Cu-Ti-Al-BASED COPPER ALLOY SHEET MATERIAL, ELECTRONIC APPARATUS COMPONENT, CURRENT-CARRYING COMPONENT, AND HEAT DISSIPATION COMPONENT

A Cu-Ti-Al-based copper alloy with optimized manufacturing processes achieves improved strength, conductivity, and reduced density, addressing the limitations of existing alloys by enhancing fatigue and spring limit values for electronic and automotive components.

JP2024144012AActive Publication Date: 2024-10-11DOWA METALTECH CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023151479
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-09-19
Publication Date
2024-10-11
Estimated Expiration
2043-09-19

AI Technical Summary

Technical Problem

Existing methods for Cu-Ti based copper alloys fail to simultaneously improve fatigue properties and spring limit values while reducing density, which is crucial for lightweight components in mobile terminals and automotive electronics.

Method used

A Cu-Ti-Al-based copper alloy with specific compositional ranges and manufacturing processes, including multiple solution treatments and controlled cold rolling, aging treatments, and cooling rates to refine crystal grains and precipitates, resulting in a material with high strength, bending workability, and reduced density.

Benefits of technology

The alloy achieves enhanced strength, conductivity, fatigue properties, and spring limit values with a reduced density, suitable for electronic device components, current-carrying parts, and heat dissipation components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144012000001
    Figure 2024144012000001
  • Figure 2024144012000002
    Figure 2024144012000002
  • Figure 2024144012000003
    Figure 2024144012000003
Patent Text Reader

Abstract

To provide a Cu-Ti-based copper alloy sheet material having all of good strength, bendability, conductivity, fatigue characteristics and spring bending elastic limit and reduced density (specific gravity).SOLUTION: There is provided a copper alloy sheet material comprising: in mass %, Ti: 1.00 to 5.00%, Al: 0.50 to 3.00%, Ag: 0 to 0.30%, B: 0 to 0.30%, Co: 0 to 1.00%, Cr: 0 to 1.00%, Fe: 0 to 1.00%, Mg: 0 to 1.00%, Mn: 0 to 2.00%, Nb: 0 to 1.00%, Ni: 0 to 1.00%, P: 0 to 0.50%, S: 0 to 0.20%, Si: 0 to 0.50%, Sn: 0 to 2.00%, V: 0 to 1.00%, Zn: 0 to 3.00%, Zr: 0 to 1.00% and a rare earth element: 0 to 3.00%, the total of elements excluding the above elements and Cu: 0.50% or less, Ti / Al being 1.50 or more with the balance substantially being Cu, and having an average crystal grain size, a number density of coarse deposit particles, a tensile strength of LD and a spring bending elastic limit of TD within predetermined ranges.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Cu-Ti-Al-based copper alloy sheet material having a reduced density (specific gravity), and to electronic device parts, current-carrying parts, and heat-dissipating parts using said sheet material as a material. [Background technology]

[0002] Among various copper alloys, Cu-Ti-based copper alloys (copper titanium) have a high level of strength and good stress relaxation resistance, and are therefore used as electrical spring parts for connectors, relays, switches, etc. In recent years, as mobile terminals such as smartphones and electronic devices for automobiles have become more highly functional, there has been an increasing demand for weight reduction in the individual components used in them. In order to meet this demand, it is important to achieve low density (low specific gravity) in the copper alloy materials used as the material for the parts. On the other hand, in order to obtain reliable parts while satisfying the demands for miniaturization and thinning, it is important to improve fatigue properties and spring limit value in addition to achieving both strength and bending workability.

[0003] Various techniques have been studied to achieve both strength and bending workability in Cu-Ti-based copper alloy materials, as seen in the following patent documents, for example. However, no method has been established to simultaneously improve fatigue properties and spring limit value while achieving low density (low specific gravity).

[0004] Patent Document 1 describes that fatigue properties of a Cu-Ti based copper alloy are improved by a process of performing cold rolling after hot rolling, and then performing heat treatment at 100 to 400° C. while performing straightening with a tension leveler. With this method, it is difficult to improve the spring limit (see Comparative Example No. 57 described later).

[0005] Patent Document 2 describes that in a Cu-Ti based copper alloy, after solution treatment, a precursor treatment is performed in which the alloy is heated at 550 to 730°C for a relatively short time, followed by cold rolling and aging treatment to improve fatigue properties. With the technique disclosed in Patent Document 2, it is difficult to obtain a material with a high spring limit value.

[0006] Patent Document 3 describes a technique for obtaining a material with a high spring limit value by performing aging treatment without cold rolling after the second solution treatment, followed by cold rolling and stress relief annealing. Since the Cu-Ti copper alloy of Patent Document 3 does not contain Al, the application of the above process tends to result in an increase in coarse precipitate particles, making it difficult to improve fatigue properties (see Comparative Example No. 58 described later).

[0007] Patent Document 4 describes that a material with a controlled grain boundary reaction phase size is obtained by performing a solution treatment once for a Cu-Ti-based copper alloy, followed by aging treatment, cooling to 300°C at 10 to 80°C / h, and then cold rolling. The spring limit value is not necessarily high. In addition, since the Cu-Ti-based copper alloy of Patent Document 4 does not contain Al, the application of the above process tends to result in a large number of coarse precipitate particles, making it difficult to improve fatigue properties (see Comparative Example No. 59 described later).

[0008] Patent Document 5 describes that a Cu-Ti based copper alloy is provided with a structure having a high integrated strength in the (311) plane by a process of performing hot rolling, cold rolling, one solution treatment, aging at 300 to 550°C, and cold rolling and stress relief annealing as necessary. Since the Cu-Ti based copper alloy of Patent Document 5 does not contain Al, the application of the above process easily causes coarsening of precipitates, making it difficult to improve fatigue properties and spring limit value (see Comparative Example No. 60 described later).

[0009] Patent Document 6 describes that a Cu-Ti based copper alloy is provided with a structure having a high integrated strength in the (420) plane by carrying out a process of performing cold rolling after hot rolling, performing a solution treatment once, and then performing cold rolling as necessary, performing aging treatment at 300 to 500°C, and performing cold rolling and low-temperature annealing as necessary. Since the solution treatment is performed once and the cooling rate after the aging treatment is not specified, it is considered that the number of coarse precipitates increases during the cooling process of the aging treatment, making it difficult to improve the fatigue properties (see Comparative Example No. 61 described later). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2014-15679 A [Patent Document 2] JP 2014-185370 A [Patent Document 3] JP 2012-62575 A [Patent Document 4] JP 2012-207254 A [Patent Document 5] JP 2013-82960 A [Patent Document 6] JP 2010-126777 A Summary of the Invention [Problem to be solved by the invention]

[0011] The techniques disclosed in the above-mentioned patent documents and the like have made it possible to obtain Cu-Ti-based copper alloy sheets having both good strength and bending workability. However, as described above, the current situation is that no method has been established for simultaneously improving the fatigue properties and spring limit value.

