Laminate, polarizing plate, and image display device

A laminate of two optically anisotropic layers with specific properties addresses light leakage and display unevenness in IPS type liquid crystal displays, ensuring reduced thickness and stability, thereby enhancing display quality.

JP2024144161APending Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024026170
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-02-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing polarizing plates in IPS type liquid crystal displays suffer from light leakage and display unevenness when viewed from oblique directions, and there is a need for thinner retardation films that maintain stability under varying environmental conditions.

Method used

A laminate comprising two optically anisotropic layers, each with specific retardation value ratios and thicknesses, is used to form a polarizing plate that reduces light leakage and color shift when viewed from oblique directions, while maintaining thinness and stability under heat.

Benefits of technology

The laminate effectively minimizes light leakage and color shift in liquid crystal displays, even under varying conditions, by optimizing the combination of optically anisotropic layers with controlled retardation values and thicknesses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144161000001_ABST
    Figure 2024144161000001_ABST
Patent Text Reader

Abstract

To provide a laminate which is thinned down and whose characteristics change due to heat is small, a polarizing plate including the laminate, and an image display device having these.SOLUTION: Provided is a laminate that includes an optical anisotropic layer X satisfying formula (1) and an optical anisotropic layer Y satisfying formula (2), and that satisfies formula (3). Formula (1): 0.960≤A≤1.040; formula (2): 0.960≤B≤1.040; formula (3): -1.20≤D / C≤0.60. [In formulas (1) to (3), A represents the ratio of the in-plane phase difference value in wavelength 450 nm to the in-plane phase difference value in wavelength 550 nm of the optical anisotropic layer X, B represents the ratio of the phase difference value in the thickness direction in wavelength 450 nm to the phase difference value in the thickness direction in wavelength 550 nm of the optical anisotropic layer Y, C represents the in-plane phase difference value in wavelength 550 nm of the optical anisotropic layer X, and D represents the phase difference value in the thickness direction in wavelength 550 nm of the optical anisotropic layer Y.]SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate including two types of optically anisotropic layers, and a polarizing plate and an image display including the laminate. [Background technology]

[0002] It is generally known that ion plane switching (IPS) liquid crystal display devices have a large amount of light leakage in black display, and are prone to contrast reduction and color shift when viewed from an oblique direction at an angle of 45 degrees to the absorption axis of the polarizer. This phenomenon occurs because the angle between the absorption axes of the polarizers arranged on the front and back sides of the liquid crystal cell does not appear to be 90 degrees.

[0003] In order to reduce the light leakage when viewed from an oblique direction, a method of disposing a retardation film between a liquid crystal cell and a polarizer has been proposed. For example, Patent Document 1 describes a method of reducing the light leakage of an IPS liquid crystal display device by disposing a stretched retardation film having a refractive index anisotropy of nx>ny>nz and a stretched retardation film having a refractive index anisotropy of nz>nx>ny. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-139747 A Summary of the Invention [Problem to be solved by the invention]

[0005] The polarizing plate in which a polarizer and a retardation film are laminated, as described in Patent Document 1, is preferably used to reduce light leakage from an IPS type liquid crystal display device, but in a liquid crystal display device having this configuration, display unevenness may be observed when the screen is viewed from an oblique direction. In addition, with the weight reduction of image display devices and the harsher usage environments, there is a demand for thinner retardation films and further suppression of changes in characteristics due to heat.

[0006] The present invention aims to provide a novel solution to the above problems, that is, a laminate combining two types of optically anisotropic layers. Another aim of the present invention is to provide a laminate that is thin and has small changes in properties due to heat, a polarizing plate including the laminate, and an image display device having the laminate and the polarizing plate. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. [1] An optically anisotropic layer X that satisfies the following formula (1) and an optically anisotropic layer Y that satisfies the following formula (2), A laminate satisfying the following formula (3): 0.960≦ A ≦1.040 (1) 0.960≦ B ≦1.040 (2) -1.20≦ D / C ≦0.60 (3) [In formula (1), A represents the ratio (Re(450) / Re(550)) of the in-plane retardation value (Re(450)) of the optically anisotropic layer X at a wavelength of 450 nm to the in-plane retardation value (Re(550)) of the optically anisotropic layer X at a wavelength of 550 nm. In formula (2), B represents the ratio (Rth(450) / Rth(550)) of the thickness direction retardation value (Rth(450)) of the optically anisotropic layer Y at a wavelength of 450 nm to the thickness direction retardation value (Rth(550)) of the optically anisotropic layer Y at a wavelength of 550 nm. In formula (3), C represents the in-plane retardation value (Re(550)) of the optically anisotropic layer X at a wavelength of 550 nm, and D represents the thickness direction retardation value (Rth(550)) of the optically anisotropic layer Y at a wavelength of 550 nm.] [2] The laminate according to [1] above, wherein the optically anisotropic layer X has a thickness of 0.5 μm or more and 5 μm or less. [3] The laminate according to [1] above, wherein the optically anisotropic layer Y has a thickness of 0.3 μm or more and 5 μm or less. [4] A polarizing plate comprising a polarizing film, the optically anisotropic layer X described in [1] above, and the optically anisotropic layer Y described in [1] above, in this order. [5] A polarizing plate comprising a polarizing film, the optically anisotropic layer Y described in [1] above, and the optically anisotropic layer X described in [1] above, in this order. [6] The polarizing plate according to [4] above, wherein the angle between the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X is 90±5°. [7] The polarizing plate according to [5] above, wherein the angle between the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X is 0±5°. [8] An image display device comprising the polarizing plate according to any one of the above items [4] to [7]. Effect of the Invention

[0008] According to the present invention, it is possible to provide a laminate which is thin and exhibits little change in characteristics due to heat, a polarizing plate including the laminate, and an image display device having these. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of a laminate of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of a polarizing plate of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of a polarizing plate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The laminate of the present invention includes an optically anisotropic layer X (hereinafter also simply referred to as "optically anisotropic layer X") that satisfies the following formula (1), and an optically anisotropic layer Y (hereinafter also simply referred to as "optically anisotropic layer Y") that satisfies the following formula (2), and satisfies the following formula (3). Hereinafter, an example of the layer structure of the laminate of the present invention will be described with reference to Fig. 1, and an example of the layer structure of the polarizing plate of the present invention will be described with reference to Figs. 2 and 3, but the present invention is not limited to these embodiments.

[0011] The laminate 10 shown in Fig. 1 comprises an optically anisotropic layer X (layer 1 in Fig. 1) and an optically anisotropic layer Y (layer 2 in Fig. 1). In the laminate 10 shown in Fig. 1, the optically anisotropic layer X satisfies the following formula (1), the optically anisotropic layer Y satisfies the following formula (2), and further the laminate 10 satisfies the following formula (3). 0.960≦ A ≦1.040 (1) 0.960≦ B ≦1.040 (2) -1.20≦ D / C ≦0.60 (3) [In formula (1), A represents the ratio (Re(450) / Re(550)) of the in-plane retardation value (Re(450)) of the optically anisotropic layer X at a wavelength of 450 nm to the in-plane retardation value (Re(550)) of the optically anisotropic layer X at a wavelength of 550 nm. In formula (2), B represents the ratio (Rth(450) / Rth(550)) of the thickness direction retardation value (Rth(450)) of the optically anisotropic layer Y at a wavelength of 450 nm to the thickness direction retardation value (Rth(550)) of the optically anisotropic layer Y at a wavelength of 550 nm. In formula (3), C represents the in-plane retardation value (Re(550)) of the optically anisotropic layer X at a wavelength of 550 nm, and D represents the thickness direction retardation value (Rth(550)) of the optically anisotropic layer Y at a wavelength of 550 nm.]

[0012] In the present invention, the in-plane retardation value (Re(λ)) of the optically anisotropic layer X at a wavelength of λ nm is calculated by the formula: Re(λ)=(nx(λ)-ny(λ))×d1, where nx(λ) represents the principal refractive index at a wavelength of λ nm in the plane of the optically anisotropic layer X, ny(λ) represents the refractive index at a wavelength of λ nm in the same plane as nx and in a direction perpendicular to the direction of nx, and d1 represents the thickness of the optically anisotropic layer X.

[0013] When the optically anisotropic layer X satisfies formula (1), the optically anisotropic layer X exhibits a characteristic in which the in-plane retardation value at a short wavelength and the in-plane retardation value at a long wavelength are almost equal. By combining such an optically anisotropic layer X with the optically anisotropic layer Y described later, when incorporated in a liquid crystal display device, a laminate having excellent effects of preventing light leakage and color shift when viewed from an oblique direction during black display can be obtained. In addition, in formula (1), the value of A is preferably 0.970 or more, more preferably 0.975 or more, and preferably 1.030 or less, more preferably 1.025 or less. If the value of A is within the above range, a laminate having excellent effects of preventing light leakage and color shift when the liquid crystal display device is viewed from an oblique direction during black display can be obtained.

[0014] The in-plane retardation value can be adjusted by the thickness (d1) of the optically anisotropic layer X. Since the in-plane retardation value is determined by the formula Re(λ)=(nx(λ)-ny(λ))×d1, a desired in-plane retardation value can be obtained by adjusting the three-dimensional refractive index and the film thickness (d1). The three-dimensional refractive index depends on the molecular structure and orientation state of the compound constituting the optically anisotropic layer X.

[0015] In addition, it is preferable that the optically anisotropic layer X satisfies the following formula (4). 100nm≦Re(550)≦160nm (4) [In formula (4), Re(λ) has the same meaning as above.] When the in-plane retardation value (Re(550)) of the optically anisotropic layer X is within the range of formula (4), the effect of preventing light leakage and color shift when viewed from an oblique direction during black display when a laminate including the optically anisotropic layer X or a polarizing plate including the laminate is applied to a liquid crystal display device is remarkable. A more preferable range of the in-plane retardation value (Re(550)) is 110 nm≦Re(550)≦150 nm.

[0016] In the present invention, the retardation value (Rth(λ)) in the thickness direction of the optically anisotropic layer Y at a wavelength of λ nm is calculated by the formula: Rth(λ)=((nx(λ)+ny(λ)) / 2-nz(λ))×d2. In the formula, nx(λ) represents the in-plane principal refractive index of the optically anisotropic layer Y at a wavelength of λ nm, ny(λ) represents the refractive index in the direction perpendicular to nx(λ) at a wavelength of λ nm, nz(λ) represents the refractive index in the thickness direction of the optically anisotropic layer Y at a wavelength of λ nm, and when nx(λ)=ny(λ), nx(λ) can be the refractive index in any direction in the plane of the optically anisotropic layer Y, and d2 represents the thickness of the optically anisotropic layer Y.

