raised portion described in JP 2022-55319 A. Specifically, the uneven surface 45 includes a convex portion 46 and a concave portion 47. The convex portion 46 and the concave portion 47 forming the irregular uneven surface 45 may have irregularity in arrangement. The convex portion 46 and the concave portion 47 may have irregularity in shape. As shown in FIG. 3, the uneven surface 45 of the raised portion 4a may be a wood surface. As shown in FIG. 3, at least one of the convex portion 46 and the concave portion 47 may be a linear portion 49 in which at least one of the orientation and the length is not constant. Both the convex portion 46 and the concave portion 47 may be linear portions 49 in which at least one of the orientation and the length is not constant.
[0026] This raised portion 4a can provide a tactile sensation in its internal region due to the step between the convex portions 46 and the concave portions 47. In other words, the raised layer 4 can provide a tactile sensation not only at the edges of the raised portion 4a, but also inside the raised portion 4a. Therefore, the unevenness of the surface of the decorative sheet 10 can be emphasized with a stronger tactile sensation.
[0027] In addition, by eliminating the regularity of the uneven surface 45, it is possible to suppress the artificial impression when observing the uneven surface 45. Therefore, the raised portion 4a can express a natural texture, and in combination with the design layer, the design can be improved synergistically.
[0028] The size of the linear portion 49 in the direction in which it extends is defined as the total length of the linear portion 49. The size of the linear portion 49 in the direction perpendicular to the direction in which it extends is defined as the width of the linear portion 49. T The size in the direction (depth direction of the paper surface) is defined as the depth of the linear portion 49.
[0029] In the decorative sheet 10 shown in FIG. 3, the protrusions 46 include protrusions D that are surrounded by recesses 47 on all sides in a plan view. The protrusions D may be irregularly arranged inside the mounded portion 4a in a plan view. The shape of a protrusion D included in one mounded portion 4a in a plan view need not be a typical geometric shape such as a triangle, rectangle, circle, or ellipse, and may be an irregular shape. The area of the protrusions D in a plan view may vary irregularly among the multiple protrusions D. That is, the areas of the multiple protrusions D in a plan view may differ from one another.
[0030] The dimensions of the projections D in a plan view can be set in consideration of realizing a tactile feel and a natural texture. The maximum dimension of the projections D along the D2 direction is preferably 30 μm or more and 500 μm or less, more preferably 100 μm or more and 300 μm or less. The maximum dimension of the projections D along the D1 direction is preferably 40 μm or more and 20,000 μm or less, more preferably 400 μm or more and 8,000 μm or less.
[0031] As shown in FIG. 3, the decorative sheet 10 may include protrusions 46 that are not partially surrounded by recesses 47, in addition to protrusions D that are entirely surrounded by recesses 47 in a plan view.
[0032] The length of the linear portions 49 is not particularly limited. Both ends of at least some of the linear portions 49 may be located on the edge of the mounded portion 4a. At least some of the linear portions 49 may include one end or both ends located inside the mounded portion 4a. That is, only one end of the linear portion 49 may be located on the edge of the mounded portion 4a. Both ends of the linear portion 49 may be located inside the mounded portion 4a. The end positions of these linear portions 49 may differ between the linear portions 49 included in one mounded portion 4a.
[0033] The width W49 of the linear portion 49 (see FIG. 3) is not particularly limited. The width W49 of the linear portion 49 may be 50 μm or more and 250 μm or less. The width W49 may be different between the multiple linear portions 49. The height difference of the linear portion 49, i.e., the height difference between the recessed portion 47 and the protruding portion 46, is D TThe height difference is the difference between the smallest (lowest) part of the recess 47 and the largest (highest) part of the protrusion 46 in the vertical direction (depth direction of the paper). The height difference is not particularly limited, but may be 10 μm or more and 200 μm or less. The height differences caused by the multiple linear portions 49 may be the same or different from each other. The height difference caused by one linear portion 49 may be constant or may vary along the longitudinal direction of the linear portion 49.
[0034] There is no particular limitation on the cross-sectional shape of the linear portion 49 in a cross section perpendicular to the longitudinal direction. The cross-sectional shape of the linear portion 49 in a cross section perpendicular to the longitudinal direction may be any shape, such as a semicircle, a semi-ellipse, a triangle, a rectangle, a pentagon, a hexagon, or any other polygon, or an irregular geometric shape.
[0035] (3)Area In the decorative sheet of the present disclosure, the ratio of the area of the protruding layer to the area of the protective layer in the thickness direction is usually 10% or more, preferably 20% or more, more preferably 30% or more, and particularly preferably 40% or more. In the present disclosure, the average distance between adjacent protruding portions 4a is a predetermined value or more, and the ratio of the area of the protruding layer 4 to the area of the protective layer 3 is a predetermined value or more, thereby obtaining a strong uneven feel. Furthermore, by having the ratio of the area of the protruding layer to the area of the protective layer within the above range, the abrasion resistance, scratch resistance, and stain resistance are improved. Meanwhile, the ratio of the area of the protruding layer is, for example, 55% or less, and preferably 50% or less.
[0036] The ratio of the area of the protruding layer to the area of the protective layer in the thickness direction is the ratio of the area of the protruding region in the measurement area where the protruding layer is provided to the area of the region in the measurement area where the protective layer is provided, viewed in the thickness direction, and is the average value calculated at 100 locations within a measurement area of 10 mm x 10 mm.
[0037] (4) Thickness The average thickness T4 of the protruding layer in the present disclosure is, for example, 2.0 times or more, may be 2.5 times or more, or may be 3.0 times or more, relative to the average thickness T3 of the protective layer. When the average thickness of the protruding layer is within the above range, the abrasion resistance, scratch resistance, and contamination resistance are improved. The specific average thickness of the protruding layer is, for example, 10 μm or more, may be 15 μm or more, or may be 20 μm or more. On the other hand, the average thickness of the protruding layer is, for example, 50 μm or less, may be 40 μm or less, or may be 30 μm or less.