[0012] The present invention aims to provide a Cu-Ti-based copper alloy sheet material which has good strength, bending workability and electrical conductivity, as well as improved fatigue characteristics and spring limit value and reduced density (specific gravity), and to provide a part making use of the properties of the sheet material. [Means for solving the problem]

[0013] In order to achieve the above object, the present specification discloses the following invention. [1] In mass%, Ti: 1.00-5.00%, Al: 0.50-3.00%, Ag: 0-0.30%, B: 0-0.30%, Co: 0-1.00%, Cr: 0-1.00%, Fe: 0-1.00%, Mg: 0-1.00%, Mn: 0-2.00%, Nb: 0-1.00%, Ni: 0-1.00%, P: 0-0.50%, S: 0-0.20%, Si: 0-0.50%, Sn: 0-2.00%, V: 0-1.00%, Zn: 0-3.00%, Zr: 0-1.00%, rare earth elements The composition is as follows: total of elements: 0 to 3.00%, total of Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr and rare earth elements: 3.00% or less, total of elements other than Ti, Al, Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr, rare earth elements and Cu: 0 to 0.50%, and the balance Cu; the content ratio of Ti to Al by mass, Ti / Al, is 1.50 or more; the average crystal grain size, as measured on a surface observed parallel to the sheet surface, is 1 to 20 μm, as measured on a surface observed parallel to the sheet surface, according to a cutting method in accordance with JIS H0501-1986; and the number density of coarse precipitate particles with a major axis of 1.0 μm or more, as measured on a surface observed parallel to the sheet surface, is 1.0 x 10 5 pieces / mm 2 The copper alloy sheet material has a tensile strength parallel to the rolling direction of 850 MPa or more, and a spring limit value perpendicular to the rolling direction of 400 MPa or more. [2] The copper alloy sheet material according to the above [1], wherein the Nb content is 0 to 0.50 mass %. [3] The copper alloy sheet material according to [1] or [2] above, in which the KAM value is 3.00° or less when a boundary with a crystal orientation difference of 15° or more is regarded as a grain boundary in an observation surface parallel to the sheet surface by EBSD (electron backscatter diffraction) with a step size of 0.1 μm. [4] The copper alloy sheet material according to any one of the above [1] to [3], having an electrical conductivity of 10.0% IACS or more. [5] The copper alloy sheet material according to any one of the above [1] to [4], wherein a ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t in a BW W-bending test according to the Japan Copper and Brass Association technical standard JCBA T307:2007 is 2.0 or less. [6] In a test using a test piece with its longitudinal direction perpendicular to the rolling direction, the fatigue limit at a load stress of 450 MPa was 10 7 The copper alloy sheet material according to any one of the above [1] to [5], wherein the copper alloy sheet material has a resistance to deformation and a temperature rise which is greater than or equal to 1000 s. [7] Density: 8.53 g / cm 3 The copper alloy sheet material according to any one of the above [1] to [6], which is: [8] An electronic device part using the copper alloy sheet material according to any one of [1] to [7] above as a material. [9] An electrical conductive part using the copper alloy sheet material according to any one of [1] to [7] above as its material.

[10] A heat dissipation component using the copper alloy sheet material according to any one of [1] to [7] above as its material.

[0014] The copper alloy sheets [1] to [7] above can be produced, for example, by the following method.

[11] A process for producing a copper alloy sheet material by subjecting an intermediate product sheet material having the above composition to a first solution treatment, a first intermediate cold rolling, a second solution treatment, a second intermediate cold rolling, and an aging treatment in the above order, The first solution treatment is carried out at a temperature of 800 to 900°C for 20 to 600 seconds. The first intermediate cold rolling is performed at a rolling ratio of 70% or more. The second solution treatment is carried out at a temperature range of 750 to 860°C for 10 to 300 seconds. The second intermediate cold rolling is performed at a rolling ratio of 15 to 50%, The aging treatment is carried out under the conditions that the maximum temperature T0 (°C) is in the range of 320°C or higher and 450°C or lower, the holding temperature range is [T0 - 10°C] or higher and T0 or lower, and the holding time in the holding temperature range is 5 to 20 hours. After performing heat holding, the average cooling rate from [T0 - 10°C] to 300°C is set to 30 to 60°C / h, and the average cooling rate from 300°C to 150°C is set to 20°C / h or lower for cooling. A method for manufacturing a copper alloy sheet.

[12] The method for manufacturing a copper alloy sheet according to

[11] above, wherein a sheet having a spring limit value in the rolling right angle direction of 400 MPa or more is obtained.

[0015] In this specification, the notation "n1~n2" indicating a numerical range means "n1 or more and n2 or less". Here, n1 and n2 are numerical values satisfying n1 < n2. The "sheet" means a sheet-like metal material formed by utilizing the malleability of the metal. A thin sheet-like metal material may also be called a "foil", and such a "foil" is also included in the "sheet" referred to here. A long sheet-like metal material wound in a coil shape is also included in the "sheet". In this specification, the thickness of the sheet-like metal material is called the "sheet thickness". The "sheet surface" is a surface perpendicular to the sheet thickness direction of the sheet. The "sheet surface" may also be called the "rolling surface".

Advantages of the Invention

[0016] According to the present invention, it has become possible to realize a Cu-Ti-based copper alloy sheet that兼备 all of high strength, bendability, conductivity, fatigue characteristics, and spring limit value, and has a low density (low specific gravity).

Embodiments for Carrying Out the Invention

[0017] [Chemical Composition] Hereinafter, "%" regarding alloy components means "mass%" unless otherwise specified. Ti (titanium) is an element that brings about the formation of a Ti modulated structure by spinodal decomposition and the formation of fine second phase particles by precipitation, and contributes to increasing the strength of the Cu-Ti-Al-based copper alloy of the present invention. It also contributes to improving stress relaxation resistance and reducing density (specific gravity). Here, the alloy with a Ti content of 1.00% or more is targeted. From the viewpoint of precipitation strengthening, the Ti content is more preferably 1.50% or more, and even more preferably 2.50% or more. Excessive Ti content is a factor that reduces hot workability and cold workability as well as bending workability, so the Ti content is set to 5.00% or less. It may be controlled to 4.50% or less, or 4.00% or less.

[0018] Al (aluminum) is an element effective in reducing the density (specific gravity) of Cu-Ti-Al copper alloys. In addition, according to the research of the inventors, it has been found that Al is an element effective in suppressing the formation of coarse precipitates in Cu-Ti-Al copper alloys. In order to fully exert these effects, the Al content is ensured to be 0.50% or more. It is more effective to make it 0.70% or more, and even more effective to make it 1.00% or more. When 0.50% or more of Al is added to a Cu-Ti copper alloy, there is a problem that it is generally difficult to achieve both strength and bending workability. However, this problem can be solved by the manufacturing method described later. However, if the Al content becomes too high, the electrical conductivity decreases, so the Al content is limited to 3.00% or less. It is preferable that the Al content is 2.80% or less.

[0019] The Ti and Al contents are adjusted so that Ti / Al, which represents the content ratio of Ti and Al in mass proportion, is 1.50 or more. If Ti / Al is too small, it is likely to cause insufficient electrical conductivity and strength, and the balance between strength and electrical conductivity may be poor. Ti / Al is necessarily 10.00 or less to satisfy the above-mentioned Ti content range and Al content range, but it may be adjusted to, for example, 7.00 or less, or 5.00 or less.