[0017] When the optically anisotropic layer Y satisfies formula (2), the optically anisotropic layer Y exhibits a characteristic in which the retardation value in the thickness direction at a short wavelength and the retardation value in the thickness direction at a long wavelength are almost equal. By combining such an optically anisotropic layer Y with the optically anisotropic layer X, a laminate having excellent effects of preventing light leakage and color shift when viewed from an oblique direction in black display can be obtained when incorporated in a liquid crystal display device. In addition, in formula (2), the value of B is preferably 0.970 or more, more preferably 0.975 or more, and preferably 1.030 or less, more preferably 1.025 or less. If the value of B is within the above range, a laminate having excellent effects of preventing light leakage and color shift when the liquid crystal display device is viewed from an oblique direction in black display can be obtained.

[0018] The thickness direction retardation value can be adjusted by the thickness (d2) of the optically anisotropic layer Y. The thickness direction retardation value is determined by the formula: Rth(λ)=((nx(λ)+ny(λ)) / 2-nz(λ))×d2, so that the desired thickness direction retardation value (Rth(λ)) can be obtained by adjusting the three-dimensional refractive index and the film thickness (d2). The three-dimensional refractive index depends on the molecular structure and the orientation state of the compound constituting the optically anisotropic layer Y.

[0019] Moreover, the optically anisotropic layer Y preferably satisfies the following formula (5), which is an index showing the degree of the effect of preventing light leakage and color shift when viewed from an oblique direction during black display. -120nm≦Rth(550)≦60nm (5) [In formula (5), Rth(550) has the same meaning as above.] From the viewpoint of further suppressing light leakage and color shift when viewed from an oblique direction during black display, the retardation value (Rth(550)) in the thickness direction of the optically anisotropic layer Y is more preferably -115 nm or more, even more preferably -110 nm or more, and more preferably 55 nm or less, even more preferably 50 nm or less.

[0020] In the present invention, a laminate including an optically anisotropic layer X satisfying the above formula (1) and an optically anisotropic layer Y satisfying the above formula (2) further satisfies the following formula (3). -1.20≦ D / C ≦0.60 (3) [In formula (3), C represents the in-plane retardation value (Re(550)) of the optically anisotropic layer X at a wavelength of 550 nm, and D represents the retardation value (Rth(550)) in the thickness direction of the optically anisotropic layer Y at a wavelength of 550 nm.]

[0021] The inventors have found through their research that when the laminate satisfies formula (3), in the case where the laminate is incorporated into a liquid crystal display device, the effect of preventing light leakage and color shift when viewed from an oblique direction during black display is remarkable.

[0022] In the formula (3), from the viewpoint of the effect of preventing light leakage and color shift when the laminate of the present invention is incorporated into a liquid crystal display device and viewed from an oblique direction during black display, the value of D / C is preferably -1.18 or more, more preferably -1.15 or more, particularly preferably -1.10 or more, and preferably 0.58 or less, more preferably 0.56 or less, particularly preferably 0.54 or less. If the value of D / C is within the above range, it is possible to obtain a laminate that is more effective in preventing light leakage and color shift when the liquid crystal display device is viewed from an oblique direction during black display.

[0023] Each component of the laminate of the present invention will be described in detail below. [Optical anisotropic layer X] The optically anisotropic layer X constituting the laminate of the present invention may be, for example, a stretched film or a cured layer of a polymerizable liquid crystal composition in which a polymerizable liquid crystal compound is cured in a state where the compound is aligned horizontally to the film plane.

[0024] Examples of stretched films include uniaxially stretched polycarbonate (PC) films, uniaxially stretched triacetyl cellulose (TAC) films, and uniaxially stretched cycloolefin polymer (COP) films. The in-plane retardation values ​​of these stretched films can be adjusted by controlling the composition of the resin constituting the stretched film, the stretching method, and the thickness of the stretched film.

[0025] The cured layer of the polymerizable liquid crystal composition in which the polymerizable liquid crystal compound is cured in a state where it is aligned in the horizontal direction relative to the film plane can be formed using nematic liquid crystal or discotic liquid crystal. The in-plane retardation value of the cured layer of the polymerizable liquid crystal composition can be adjusted by controlling the type of the polymerizable liquid crystal compound, the alignment state of the cured layer of the polymerizable liquid crystal compound, and the thickness of the cured layer.

[0026] The thickness of the optically anisotropic layer X is preferably 0.5 μm or more and 5 μm or less, more preferably 0.6 μm or more and 4.5 μm or less, and even more preferably 0.7 μm or more and 4 μm or less. Since a thinner thickness is preferable, as described below, the optically anisotropic layer X is preferably a cured product of a polymerizable liquid crystal composition in which a polymerizable liquid crystal compound is cured in a state where it is aligned in the horizontal direction relative to the film plane (hereinafter, also referred to as a "horizontally aligned liquid crystal cured film"), and more preferably a liquid crystal cured film in which a polymerizable liquid crystal compound having at least one radical polymerizable group is cured in a state where it is aligned horizontally relative to the in-plane direction of the cured film. By the optically anisotropic layer X being a horizontally aligned liquid crystal cured film having a thickness that satisfies the above range, it is possible to achieve a reduction in the weight of the image display device, and further, as described below, it is possible to obtain a laminate with small changes in characteristics due to heat.

[0027] In the present invention, the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition that forms the horizontally aligned liquid crystal cured film means a liquid crystal compound having a polymerizable group, and in particular, a polymerizable liquid crystal compound having at least one radically polymerizable group is preferred. The polymerizable group refers to a group that can participate in a polymerization reaction by an active radical or an acid generated from a polymerization initiator. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, a radical polymerizable group is preferable, an acryloyloxy group, a methacryloyloxy group, a vinyl group, and a vinyloxy group are more preferable, and an acryloyloxy group and a methacryloyloxy group are even more preferable.

[0028] The liquid crystallinity exhibited by the polymerizable liquid crystal compound may be thermotropic liquid crystal or lyotropic liquid crystal, but thermotropic liquid crystal is preferred in terms of enabling precise control of the film thickness.

[0029] The polymerizable liquid crystal compound generally includes a polymerizable liquid crystal compound exhibiting a positive wavelength dispersion and a polymerizable liquid crystal compound exhibiting a reverse wavelength dispersion, and either one type of polymerizable liquid crystal compound may be used alone, or both types of polymerizable liquid crystal compounds may be used in combination. From the viewpoint of preventing light leakage and color shift when viewed from an oblique direction during black display, it is preferable to adjust the composition of the optically anisotropic layer X so that it satisfies the above formula (1).

[0030] The polymerizable liquid crystal compound exhibiting reverse wavelength dispersion is preferably a compound having the following characteristics (A) to (D). (A) A compound capable of forming a nematic phase or a smectic phase. (B) The polymerizable liquid crystal compound has π electrons in the long axis direction (a). (C) It has π electrons in a direction intersecting with the long axis direction (a) [intersecting direction (b)]. (D) The total number of π electrons present in the long axis direction (a) is N(πa), and the total number of molecular weights present in the long axis direction is N(Aa), where N(πa) is the total number of π electrons present in the long axis direction, and N(Aa) is the total number of molecular weights present in the long axis direction. The π electron density in the long axis direction (a) of a polymerizable liquid crystal compound is defined by the following formula (i): D(πa)=N(πa) / N(Aa) (i) The total number of π electrons present in the cross direction (b) is N(πb), and the total number of molecular weights present in the cross direction (b) is N(Ab), where N(πb) is the total number of π electrons present in the cross direction (b), and the π electron density in the cross direction (b) of the polymerizable liquid crystal compound is defined by the following formula (ii): D(πb)=N(πb) / N(Ab) (ii) and the formula (iii) 0≦[D(πa) / D(πb)]<1 (iii) [That is, the π electron density in the intersecting direction (b) is greater than the π electron density in the long axis direction (a)]. As described above, the polymerizable liquid crystal compound having π electrons on the long axis and in the direction intersecting therewith has, for example, a T-shaped structure.

[0031] In the above features (A) to (D), the long axis direction (a) and the number of π electrons N are defined as follows. The long axis direction (a) is, for example, in the case of a compound having a rod-like structure, the long axis direction of the rod. The number of π electrons present in the long axis direction (a), N(πa), does not include the π electrons lost due to the polymerization reaction. The number of π electrons present along the long axis (a), N(πa), is the total number of π electrons on the long axis and those conjugated with it, and includes, for example, the number of π electrons present in rings present along the long axis (a) that satisfy Hückel's rule. The number of π electrons present in the intersecting direction (b), N(πb), does not include the π electrons lost due to the polymerization reaction. A polymerizable liquid crystal compound that satisfies the above conditions has a mesogenic structure in the long axis direction, and this mesogenic structure allows the compound to exhibit a liquid crystal phase (nematic phase, smectic phase).

[0032] A polymerizable liquid crystal compound satisfying the above (A) to (D) is applied onto a film (layer) that forms a liquid crystal cured film, and heated to a temperature equal to or higher than the phase transition temperature, thereby forming a liquid crystal phase such as a nematic phase or a smectic phase. In the liquid crystal phase formed by the orientation of this polymerizable liquid crystal compound, the long axis directions of the polymerizable liquid crystal compounds are usually oriented so that they are parallel to each other, and this long axis direction is the orientation direction of the liquid crystal phase. When such a polymerizable liquid crystal compound is made into a film and polymerized in the liquid crystal phase state, a polymer film can be formed that is made of a polymer polymerized in a state of being oriented in the long axis direction (a). This polymer film absorbs ultraviolet light by π electrons in the long axis direction (a) and π electrons in the cross direction (b). Here, the maximum absorption wavelength of ultraviolet light absorbed by π electrons in the cross direction (b) is defined as λbmax. λbmax is usually 300 nm to 400 nm. The π electron density satisfies the above formula (iii), and the π electron density in the cross direction (b) is greater than the π electron density in the long axis direction (a), resulting in a polymer film in which the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the cross direction (b) is greater than the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the long axis direction (a). The ratio (the ratio of the absorbance in the cross direction (b) of linearly polarized ultraviolet light / the absorbance in the long axis direction (a)) is, for example, greater than 1.0, preferably 1.2 or more, and usually 30 or less, for example 10 or less.

[0033] Polymerizable liquid crystal compounds having the above characteristics generally exhibit reverse wavelength dispersion. Specifically, for example, a compound represented by the following formula (X) (hereinafter, also referred to as "polymerizable liquid crystal compound (X)") can be mentioned.

[0034] [ka]

[0035] In formula (X), Ar represents a divalent group having an aromatic group which may have a substituent. The aromatic group referred to here refers to a ring structure having a π electron number of [4n+2] according to the Huckel rule, and may have two or more Ar groups, such as those exemplified by (Ar-1) to (Ar-23) described later, via a divalent linking group. Here, n represents an integer. When a ring structure is formed by including heteroatoms such as -N= or -S-, the Huckel rule is satisfied including the non-covalent bond electron pairs on these heteroatoms, and aromaticity is also included. The aromatic group preferably contains at least one of a nitrogen atom, an oxygen atom, and a sulfur atom. The aromatic group contained in the divalent group Ar may have one or more aromatic groups. When there is one aromatic group, the divalent group Ar may be a divalent aromatic group which may have a substituent. When the divalent group Ar contains two or more aromatic groups, the two or more aromatic groups may be bonded to each other via a divalent bonding group such as a single bond, -CO-O-, or -O-. G 1 and G 2 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. L 1 , L 2 , B 1and B. 2 each independently represents a single bond or a divalent linking group. k and l each independently represent an integer of 0 to 3, and satisfy the relationship of 1≦k+l. Here, when 2≦k+l, B 1 and B. 2 , G 1 and G 2 may be the same as or different from each other. E 1 and E 2 each independently represents an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms. In addition, a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and -CH2- contained in the alkanediyl group may be substituted with -O-, -S-, -SiH2-, or -C(=O)-. P 1 and P 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.