[0038] The average thickness of the raised layer is determined by measuring the thickness T4 of the raised portion 4a at 100 points on an image of the cross section of the decorative sheet taken with a scanning electron microscope (SEM), and excluding the minimum 10 points and the maximum 10 points, for a total of 80 points. If the raised portion has an uneven surface, the thickness is measured at the convex parts. The same applies to the average thickness of the protective layer.
[0039] (5) Composition (i) Filler The raised portion preferably contains a filler. That is, the raised layer preferably contains a filler. Examples of the filler include organic particles and inorganic particles. Examples of the organic particles include beads made of resins such as acrylic resins, urethane resins, silicone resins, and polyamide resins such as nylon. Examples of the inorganic particles include beads made of inorganic materials such as silica, alumina, zirconia, titania (titanium dioxide), kaolinite, calcium carbonate, and barium sulfate. The above-mentioned particles may be used alone or in combination of two or more kinds.
[0040] The average particle size of inorganic particles is not particularly limited. The average particle size of inorganic particles is, for example, 2 μm or more, may be 3 μm or more, or may be 5 μm or more. On the other hand, the average particle size of inorganic particles is, for example, 12 μm or less, may be 10 μm or less. In this specification, the average particle size is D50 according to the volume-based particle size distribution measured by a laser diffraction scattering method.
[0041] The content of the inorganic particles in the mound portion may be 2 parts by mass or more, preferably 5 parts by mass or more, may be 15 parts by mass or more, or may be 18 parts by mass or more, relative to 100 parts by mass of the resin component in the mound portion. On the other hand, the content of the inorganic particles in the mound portion may be, for example, 38 parts by mass or less, 28 parts by mass or less, or may be 25 parts by mass or less.
[0042] The average particle size of the organic particles is not particularly limited. The average particle size of the organic particles is, for example, 20 μm or more, and may be 30 μm or more. On the other hand, the average particle size of the organic particles is, for example, 60 μm or less, and may be 50 μm or less.
[0043] The content of the organic particles in the protruding portion is preferably 7 parts by mass or more, and may be 10 parts by mass or more, relative to 100 parts by mass of the resin component of the protruding portion. On the other hand, the content of the organic particles in the protruding layer may be, for example, 38 parts by mass or less, 33 parts by mass or less, or 25 parts by mass or less.
[0044] When the protuberance contains both organic and inorganic particles as fillers, the content of the organic particles relative to the content of the fillers in the protuberance is, for example, 20% by mass or more, or may be 30% by mass or more, or may be 40% by mass or more, while the content of the organic particles is, for example, 80% by mass or less, or may be 70% by mass or less, or may be 60% by mass or less.
[0045] When the protuberance contains both organic and inorganic particles as fillers, the content of the inorganic particles relative to the content of the fillers in the protuberance is, for example, 20% by mass or more, or may be 30% by mass or more, or may be 40% by mass or more, while the content of the inorganic particles is, for example, 80% by mass or less, or may be 70% by mass or less, or may be 60% by mass or less.
[0046] (ii) Resin component The material constituting the protruding portion contains a resin component. The resin component is typically a cured product (crosslinked structure) of a curable resin X. Alternatively, the resin component may be a thermoplastic resin. In particular, the protruding portion preferably contains a cured product of a curable resin X. The curable resin X may be, for example, at least one selected from a two-component curing resin, a thermosetting resin, and an ionizing radiation curing resin.
[0047] Examples of two-component curing resins include two-component curing urethane resins that use a polyol compound as a base compound and an isocyanate compound as a curing agent, two-component curing epoxy resins, two-component curing urethane-modified acrylic resins, and two-component curing polyester resins.
[0048] Examples of the thermosetting resin include acrylic resins, urethane resins, phenolic resins, melamine resins, epoxy resins, unsaturated polyester resins, and silicone resins.
[0049] The ionizing radiation curable resin is a composition containing a compound having an ionizing radiation curable functional group. Examples of the ionizing radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl group, vinyl group, and allyl group, as well as epoxy group and oxetanyl group. The ionizing radiation curable resin may be a compound having an ethylenically unsaturated bond group. The ionizing radiation curable resin may be a compound having two or more ethylenically unsaturated bond groups, and preferably may be a polyfunctional (meth)acrylate compound having two or more ethylenically unsaturated bond groups. The polyfunctional (meth)acrylate compound may be a monomer or oligomer. The ionizing radiation means an electromagnetic wave or a charged particle beam that has an energy quantum capable of polymerizing or crosslinking molecules. Examples of the ionizing radiation include ultraviolet rays (UV) and electron beams (EB). The ionizing radiation may be an electromagnetic wave such as X-rays and gamma rays, or a charged particle beam such as alpha rays and ion beams.
[0050] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxy diacrylate, bisphenol A tetrapropoxy diacrylate, and 1,6-hexanediol diacrylate. Examples of trifunctional or higher (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and isocyanuric acid-modified tri(meth)acrylate. The above (meth)acrylate monomers may have a part of the molecular skeleton modified. The above (meth)acrylate monomers may be modified with ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, alkyl, cyclic alkyl, aromatic, bisphenol, or the like.
[0051] Examples of the polyfunctional (meth)acrylate oligomer include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, and polyether (meth)acrylate. The urethane (meth)acrylate can be obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate. The epoxy (meth)acrylate may be a (meth)acrylate obtained by reacting a trifunctional or higher aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like with (meth)acrylic acid, a (meth)acrylate obtained by reacting a bifunctional or higher aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like with a polybasic acid and (meth)acrylic acid, or a (meth)acrylate obtained by reacting a bifunctional or higher aromatic epoxy resin, alicyclic epoxy resin, aliphatic epoxy resin, or the like with a phenol and (meth)acrylic acid. The ionizing radiation curable resins may be used alone or in combination of two or more.
[0052] When the ionizing radiation curable resin is an ultraviolet curable resin, the composition may contain additives such as a photopolymerization initiator and a photopolymerization accelerator. In the case of a compound having an ethylenically unsaturated group, the photopolymerization initiator may be one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl dimethyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc. The photopolymerization accelerator can reduce polymerization inhibition caused by air during curing and increase the curing speed. The photopolymerization accelerator may be one or more selected from p-dimethylaminobenzoic acid isoamyl ester, p-dimethylaminobenzoic acid ethyl ester, etc.