[0020] Ag (silver), B (boron), Co (cobalt), Cr (chromium), Fe (iron), Mg (magnesium), Mn (manganese), Nb (niobium), Ni (nickel), P (phosphorus), S (sulfur), Si (silicon), Sn (tin), V (vanadium), Zn (zinc), Zr (zirconium), and rare earth elements are optional elements. One or more of these can be contained as necessary. For example, Ni, Co, Fe, and Nb form intermetallic compounds with Ti to contribute to improving strength. In addition, the intermetallic compounds of these elements suppress the coarsening of crystal grains, making it possible to perform solution treatment at higher temperatures in the production of copper alloy sheet materials, which is advantageous in fully dissolving Ti. Suppressing the coarsening of crystal grains is also advantageous in terms of fatigue properties. Fe in particular is useful for improving strength and fatigue properties. Ag and Sn have a solid solution strengthening effect and an effect of improving stress relaxation resistance. Zn improves solderability and strength, and is also effective in improving castability. Mg has the effect of improving stress relaxation resistance and desulfurization. Si can form a compound with Ti, which contributes to pinning during recrystallization in the production of copper alloy sheet material and can reduce the grain size. Cr and Zr are effective in dispersion strengthening and suppressing grain coarsening. Mn and V are likely to form high melting point compounds with S and the like, and B and P have the effect of refining the cast structure, so they can each contribute to improving hot workability. Rare earth elements (REM) are Sc (scandium), Y (yttrium), and lanthanoid elements (excluding Pm (promethium)) in Group 3 of the periodic table. The inclusion of rare earth elements is effective in refining grains and dispersing precipitates. Misch metal (a mixture of rare earth elements) may be used as a source of rare earth elements.

[0021] The contents of the above optional elements can be in the ranges of Ag: 0-0.30%, B: 0-0.30%, Co: 0-1.00%, Cr: 0-1.00%, Fe: 0-1.00%, Mg: 0-1.00%, Mn: 0-2.00%, Nb: 0-1.00%, Ni: 0-1.00%, P: 0-0.50%, S: 0-0.20%, Si: 0-0.50%, Sn: 0-2.00%, V: 0-1.00%, Zn: 0-3.00%, Zr: 0-1.00%, and the sum of rare earth elements: 0-3.00%. The rare earth elements may include, for example, one or more selected from La (lanthanum): 2.00% or less, Ce (cerium): 1.80% or less, Pr (praseodymium): 0.30% or less, Nd (neodymium): 0.80% or less, Sm (samarium): 2.50% or less, and Y (yttrium): 2.50% or less, with the total content of rare earth elements being 3.00% or less. In the above, the Nb content may be specified to be 0 to 0.50%.

[0022] Furthermore, the contents of the above optional elements are more preferably within the ranges of Ag: 0-0.20%, B: 0-0.20%, Co: 0-0.50%, Cr: 0-0.50%, Fe: 0-0.50%, Mg: 0-0.50%, Mn: 0-1.80%, Nb: 0-0.30%, Ni: 0-0.50%, P: 0-0.20%, S: 0-0.10%, Si: 0-0.20%, Sn: 0-1.50%, V: 0-0.50%, Zn: 0-2.00%, Zr: 0-0.50%, and the total of rare earth elements: 0-2.00%. In this case, the content range of rare earth elements taking into consideration economic efficiency and manufacturability can be, for example, a range including one or more selected from La: 0.60% or less, Ce: 0.70% or less, Pr: 0.10% or less, Nd: 0.20% or less, Sm: 1.00% or less, and Y: 1.00% or less, with the total content of rare earth elements being 1.50% or less.

[0023] The contents of the above optional elements may be controlled within the following ranges: Ag: 0-0.15%, B: 0-0.15%, Co: 0-0.20%, Cr: 0-0.20%, Fe: 0-0.20%, Mg: 0-0.45%, Mn: 0-1.50%, Nb: 0-0.15%, Ni: 0-0.20%, P: 0-0.15%, S: 0-0.04%, Si: 0-0.03%, Sn: 0-1.30%, V: 0-0.20%, Zn: 0-1.80%, Zr: 0-0.20%, and rare earth elements total: 0-1.00%. In this case, a more preferable content range of rare earth elements that takes into further consideration economic efficiency and manufacturability can be, for example, a range including one or more selected from La: 0.35% or less, Ce: 0.32% or less, Pr: 0.04% or less, Nd: 0.10% or less, Sm: 0.50% or less, and Y: 0.50% or less, with the total content of rare earth elements being 0.80% or less.

[0024] The total content of the above optional elements Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr and rare earth elements is in the range of 3.00% or less (including 0%). The upper limit of the total content of these optional elements is preferably 2.00% or less, and may be controlled to 1.60% or less.

[0025] Elements other than those mentioned above are also permitted to be contained within a range that does not impede the objectives of the present invention (good strength, bending workability, electrical conductivity, fatigue properties, spring limit value, and low density). Specifically, the total content of elements other than Ti, Al, Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr, rare earth elements, and Cu (copper) may be controlled to 0.50% or less (including 0%), or may be controlled to 0.10% or less (including 0%).

[0026] As an embodiment of the alloy composition in which the total content of elements other than Ti, Al, Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr, rare earth elements, and Cu (copper) is 0.10% or less, for example, "in mass%, Ti: 1.00 to 5.00%, Al: 0.50 to 3.00%, Ag: 0 to 0.30%, B: 0 to 0.30%, Co: 0 to 1.00%, Cr: 0 to 1.00%, Fe: 0 to 1.00%, Mg: 0 to 1.00%, Mn: 0 to 2.00%, Nb: 0 to 1.00% or 0 to 0.50%, Ni: 0-1.00%, P: 0-0.50%, S: 0-0.20%, Si: 0-0.50%, Sn: 0-2.00%, V: 0-1.00%, Zn: 0-3.00%, Zr: 0-1.00%, total rare earth elements: 0-3.00%, total of Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr and rare earth elements: 3.00% or less, balance Cu and unavoidable impurities, Ti / Al content ratio by mass percentage is 1.50 or more. In this case, unavoidable impurities refer to elements that are inevitably mixed in during manufacturing and are other than the elements listed above.

[0027] [Average grain size] In the Cu-Ti-Al-based copper alloy sheet material having the above-mentioned chemical composition, when the average grain size is 1 to 20 μm according to the cutting method in accordance with JIS H0501-1986 on the observation surface parallel to the sheet surface, good bending workability and fatigue properties are obtained. The above-mentioned average grain size is more preferably 15 μm or less, and even more preferably 5 μm or less. In a structure state in which the average grain size is less than 1 μm, non-recrystallized grains may be mixed, and from the viewpoint of maintaining stable and good bending workability, it is advantageous for the average grain size to be 1 μm or more. The manufacturing process described below in which the solution treatment is performed twice is effective for refining the grains. In addition, the cutting method specified in JIS H0501-1986 states that "the average value of the cutting length (mm) is displayed," but since the grain size targeted in the present invention is very small compared to this default display unit, here, a measurement in accordance with the method of the standard is performed in a higher magnification observation field to obtain the average grain size in μm units.