[0036] G 1 and G 2 are each independently preferably a 1,4-phenylenediyl group optionally substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group optionally substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, more preferably a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group, and particularly preferably an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group. In addition, there are multiple G 1 and G 2 At least one of L is preferably a divalent alicyclic hydrocarbon group. 1 or L 2 G binds to 1 and G 2It is more preferable that at least one of the groups is a divalent alicyclic hydrocarbon group.

[0037] L 1 and L 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -, -R a3 COOR a4 -, -R a5 O.C.O.R. a6 -, R a7 OC=OOR a8 -, -N=N-, -CR c =CR d -, or -C≡C-, where R a1 ~R a8 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms; R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 are each independently preferably a single bond, -OR a2-1 -, -CH2-, -CH2CH2-, -COOR a4-1 -OR- a6-1 -, where R a2-1 , R a4-1 , R a6-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and L 2 are each independently more preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or -OCO-.

[0038] B 1 and B. 2 are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -, -R a11 COOR a12 -, -R a13 O.C.O.R. a14 - or R a15 OC=OORa16 -, where R a9 ~R a16 each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B. 2 are each independently preferably a single bond, -OR a10-1 -, -CH2-, -CH2CH2-, -COOR a12-1 -OR- a14-1 -, where R a10-1 , R a12-1 , R a14-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. B 1 and B. 2 are each independently more preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or -OCOCH2CH2-.

[0039] From the viewpoint of expressing reverse wavelength dispersion, k and l are preferably in the range of 2≦k+l≦6, preferably k+l=4, and more preferably k=2 and l=2. When k=2 and l=2, a symmetrical structure is obtained, which is preferable.

[0040] P 1 or P 2 Examples of the polymerizable group represented by the formula (I) include an epoxy group, a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, an acryloyloxy group, a methacryloyloxy group, a vinyl group, and a vinyloxy group are preferred, and an acryloyloxy group and a methacryloyloxy group are more preferred.

[0041] It is preferable that Ar has at least one selected from an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, and an electron-withdrawing group. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, and an anthracene ring, and the like, and the benzene ring and the naphthalene ring are preferable. Examples of the aromatic heterocycle include a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, and a phenanthroline ring. Among them, it is preferable that Ar has a thiazole ring, a benzothiazole ring, or a benzofuran ring, and it is more preferable that Ar has a benzothiazole group. In addition, when Ar contains a nitrogen atom, it is preferable that the nitrogen atom has π electrons.

[0042] In formula (X), the total number of π electrons contained in the divalent aromatic group represented by Ar is N π is preferably 8 or more, more preferably 10 or more, even more preferably 14 or more, and particularly preferably 16 or more. Also, it is preferably 30 or less, more preferably 26 or less, and even more preferably 24 or less.

[0043] Examples of the aromatic group represented by Ar include the following groups.

[0044] [ka]

[0045] In formulae (Ar-1) to (Ar-23), * represents a linking portion, Z 0 , Z 1 and Z 2each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms. 0 , Z 1 and Z 2 may contain a polymerizable group.

[0046] Q 1 and Q 2 are each independently -CR 2’ R 3’ -, -S-, -NH-, -NR 2’ -, -CO- or -O-; R 2’ and R 3’ each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.

[0047] J 1 , and J. 2 each independently represents a carbon atom or a nitrogen atom.

[0048] Y 1 , Y 2 and Y 3 each independently represents an optionally substituted aromatic hydrocarbon group or an optionally substituted aromatic heterocyclic group.

[0049] W 1 and W 2 each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom; and m represents an integer of 0 to 6.

[0050] Y 1 , Y 2 and Y 3Examples of the aromatic hydrocarbon group in the formula (I) include aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and a biphenyl group, of which a phenyl group and a naphthyl group are preferred, and a phenyl group is more preferred. Examples of the aromatic heterocyclic group in the formula (I) include aromatic heterocyclic groups having 4 to 20 carbon atoms and containing at least one heteroatom, such as a nitrogen atom, an oxygen atom, or a sulfur atom, such as a furyl group, a pyrrolyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group, of which a furyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group are preferred.

[0051] Y 1 , Y 2 and Y 3 may each independently be an optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring assembly. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring assembly.

[0052] Z 0 , Z 1 and Z 2 are each preferably independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms; Z 0 is more preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group; Z 1 and Z 2 is more preferably a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, or a cyano group. 0 , Z 1 and Z 2 may contain a polymerizable group.

[0053] Q 1 and Q 2 -NH-, -S-, -NR 2’ -, -O- are preferred, R 2’ is preferably a hydrogen atom, and among these, -S-, -O-, and -NH- are particularly preferable.

[0054] Among the formulae (Ar-1) to (Ar-23), the formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.

[0055] In formulas (Ar-16) to (Ar-23), Y 1 is the nitrogen atom to which it is bonded and Z 0 and may form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include those mentioned above as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. This aromatic heterocyclic group may have a substituent. In addition, Y 1 is the nitrogen atom to which it is bonded and Z 0 In addition, it may be the above-mentioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group, for example, a benzofuran ring, a benzothiazole ring, a benzoxazole ring, etc.

[0056] In the present invention, as the polymerizable liquid crystal compound forming the horizontally aligned liquid crystal cured film, for example, a compound containing a group represented by the following formula (Y) (hereinafter also referred to as "polymerizable liquid crystal compound (Y)") may be used. The polymerizable liquid crystal compound (Y) generally tends to exhibit positive wavelength dispersion. The polymerizable liquid crystal compound may be used alone or in combination of two or more kinds, and the polymerizable liquid crystal compound (X) may be used in combination with the polymerizable liquid crystal compound (Y).

[0057] P11-B11-E11-B12-A11-B13- (Y) In formula (Y), P11 represents a polymerizable group. A11 represents a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. A hydrogen atom contained in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, or a nitro group, and a hydrogen atom contained in the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms may be substituted with a fluorine atom. B11 is -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -CO-NR 16 -, -NR 16 Represents -CO-, -CO-, -CS- or a single bond. R 16 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. B12 and B13 each independently represent -C≡C-, -CH=CH-, -CH2-CH2-, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -, -NR 16 It represents -C(=O)-, -OCH2-, -OCF2-, -CH2O-, -CF2O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH- or a single bond. E11 represents an alkanediyl group having 1 to 12 carbon atoms, and a hydrogen atom contained in the alkanediyl group may be substituted with an alkoxy group having 1 to 5 carbon atoms, and a hydrogen atom contained in the alkoxy group may be substituted with a halogen atom. In addition, -CH2- constituting the alkanediyl group may be substituted with -O- or -CO-.]

[0058] The number of carbon atoms in the aromatic hydrocarbon group and alicyclic hydrocarbon group of A11 is preferably in the range of 3 to 18, more preferably in the range of 5 to 12, and particularly preferably 5 or 6. A11 is preferably a cyclohexane-1,4-diyl group or a 1,4-phenylene group.

[0059] E11 is preferably a linear alkanediyl group having 1 to 12 carbon atoms. -CH2- constituting the alkanediyl group may be replaced with -O-. Specific examples include linear alkanediyl groups having 1 to 12 carbon atoms, such as a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a nonane-1,9-diyl group, a decane-1,10-diyl group, an undecane-1,11-diyl group, and a dodecane-1,12-diyl group; -CH2-CH2-O-CH2-CH2-, -CH2-CH2-O-CH2-CH2-O-CH2-CH2-, and -CH2-CH2-O-CH2-CH2-O-CH2-CH2-O-CH2-CH2-. As B11, -O-, -S-, -CO-O-, and -O-CO- are preferable, and among them, -CO-O- is more preferable. As B12 and B13, each independently, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)- or -OC(=O)-O- is preferable, and among them, -O- or -OC(=O)-O- is more preferable.

[0060] As the polymerizable group represented by P11, a radically polymerizable group or a cationic polymerizable group is preferred from the viewpoint of high polymerization reactivity, particularly high photopolymerization reactivity. In addition, the polymerizable group is preferably a group represented by the following formulae (P-11) to (P-15), since it is easy to handle and the liquid crystal compound can be easily produced.

[0061] [ka] [In formulas (P-11) to (P-15), R 17 ~R 21 each independently represents an alkyl group having 1 to 6 carbon atoms or a hydrogen atom.

[0062] Specific examples of the groups represented by formulae (P-11) to (P-15) include groups represented by the following formulae (P-16) to (P-20).

[0063] [ka]

[0064] P11 is preferably a group represented by formula (P-14) to formula (P-20), and more preferably a vinyl group, a p-stilbene group, an epoxy group or an oxetanyl group. The group represented by P11-B11- is more preferably an acryloyloxy group or a methacryloyloxy group.

[0065] Examples of the polymerizable liquid crystal compound (Y) include compounds represented by formula (I), formula (II), formula (III), formula (IV), formula (V) or formula (VI). P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12 (I) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11 (II) P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12 (III) P11-B11-E11-B12-A11-B13-A12-B14-A13-F11 (IV) P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12 (V) P11-B11-E11-B12-A11-B13-A12-F11 (VI) (In the formula, A12 to A14 each independently have the same meaning as A11, B14 to B16 each independently have the same meaning as B12, B17 has the same meaning as B11, and E12 has the same meaning as E11. F11 represents a hydrogen atom, an alkyl group having 1 to 13 carbon atoms, an alkoxy group having 1 to 13 carbon atoms, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxy group, a methylol group, a formyl group, a sulfo group (-SO3H), a carboxy group, an alkoxycarbonyl group having 1 to 10 carbon atoms, or a halogen atom, and -CH2- constituting the alkyl group and the alkoxy group may be replaced with -O-.

[0066] Specific examples of the polymerizable liquid crystal compound (Y) include compounds having a polymerizable group among the compounds described in “3.8.6 Network (completely crosslinked type)” and “6.5.1 Liquid crystal materials b. Polymerizable nematic liquid crystal materials” in Liquid Crystal Handbook (edited by Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000), and the polymerizable liquid crystals described in JP-A Nos. 2010-31223, 2010-270108, 2011-6360, and 2011-207765.

[0067] Specific examples of the polymerizable liquid crystal compound (Y) include compounds represented by the following formulae (I-1) to (I-4), (II-1) to (II-4), (III-1) to (III-26), (IV-1) to (IV-26), (V-1) to (V-2), and (VI-1) to (VI-6). In the following formulae, k1 and k2 each independently represent an integer of 2 to 12. These polymerizable liquid crystal compounds (Y) are preferred in terms of ease of synthesis or availability.