[0053] Examples of thermoplastic resins include acrylic resins, cellulose resins, urethane resins, vinyl chloride resins, polyester resins, polyolefin resins, polycarbonate, nylon, polystyrene, and ABS resins.
[0054] The protruding layer may be transparent or colored. The material used for the protruding layer may be colored by adding a colorant (pigment or dye) to the composition. The colorant may be a known or commercially available pigment or dye. One type of colorant may be used alone, or two or more types may be used in combination. The amount of colorant added may be appropriately set depending on the desired color tone, etc.
[0055] The protruding layer may contain various additives such as a foaming agent, a flame retardant, a lubricant, an antistatic agent, an antioxidant, an ultraviolet absorbing agent, a light stabilizer, a radical scavenger, and a soft component (for example, rubber).
[0056] As a method for forming the raised layer, for example, a raised layer forming ink containing a curable resin X is applied to the surface of the protective layer opposite the design layer by gravure printing using a plate or a lattice, and then cured as necessary to form the raised portion. When the raised portion has the above-mentioned uneven surface, for example, the plate described in JP-A-2022-55319 can be used.
[0057] When the ink for forming the protruding layer contains an electron beam curable resin as the curable resin X, the cured product of the electron beam curable resin is usually obtained by irradiating it with an electron beam. Examples of the electron beam source include various electron beam accelerators such as Cockcroft-Walt type, Van de Graff type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type. The energy of the electron beam is, for example, 100 kV or more and 1000 kV or less, or may be 100 kV or more and 300 kV or less. The irradiation dose of the electron beam is, for example, 2 Mrad or more and 15 Mrad or less.
[0058] When the ink for forming the protruding layer contains an ultraviolet-curable resin as the curable resin X, the ultraviolet-curable resin is usually cured by irradiating it with ultraviolet light. Examples of ultraviolet light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps. The wavelength of the ultraviolet light is, for example, 190 nm or more and 380 nm or less.
[0059] When the ink for forming the protruding layer contains a thermosetting resin as the curable resin X, the ink is usually heated to obtain a cured product of the thermosetting resin. The heating temperature is appropriately set according to the type of the thermosetting resin. The ink for forming the protruding layer may contain a curing agent such as a crosslinking agent and a polymerization initiator, and a polymerization accelerator, in addition to the thermosetting resin. Examples of the curing agent include isocyanates, organic sulfonates, organic amines, peroxides (e.g., methyl ethyl ketone peroxide), and radical initiators (azoisobutylnitrile).
[0060] The ink for forming the protruding layer may contain a solvent as necessary. Examples of the solvent include water, hydrocarbon compounds such as toluene and xylene, alcohol compounds such as methanol, ethanol and methyl glycol, ketone compounds such as acetone and methyl ethyl ketone, ester compounds such as methyl formate, ethyl acetate and butyl acetate, nitrogen-containing compounds such as N-methylpyrrolidone and N,N-dimethylformamide, ether compounds such as tetrahydrofuran and dioxane, halogenated hydrocarbon compounds such as methylene chloride and chloroform, and dimethyl sulfoxide.
[0061] 2.Protective layer As shown in Fig. 1, the protective layer 3 in the present disclosure is disposed between the design layer 2 and the protruding layer 4. The protective layer in the present disclosure may be disposed partially or entirely on the base layer described below. In particular, it is preferable that the protective layer is disposed entirely on the base layer. Also, as shown in Fig. 1, it is preferable that the protective layer 3 is in direct contact with the protruding layer 4. The decorative sheet of the present disclosure can obtain a natural and authentic design with a small layer structure.
[0062] The 60° gloss value of the protective layer in the present disclosure is not particularly limited as long as it is smaller than the 60° gloss value of the protruding layer, but is, for example, equal to or less than 3, and may be equal to or less than 2. On the other hand, the 60° gloss value of the protective layer is, for example, equal to or greater than 1.
[0063] The protective layer is not particularly limited as long as it protects the design layer and has a predetermined 60° gloss value. The material constituting the protective layer contains, for example, a resin component. Examples of the resin component include the same types as those exemplified for the above-mentioned raised layer.
[0064] The protective layer contains, for example, a matting agent. For example, the same type of the inorganic particles as exemplified in the above-mentioned protruding layer can be used as the matting agent. The average particle size of the inorganic particles used in the protective layer is, for example, 1 μm or more, may be 3 μm or more, or may be 5 μm or more. On the other hand, the average particle size of the inorganic particles used in the protective layer is, for example, 20 μm or less, and may be 15 μm or less.
[0065] The content of the inorganic particles in the protective layer is preferably 10 parts by mass or more, and may be 20 parts by mass or more, relative to 100 parts by mass of the resin component of the protective layer, while the content of the inorganic particles in the protective layer may be, for example, 40 parts by mass or less, or may be 30 parts by mass or less.
[0066] The average thickness of the protective layer is not particularly limited, but is, for example, 1 μm or more, and preferably 5 μm or more. When the average thickness of the protective layer is in the above range, the abrasion resistance, scratch resistance, and cellophane tape resistance are improved. On the other hand, the average thickness of the protective layer is, for example, 50 μm or less, may be 30 μm or less, or may be 20 μm or less. When the thickness of the protective layer is in the above range, for example, when the protective layer contains silica, the increase in the cloudiness caused by silica can be suppressed, and the visibility of the design layer is improved. Furthermore, the protective layer does not become too hard, and surface cracks when folded can be suppressed.
[0067] 3. Design layer The decorative layer in the present disclosure is disposed between the base layer and the protective layer. The decorative layer preferably has a pattern.
[0068] Examples of patterns of the design layer include organic patterns, inorganic patterns, and abstract patterns. Organic patterns are patterns derived from the life activities of living organisms such as animals and plants. Inorganic patterns are patterns that do not fall under the category of organic patterns. Abstract patterns are patterns that interpret objects (e.g., images that exist in nature) abstractly and do not express a clear shape. Examples of organic patterns include wood grain patterns, leather patterns, floral patterns, and botanical patterns. Examples of inorganic patterns include stone patterns, concrete patterns, sand patterns, cloth patterns, metal patterns, tile patterns, and brick masonry patterns. Examples of abstract patterns include flickering patterns (e.g., ink flickering patterns), smoke patterns, and marble patterns.