[0028] [Number density of coarse precipitate particles] Reducing the amount of coarse precipitates is extremely effective in improving fatigue properties. In the present invention, the number density of coarse precipitate particles with a major axis of 1.0 μm or more on an observation surface parallel to the sheet surface is 1.0 × 10 5 pieces / mm 2 The number density of coarse precipitate particles is 8.5×10 4 pieces / mm 2 It is more effective to set the number density of the coarse precipitate particles to 8.5×10 or less. 4 pieces / mm 2 It is more advantageous for improving fatigue properties that the average grain size is 15 μm or less and the average grain size is 15 μm or less. The fewer the coarse precipitate particles, the better. However, it is difficult in manufacturing to completely prevent the formation of coarse precipitate particles. Usually, the number density of the coarse precipitate particles is 5.0×10 2 pieces / mm 2 That's all. The number density of the coarse precipitate particles can be determined by the following method.

[0029] (How to determine the number density of coarse precipitate particles) The plate surface was electrolytically polished under the following electrolytic polishing conditions to dissolve only the Cu base of the copper alloy plate material, exposing the precipitate particles. The surface was then observed with a field emission scanning electron microscope (FE-SEM) at an acceleration voltage of 15 kV and a magnification of 5,000 times. The total number of precipitate particles with a major axis of 1.0 μm or more observed on the FE-SEM image was calculated based on the total observation area (mm 2 ) is the number density of coarse precipitate particles (particles / mm 2 ) for the secondary electron image of the FE-SEM, the focus is adjusted at a magnification of 5000x, and the color tone is then adjusted using auto-contrast. At this time, the image in the same field of view may be burned by the electron beam, causing a change in color tone, so observation is carried out in a field of view different from the one used for auto-contrast. This is done to prevent variation in the precipitate number density results due to adjustment of the brightness threshold value in the binarization process of coarse precipitates, which will be described later. The total observation area is a total of 0.1 mm2, measured using multiple randomly set non-overlapping observation fields. 2That is all. Precipitate particles that partly protrude from the observation field are counted if the portion that appears within the observation field is assumed to be the entire particle and its major axis is 1.0 μm or more. Regarding the measurement of the major axis of precipitate particles, the SEM image (secondary electron image) is binarized using image analysis software to identify the areas where precipitate particles exist, the outline of each precipitate particle is approximated as an ellipse, and the length of the major axis of that ellipse (however, if the ellipse is a perfect circle, the diameter of the circle) can be used as the major axis.

[0030] (Electrolytic polishing conditions) Electrolyte: Distilled water, phosphoric acid, ethanol, and 2-propanol mixed in a volume ratio of 10:5:5:1 Liquid temperature: 20℃ Voltage: 15V ·Electrolysis time: 20 seconds

[0031] [Spring limit value] The spring limit is measured by a method conforming to the moment test specified in JIS H3130:2018. Although the standard states that "test pieces are taken in the rolling direction of the plate or strip," in this case, a test piece whose longitudinal direction is the transverse direction (TD) is adopted in order to evaluate with stricter standards. The transverse direction is the direction perpendicular to the rolling direction and the plate thickness direction. Except for the use of a test piece whose longitudinal direction is transverse to the rolling direction, the moment test for alloy number C1990 described in JIS H3130:2018 is adopted. As a result of the investigation, in order to obtain high reliability in current-carrying spring parts that may be bent into complex shapes, it is advantageous for the spring limit value by this test to be 400 MPa or more. It is more effective for this spring limit value to be 550 MPa or more, and it can also be adjusted to 700 MPa or more. The spring limit value is usually 1000 MPa or less.

[0032] [Tensile strength] The tensile strength in the rolling direction (LD) of the copper alloy sheet material of the present invention is preferably 850 MPa or more, more preferably 880 MPa or more. It is also possible to adjust the tensile strength in the rolling direction to a strength level of 1000 MPa or more. The upper limit of the tensile strength is not particularly limited, but it may be adjusted to, for example, a range of 1400 MPa or less, or may be adjusted to a range of 1200 MPa or less.

[0033] [KAM value] In order to achieve an excellent spring limit value of the level specified in the present invention, it is preferable that the KAM value is not too high. The KAM value is one of the indices that can evaluate the lattice strain in the crystal grains. As a result of the study, in the copper alloy sheet material of the present invention, the KAM value is preferably 3.00° or less when the boundary with a crystal orientation difference of 15° or more is regarded as the crystal grain boundary in the measurement by EBSD (electron backscatter diffraction) of the observation surface parallel to the sheet surface with a step size of 0.1 μm. As long as a sufficient spring limit value is obtained, the lower limit of the KAM value is not particularly limited, but it is usually sufficient to adjust it to a range of 0.20° or more. From the viewpoint of an excellent spring limit value and manufacturability, the KAM value is more preferably in the range of 0.45 to 2.00°. The KAM value can be obtained by the following method.

[0034] (How to calculate KAM value) The plate surface (rolled surface) of the plate material sample to be measured is buffed and then smoothed by ion milling to obtain an observation surface. Within the observation surface, an observation area with a field of view equivalent to an observation magnification of 2000 times (for example, five rectangular areas of 45 μm in the direction perpendicular to the rolling × 60 μm in the rolling direction) is randomly set, and the observation area is irradiated with an electron beam at a step size of 0.1 μm by EBSD (electron backscatter diffraction) to collect crystal orientation data. Based on the data, a kernel average misorientation (KAM) value is calculated using EBSD data analysis software, assuming that the boundary where the crystal orientation difference between adjacent measurement points is 15° or more is a grain boundary. The KAM value corresponds to the average value of all the crystal orientation differences between adjacent spots (hereinafter referred to as "adjacent spot misorientation") measured for electron beam irradiation spots arranged at a pitch of 0.1 μm, and only the measurement values ​​of the adjacent spot misorientation differences that are less than 15° are extracted. In calculating the KAM value, twin boundaries are also considered as grain boundaries.

[0035] [conductivity] Considering the applications of Cu-Ti-Al based copper alloy sheets, the electrical conductivity is preferably 10.0% IACS or more. There is no particular upper limit to the electrical conductivity, but it is usually adjusted to be within the range of 20.0% IACS or less.

[0036] [Bending workability] Bending is often performed when processing into current-carrying parts, etc. Considering the applications of Cu-Ti-Al alloy sheets, if they have bending workability in which the ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the sheet thickness t is 2.0 or less in a BW W-bend test according to the Japan Copper and Brass Association technical standard JCBA T307:2007, they can be highly reliable when processed into many current-carrying parts and heat-dissipating parts. It is more preferable that MBR / t at BW is 1.0 or less, and even more preferable that it is 0.7 or less. It is also possible to obtain a sheet with MBR / t at BW of 0.0 (no cracks occurring in tight bending). BW (Bad Way) means that the bending axis is parallel to the rolling direction.