[0068] [ka]

[0069] [ka]

[0070] [ka]

[0071]

change

[0072]

change

[0073]

change

[0074]

change

[0075]

change

[0076]

change

[0077] In the present invention, the horizontally aligned liquid crystal cured film preferably has at least one maximum absorption between 300 and 400 nm, and the polymerizable liquid crystal composition forming the horizontally aligned liquid crystal cured film preferably contains at least one polymerizable liquid crystal compound having a maximum absorption wavelength between 300 and 400 nm. When the polymerizable liquid crystal composition contains a photopolymerization initiator, the polymerization reaction and gelation of the polymerizable liquid crystal compound may proceed during long-term storage. However, if the maximum absorption wavelength of the polymerizable liquid crystal compound is 300 to 400 nm, the generation of reactive species from the photopolymerization initiator and the polymerization reaction and gelation of the polymerizable liquid crystal compound due to the reactive species can be effectively suppressed even if the polymerizable liquid crystal compound is exposed to ultraviolet light during storage. Therefore, it is advantageous in terms of long-term stability of the polymerizable liquid crystal composition, and the alignment property and uniformity of the film thickness of the obtained liquid crystal cured film can be improved. The maximum absorption wavelength of the polymerizable liquid crystal compound can be measured using a UV-visible spectrophotometer in a solvent. The solvent is a solvent that can dissolve the polymerizable liquid crystal compound, and examples of the solvent include chloroform.

[0078] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition forming the horizontally aligned liquid crystal cured film is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and even more preferably 90 to 95 parts by mass, based on 100 parts by mass of the solid content of the polymerizable liquid crystal composition. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous in terms of the alignment of the obtained liquid crystal cured film. In the present invention, the solid content of the polymerizable liquid crystal composition means all components excluding volatile components such as organic solvents from the polymerizable liquid crystal composition.

[0079] The polymerizable liquid crystal composition used for forming the horizontally aligned liquid crystal cured film may further contain, in addition to the polymerizable liquid crystal compound, additives such as a solvent, a polymerization initiator, a leveling agent, an antioxidant, a photosensitizer, etc. Each of these components may be used alone or in combination of two or more.

[0080] The polymerizable liquid crystal composition used for forming the horizontally aligned liquid crystal cured film is preferably dissolved in a solvent and applied onto a substrate, a horizontal alignment film, etc. The solvent is preferably a solvent capable of dissolving the polymerizable liquid crystal compound, and is preferably a solvent inactive to the polymerization reaction of the polymerizable liquid crystal compound. Examples of the solvent include alcohol solvents such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as ethylcyclohexane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone (NMP), and 1,3-dimethyl-2-imidazolidinone. These solvents can be used alone or in combination of two or more. Among these, alcohol solvents, ester solvents, ketone solvents, chlorine-containing solvents, amide solvents and aromatic hydrocarbon solvents are preferred.

[0081] The content of the solvent in the polymerizable liquid crystal composition is preferably 50 to 98 parts by weight, more preferably 70 to 95 parts by weight, relative to 100 parts by weight of the polymerizable liquid crystal composition. Therefore, the solid content per 100 parts by weight of the polymerizable liquid crystal composition is preferably 2 to 50 parts by weight. If the solid content is 50 parts by weight or less, the viscosity of the polymerizable liquid crystal composition is low, so that the thickness of the film becomes approximately uniform and unevenness tends to be less likely to occur. The solid content can be appropriately determined in consideration of the thickness of the liquid crystal cured film to be produced.

[0082] The polymerization initiator is a compound that generates reactive species by the contribution of heat or light and can initiate a polymerization reaction of a polymerizable liquid crystal compound, etc. Examples of the reactive species include active species such as radicals, cations, and anions. Among them, a photopolymerization initiator that generates radicals by light irradiation is preferred from the viewpoint of easy reaction control.

[0083] Examples of photopolymerization initiators include benzoin compounds, benzophenone compounds, benzyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, oxime compounds, triazine compounds, iodonium salts, and sulfonium salts.Specific examples include Irgacure (registered trademark) 907, Irgacure 184, Irgacure 651, Irgacure 819, Irgacure 250, Irgacure 369, Irgacure 379, Irgacure 127, Irgacure 2959, Irgacure 754, Irgacure 379EG (all manufactured by BASF Japan Ltd.), Seikuol BZ, Seikuol Z, Seikuol BEE (all manufactured by Seiko Chemical Co., Ltd.), Kayacure (registered trademark) Examples of suitable antibacterial agents include ADEKA CURE BP100 (manufactured by Nippon Kayaku Co., Ltd.), Kayacure UVI-6992 (manufactured by Dow), ADEKA OPTOMER SP-152, ADEKA OPTOMER SP-170, ADEKA OPTOMER N-1717, ADEKA OPTOMER N-1919, ADEKA ARCLES NCI-831, ADEKA ARCLES NCI-930 (all manufactured by ADEKA Corporation), TAZ-A, TAZ-PP (all manufactured by Nippon SiberHegner AG) and TAZ-104 (manufactured by Sanwa Chemical Co., Ltd.).

[0084] The photopolymerization initiator can fully utilize the energy emitted from the light source and has excellent productivity, so that the maximum absorption wavelength is preferably 300 nm to 400 nm, and more preferably 300 nm to 380 nm, and among them, an α-acetophenone-based polymerization initiator or an oxime-based photopolymerization initiator is preferable.

[0085] Examples of α-acetophenone compounds include 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one, and 2-dimethylamino-1-(4-morpholinophenyl)-2-(4-methylphenylmethyl)butan-1-one, and more preferably 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one and 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one. Examples of commercially available α-acetophenone compounds include Irgacure 369, 379EG, and 907 (all manufactured by BASF Japan Co., Ltd.) and Seikuol BEE (manufactured by Seiko Chemical Co., Ltd.).

[0086] The oxime-based photopolymerization initiator generates radicals such as phenyl radicals and methyl radicals when irradiated with light. The polymerization of the polymerizable liquid crystal compound proceeds favorably by these radicals, and among them, the oxime-based photopolymerization initiator that generates methyl radicals is preferred in terms of high initiation efficiency of the polymerization reaction. In addition, from the viewpoint of proceeding the polymerization reaction more efficiently, it is preferable to use a photopolymerization initiator that can efficiently utilize ultraviolet light with a wavelength of 350 nm or more. As the photopolymerization initiator that can efficiently utilize ultraviolet light with a wavelength of 350 nm or more, a triazine compound or a carbazole compound containing an oxime structure is preferred, and from the viewpoint of sensitivity, a carbazole compound containing an oxime ester structure is more preferred. Examples of the carbazole compound containing an oxime structure include 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime), and the like. Commercially available oxime ester photopolymerization initiators include Irgacure OXE-01, Irgacure OXE-02, Irgacure OXE-03 (all manufactured by BASF Japan Ltd.), ADEKA Optomer N-1919, ADEKA Arcles NCI-831 (all manufactured by ADEKA Corporation), and the like.

[0087] The content of the photopolymerization initiator is usually 0.1 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 1 to 15 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. Within the above range, the reaction of the polymerizable group proceeds sufficiently, and the alignment of the polymerizable liquid crystal compound is unlikely to be disturbed.

[0088] A leveling agent is an additive that has the function of adjusting the fluidity of a polymerizable liquid crystal composition and making the coating film obtained by applying the composition flatter. Examples of the leveling agent include silicone-based, polyacrylate-based and perfluoroalkyl-based leveling agents. As the leveling agent, a commercially available product may be used. Specific examples of the leveling agent include DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, FZ2123 (all manufactured by Toray Dow Corning Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, TSF4460 (all manufactured by Momentive Performance Materials Co., Ltd.). Japan LLC), Fluorinert (registered trademark) FC-72, FC-40, FC-43, FC-3283 (all manufactured by Sumitomo 3M Limited), Megafac (registered trademark) R-08, R-30, R-90, F-410, F-411, F-443, F-445, F-470, F-477, F-479, F-482, F-483, F-556 (all manufactured by DIC Corporation), F-top (trade name) EF301, EF3 03, EF351, EF352 (all manufactured by Mitsubishi Materials Electronics Co., Ltd.), Surflon (registered trademark) S-381, S-382, S-383, S-393, SC-101, SC-105, KH-40, SA-100 (all manufactured by AGC Seimi Chemical Co., Ltd.), trade names E1830, E5844 (manufactured by Daikin Fine Chemical Research Institute Co., Ltd.), BM-1000, BM-1100, BYK-352, BYK-353 and BYK-361N (all trade names: manufactured by BM Chemie), etc. The leveling agent can be used alone or in combination of two or more kinds.

[0089] The content of the leveling agent is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, it is easy to align the polymerizable liquid crystal compound, and the obtained liquid crystal cured film tends to be smoother, which is preferable.

[0090] By blending an antioxidant, the polymerization reaction of the polymerizable liquid crystal compound can be controlled. The antioxidant may be a primary antioxidant selected from phenol-based antioxidants, amine-based antioxidants, quinone-based antioxidants, and nitroso-based antioxidants, or a secondary antioxidant selected from phosphorus-based antioxidants and sulfur-based antioxidants. In order to polymerize the polymerizable liquid crystal compound without disturbing the alignment of the polymerizable liquid crystal compound, the content of the antioxidant is usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. The antioxidant may be used alone or in combination of two or more kinds.

[0091] In addition, the photopolymerization initiator can be made highly sensitive by using a photosensitizer. Examples of the photosensitizer include xanthones such as xanthone and thioxanthone; anthracenes having a substituent such as anthracene and alkyl ether; phenothiazine; and rubrene. The photosensitizer can be used alone or in combination of two or more kinds. The content of the photosensitizer is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound.

[0092] The polymerizable liquid crystal composition used for forming the horizontally aligned liquid crystal cured film can be obtained by stirring the polymerizable liquid crystal compound, a solvent, a photopolymerization initiator, and components other than the polymerizable liquid crystal compound at a predetermined temperature.

[0093] [Optical anisotropic layer Y] The optically anisotropic layer Y constituting the laminate of the present invention may be, for example, a cured product of a polymerizable liquid crystal composition in which the polymerizable liquid crystal compound is cured in a state where it is aligned in a direction perpendicular to the film plane (hereinafter, also referred to as a "vertically aligned liquid crystal cured film"). In the present invention, the vertically aligned liquid crystal cured film preferably contains a vertical alignment promoter. That is, in the present invention, the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film preferably contains a vertical alignment promoter. In the present invention, the vertical alignment promoter means a material that promotes the liquid crystal alignment of the polymerizable liquid crystal compound in a direction perpendicular to the film plane. By forming the vertically aligned liquid crystal cured film from a polymerizable liquid crystal composition containing a vertical alignment promoter, the vertically aligned liquid crystal cured film can be formed without a vertical alignment film. As a result, in the laminate of the present invention, it is not necessary to form a vertical alignment film, and the manufacturing process of the laminate is simplified, and the laminate can be manufactured with good productivity.