[0069] The design layer has, for example, a pattern layer. The design layer may have a solid layer on the substrate layer side of the pattern layer. In the present disclosure, the pattern layer means a layer formed partially (particularly in a pattern) on one side of the substrate layer. The solid layer means a layer formed on the entire surface of one side of the substrate layer.
[0070] The design layer contains, for example, a colorant and a resin component. Examples of the colorant include inorganic pigments such as carbon black, titanium white, zinc oxide, red iron oxide, Prussian blue, and cadmium red; organic pigments such as azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; and luminous pigments. Dyes may also be used as the colorant.
[0071] Examples of the resin component include (meth)acrylic resins, ester urethane resins, acrylamide resins, ethylene oxide resins, N-vinylpyrrolidone resins, ester resins, amide resins, vinyl acetate resins, vinyl chloride resins, urethane (meth)acrylic resins, natural rubber, synthetic rubber, cellulose derivatives, etc. Among these, (meth)acrylic resins and urethane (meth)acrylic resins are preferred.
[0072] The design layer may contain additives such as fillers (e.g., silica), extender pigments (e.g., organic beads), neutralizers, surfactants, etc., as necessary. The thickness of the design layer is not particularly limited, but is, for example, 0.1 μm or more and 20 μm or less.
[0073] The method for forming the design layer includes, for example, a coating method using an ink for forming the design layer containing a colorant, a binder resin, and a solvent (or a dispersion medium). For example, the ink for forming the design layer is applied to one side of the base layer and dried to obtain the design layer.
[0074] Examples of the solvent (or dispersion medium) include petroleum-based organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ester-based organic solvents such as ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and 2-ethoxyethyl acetate; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and propylene glycol; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based organic solvents such as diethyl ether, dioxane, and tetrahydrofuran; chlorine-based organic solvents such as dichloromethane, carbon tetrachloride, trichloroethylene, and tetrachloroethylene; and inorganic solvents such as water.
[0075] Examples of the coating method include printing. Examples of the printing method include gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, and inkjet printing. Examples of the coating method for forming a solid layer include various coating methods such as roll coating, knife coating, air knife coating, die coating, lip coating, comma coating, kiss coating, flow coating, and dip coating.
[0076] 4.Base material layer The decorative sheet in the present disclosure has a base layer. The base layer is a member that supports the design layer, the protective layer, and the raised layer. By having the base layer, the decorative sheet has various performances such as mechanical strength, post-processing suitability, and design, and therefore the usability as a sheet is improved.
[0077] The substrate layer is not particularly limited, and examples thereof include a resin substrate, a glass substrate, a metal substrate, and a fiber substrate. The type of substrate layer is appropriately selected depending on the application of the decorative sheet.
[0078] Examples of the resin used in the resin substrate include various synthetic resins and various natural resins. Examples of the synthetic resin include thermoplastic resins and curable resins. Considering the manufacturing suitability, handling suitability, and post-processing suitability of the decorative sheet, thermoplastic resins are preferred.
[0079] Examples of thermoplastic resins include olefin resins such as polyethylene, polypropylene, polymethylpentene, ionomers, and various olefin-based thermoplastic elastomers; vinyl chloride resins such as polyvinyl chloride, polyvinylidene chloride, and vinyl chloride-vinyl acetate copolymers; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, ethylene glycol-terephthalic acid-isophthalic acid copolymers, and polyester-based thermoplastic elastomers; acrylic resins such as polymethyl (meth)acrylate, polyethyl (meth)acrylate, polybutyl (meth)acrylate, and methyl (meth)acrylate-butyl (meth)acrylate copolymers; polyamide resins such as nylon 6 and nylon 66; cellulose resins such as cellulose triacetate, cellophane, and celluloid; styrene resins such as polystyrene, acrylonitrile-styrene copolymers, and acrylonitrile-butadiene-styrene copolymers (ABS resins); polyvinyl alcohol, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, polycarbonate resins, polyarylate resins, and polyimide resins.
[0080] Examples of the curable resin include ionizing radiation curable resins and thermosetting resins.
[0081] Natural resins include, for example, natural rubber, rosin, and amber.
[0082] Examples of metals used for the metal substrate include aluminum or aluminum alloys such as duralumin, iron or iron alloys such as carbon steel and stainless steel, copper or copper alloys such as brass and bronze, gold, silver, chromium, nickel, cobalt, tin, and titanium. The metal substrate may have a plating film or an anodized film on the surface.
[0083] Examples of fibrous materials used in the fiber substrate include paper such as tissue paper, craft paper, fine paper, Japanese paper, titanium paper, linter paper, parchment paper, glassine paper, backing paper for wallpaper, paperboard, and base paper for gypsum board; woven or nonwoven fabrics made of fibers such as polyester resin fiber, acrylic resin fiber, protein or cellulose-based natural fibers such as silk, cotton, and hemp, glass fiber, and carbon fiber. Various resins such as acrylic resin, styrene-butadiene rubber, melamine resin, and urethane resin may be added to the fiber substrate. When the fiber substrate is a paper substrate, the strength between the fibers of the paper substrate or the interlayer strength between the paper substrate and other substrates can be improved. In addition, fluffing can be suppressed. The resin may be added by impregnating the paper substrate after papermaking, or by filling the resin during papermaking. Examples of paper substrates to which resin has been added include inter-paper reinforced paper and resin-impregnated paper.
[0084] The substrate layer may contain additives as necessary. In the case of a resin substrate, examples of additives include inorganic fillers, flame retardants, lubricants, foaming agents, antioxidants, ultraviolet absorbers, light stabilizers, and colorants. Various additives can be used alone or in combination. The content of the additives is not particularly limited as long as it does not impair the surface properties and processing properties, and can be appropriately set according to the required properties.