[0037] In addition, JCBA T307:2007 states that "This standard applies to the evaluation of bending workability of copper and copper alloy thin plate strips having a thickness of 0.1 mm or more and 0.8 mm or less." According to the study by the inventors, it was confirmed that the bending workability can be evaluated by the W-bend test method described in the standard even for Cu-Ti-Al-based copper alloy sheets having a thickness of less than 0.1 mm. Therefore, in the present invention, the W-bend test method in BW shown in JCBA T307:2007 is extended to the case of a sheet thickness of less than 0.1 mm (for example, 0.02 mm or more and less than 0.1 mm) and is applied as it is.

[0038] [Fatigue properties] In order to obtain high reliability in current-carrying spring parts that may be bent into complex shapes, a fatigue limit of 10 MPa at a load stress of 450 MPa must be achieved in a reversed-swing fatigue test using a cantilever resonance method with a test piece whose longitudinal direction is perpendicular to the rolling direction (TD). 7 cycles, i.e., 1.0×10 7 It is preferable that no "fatigue" occurs during the cycle, and the 7 It is more preferable that no "fatigue" occurs during the cycle. 8 Fatigue occurs in cycles of 3.0×10 8 Fatigue may occur within less than one cycle. "Fatigue" can be determined by monitoring the decrease in resonant frequency associated with a decrease in Young's modulus.

[0039] [density] Since the order of atomic weights of Cu, Ti, and Al is Cu>Ti>Al, increasing the Al content is the most effective way to reduce the density (specific gravity) of a Cu-Ti-Al based copper alloy, and the Ti content also has a large effect. 3 In Cu-Ti-Al-based copper alloy sheet materials, it is possible to reduce the density to 8.53 g / cm while simultaneously providing good strength, bending workability, electrical conductivity, fatigue properties, and spring limit value. 3It has been difficult to reduce the density to below 7.80 g / cm using conventional techniques. 3 The adjustment may be made within the above range.

[0040] [Manufacturing method] The copper alloy sheet material described above can be manufactured, for example, by the following manufacturing process. Melting and casting → heating of the cast piece → hot processing → rough cold rolling → 1st solution treatment → 1st intermediate cold rolling → 2nd solution treatment → 2nd intermediate cold rolling → aging treatment Although not described in the above steps, facing is performed as necessary after the hot working, and pickling, polishing, or further degreasing is performed as necessary after each heat treatment. Each of the above steps will be described below.

[0041] [Melting and Casting] A cast piece having the chemical composition specified in the present invention may be produced using a crucible furnace, etc. To prevent oxidation of Ti and Al, it is preferable to carry out the process in an inert gas atmosphere or in a vacuum melting furnace.

[0042] [Slab heating] The heating of the slab before hot working can be carried out, for example, by holding it at 900 to 1000° C. for 0.5 to 5 hours.

[0043] [Hot processing, rough cold rolling] The method of hot working is not particularly limited. Usually, hot rolling or hot forging is adopted. In the case of hot rolling, the total hot rolling reduction ratio may be, for example, 60 to 99%. After the hot working is completed, it is preferable to rapidly cool the material by water cooling or the like. Then, cold rolling is performed. The cold rolling at this stage is called "rough cold rolling" in this specification. The rolling reduction ratio in the rough cold rolling can be, for example, 50 to 99%. In this way, an intermediate product sheet material to be subjected to the first solution treatment can be obtained. Here, the rolling ratio is represented by the following formula (1) (the same applies to each of the following steps). Reduction ratio (%) = 100 × (t0-t1) / t0…(1) t0: thickness before rolling (mm) t1: thickness after rolling (mm)

[0044] [First solution treatment] The intermediate product sheet material is subjected to a first solution treatment. In this solution treatment, the strain introduced by hot working and rough cold rolling is utilized to recrystallize, and the coarse grain boundary reaction type precipitates and granular precipitates generated after casting or during hot working are sufficiently dissolved. If the precipitates are not sufficiently dissolved at the stage of this first solution treatment, the precipitates remain until the final process, and the desired characteristics cannot be obtained. In the first solution treatment, it is advantageous to introduce a large amount of heat energy in order to prioritize the dissolution. In this case, recrystallized grains are likely to grow, but this is not a problem because the grains are refined in the subsequent second solution treatment. The first solution treatment is performed under conditions of holding at a temperature range of 800 to 900°C for 20 to 600 seconds.

[0045] [First intermediate cold rolling] The cold rolling applied to the material after the first solution treatment is called the first cold rolling. The purpose of the first cold rolling is to reduce the plate thickness as well as to introduce strain. If the introduction of strain is insufficient, the nucleation sites for recrystallization cannot be sufficiently secured in the subsequent second solution treatment, making it difficult to refine the crystal grains. In the first intermediate cold rolling, the rolling reduction is 70% or more. It is more effective to set the rolling reduction to 85% or more, and even more effective to set it to 90% or more. There is no particular upper limit to the rolling reduction, but it is usually set to 99% or less depending on the capacity of the cold rolling mill.

[0046] [Second solution treatment] In the material that has undergone the first intermediate cold rolling, the precipitates have already been sufficiently dissolved, and strain has been introduced into the crystals of the matrix (metallic base). The sheet material in this structure is then subjected to a second solution treatment. In this solution treatment, the strain introduced in the first intermediate cold rolling is used to cause new recrystallization from many places, resulting in finer grains. Since the main purpose is not to dissolve the precipitates, but to refine the grains by recrystallization, the allowable upper limit of the heating temperature is lower than that of the first solution treatment. Specifically, the temperature is held in the range of 750 to 860°C for 10 to 300 seconds. If the heating temperature is too high, grain growth accompanied by grain boundary movement between recrystallized grains is likely to occur, and the grains may become coarse. If the heating temperature is too low, precipitation is likely to occur instead of recrystallization, making it difficult to generate sufficient fine precipitates in the aging treatment described below.

[0047] [Second intermediate cold rolling] The cold rolling applied to the material after the second solution treatment is called the second intermediate cold rolling. In the second intermediate cold rolling, an appropriate amount of strain is introduced so that the formation of fine precipitates in the crystal grains is promoted in the subsequent aging treatment. This strain also contributes to improving the strength. If too much strain is introduced, excessive strain remains after the aging treatment, and the final improvement in bending workability and spring limit value tends to be insufficient. In the second intermediate cold rolling, the rolling reduction is in the range of 15 to 50%. It may also be controlled in the range of 15 to 35%.

[0048] [Aging process] The material that has undergone the second intermediate cold rolling is subjected to aging treatment that specifies the conditions of the heating and cooling processes. In the heating and holding process, the maximum temperature T0 (℃) is set to 320℃ or higher and 450℃ or lower, and the temperature is held in the holding temperature range of [T0-10℃] or higher and T0 or lower for 5 to 20 hours. The start point of the holding is the point at which [T0-10℃] is first reached, and the end point is the point at which the temperature range from [T0-10℃] or higher to [T0-10℃] or lower is first entered into a temperature range lower than [T0-10℃]. In the heating and holding process, the energy of the strain introduced in the second intermediate cold rolling is used to generate fine precipitates from many sites within the crystal grains, improving strength, electrical conductivity, and fatigue properties. If the maximum temperature T0 is too high, the size of the fine precipitates increases and the number density decreases, which tends to result in insufficient improvements in strength, bending workability, and fatigue properties. If the maximum attainable temperature T0 is too low, or if the holding time in the above-mentioned holding temperature range is too short, the amount of precipitates generated will be insufficient, and the improvement in strength and electrical conductivity will tend to be insufficient.