[0094] Examples of the vertical alignment promoter that promotes the vertical alignment of the polymerizable liquid crystal compound include an ionic compound consisting of nonmetallic atoms and a nonionic silane compound, etc. It is preferable that the vertically aligned liquid crystal cured film contains at least one of the nonionic silane compound and the ionic compound consisting of nonmetallic atoms, and it is more preferable that the vertically aligned liquid crystal cured film contains both the nonionic silane compound and the ionic compound consisting of nonmetallic atoms.

[0095] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains a nonionic silane compound, the nonionic silane compound reduces the surface tension of the polymerizable liquid crystal composition, and in the dried coating film formed from the polymerizable liquid crystal composition, the nonionic silane compound tends to be unevenly distributed at the interface between the dried coating film and the air, increasing the vertical alignment control force for the polymerizable liquid crystal compound, and the polymerizable liquid crystal compound tends to be aligned in the vertical direction to the film plane in the dried coating film. This makes it possible to form a liquid crystal cured film while maintaining the vertical alignment state of the polymerizable liquid crystal compound.

[0096] The nonionic silane compound is a nonionic compound that contains Si element. Examples of the nonionic silane compound include silicon polymers such as polysilane, silicone resins such as silicone oil and silicone resin, and organic and inorganic silane compounds such as silicone oligomers, silsesquioxanes and alkoxysilanes (more specifically, silane coupling agents, etc.).

[0097] The nonionic silane compound may be a silicone monomer type or a silicone oligomer (polymer) type. The nonionic silane compound may be used alone or in combination of two or more types.

[0098] The silane coupling agent is a compound containing an Si element having at least one functional group selected from the group consisting of vinyl group, epoxy group, styryl group, methacryl group, acrylic group, amino group, isocyanurate group, ureido group, mercapto group, isocyanate group, carboxy group, and hydroxyl group at the end, and at least one alkoxysilyl group or silanol group. By appropriately selecting these functional groups, it is possible to impart unique effects such as improving the mechanical strength of the vertically aligned liquid crystal cured film, modifying the surface of the vertically aligned liquid crystal cured film, and improving the adhesion between the vertically aligned liquid crystal cured film and an adjacent layer. From the viewpoint of adhesion, it is preferable that the silane coupling agent is a silane coupling agent having an alkoxysilyl group and another different reactive group (for example, the above-mentioned functional group). Furthermore, it is preferable that the silane coupling agent is a silane coupling agent having an alkoxysilyl group and a polar group. When the silane coupling agent has at least one alkoxysilyl group and at least one polar group in its molecule, the vertical alignment of the polymerizable liquid crystal compound is more easily improved, and the vertical alignment promotion effect tends to be significantly obtained.The polar group can be, for example, an epoxy group, an amino group, an isocyanurate group, a mercapto group, a carboxy group, and a hydroxy group.The polar group may have a suitable substituent or a protective group in order to control the reactivity of the silane coupling agent.

[0099] Commercially available silane coupling agents include, for example, KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, KBE- 502, KBE-503, KBM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBM-9659, KBE-585, KBM-802, KBM-803, KBE-846, and KBE-9007 manufactured by Shin-Etsu Chemical Co., Ltd.

[0100] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains a nonionic silane compound, the content thereof is usually preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition. When the content of the nonionic silane compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining good coatability of the polymerizable liquid crystal composition.

[0101] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains an ionic compound consisting of a nonmetallic atom, in the dried coating film formed from the polymerizable liquid crystal composition, a vertical alignment regulating force for the polymerizable liquid crystal compound is exerted due to electrostatic interaction, and the polymerizable liquid crystal compound tends to be aligned in the vertical direction to the film plane in the dried coating film. As a result, the liquid crystal cured film can be formed while maintaining the vertically aligned state of the polymerizable liquid crystal compound.

[0102] Examples of ionic compounds consisting of nonmetallic atoms include onium salts (more specifically, quaternary ammonium salts in which the nitrogen atom has a positive charge, tertiary sulfonium salts, and quaternary phosphonium salts in which the phosphorus atom has a positive charge). Among these onium salts, quaternary onium salts are preferred from the viewpoint of further improving the vertical alignment property of the polymerizable liquid crystal compound, and quaternary phosphonium salts or quaternary ammonium salts are more preferred from the viewpoint of improving availability and mass productivity. The onium salt may have two or more quaternary onium salt sites in the molecule, and may be an oligomer or polymer.

[0103] The molecular weight of the ionic compound consisting of nonmetallic atoms is preferably 100 or more and 10,000 or less. When the molecular weight is within the above range, it is easy to improve the vertical alignment property of the polymerizable liquid crystal compound while ensuring the coatability of the polymerizable composition. The molecular weight of the ionic compound is more preferably 5000 or less, and further preferably 3000 or less.

[0104] The cationic component of the ionic compound consisting of nonmetallic atoms may be, for example, an inorganic cation or an organic cation. Among them, organic cations are preferred because they are less likely to cause alignment defects in the polymerizable liquid crystal compound. Examples of organic cations include imidazolium cations, pyridinium cations, ammonium cations, sulfonium cations, and phosphonium cations.

[0105] Ionic compounds consisting of nonmetallic atoms generally have counter anions. Examples of anion components that are counter ions of the cationic components include inorganic anions and organic anions. Among them, organic anions are preferred because they are less likely to cause alignment defects in the polymerizable liquid crystal compound. It is not necessary that the cations and anions correspond one-to-one.

[0106] Specific examples of the anion component include the following: Chloride anion [Cl - 〕, Bromide anion [Br - 〕, Iodide anion [I - 〕, Tetrachloroaluminate anion [AlCl4 - 〕, Heptachlorodialuminate anion [Al2Cl7 - 〕, Tetrafluoroborate anion [BF4 - 〕, Hexafluorophosphate anion [PF6 - 〕, Perchlorate anion [ClO4 - 〕, Nitrate anion [NO3 - 〕, Acetate anion [CH3COO - 〕, Trifluoroacetate anion [CF3COO - 〕, Fluorosulfonate anion [FSO3 - 〕, Methanesulfonate anion [CH3SO3 - 〕, Trifluoromethanesulfonate anion [CF3SO3 - 〕, p-Toluenesulfonate anion [p-CH3C6H4SO3 - 〕, Bis(fluorosulfonyl)imide anion [(FSO2)2N - 〕, Bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N - 〕, Tris(trifluoromethanesulfonyl)methanide anion [(CF3SO2)3C - 〕, Hexafluoroarsenate anion [AsF6 - 〕, Hexafluoroantimonate anion [SbF6 - 〕, Hexafluoroniobate anion [NbF6 - 〕, Hexafluorotantalate anion [TaF6 - 〕, Dimethylphosphinate anion [(CH3)2POO - 〕, (Poly)hydrofluorofluoride anion [F(HF) n - (for example, n is an integer from 1 to 3), Dicyanamide anion [(CN)2N - 〕, Thiocyanine anion (SCN - 〕, Perfluorobutanesulfonate anion [C4F9SO3 - 〕, Bis(pentafluoroethanesulfonyl)imide anion [(C2F5SO2)2N - 〕, Perfluorobutanoate anion [C3F7COO - ], and (Trifluoromethanesulfonyl)(trifluoromethanecarbonyl)imide anion 〔(CF3SO2)(CF3CO)N - 〕.

[0107] Specific examples of the ionic compound consisting of nonmetallic atoms can be appropriately selected from the combinations of the above-mentioned cationic and anionic components. Specific examples of the compound consisting of a combination of a cationic component and an anionic component include the following.

[0108] (Pyridinium salts) N-Hexylpyridinium hexafluorophosphate, N-octylpyridinium hexafluorophosphate, N-methyl-4-hexylpyridinium hexafluorophosphate, N-butyl-4-methylpyridinium hexafluorophosphate, N-octyl-4-methylpyridinium hexafluorophosphate, N-Hexylpyridinium bis(fluorosulfonyl)imide, N-Octylpyridinium bis(fluorosulfonyl)imide, N-methyl-4-hexylpyridinium bis(fluorosulfonyl)imide, N-butyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-octyl-4-methylpyridinium bis(fluorosulfonyl)imide, N-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-Octylpyridinium bis(trifluoromethanesulfonyl)imide, N-methyl-4-hexylpyridinium bis(trifluoromethanesulfonyl)imide, N-butyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-octyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide, N-Hexylpyridinium p-toluenesulfonate, N-Octylpyridinium p-toluenesulfonate, N-methyl-4-hexylpyridinium p-toluenesulfonate, N-Butyl-4-methylpyridinium p-toluenesulfonate, and N-Octyl-4-methylpyridinium p-toluenesulfonate.

[0109] (Imidazolium salt) 1-ethyl-3-methylimidazolium hexafluorophosphate, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium p-toluenesulfonate, 1-Butyl-3-methylimidazolium methanesulfonate, etc.

[0110] (Pyrrolidinium salts) N-butyl-N-methylpyrrolidinium hexafluorophosphate, N-butyl-N-methylpyrrolidinium bis(fluorosulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-Butyl-N-methylpyrrolidinium p-toluenesulfonate, etc.

[0111] (Ammonium salt) tetrabutylammonium hexafluorophosphate, Tetrabutylammonium bis(fluorosulfonyl)imide, Tetrahexylammonium bis(fluorosulfonyl)imide, trioctylmethylammonium bis(fluorosulfonyl)imide, (2-hydroxyethyl)trimethylammonium bis(fluorosulfonyl)imide, tetrabutylammonium bis(trifluoromethanesulfonyl)imide, tetrahexylammonium bis(trifluoromethanesulfonyl)imide, trioctylmethylammonium bis(trifluoromethanesulfonyl)imide, (2-hydroxyethyl)trimethylammonium bis(trifluoromethanesulfonyl)imide, tetrabutylammonium p-toluenesulfonate, Tetrahexylammonium p-toluenesulfonate, Trioctylmethylammonium p-toluenesulfonate, (2-hydroxyethyl)trimethylammonium p-toluenesulfonate, (2-Hydroxyethyl)trimethylammonium dimethylphosphinate 1-(3-trimethoxysilylpropyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylpropyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylbutyl)-1,1,1-tributylammonium bis(trifluoromethanesulfonyl)imide, 1-(3-trimethoxysilylbutyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide, N-{(3-triethoxysilylpropyl)carbamoyloxyethyl)}-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide, and N-[2-{3-(3-trimethoxysilylpropylamino)-1-oxopropoxy}ethyl]-N,N,N-trimethylammonium bis(trifluoromethanesulfonyl)imide.

[0112] (phosphonium salts) tributyl(2-methoxyethyl)phosphonium bis(trifluoromethanesulfonyl)imide, tributylmethylphosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-trimethyl-1-[4-(trimethoxysilyl)butyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-tributyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide, 1,1,1-tributyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, and 1,1,1-Tributyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide. These ionic compounds may be used alone or in combination of two or more. Among them, ionic compounds made of phosphonium salts or ammonium salts are preferred.