[0085] The substrate layer may be a single layer or a laminate of two or more layers. In the case of a laminate, the substrate layer may have two or more layers of the same type of substrate, or may have two or more layers of different types of substrate.
[0086] The substrate layer may be transparent or opaque.
[0087] The substrate layer may be colored. The coloring mode is not particularly limited, and may be transparent or opaque (hiding), which can be selected arbitrarily.
[0088] When the base layer is colored, it may contain a colorant. Examples of colorants include inorganic pigments such as white pigments such as titanium white, iron black, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, phthalocyanine blue, nickel-azo complex, azomethine azo-based black pigment, and perylene-based black pigment; metal pigments made of scaly foil such as aluminum and brass; and pearlescent (pearl) pigments made of scaly foil such as titanium dioxide-coated mica and basic lead carbonate. For example, when the surface hue of the adherend on which the decorative sheet is laminated varies, in order to conceal the surface hue and improve the stability of the color tone of the decorative layer, an inorganic pigment such as a white pigment may be used.
[0089] The substrate layer may be surface-treated to enhance adhesion with layers in contact with the substrate layer, such as adhesion with a decorative layer and adhesion with an adhesive layer. Examples of the surface treatment include physical surface treatments such as oxidation and roughening, and chemical surface treatments. Examples of the oxidation method include corona discharge treatment, chromium oxidation treatment, flame treatment, hot air treatment, and ozone-ultraviolet treatment. Examples of the roughening method include sandblasting and solvent treatment. These surface treatments are appropriately selected depending on the type of substrate layer, but in consideration of the effect and operability of the surface treatment, corona discharge treatment is generally preferred.
[0090] When the substrate layer is a laminate, an adhesive layer or a primer layer may be disposed between adjacent layers in order to improve the adhesion between the layers.
[0091] The thickness of the base layer is not particularly limited and is appropriately selected depending on the material of the base layer. In the case of a base layer containing a resin, the thickness of the base layer is, for example, 10 μm to 300 μm, may be 20 μm to 200 μm, or may be 40 μm to 100 μm. In addition, in the case where the base layer is a paper base, the basis weight is, for example, 20 g / m 2 More than 150g / m 2 Less than or equal to 30 g / m 2 More than 100g / m 2 It may be the following.
[0092] 5. Other layers As shown in Fig. 1, the decorative sheet of the present disclosure has at least a base layer 1, a design layer 2, a protective layer 3, and a raised layer 4. Meanwhile, the decorative sheet of the present disclosure may have other layers in addition to these layers. Examples of the other layers include a transparent resin layer, an adhesive layer, a separator layer, and a primer layer.
[0093] (1)Transparent resin layer The decorative sheet in the present disclosure may have a transparent resin layer between the protective layer and the design layer. The transparent resin layer can increase the strength of the decorative sheet.
[0094] The transparent resin layer may be transparent enough to allow the design layer to be visually recognized, and may be colorless and transparent, colored and transparent, or translucent.
[0095] Examples of resins constituting the transparent resin layer include polyolefin resins, polyester resins, polycarbonate resins, acrylonitrile-butadiene-styrene resins (hereinafter also referred to as "ABS resins"), acrylic resins, and vinyl chloride resins. In consideration of processability, polyolefin resins and vinyl chloride resins are preferred. The resins may be used alone or in combination.
[0096] The transparent resin layer contains additives as necessary. Examples of the additives include weather resistance agents such as ultraviolet absorbers and light stabilizers. The weather resistance agent may be appropriately selected from those described above.
[0097] Taking into consideration processability, the thickness of the transparent resin layer is, for example, 20 μm or more and 150 μm or less, or may be 40 μm or more and 120 μm or less, or may be 60 μm or more and 100 μm or less.
[0098] Examples of methods for forming the transparent resin layer include a method of applying a resin composition and a method of laminating a resin film by dry lamination.
[0099] (2) Back adhesive layer The decorative sheet of the present disclosure may have a back adhesive layer on the side of the base layer opposite the design layer. The back adhesive layer is, for example, a member for attaching the decorative sheet to an adherend.
[0100] The back adhesive layer may be transparent or opaque.
[0101] The adhesive used for the back surface adhesive layer may be, for example, a curing adhesive or a pressure-sensitive adhesive. Specific examples include a urethane adhesive, an acrylic adhesive, an epoxy adhesive, and a rubber adhesive. In addition, OCA (Optically Clear Adhesive) or OCR (Optically Clear Resin) may also be used for the back surface adhesive layer.
[0102] From the viewpoint of efficiently obtaining a desired adhesive strength, the thickness of the back surface adhesive layer is, for example, 5 μm or more and 100 μm or less, optionally 10 μm or more and 75 μm or less, or optionally 20 μm or more and 50 μm or less.
[0103] Examples of methods for forming the back surface adhesive layer include a method of applying an adhesive composition and a method of laminating an adhesive film by dry lamination.
[0104] (3) Primer layer The decorative sheet of the present disclosure may have a primer layer in order to improve the interlayer adhesion of the multiple layers that make up the decorative sheet. The primer layer may be disposed between any of the layers.
[0105] The primer layer is mainly composed of a binder resin, and may contain additives such as an ultraviolet absorber and a light stabilizer, if necessary.
[0106] Examples of binder resins include urethane resin, acrylic polyol resin, acrylic resin, ester resin, amide resin, butyral resin, styrene resin, urethane-acrylic copolymer, polycarbonate-based urethane-acrylic copolymer (urethane-acrylic copolymer derived from a polymer (polycarbonate polyol) having a carbonate bond in the polymer main chain and having two or more hydroxyl groups at the end and side chain), vinyl chloride-vinyl acetate copolymer resin, vinyl chloride-vinyl acetate-acrylic copolymer resin, chlorinated propylene resin, nitrocellulose resin (nitrocellulose), and cellulose acetate resin. These can be used alone or in combination of multiple types.