[0049] In the cooling process of the aging treatment, in the temperature range from the above-mentioned holding temperature range to 300°C, excessive growth of precipitate particles generated in the above-mentioned holding temperature range is suppressed, new precipitates are generated with the temperature drop, and residual stress is reduced. It is effective to set the residence time in the temperature range up to 300°C as short as possible within a range in which the amount of new precipitates generated during the temperature drop can be sufficiently secured. Specifically, it is effective to control the average cooling rate in the temperature range from [T0-10°C] to 300°C (hereinafter, this temperature range may be referred to as the "first cooling temperature range") to 30 to 60°C / h. If the average cooling rate in the first cooling temperature range is too fast, the progress of the precipitation reaction accompanying the temperature drop may be insufficient, resulting in insufficient improvement in electrical conductivity. In addition, the reduction of residual stress may be insufficient, resulting in insufficient improvement in spring limit value. If the average cooling rate in the first cooling temperature range is too slow, coarse precipitates may increase, resulting in deterioration of fatigue properties.

[0050] In the cooling process of the aging treatment, in the temperature range of 300°C or less, the residual stress is reduced. Therefore, it is effective to make the residence time in the temperature range of 300°C or less long within the range that allows productivity. Specifically, it is effective to control the average cooling rate in the temperature range from 300°C to 150°C (hereinafter, this temperature range may be referred to as the "second cooling temperature range") to 20°C / h or less. If the average cooling rate in the second cooling temperature range is too fast, the reduction of the residual stress may be insufficient and the improvement of the spring limit value may be insufficient. Since an excessively slow average cooling rate in the second cooling temperature range leads to a decrease in productivity, the average cooling rate in the second cooling temperature range may usually be set to a range of 10°C / h or more.

[0051] If cold rolling or annealing is performed after the above-mentioned aging treatment, the structure formed by the aging treatment may be damaged, and good strength, bending workability, electrical conductivity, fatigue properties, and spring limit value may not be achieved at the same time. Therefore, it is desirable to make the above-mentioned aging treatment the final step among the steps involving processing and thermal history in the manufacturing process of the copper alloy sheet material. The final plate thickness may be in the range of 0.02 to 0.50 mm, for example.

[0052] [Electronic device parts, current-carrying parts, heat-dissipating parts] The copper alloy sheet material of the present invention described above has good strength, bending workability, electrical conductivity, fatigue properties, and spring limit value, and also has a reduced density (specific gravity). Therefore, electronic device parts, current-carrying parts, and heat-dissipating parts formed by processes including press working and bending using this sheet material as a material meet the demands for high functionality of recent mobile terminals and electronic devices for automobiles. EXAMPLES

[0053] Copper alloys having the chemical compositions shown in Table 1 were melted and cast. The resulting slabs (thickness: 50 mm) were heated at the temperatures and times shown in Tables 2 and 3, and then hot rolled to the thicknesses shown in Tables 2 and 3, and water-cooled. After hot rolling, the oxide layer on the surface was removed by mechanical polishing (face grinding), and each hot-rolled material was cold rolled to the thicknesses shown in the "Rough cold rolling" column in Tables 2 and 3.

[0054] Thereafter, except for some examples (comparative examples No. 57 to 61), the first solution treatment, the first intermediate cold rolling, the second solution treatment, the second intermediate cold rolling, and the aging treatment were performed in the above order under the conditions shown in Tables 2 and 3. The aging treatment was performed in a nitrogen atmosphere using a batch-type heat treatment furnace. The "-" (hyphen) mark in Tables 2 and 3 means that a process was omitted. In No. 57, after rough cold rolling, straightening was performed with a tension leveler at a heating rate of 20°C / s, an ultimate temperature of 200°C, and a tension of 120 MPa, and then cold rolling and solution treatment were performed, and cold rolling before the aging treatment was omitted. In No. 58, the second intermediate cold rolling was omitted. In Nos. 59 and 60, intermediate cold rolling was not performed, and the material that had been solution treated once was subjected to the aging treatment. In No. 61, the second solution treatment and the second intermediate cold rolling were omitted.

[0055] Aging treatment was performed in a nitrogen atmosphere using a batch-type heat treatment furnace. After heating, the maximum temperature T0 (℃) listed in Tables 2 and 3 was maintained, and then cooling was started. In other words, after reaching the maximum temperature T0, the temperature was controlled to a constant temperature until cooling was started. The "time" listed in the "Heating retention" column of Tables 2 and 3 is the time during which the material temperature was maintained in the temperature range of [T0-10℃] or more and T0 or less. Here, the temperature was maintained at a constant temperature T0 until cooling was started, so the "time" listed in the "Heating retention" column of Tables 2 and 3 includes the time required to reach T0 from [T0-10℃] before the end of heating, and the time required to reach T0 from T0 after cooling was started. In the cooling process, the average cooling rate in the first cooling temperature range from [T0-10℃] to 300℃ and the average cooling rate in the second cooling temperature range from 300℃ to 150℃ were controlled as listed in Tables 2 and 3.

[0056] With the exception of some examples (Comparative Examples Nos. 56 to 61), the test materials were sheets that had been subjected to the above-mentioned aging treatment. For Nos. 56 to 61, the test materials were sheets that had been subjected to finish cold rolling or further low-temperature annealing under the conditions shown in Table 3 after the aging treatment. Tables 2 and 3 show the thickness of the final sheet material (test material). The following investigations were carried out for each test material. The density (specific gravity) was measured using a block sample cut out from the material at the stage when the slab heating was completed.

[0057] (Elemental analysis) O (oxygen) and N (nitrogen) were quantified using an oxygen / nitrogen / hydrogen analyzer (LECO, ONH-836), H (hydrogen) was quantified using a hydrogen analyzer (HORIBA, EMGA-921), C (carbon) and S (sulfur) were quantified using a carbon-sulfur analyzer (LECO, CS844), elements in the second to sixth periods (excluding C, N, O, group 17 elements, group 18 elements, Tc (technetium), Po (polonium), and Pm (promethium)) were quantified using an ICP-MS (Agilent, 7900), and F (fluorine), Cl (chlorine), and Br (bromine) were quantified using a combustion-ion chromatography apparatus (Thermo Scientific, DIONEX ICS-1600). These measurements allow the quantification of virtually all elements that may be contained in the copper alloy sheet material. As a result, it was confirmed that both the test materials of the present invention and the comparative examples met the requirements of a total of Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr and rare earth elements of 3.00% or less, and a total of elements other than Ti, Al, Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr, rare earth elements, and Cu of 0 to 0.50%. In all examples, the total content of elements other than Ti, Al, Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr, rare earth elements, and Cu was 0.10% or less.