[0113] From the viewpoint of further improving the vertical alignment of the polymerizable liquid crystal compound, the ionic compound preferably has a Si element and / or an F element in the molecular structure of the cationic moiety. When the ionic compound has a Si element and / or an F element in the molecular structure of the cationic moiety, the ionic compound is easily segregated on the surface of the vertically aligned liquid crystal cured film. Among them, the following ionic compounds (i) to (iii) are preferred as ionic compounds whose constituent elements are all nonmetallic elements.

[0114] (Ionic compound (i))

[0115] [ka] (Ionic compound (ii))

[0116] [ka] (Ionic compound (iii))

[0117] [ka]

[0118] For example, the vertical alignment of the polymerizable liquid crystal compound can be further improved by applying a method of treating the substrate surface with a surfactant having an alkyl group with a relatively long chain length to improve the alignment of the liquid crystal (see, for example, Chapter 2, Liquid Crystal Orientation and Physical Properties, of the Liquid Crystal Handbook (published by Maruzen Co., Ltd.)). In other words, by treating the substrate surface with an ionic compound having an alkyl group with a relatively long chain length, the vertical alignment of the polymerizable liquid crystal compound can be effectively improved.

[0119] Specifically, it is preferable that the ionic compound composed of nonmetallic atoms satisfies the following formula (10). 5 <M<16 (10) In formula (10), M is expressed by the following formula (11). M = (number of covalent bonds from the positively charged atom to the end of the molecular chain of the substituent with the most covalent bonds to the end of the molecular chain among the substituents directly bonded to the positively charged atom) ÷ (number of positively charged atoms) (11) When the ionic compound consisting of a nonmetallic atom satisfies the above condition (10), the vertical alignment property of the polymerizable liquid crystal compound can be effectively improved.

[0120] In addition, when there are two or more positively charged atoms in the molecule of an ionic compound consisting of nonmetallic atoms, for a substituent having two or more positively charged atoms, the number of covalent bonds from the positively charged atom considered as the base point to the nearest other positively charged atom is considered to be the "number of covalent bonds from the positively charged atom to the molecular chain end" described in the above definition of M. In addition, when an ionic compound consisting of nonmetallic atoms is an oligomer or polymer having two or more repeating units, the constituent unit is considered as one molecule and the above M is calculated. When a positively charged atom is incorporated in a ring structure, the number of covalent bonds from the ring structure to the atom having the same positive charge, or the number of covalent bonds to the end of the substituent bonded to the ring structure, whichever is larger, is considered to be the "number of covalent bonds from the positively charged atom to the molecular chain end" described in the above definition of M.

[0121] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains an ionic compound consisting of non-metallic atoms, the content thereof is usually preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition. When the content of the ionic compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining good coatability of the polymerizable liquid crystal composition.

[0122] Since the polymerizable liquid crystal composition for forming the vertically aligned liquid crystal cured film contains both a nonionic silane compound and an ionic compound consisting of nonmetallic atoms, the vertical alignment of the polymerizable liquid crystal compound is more easily promoted in the dried coating film formed from the polymerizable liquid crystal composition for forming the vertically aligned liquid crystal cured film due to the electrostatic interaction derived from the ionic compound and the surface tension reducing effect derived from the nonionic silane compound. This makes it possible to form a liquid crystal cured film while maintaining the polymerizable liquid crystal compound in a more precisely vertically aligned state.

[0123] The vertically aligned liquid crystal cured film is preferably a cured product of a polymerizable liquid crystal composition containing the above-mentioned alignment promoter and at least one polymerizable liquid crystal compound, and more preferably a liquid crystal cured film obtained by curing a polymerizable liquid crystal compound having at least one radically polymerizable group in a state where the polymerizable liquid crystal compound is aligned vertically to the in-plane direction of the liquid crystal cured film. In the present invention, the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film means a liquid crystal compound having a polymerizable group similar to that shown in the horizontally aligned liquid crystal cured film, and in particular, a liquid crystal compound having at least one radically polymerizable group is preferred. The polymerizable liquid crystal compound is not particularly limited, and for example, a polymerizable liquid crystal compound conventionally known in the field of retardation films can be used.

[0124] As the optically anisotropic layer Y of the present invention, the vertically aligned liquid crystal cured film is preferably formed on a layer having no vertical alignment regulating force without a vertical alignment film. Since the vertically aligned liquid crystal cured film in the laminate of the present invention can be formed without a vertical alignment film, the number of steps for producing the laminate is reduced, resulting in a laminate that can be produced with good productivity.

[0125] The polymerizable liquid crystal compound constituting the vertically aligned liquid crystal cured film is not particularly limited, and for example, a polymerizable liquid crystal compound conventionally known in the field of retardation films can be used. Specifically, the polymerizable liquid crystal compound (X) or the polymerizable liquid crystal compound (Y) exemplified as the polymerizable liquid crystal compound usable for forming the horizontally aligned liquid crystal cured film can be used, and among them, it is preferable to include at least one polymerizable liquid crystal compound exhibiting so-called reverse wavelength dispersion, and for example, the polymerizable liquid crystal compound (X) can be suitably used. In the polymerizable liquid crystal composition for forming the vertically aligned liquid crystal cured film, the polymerizable liquid crystal compound can be used alone or in combination of two or more kinds, and the polymerizable liquid crystal compound (X) and the polymerizable liquid crystal compound (Y) may be used in combination.

[0126] The thickness of the optically anisotropic layer Y is from 0.3 μm to 5 μm, more preferably from 0.4 μm to 4.5 μm, and further preferably from 0.5 μm to 4 μm. When the optically anisotropic layer Y is a horizontally aligned liquid crystal cured film having a thickness in the above range, it is possible to achieve a reduction in the weight of the image display device.

[0127] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition used for forming the vertically aligned liquid crystal cured film is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and further preferably 90 to 95 parts by mass, based on 100 parts by mass of the solid content of the polymerizable liquid crystal composition. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous from the viewpoint of the alignment of the obtained liquid crystal cured film.

[0128] The polymerizable liquid crystal composition used for forming the vertically aligned liquid crystal cured film may further contain additives such as a solvent, a polymerization initiator, a leveling agent, an antioxidant, a photosensitizer, etc., in addition to the polymerizable liquid crystal compound or the polymerizable liquid crystal compound and the vertical alignment promoter. These components include the same ones as those exemplified above as the components that can be used in the horizontally aligned liquid crystal cured film, and each of them may be used alone or in combination of two or more.

[0129] The polymerizable liquid crystal composition used for forming the vertically aligned liquid crystal cured film can be obtained by stirring the polymerizable liquid crystal compound and components other than the polymerizable liquid crystal compound, such as a solvent and a photopolymerization initiator, at a predetermined temperature.

[0130] [Method for producing laminate] The laminate of the present invention includes an optically anisotropic layer X and an optically anisotropic layer Y. As described above, the optically anisotropic layer X may be, for example, a stretched film or a cured layer of a polymerizable liquid crystal composition cured in a state where the polymerizable liquid crystal compound is aligned in a horizontal direction relative to the film plane (horizontally aligned liquid crystal cured film). The optically anisotropic layer Y may be, for example, a cured layer of a polymerizable liquid crystal composition cured in a state where the polymerizable liquid crystal compound is aligned in a vertical direction relative to the film plane (vertically aligned liquid crystal cured film).

[0131] The laminate of the present invention is, for example, A laminate having an optically anisotropic layer Y directly on an optically anisotropic layer X can be produced by forming a coating film of a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film, which contains a polymerizable liquid crystal compound, on a stretched film, and forming a vertically aligned liquid crystal cured film from the coating film (hereinafter, also referred to as a "vertically aligned liquid crystal cured film forming process").

[0132] The laminate of the present invention is, for example, A laminate having an optically anisotropic layer X and a direct optically anisotropic layer Y can be produced by a method including, in this order, a step of forming a coating film of a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film, which contains a polymerizable liquid crystal compound, and forming a horizontally aligned liquid crystal cured film from the coating film (hereinafter also referred to as a "horizontally aligned liquid crystal cured film forming step"), and a vertically aligned liquid crystal cured film forming step.

[0133] In the laminate of the present invention, when the optically anisotropic layer X is formed of a horizontally aligned liquid crystal cured film, It is preferable to include a step of forming a coating film of a composition for forming a horizontal alignment film and forming a horizontal alignment film from the coating film (hereinafter, also referred to as a "horizontal alignment film forming step") before forming the horizontal alignment film cured film, and it is preferable that the horizontal alignment film forming step and the horizontal alignment liquid crystal cured film forming step are performed continuously in this order. By the manufacturing method including the horizontal alignment film forming step, an optically anisotropic layer X consisting of a horizontal alignment liquid crystal cured film formed on a horizontal alignment film is obtained.

[0134] In the horizontally aligned liquid crystal cured film forming step, the horizontally aligned liquid crystal cured film is, for example, A step of applying a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film onto a substrate or an alignment film to obtain a coating film; drying the coating to form a dry coating; and A process of irradiating the dried coating with active energy rays to form a horizontally aligned liquid crystal cured film. The composition can be produced by a method comprising the steps of:

[0135] The formation of a coating film of the polymerizable liquid crystal composition can be carried out, for example, by applying the polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film onto a substrate or an alignment film described below. Examples of the substrate include glass substrates and film substrates, but resin film substrates are preferred from the viewpoint of processability. Examples of the resin constituting the film substrate include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; plastics such as polyphenylene sulfide and polyphenylene oxide. Such resins can be formed into a film by known means such as solvent casting and melt extrusion to form a substrate. The substrate surface may have a protective layer formed from an acrylic resin, a methacrylic resin, an epoxy resin, an oxetane resin, a urethane resin, a melamine resin, or the like, and may be subjected to a surface treatment such as a release treatment such as silicone treatment, a corona treatment, or a plasma treatment.

[0136] Commercially available products may be used as the substrate. Examples of commercially available cellulose ester substrates include cellulose ester substrates manufactured by Fuji Photo Film Co., Ltd., such as Fujitac Film; cellulose ester substrates manufactured by Konica Minolta Opto Co., Ltd., such as "KC8UX2M", "KC8UY", and "KC4UY". Examples of commercially available cyclic olefin resins include cyclic olefin resins manufactured by Ticona (Germany), such as "Topas (registered trademark)", cyclic olefin resins manufactured by JSR Corporation, such as "Arton (registered trademark)", cyclic olefin resins manufactured by Zeon Corporation, such as "ZEONOR (registered trademark)" and "ZEONEX (registered trademark)", and cyclic olefin resins manufactured by Mitsui Chemicals, Inc., such as "Apel" (registered trademark). Commercially available cyclic olefin resin substrates may also be used. Commercially available cyclic olefin resin substrates include cyclic olefin resin substrates manufactured by Sekisui Chemical Co., Ltd., such as "S-Cina (registered trademark)" and "SCA40 (registered trademark)"; cyclic olefin resin substrates manufactured by Optes Inc., such as "ZEONORFILM (registered trademark)"; and cyclic olefin resin substrates manufactured by JSR Corporation, such as "ARTONFILM (registered trademark)."