[0107] The binder resin may be a resin obtained by adding a curing agent such as an isocyanate-based curing agent or an epoxy-based curing agent to the above-mentioned resin to crosslink and harden it. For example, a resin obtained by crosslinking and hardening a polyol-based resin such as an acrylic polyol resin with an isocyanate-based curing agent is preferred, and a resin obtained by crosslinking and hardening an acrylic polyol resin with an isocyanate-based curing agent is more preferred.
[0108] The thickness of the primer layer is, for example, 0.5 μm or more, may be 1 μm or more, or may be 2 μm or more, and the thickness of the primer layer is, for example, 10 μm or less, may be 8 μm or less, or may be 6 μm or less.
[0109] The primer layer can be formed by applying a resin composition, and then drying and curing the composition as necessary.
[0110] (4) Separator layer The decorative sheet of the present disclosure may have a separator layer on the side of the back adhesive layer opposite the base layer. The separator layer is a member that protects the back adhesive layer, and is peeled off when the decorative sheet is attached to an adherend. As the separator layer, a conventionally known one can be used.
[0111] B. Decorative materials The decorative member in the present disclosure has a base and the above-mentioned decorative sheet. Fig. 5 is a schematic cross-sectional view illustrating a decorative member in the present disclosure. The decorative member 100 shown in Fig. 5 has a base 50, an adhesive layer 40, and the above-mentioned decorative sheet 10, in this order. As shown in Fig. 5, the protruding layer 4 of the decorative sheet 10 constitutes the outermost layer of the decorative member 100. The decorative sheet 10 is arranged so that the surface on the base layer 1 side faces the base 50 side.
[0112] According to the present disclosure, since it has the decorative sheet described above, it is a decorative component that has a strong feel and a sense of realism.
[0113] 1. Decorative sheet The decorative sheet in this disclosure is similar to that described above in "A. Decorative sheet," and so a description thereof will be omitted here.
[0114] 2.Base The substrate in the present disclosure is a member that is decorated with a decorative sheet. An example of the substrate is a resin member. Examples of resins used in the resin member include vinyl chloride resins, acrylic resins, ester resins, styrene resins, olefin resins, acrylonitrile-butadiene-styrene copolymers (ABS resins), phenolic resins, cellulose resins, and rubber. Another example of the substrate is a wood member. Examples of the wood member include wood veneer, wood plywood, particle board, and wood fiberboard. Examples of wood used in the wood member include cedar, cypress, pine, and lauan.
[0115] Another example of the substrate is a metal member. Examples of metals used for the metal member include iron, iron alloys (e.g., carbon steel and stainless steel), and aluminum. Another example of the substrate is a ceramic member. The material of the ceramic member may be ceramics such as glass or porcelain, a non-cement ceramic material such as gypsum, or a non-ceramic ceramic material such as ALC (aerated lightweight concrete).
[0116] The shape of the substrate is not particularly limited, and may be, for example, a plate, a sheet, or a three-dimensional shape. The substrate may have a flat surface, a curved surface, or both a flat surface and a curved surface. The substrate may have at least one of a convex portion, a concave portion, a convex streak portion, a concave streak portion, and a through portion.
[0117] 3.Adhesive layer The decorative member of the present disclosure may have an adhesive layer (second adhesive layer) between the substrate and the decorative sheet. The second adhesive layer disposed between the substrate and the decorative sheet may be made of, for example, the same resin as the back adhesive layer described above. In addition, when the decorative sheet has the back adhesive layer described above, the decorative sheet and the substrate may be in direct contact with each other.
[0118] 4. Decorative materials The decorative member in the present disclosure has the above-mentioned decorative sheet and substrate. The uses of the decorative member in the present disclosure are not particularly limited, and examples thereof include architectural members such as walls, ceilings, floors, roofs, eaves, fences, and gates; fittings or fixtures such as window frames, doors, handrails, skirting boards, moldings, and other building materials; general furniture such as chests, shelves, and desks; kitchen furniture such as dining tables and sinks; various furniture used around water such as kitchens, toilets, bathrooms, and washbasins; surface decorative panels such as cabinets for home appliances and office automation equipment; and interior or exterior components for vehicles. The decorative material in the present disclosure may be a component used outdoors (exterior component) or a component used indoors (interior component).
[0119] The decorative member of the present disclosure can be obtained, for example, by laminating a decorative sheet and a substrate. Specifically, the substrate and the decorative sheet are laminated such that a surface of the substrate (a surface requiring decoration) faces a surface of the decorative sheet facing the base layer.
[0120] As a method for producing a decorative member, for example, a method is exemplified in which the decorative sheet is attached to the substrate so that the back adhesive layer of the decorative sheet of the present disclosure is in direct contact with the surface of the substrate. Another method for producing a decorative member is to laminate the decorative sheet to the substrate via a second adhesive layer so that the surface of the decorative sheet of the present disclosure facing the base layer side of the decorative sheet of the present disclosure faces the surface of the substrate.
[0121] Methods for laminating the base and the decorative sheet include, for example, lamination, wrapping, and vacuum forming. In the lamination method, for example, the decorative sheet is pressed onto a plate-shaped base with a pressure roller. In the wrapping method, for example, the decorative sheet is supplied and sequentially pressure-bonded to the multiple sides constituting the base with multiple rollers in different orientations. When a hot melt adhesive (heat-sensitive adhesive) is used to laminate the decorative sheet and the base, the heating temperature is, for example, 150°C or higher and 200°C or lower. Furthermore, when a reactive hot melt adhesive is used, the heating temperature is, for example, 100°C or higher and 130°C or lower.
[0122] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0123] [Example 1] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curing resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protruding layer ink 1 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70° C. for 24 hours to obtain the decorative sheet of Example 1. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 1.
[0124] <Ink for top layer 1> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 33 parts by weight (spherical urethane beads, average particle size 50 μm) Solvent (butyl acetate, ethyl acetate)
[0125] [Example 2] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curable resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protruding layer ink 2 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70° C. for 24 hours to obtain the decorative sheet of Example 2. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 1.
[0126] <Ink for top layer 2> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 11 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles: 9 parts by weight (silica particles, average particle size 3 μm) Solvent (butyl acetate, ethyl acetate)
[0127] [Example 3] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curing resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protruding layer ink 3 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70° C. for 24 hours to obtain the decorative sheet of Example 3. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 1.