[0058] (Average grain size) The plate surface of the test material was polished, and the surface finished by electrolytic polishing was etched using the electrolytic polishing conditions described in the above-mentioned "Method of determining the number density of coarse precipitate particles" to prepare an observation surface. The observation surface was observed with an optical microscope at a magnification of 1000 times, and an observation image was obtained. A total of three straight lines parallel to the rolling direction were drawn, and the number of grain boundaries cut by each straight line was counted using a cutting method in accordance with JIS H0501-1986, to calculate the average grain size in the observation field. This operation was performed on five randomly selected fields, and the arithmetic mean value of the average grain size values ​​obtained in each field was adopted as the average grain size of the plate material. The optical microscope used was a LEXT OLS4000 manufactured by OLYMPUS Corporation.

[0059] (Number density of coarse precipitate particles) The number density of the coarse precipitate particles was determined according to the above-mentioned "Method for determining the number density of coarse precipitate particles".

[0060] The image analysis software used to measure the major axis of the precipitate particles was Image J (National Institutes of Health (NIH), Version 1.52a). The analysis conditions for this software were as follows: select Analyze, then Set Scale, and on the "Set Scale" screen that appears, measure the number of pixels of the scale bar length of the captured FE-SEM image and enter it in Distance in pixels. Next, enter the length of the scale bar (μm) in Known distance, set Pixel aspect ratio to 1.0, and Unit of length to μm, so that the size of the precipitates can be recognized on the software. After that, on the "Resize Image Canvas" screen, set Width to 1280 pixels, Height to 950 pixels, and Position to Top-Center, and display the image of the FE-SEM image portion excluding the scale bar portion. After setting this scale and deleting the scale bar display portion, the brightness was inverted on the "Threshold" screen, which can be displayed by successively selecting Image, Adjust, and Threshold, so that the lowest brightness pixel among all pixels had a brightness of 255 and the highest brightness pixel had a brightness of 0, and the threshold was set to a value that would make the proportion of pixels below that value closest to 5% of all pixels, thereby binarizing and identifying the areas where precipitate particles exist. After that, on the "Analyze Particles" screen of the same software, the area of ​​one independent precipitate region was set to 0.1 μm 2 To exclude particles with a major axis of 1.0 μm or more, Size was set to "0.10-Infinity." Furthermore, Circularity was set to 0.00-1.00, and the Fit Ellipse item was checked on the Set Measurements screen. Particle analysis was performed, and the number density of precipitate particles with a major axis (displayed as the Major item name) of 1.0 μm or more in the field of view was calculated.

[0061] (KAM value) The plate surface of the sample cut from the test material was buffed and then ion milled to prepare the sample surface for EBSD (electron backscatter diffraction) measurement. The sample surface was observed with an FE-SEM (JSM-7200F manufactured by JEOL Ltd.) at an acceleration voltage of 15 kV and a magnification of 2000 times, and crystal orientation data was collected with a step size of 0.1 μm by the EBSD method using an EBSD device (Symmetry manufactured by Oxford Instruments) installed in the FE-SEM for a rectangular measurement area of ​​45 μm in the direction perpendicular to the rolling direction × 60 μm in the rolling direction. Based on the crystal orientation data measured for the measurement area of ​​5 fields of view, the KAM value was calculated according to the above-mentioned "How to calculate the KAM value". OIM-Analysis 7.3.1 manufactured by TSL Solutions Co., Ltd. was used as the software for EBSD data analysis.

[0062] (Spring limit value) A test piece cut from the test material with its longitudinal direction perpendicular to the rolling direction (TD) was used to carry out a moment test for alloy number C1990 described in JIS H3130:2018 to determine the spring limit value.

[0063] (Tensile strength) Tensile test pieces (JIS No. 5) were taken from each test material in the rolling direction (TD), and tensile tests were performed according to JIS Z2241 with the number of tests being n = 3 to measure the tensile strength. The average value of n = 3 was used as the performance value of the test material.

[0064] (conductivity) The electrical conductivity of each test material was measured by the double bridge average cross-sectional area method in accordance with JIS H0505.

[0065] (MBR / t for 90°W bend) The ratio MBR / t of the minimum bending radius MBR at which cracks do not occur to the plate thickness t was determined by a BW W-bend test according to the Japan Copper and Brass Association technical standard JCBA T307:2007. The test piece size was 30 mm in the direction perpendicular to the rolling direction and 10 mm in the rolling direction. A bending test in which the bending radius was changed stepwise was performed for one bending radius with n=3 tests, and the minimum bending radius at which cracks were not observed on the bent surface in all three test pieces was determined as the MBR for that test material. The presence or absence of cracks on the bent surface was determined according to JCBA T307:2007. For samples that were judged to have "large wrinkles" in the appearance observation of the bent surface, a specimen was prepared by cutting the deepest wrinkled part perpendicular to the bending axis direction, and the polished cross section was observed with an optical microscope to check whether cracks had occurred that progressed into the plate thickness. If no such cracks occurred, it was judged to have "no cracks observed."

[0066] (Fatigue limit) A test piece 3 mm wide and 20 mm long, with the width direction being the rolling direction (LD) and the length direction being the direction perpendicular to the rolling direction (TD), was cut out from the test material, and a reversed-swing fatigue test was performed using a cantilever resonance method with a fatigue testing device (Nippon Technoplus Co., Ltd., RF-RT) at a load stress of 450 MPa. The change in the resonance frequency was monitored during the test, and the number of cycles at which the resonance frequency reached 98% of the initial value was taken as the fatigue limit of the test piece. This operation was performed on five test pieces made from one test material, and the average value of the fatigue limits was adopted as the fatigue limit of the test material.

[0067] (density) A block sample having a mass of 10 g was cut out from the material after the heating of the slab, and the density at room temperature (20°C) was measured by the Archimedes method (underwater gravimetry). The above results are shown in Tables 4 and 5.

[0068] [Table 1]

[0069] [Table 2]

[0070] [Table 3]

[0071] [Table 4]

[0072] [Table 5]

[0073] All of the plate materials of the present invention, whose chemical composition and manufacturing conditions were strictly controlled in accordance with the above-mentioned regulations, had high levels of strength, bending workability, electrical conductivity, fatigue properties, and spring limit value, and also had an excellent density (specific gravity) reduction effect.