[0137] From the viewpoints of thinning the laminate, ease of peeling the substrate, and ease of handling the substrate, the thickness of the substrate is usually 5 to 300 μm, and preferably 10 to 150 μm. When the substrate is disposed in the laminate of the present invention, the substrate is preferably optically isotropic from the viewpoint of optical compensation described later. In the present invention, being optically isotropic means that the in-plane retardation value of the substrate is 3 nm or less.

[0138] Examples of a method for applying the polymerizable liquid crystal composition to a substrate or the like include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.

[0139] Next, the solvent is removed by drying or the like to form a dried coating film. Examples of drying methods include natural drying, ventilation drying, heat drying, and reduced pressure drying. In this case, the coating film obtained from the polymerizable liquid crystal composition is heated to dry and remove the solvent from the coating film, and the polymerizable liquid crystal compound can be aligned in a horizontal direction relative to the coating film plane. The heating temperature of the coating film can be appropriately determined in consideration of the materials of the polymerizable liquid crystal compound used and the substrate on which the coating film is formed, but it is usually necessary that the temperature be equal to or higher than the liquid crystal phase transition temperature in order to phase-transition the polymerizable liquid crystal compound to a liquid crystal phase state. In order to make the polymerizable liquid crystal compound horizontally aligned while removing the solvent contained in the polymerizable liquid crystal composition, the composition can be heated to a temperature equal to or higher than the liquid crystal phase transition temperature (smectic phase transition temperature or nematic phase transition temperature) of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition. The liquid crystal phase transition temperature can be measured using, for example, a polarizing microscope equipped with a temperature control stage, a differential scanning calorimeter (DSC), a thermogravimetric differential thermal analyzer (TG-DTA), etc. When two or more polymerizable liquid crystal compounds are used in combination, the phase transition temperature means a temperature measured in the same manner as when one type of polymerizable liquid crystal compound is used, using a mixture of polymerizable liquid crystal compounds in which all polymerizable liquid crystal compounds constituting the polymerizable liquid crystal composition are mixed in the same ratio as the composition in the polymerizable liquid crystal composition. It is generally known that the liquid crystal phase transition temperature of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition may be lower than the liquid crystal phase transition temperature of the polymerizable liquid crystal compound alone.

[0140] The heating time can be appropriately determined depending on the heating temperature, the type of polymerizable liquid crystal compound used, the type and boiling point of the solvent, and the amount thereof, but is usually 15 seconds to 10 minutes, and preferably 0.5 to 5 minutes.

[0141] The removal of the solvent from the coating film may be performed simultaneously with or separately from the heating of the polymerizable liquid crystal compound to a temperature equal to or higher than the liquid crystal phase transition temperature, but is preferably performed simultaneously from the viewpoint of improving productivity. Before heating the polymerizable liquid crystal compound to a temperature equal to or higher than the liquid crystal phase transition temperature, a preliminary drying step may be provided to adequately remove the solvent in the coating film obtained from the polymerizable liquid crystal composition under conditions in which the polymerizable liquid crystal compound contained in the coating film is not polymerized. Examples of the drying method in the preliminary drying step include natural drying, ventilation drying, heat drying, and reduced pressure drying, and the drying temperature (heating temperature) in the drying step can be appropriately determined depending on the type of polymerizable liquid crystal compound used, the type of solvent, its boiling point, and its amount, etc.

[0142] Next, in the obtained dried coating film, the polymerizable liquid crystal compound is polymerized while maintaining the horizontal alignment state of the polymerizable liquid crystal compound, thereby forming a horizontally aligned liquid crystal cured film. Examples of polymerization methods include thermal polymerization and photopolymerization, but photopolymerization is preferred from the viewpoint of easy control of the polymerization reaction. In photopolymerization, the light irradiated to the dried coating film is appropriately selected according to the type of polymerization initiator contained in the dried coating film, the type of polymerizable liquid crystal compound (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof. Specific examples thereof include one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, and active electron beams. Among them, ultraviolet light is preferred in terms of easy control of the progress of the polymerization reaction and the ability to use photopolymerization devices that are widely used in this field, and it is preferable to select the types of polymerizable liquid crystal compound and polymerization initiator contained in the polymerizable liquid crystal composition so that they can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can also be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means during polymerization. By adopting such a cooling means, polymerization of the polymerizable liquid crystal compound can be performed at a lower temperature, and even if a substrate with relatively low heat resistance is used, a horizontally aligned liquid crystal cured film can be appropriately formed. In addition, it is also possible to promote the polymerization reaction by increasing the polymerization temperature within a range in which defects due to heat during light irradiation (such as deformation of the substrate due to heat) do not occur. During photopolymerization, a patterned cured film can also be obtained by performing masking and development.

[0143] Examples of the light source of the active energy rays include a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave excited mercury lamp, and a metal halide lamp.

[0144] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.

[0145] In the present invention, the coating film of the polymerizable liquid crystal composition for forming the horizontally aligned cured liquid crystal film is preferably formed on a horizontal alignment film having an alignment control force in the horizontal direction with respect to the plane of the obtained cured liquid crystal film, since the degree of alignment order of the horizontally aligned cured liquid crystal film can be increased. Therefore, in the laminate of the present invention, it is preferable that the optically anisotropic layer X is formed on the horizontal alignment film, and the horizontal alignment film and the horizontally aligned cured liquid crystal film are included in this order. The alignment control force of the alignment film can be arbitrarily adjusted by the type of alignment film, surface condition, rubbing conditions, etc., and when the alignment film is formed from a photoalignable polymer, it can be arbitrarily adjusted by the polarized light irradiation conditions, etc.

[0146] The horizontal alignment film is preferably one that has solvent resistance such that the polymerizable liquid crystal composition is not dissolved by application or the like, and also has heat resistance in the heat treatment for removing the solvent and for aligning the polymerizable liquid crystal compound described below. Examples of the alignment film include an alignment film containing an alignment polymer, a photo-alignment film, a groove alignment film having a concave-convex pattern or a plurality of grooves on the surface, and a stretched film stretched in the alignment direction, and the like, and a photo-alignment film is preferred from the viewpoint of the accuracy of the alignment angle and the quality.

[0147] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among them, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.

[0148] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an "alignment polymer composition") to a substrate and removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing (rubbing method). Examples of the solvent include the same solvents as those exemplified above as solvents that can be used in the polymerizable liquid crystal composition.

[0149] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably about 0.1 to 10%.

[0150] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).

[0151] The method for applying the alignable polymer composition to the substrate may be the same as the above-mentioned example of the method for applying the polymerizable liquid crystal composition to the substrate.

[0152] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0153] In order to impart an orientation control force to the orientation film, a rubbing treatment can be performed as necessary (rubbing method). A method for imparting an orientation control force by the rubbing method includes a method in which an orientation polymer composition is applied to a substrate and annealed to bring an orientation polymer film formed on the substrate surface into contact with a rotating rubbing roll wrapped with a rubbing cloth. If masking is performed during the rubbing treatment, multiple regions (patterns) with different orientation directions can also be formed on the orientation film.

[0154] In a preferred embodiment of the present invention, the horizontal alignment film is a photo-alignment film formed from a polymer having a (meth)acryloyl group. When the horizontal alignment film has a polymerizable group similar to or the same as that of the polymerizable liquid crystal compound constituting the horizontal alignment liquid crystal cured film, the adhesion between the horizontal alignment film and the horizontal alignment liquid crystal cured film tends to be increased, so it is preferable that the horizontal alignment film is formed from a polymer having a (meth)acryloyl group, and the horizontal alignment liquid crystal cured film is formed from a polymerizable liquid crystal composition containing a polymerizable liquid crystal compound having a (meth)acryloyl group.

[0155] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film forming composition") to a substrate, removing the solvent, and then irradiating the substrate with polarized light (preferably polarized UV). Photo-alignment films are also advantageous in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.

[0156] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that induce molecular alignment or are the origin of liquid crystal alignment ability, such as isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, caused by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.

[0157] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazole groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.

[0158] Among them, photoreactive groups involved in photodimerization reaction are preferred, and azo groups, cinnamoyl groups, and chalcone groups are preferred in that the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film excellent in thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, a polymer having an azo group or a cinnamoyl group is preferred, and a polymer having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred from the viewpoint of improving adhesion between the horizontal alignment film and the horizontal alignment liquid crystal cured film.

[0159] A photo-alignment layer can be formed on a substrate by applying the composition for forming a photo-alignment film on the substrate. The solvent contained in the composition can be the same as the solvents exemplified above as the solvents usable for the polymerizable liquid crystal composition, and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.

[0160] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the intended photo-alignment film, but is preferably at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, based on the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.

[0161] The method of applying the composition for forming a photo-alignment film to a substrate may be the same as the method of applying the oriented polymer composition to a substrate. Examples of the method of removing the solvent from the applied composition for forming a photo-alignment film include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0162] The polarized light may be irradiated by directly irradiating the polarized UV light onto the composition for forming a photo-aligned film coated on the substrate after removing the solvent, or by irradiating the polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The light from the light source can be irradiated by passing through an appropriate polarizer to irradiate the polarized UV light. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.

[0163] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.

[0164] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film with multiple equally spaced linear grooves, the liquid crystal molecules are aligned in the direction along the grooves.

[0165] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form an uneven pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to a substrate and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on a substrate to form unevenness, followed by curing.

[0166] The thickness of the alignment film (alignment film containing an alignment polymer or photoalignment film) is usually 100 to 5000 nm, preferably 100 to 1000 nm, more preferably 100 to 500 nm, further preferably 100 to 300 nm, and particularly preferably 100 to 250 nm. When the thickness of the alignment film is within the above range, it has sufficient horizontal alignment control power, and the alignment film in the laminate is less likely to suffer from cohesive failure.

[0167] When the optically anisotropic layer Y in the laminate of the present invention is formed of a vertically aligned liquid crystal cured film, In the vertical alignment liquid crystal cured film forming step, the vertical alignment liquid crystal cured film is, for example, A step of applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto a stretched film (optically anisotropic layer X) to obtain a coating film; drying the coating to form a dry coating; and A process of irradiating the dried coating with active energy rays to form a vertically aligned liquid crystal cured film. It is possible to produce a laminate having an optically anisotropic layer Y directly on an optically anisotropic layer X by the method comprising the steps of:

[0168] The formation of the coating film of the polymerizable liquid crystal composition can be carried out, for example, by coating the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film on a stretched film. The coating method of the polymerizable liquid crystal composition can be the same as the method that can be adopted in the production method of the horizontally aligned liquid crystal cured film.