[0128] <Ink for top layer 3> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 11 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles 4.5 parts by weight (silica particles, average particle size 12 μm) Solvent (butyl acetate, ethyl acetate)
[0129] [Example 4] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curing resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protruding layer ink 4 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70° C. for 24 hours to obtain the decorative sheet of Example 4. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 1.
[0130] <Ink for top layer 4> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Inorganic particles: 28 parts by weight (silica particles, average particle size 3 μm) Solvent (butyl acetate, ethyl acetate)
[0131] [Example 5] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curable resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 8 μm. Next, a protruding layer ink 5 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70° C. for 24 hours to obtain the decorative sheet of Example 5. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 1.
[0132] <Ink for top layer 5> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 7.6 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles: 15 parts by weight (silica particles, average particle size 6 μm) Solvent (butyl acetate, ethyl acetate)
[0133] [Example 6] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curable resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 1 μm. Next, a protruding layer ink 6 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70° C. for 24 hours to obtain the decorative sheet of Example 6. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 1.
[0134] <Ink for top layer 6> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 7.6 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Inorganic particles: 15 parts by weight (silica particles, average particle size 8 μm) Solvent (butyl acetate, ethyl acetate)
[0135] [Comparative Examples 1 to 3] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curing resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 3 μm. Next, a protruding layer ink 7 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was carried out at 70°C for 24 hours to obtain the decorative sheets of Comparative Examples 1 to 3. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 2.
[0136] <Ink for top layer 7> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 16 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 50 μm) Solvent (butyl acetate, ethyl acetate)
[0137] [Comparative Example 4] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curable resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 3 μm. Next, a protruding layer ink 8 having the following formulation was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70°C for 24 hours to obtain the decorative sheet of Comparative Example 4. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness of the raised layer were the values shown in Table 2.
[0138] <Ink for top layer 8> Two-component curing resin 100 parts by weight (base: acrylic polyol, curing agent: hexamethylene diisocyanate) Organic particles: 16 parts by weight (spherical polymethyl methacrylate particles, average particle diameter 30 μm) Solvent (butyl acetate, ethyl acetate)
[0139] [Comparative Example 5] (Making decorative sheets) The base material is colored base paper for building materials ("CHPS45 (model number)", basis weight: 45g / m 2(manufactured by Tenma Tokushushi Co., Ltd.) was prepared. A resin composition containing acrylic resin as a binder and titanium white, red iron oxide and yellow lead as colorants was applied to one side of the substrate by gravure printing to form a solid layer having a thickness of 5 μm. Next, a picture layer with a wood grain pattern was formed on the solid layer using a resin composition containing nitrocellulose as a binder and a colorant mainly composed of red iron oxide. This formed a design layer including a solid layer and a picture layer on the substrate. Next, a protective layer ink containing a two-component curing resin (main agent: acrylic polyol, curing agent: hexamethylene diisocyanate) and a matting agent (silica particles with an average particle size of 2 μm, 23 parts by mass relative to 100 parts by mass of the resin component of the protective layer) was applied to the entire surface of the design layer and dried to form a protective layer with an average thickness of 5 μm. Next, a protruding layer ink 7 having the above formula was applied to a part of the protective layer and dried to form a protruding layer having a plurality of protruding parts. Thereafter, heat curing was performed at 70°C for 24 hours to obtain a decorative sheet of Comparative Example 5. The raised portions were formed so that the ratio of the area of the raised layer to the area of the protective layer in the thickness direction, the average distance between adjacent raised portions, and the average thickness T4 of the raised layer were the values shown in Table 2.
[0140] [60° gloss value of protective layer and top layer] The 60° gloss values of the protruding layer and protective layer in the decorative sheets obtained in the Examples and Comparative Examples were measured by the following method. The results are shown in Tables 1 and 2. (Measurement method) The decorative sheet was placed with the raised layer side facing up, and the 60° specular gloss of the raised layer was measured from the raised layer side using a gloss meter ("Microgloss (model name)", manufactured by BYK Gardner) in accordance with method 3 of JIS Z 8741:1997. The 60° gloss value of the raised layer was taken as the average value of the measurements at any 10 points on the raised part. At each measurement point, the raised part was located at the center of the measurement point of the gloss meter, and measurements were made so that 50% or more of the area of the measurement point overlapped with the raised part. The 60° specular gloss of the protective layer was also measured using a similar method.
[0141] [Realism evaluation] A total of 20 subjects, five each from their 20s, 30s, 40s, and 50s, evaluated the realness of the decorative sheets obtained in the Examples and Comparative Examples. Visual observation was made from the raised layer side of the decorative sheet to evaluate the realness created by the raised layer and protective layer. The evaluation was performed under fluorescent lighting in a room that blocked out external light, and was based on the following evaluation criteria. The evaluation criteria for the realness were that the difference in gloss between the area with the raised portion and the area without the raised portion was sufficiently noticeable, and that the difference in gloss was not too large. (Evaluation Criteria) A: More than 15 out of 20 people answered that it felt authentic. B: Of 20 people, between 11 and 14 answered that it felt real. C: Between 5 and 10 out of 20 people answered that it felt real. D: Fewer than 4 out of 20 people answered that it felt real.
[0142] [Tactile evaluation] A total of 20 subjects, five each from their 20s, 30s, 40s, and 50s, evaluated the tactile sensation of the decorative sheets obtained in the Examples and Comparative Examples. Each subject touched the surface of the raised layer of the decorative sheet with the pad of the index finger of their dominant hand and evaluated whether or not the tactile sensation was high. The evaluation criteria for the tactile sensation were "whether or not the unevenness was strongly felt."
[0143] (Evaluation Criteria) A: More than 15 out of 20 people answered that they could feel the touch. B: Of 20 people, 11 to 14 people answered that they could feel the touch. C: Five to ten out of twenty people answered that they could feel the touch. D: Four or fewer people answered that they could feel the touch.