[0074] In contrast, the comparative examples gave the following results: In No. 41, the Al content was insufficient, so the density (specific gravity) was not reduced sufficiently. Also, the remaining coarse precipitates were not eliminated sufficiently, so the fatigue properties were poor. No. 42 had poor conductivity because the Al content was too high. No. 43 had an insufficient Ti content, so the strength was low and the reduction in density (specific gravity) was also insufficient. No. 44 had poor bending workability because the Ti content was too high. In No. 45, the temperature of the first solution treatment was low, which is thought to have resulted in insufficient solid solution of the precipitated phase and insufficient precipitation of fine precipitates during aging treatment, resulting in low strength. In addition, the number of coarse precipitates increased, resulting in poor fatigue properties. In No. 46, the temperature of the first solution treatment was too high, causing the crystal grains to become coarse, and the crystal grains could not be sufficiently refined in the second solution treatment, resulting in poor fatigue properties and bending workability. In No. 47, the reduction ratio in the first intermediate cold rolling was too low, resulting in insufficient strain introduction, and in the subsequent second solution treatment, the growth of the crystal grains became uneven, leading to the phenomenon in which larger crystal grains absorbed smaller ones, making it impossible to refine the crystal grains. As a result, the bending workability and fatigue properties were poor. In No. 48, the reduction ratio of the second intermediate cold rolling was too low, so the introduction of strain was insufficient, and the subsequent aging treatment led to insufficient formation of fine precipitates within the crystal grains, resulting in low strength. Also, the aging treatment promoted the progression of precipitation at the crystal grain boundaries due to the lack of strain, resulting in an increase in coarse precipitates, resulting in poor fatigue properties. In No. 49, the reduction ratio in the second intermediate cold rolling was too high, which resulted in the introduction of a lot of strain, resulting in a structure with a high KAM value and a low spring limit value. In No. 50, the heating temperature during aging treatment was low, which resulted in insufficient precipitation and low strength and electrical conductivity. In No. 51, it is believed that the heating temperature during aging treatment was too high, which resulted in little formation of fine precipitates, and therefore low strength. In No. 52, the cooling rate in the first cooling temperature range in the aging treatment was too slow, which resulted in the formation of a large amount of coarse precipitates during the cooling process, resulting in poor fatigue properties. For No. 53, the cooling rate in the first cooling temperature range during aging treatment was too high, so the progress of precipitation during the cooling process was insufficient, resulting in poor electrical conductivity. Also, the removal of residual stress in the first cooling temperature range was insufficient, resulting in a low spring limit value. For No. 54, the cooling rate in the second cooling temperature range during the aging treatment was too slow, so the residual stress was not sufficiently removed during the cooling process, and the spring limit value was low. No. 55 did not contain any aluminum, so the density (specific gravity) was not reduced sufficiently. Also, the remaining coarse precipitates were not eliminated sufficiently, so the fatigue properties were poor. No. 56 was cold-rolled after aging treatment, and therefore the processing strain could not be sufficiently removed even after low-temperature annealing, resulting in a structure with a high KAM value and a low spring limit value. No. 57 had no added aluminum, so the density (specific gravity) was not reduced sufficiently. The first solution treatment was not performed, so the grain size was large, and the fatigue properties were poor. Cold rolling was not performed between the solution treatment and the aging treatment, so it is believed that the generation of fine precipitates during the aging treatment was insufficient, and the strength was low. Because the strength was low, the bending workability was relatively good. Since the material had been straightened using a tension leveler, it is believed that the tensile residual stress increased, and the spring limit value was low. No. 58 was cold-rolled after aging treatment, but by performing a second solution treatment and omitting the second intermediate cold rolling, the increase in KAM value was suppressed and the spring limit value was increased. However, since no Al was added, the density (specific gravity) was not reduced sufficiently and the remaining coarse precipitates could not be fully eliminated, resulting in poor fatigue properties. No. 59 had poor fatigue properties because it did not contain any aluminum and the density (specific gravity) was not reduced sufficiently and the remaining coarse precipitates were not eliminated sufficiently. The cold rolling was performed after aging treatment, resulting in a structure with a high KAM value and a low spring limit value. No. 60 had poor fatigue properties because no Al was added and the density (specific gravity) was not sufficiently reduced and the remaining coarse precipitates were not sufficiently eliminated. In No. 61, the Al content was insufficient, so the density (specific gravity) was not reduced sufficiently. In addition, the Al content was low, and the heating temperature during the aging treatment was high, and the cooling rate in the first cooling temperature range was low, which resulted in a large number of coarse precipitates and poor fatigue properties.

Claims

1. In mass percent, Ti: 1.00-5.00%, Al: 0.50-3.00%, Ag: 0-0.30%, B: 0-0.30%, Co: 0-1.00%, Cr: 0-1.00%, Fe: 0-1.00%, Mg: 0-1.00%, Mn: 0-2.00%, Nb: 0-1.00%, Ni: 0-1.00%, P: 0-0.50%, S: 0-0.20%, Si: 0-0.50%, Sn: 0-2.00%, V: 0-1.00%, Zn: 0-3.00%, Zr: 0-1.00%, rare earth elements. The composition is as follows: total: 0 to 3.00%, total of Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr and rare earth elements: 3.00% or less, total of elements other than Ti, Al, Ag, B, Co, Cr, Fe, Mg, Mn, Nb, Ni, P, S, Si, Sn, V, Zn, Zr, rare earth elements, and Cu: 0 to 0.50%, and balance Cu. The composition is such that the content ratio of Ti to Al by mass, Ti / Al, is 1.50 or more, the average crystal grain size in a plane observed parallel to the plate surface is 1 to 20 μm according to a cutting method in accordance with JIS H0501-1986, and the number density of coarse precipitate particles having a major axis of 1.0 μm or more in a plane observed parallel to the plate surface is 1.0×10 5 pieces / mm 2 The copper alloy sheet material has a tensile strength of 850 MPa or more in a direction parallel to the rolling direction and a spring limit value of 400 MPa or more in a direction perpendicular to the rolling direction.

2. The copper alloy sheet material according to claim 1, wherein the Nb content is 0 to 0.50 mass%.

3. 2. The copper alloy sheet according to claim 1, wherein the KAM value is 3.00° or less when a boundary having a crystal orientation difference of 15° or more is regarded as a grain boundary in a measurement of an observation surface parallel to the sheet surface by EBSD (electron backscatter diffraction) with a step size of 0.1 μm.

4. 2. The copper alloy sheet material according to claim 1, having an electrical conductivity of 10.0% IACS or more.

5. 2. The copper alloy sheet material according to claim 1, wherein a ratio MBR / t of a minimum bending radius MBR at which cracks do not occur to a sheet thickness t in a B.W. W-bending test according to Japan Copper and Brass Association technical standard JCBA T307:2007 is 2.0 or less.

6. In a reverse fatigue test using a cantilever resonance method with a test piece whose longitudinal direction is perpendicular to the rolling direction, the fatigue limit at a load stress of 450 MPa was 10 7 The copper alloy sheet material according to claim 1, wherein the copper alloy sheet material has a temperature of 1000° C. or more than 1000° C.

7. Density is 8.53 g / cm 3 The copper alloy sheet material according to claim 1, wherein:

8. An electronic device part using the copper alloy sheet material according to any one of claims 1 to 7 as a material.

9. An electric current-carrying part using the copper alloy sheet material according to any one of claims 1 to 7 as a material.

10. A heat dissipation part using the copper alloy sheet material according to any one of claims 1 to 7 as a material.

Citation Information

Patent Citations

  • JP1975110927A

  • Titanium-copper

    JP2007254803A

  • Copper alloy sheet, and method for producing the same

    JP2010126777A

  • Copper alloy sheet and method for manufacturing the same, and electric and electronic component

    JP2011026635A

  • Cu-Ti-BASED COPPER ALLOY PLATE, MANUFACTURING METHOD THEREFOR AND ELECTRIC CONDUCTION PARTS

    JP2014185370A