[0144] [Wear resistance evaluation] For the decorative sheets obtained in the Examples and Comparative Examples, an abrasion resistance test was carried out on the surface of the raised layer by a method conforming to the provisions of JIS K7204. The test conditions were a load of 500g for each of the two abrasive wheels (CS-10) and a rotation speed of 250 rpm. After the abrasion test, the decorative sheets were visually observed to determine the pattern remaining rate and evaluated according to the following evaluation criteria.
[0145] (Evaluation Criteria) A: Pattern survival rate over 90% B: Pattern remaining rate: 70% to less than 90% C: Pattern remaining rate 50% to less than 70% D: Less than 50% of the handle remains
[0146] [Evaluation of cellophane tape resistance] For the decorative sheets obtained in the examples and comparative examples, a 60 mm x 24 mm piece of Cellotape (registered trademark) (manufactured by Nichiban Co., Ltd., 24 mm width) was attached to the surface of the raised layer. It was then rapidly peeled off at an angle of 45°. This was repeated 10 times, and the presence or absence of peeled parts after the test was evaluated. A: No peeling B: Peeling occurs
[0147] [Table 1]
[0148] [Table 2]
[0149] As shown in Table 1, the decorative sheets obtained in Examples 1 to 6 were confirmed to have a strong tactile sensation while also having a sense of the real thing. On the other hand, as shown in Table 2, the decorative sheets obtained in Comparative Examples 1 to 5 were confirmed to have a high gloss value for the raised layer and a poor sense of the real thing because organic particles with a large average particle size were used in the raised layer. In addition, it was confirmed that the decorative sheets obtained in Comparative Examples 3 and 4 did not have a strong tactile sensation because the average spacing between the raised parts was short.
[0150] Thus, in the present disclosure, for example, the following inventions are provided:
[0151] [1] A decorative sheet having a base layer, a design layer, a protective layer, and a raised layer having a patterned raised portion, in this order in a thickness direction, The 60° gloss value of the protective layer is smaller than the 60° gloss value of the protruding layer, The 60° gloss value of the above-mentioned layer is 20 or less, In the thickness direction, the ratio of the area of the protruding layer to the area of the protective layer is 10% or more; A decorative sheet, wherein the average distance between adjacent raised portions is 1.6 mm or more.
[0152] [2] The decorative sheet according to [1], wherein the protective layer has a 60° gloss value of 3 or less.
[0153] [3] The decorative sheet according to [1] or [2], wherein the 60° gloss value of the protruding layer is 4 or more.
[0154] [4] The decorative sheet according to any one of [1] to [3], wherein the average distance between adjacent raised portions is 4.0 mm or less.
[0155] [5] The decorative sheet according to any one of [1] to [4], wherein the average thickness of the protruding layer is at least twice the average thickness of the protective layer.
[0156] [6] The decorative sheet according to any one of [1] to [5], wherein the average thickness of the raised layer is 15 μm or more.
[0157] [7] The decorative sheet according to any one of [1] to [6], wherein the average thickness of the protective layer is 5 μm or more.
[0158] [8] A decorative sheet according to any one of [1] to [7], wherein the raised portion contains a filler.
[0159] [9] The decorative sheet according to [8], wherein the filler is inorganic particles.
[0160]
[10] The decorative sheet according to [9], wherein the content of the inorganic particles in the protruding portion is 2 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of the protruding portion.
[0161]
[11] The decorative sheet according to [9] or
[10] , wherein the average particle size of the inorganic particles is 2 μm or more and 12 μm or less.
[0162]
[12] The decorative sheet according to [8], wherein the filler is organic particles.
[0163]
[13] The decorative sheet according to
[12] , wherein the content of the organic particles in the raised portion is 7 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of the raised portion.
[0164]
[14] The decorative sheet according to
[12] or
[13] , wherein the average particle size of the organic particles is 20 μm or more and 60 μm or less.
[0165]
[15] A substrate; [1] to
[14] , and A decorative member having the above structure. [Explanation of symbols]
[0166] 1...Base material layer 2…Design layer 3…Protective layer 4…Morijo layer 4a…More part 10...Decorative sheet
Claims
1. A decorative sheet having a base layer, a design layer, a protective layer, and a raised layer having a patterned raised portion, in this order in a thickness direction, The 60° gloss value of the protective layer is smaller than the 60° gloss value of the protruding layer, The 60° gloss value of the raised layer is 20 or less, In the thickness direction, a ratio of an area of the protruding layer to an area of the protective layer is 10% or more; The decorative sheet, wherein the average distance between adjacent raised portions is 1.6 mm or more.
2. 2. The decorative sheet according to claim 1, wherein the 60° gloss value of said protective layer is 3 or less.
3. 2. The decorative sheet according to claim 1, wherein the 60° gloss value of said raised layer is 4 or more.
4. 2. The decorative sheet according to claim 1, wherein the average distance between adjacent raised portions is 4.0 mm or less.
5. 2. The decorative sheet according to claim 1, wherein the average thickness of said raised layer is at least twice as large as the average thickness of said protective layer.
6. 2. The decorative sheet according to claim 1, wherein the average thickness of the raised layer is 15 μm or more.
7. 2. The decorative sheet according to claim 1, wherein the protective layer has an average thickness of 5 μm or more.
8. The decorative sheet according to claim 1 , wherein the raised portion contains a filler.
9. The decorative sheet according to claim 8 , wherein the filler is an inorganic particle.
10. 10. The decorative sheet according to claim 9, wherein the content of said inorganic particles in said raised portion is 2 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of said raised portion.
11. 10. The decorative sheet according to claim 9, wherein the inorganic particles have an average particle size of 2 μm or more and 12 μm or less.
12. The decorative sheet according to claim 8 , wherein the filler is an organic particle.
13. 13. The decorative sheet according to claim 12, wherein the content of said organic particles in said raised portion is 7 parts by mass or more and 38 parts by mass or less per 100 parts by mass of the resin component of said raised portion.
14. The decorative sheet according to claim 12, wherein the average particle size of the organic particles is 20 μm or more and 60 μm or less.
15. A substrate; A decorative sheet according to any one of claims 1 to 14, A decorative member having the above structure.
Citation Information
Patent Citations
Decorative sheet
JP2008087158A