[0169] In the vertical alignment liquid crystal cured film forming step, the vertical alignment liquid crystal cured film is, for example, A step of applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto the horizontally aligned liquid crystal cured film to obtain a coating film; drying the coating to form a dry coating; and A process of irradiating the dried coating with active energy rays to form a vertically aligned liquid crystal cured film. It is possible to produce a laminate having an optically anisotropic layer Y directly on an optically anisotropic layer X by the method comprising the steps of:

[0170] The formation of a coating film of the polymerizable liquid crystal composition can be carried out, for example, by coating a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film on a horizontally aligned liquid crystal cured film. Examples of a method for coating the polymerizable liquid crystal composition include the same methods as those that can be adopted in the method for producing a horizontally aligned liquid crystal cured film.

[0171] The coating film of the polymerizable liquid crystal composition can be formed, for example, by applying the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto the above-mentioned substrate. As the substrate, those exemplified in the method for producing a horizontally aligned liquid crystal cured film can be used. When the substrate is disposed in the laminate of the present invention, the substrate is preferably optically isotropic from the viewpoint of optical compensation described later. In the present invention, being optically isotropic means that the in-plane retardation value of the substrate is 3 nm or less.

[0172] In the laminate of the present invention, the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film may be laminated via another layer, as long as the effect of the present invention is not affected. Such another layer may be, for example, an adhesive layer. When the laminate of the present invention includes an adhesive layer, the thickness of the adhesive layer is preferably 0.1 to 30 μm, more preferably 0.5 to 20 μm.

[0173] Examples of the adhesive layer include pressure-sensitive adhesives and energy ray curable adhesives. Among these, acrylic adhesives, epoxy adhesives, and urethane adhesives are preferred because they have high transparency and excellent heat resistance.

[0174] The laminate of the present invention may also include, as the other layer, a cured resin layer or a hard coat layer intended to increase or reinforce the mechanical strength of the liquid crystal cured film. When the laminate of the present invention includes the other layer between the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film, the thickness of the other layer is preferably 0.1 to 4 μm, more preferably 0.5 to 3 μm. When the laminate of the present invention includes the other layer between the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film, the other layer may be formed after the horizontally aligned liquid crystal cured film is formed, and then a coating film of a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film may be formed on the other layer.

[0175] The cured resin layer can be formed from, for example, an acrylic resin, a methacrylic resin, an epoxy resin, an oxetane resin, a urethane resin, a melamine resin, etc. By providing the cured resin layer, even if the liquid crystal cured film formed adjacent to the cured resin layer is thin, the cured resin layer can sufficiently compensate for the strength of the liquid crystal cured film as a protective layer or a reinforcing layer.

[0176] After the coating film of the polymerizable liquid crystal composition is formed, the solvent is removed by drying or the like to form a dried coating film. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying. From the viewpoint of productivity, heat drying is preferred, and the heating temperature in this case is preferably such that the solvent can be removed and is equal to or higher than the phase transition temperature of the polymerizable liquid crystal compound. The procedure and conditions in this step may be the same as those that can be adopted in the manufacturing method of the horizontally aligned liquid crystal cured film.

[0177] The obtained dried coating film is irradiated with active energy rays (more specifically, ultraviolet rays, etc.) to polymerize the polymerizable liquid crystal compound while maintaining the state in which the polymerizable liquid crystal compound is aligned in the vertical direction relative to the coating film plane, thereby forming a vertically aligned liquid crystal cured film. As the polymerization method, a method similar to the method that can be adopted in the manufacturing method of the horizontally aligned liquid crystal cured film can be used.

[0178] The laminate of the present invention may be a laminate in which an optically anisotropic layer X is disposed on an optically anisotropic layer Y. A laminate in which an optically anisotropic layer X is disposed on an optically anisotropic layer Y is A step of applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto a substrate to obtain a coating film; drying the coating film to form a dry coating film; A step of irradiating the dried coating film with active energy rays to form a vertically aligned liquid crystal cured film; A step of applying a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film on the vertically aligned liquid crystal cured film to obtain a coating film; drying the coating to form a dry coating; and A step of irradiating the dried coating film with active energy rays to form a horizontally aligned liquid crystal cured film; It can be produced by a method comprising the steps of:

[0179] In the laminate of the present invention, when the optically anisotropic layer X is formed on the optically anisotropic layer Y, it is preferable to include a step of forming a horizontal alignment film by a horizontal alignment film forming step before forming the horizontal alignment liquid crystal cured film. Here, the horizontal alignment film forming step can be the same step as the method exemplified in the horizontal alignment liquid crystal cured film forming step described above.

[0180] [Polarizing Plate] The present invention includes a polarizing plate comprising the laminate of the present invention and a polarizing film. The polarizing film is a film having a polarizing function, and examples of the polarizing film include a stretched film having a dye having anisotropy adsorbed thereon, a film coated with a dye having anisotropy, and the like, which includes a polarizer, etc. Examples of the dye having anisotropy include a dichroic dye.

[0181] A film including, as a polarizer, a stretched film having adsorbed thereon a dye having absorption anisotropy is usually produced by uniaxially stretching a polyvinyl alcohol-based resin film, dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, treating the polyvinyl alcohol-based resin film having the adsorbed dichroic dye with an aqueous boric acid solution, and washing the film with water after the treatment with the aqueous boric acid solution, and then sandwiching the film between a transparent protective film via an adhesive on at least one surface of the polarizer produced through these steps.

[0182] Polyvinyl alcohol resins are obtained by saponifying polyvinyl acetate resins. As polyvinyl acetate resins, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith are used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.

[0183] The degree of saponification of the polyvinyl alcohol resin is usually about 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can also be used. The degree of polymerization of the polyvinyl alcohol resin is usually about 1,000 to 10,000, preferably in the range of 1,500 to 5,000.

[0184] Such a polyvinyl alcohol-based resin is used as a raw film for a polarizing film. The method for forming a film of the polyvinyl alcohol-based resin is not particularly limited, and the film can be formed by a known method. The thickness of the polyvinyl alcohol-based raw film can be, for example, about 10 to 150 μm.

[0185] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. It is also possible to perform the uniaxial stretching at these multiple stages. In the uniaxial stretching, the film may be uniaxially stretched between rolls having different peripheral speeds, or may be uniaxially stretched using a heated roll. The uniaxial stretching may be dry stretching in which the film is stretched in the air, or wet stretching in which the polyvinyl alcohol-based resin film is stretched in a swollen state using a solvent. The stretching ratio is usually about 3 to 8 times.

[0186] Dyeing of a polyvinyl alcohol-based resin film with a dichroic dye is carried out, for example, by a method of immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye.

[0187] Specifically, iodine or a dichroic organic dye is used as the dichroic pigment. Examples of the dichroic organic dye include a dichroic direct dye made of a disazo compound such as CIDIRECT RED 39, and a dichroic direct dye made of a compound such as trisazo or tetrakisazo. It is preferable that the polyvinyl alcohol resin film is immersed in water before the dyeing process.

[0188] When iodine is used as the dichroic dye, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing iodine and potassium iodide is usually adopted. The content of iodine in this aqueous solution is usually about 0.01 to 1 part by mass per 100 parts by mass of water. The content of potassium iodide is usually about 0.5 to 20 parts by mass per 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is usually about 20 to 40°C. The immersion time in this aqueous solution (dyeing time) is usually about 20 to 1,800 seconds.

[0189] On the other hand, when a dichroic organic dye is used as the dichroic pigment, a method of dyeing a polyvinyl alcohol resin film by immersing it in an aqueous solution containing a water-soluble dichroic dye is usually adopted. The content of the dichroic organic dye in this aqueous solution is usually 1×10 -4 ~10 parts by mass, preferably 1 × 10 -3 ~1 part by mass, more preferably 1 × 10 -3 ~1×10 -2 The amount of the dye in the aqueous solution is expressed by parts by mass. This aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing assistant. The temperature of the aqueous dichroic dye solution used for dyeing is usually about 20 to 80° C. The immersion time in the aqueous solution (dyeing time) is usually about 10 to 1,800 seconds.

[0190] The boric acid treatment after dyeing with a dichroic dye can usually be carried out by immersing the dyed polyvinyl alcohol resin film in an aqueous boric acid solution. The content of boric acid in this aqueous boric acid solution is usually about 2 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. When iodine is used as the dichroic dye, this aqueous boric acid solution preferably contains potassium iodide, and in this case, the content of potassium iodide is usually about 0.1 to 15 parts by mass, preferably 5 to 12 parts by mass, per 100 parts by mass of water. The immersion time in the aqueous boric acid solution is usually about 60 to 1,200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the boric acid treatment is usually 50°C or higher, preferably 50 to 85°C, and more preferably 60 to 80°C.

[0191] The polyvinyl alcohol-based resin film after the boric acid treatment is usually washed with water. The washing can be performed, for example, by immersing the boric acid-treated polyvinyl alcohol-based resin film in water. The temperature of the water used in the washing is usually about 5 to 40° C. The immersion time is usually about 1 to 120 seconds.

[0192] After washing with water, a drying treatment is carried out to obtain a polarizer. The drying treatment can be carried out, for example, using a hot air dryer or a far-infrared heater. The temperature of the drying treatment is usually about 30 to 100°C, and preferably 50 to 80°C. The time of the drying treatment is usually about 60 to 600 seconds, and preferably 120 to 600 seconds. The moisture content of the polarizer is reduced to a practical level by the drying treatment. The moisture content is usually about 5 to 20 mass%, and preferably 8 to 15 mass%. If the moisture content is less than 5 mass%, the polarizer loses its flexibility, and the polarizer may be damaged or broken after drying. If the moisture content exceeds 20 mass%, the thermal stability of the polarizer may be deteriorated.

[0193] The polyvinyl alcohol-based resin film is then uniaxially stretched, dyed with a dichroic dye, treated with boric acid, washed with water and dried to obtain a polarizer having a thickness preferably of 5 to 40 μm.

[0194] Examples of the film coated with a dye having absorption anisotropy include a film obtained by coating a composition containing a dichroic dye having liquid crystal properties or a composition containing a dichroic dye and a polymerizable liquid crystal. The film preferably has a protective film on one or both sides. Examples of the protective film include the same resin film as the above-mentioned example of a substrate that can be used for producing a horizontally aligned liquid crystal cured film.

[0195] The film coated with the dye having absorption anisotropy is preferably thin, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the film is usually 20 μm or less, preferably 5 μm or less, and more preferably 0.5 to 3 μm.

[0196] Specific examples of the film coated with a dye having absorption anisotropy include the films described in JP-A-2012-33249 and the like.

[0197] A transparent protective film may be laminated on at least one surface of the polarizer thus obtained, for example, via an adhesive layer. As the transparent protective film, a transparent film similar to the resin film exemplified above as the substrate usable for producing the liquid crystal cured film can be used.

[0198] The polarizing plate of the present invention is composed of the laminate of the present invention and a polarizing film, and can be obtained, for example, by laminating the laminate of the present invention and the polarizing film via a pressure-sensitive adhesive layer or the like.

[0199] In one embodiment of the present invention, when the laminate of the present invention and a polarizing film are laminated, a polarizing plate 20 including a polarizing film 3, an optically anisotropic layer X (layer 1 in FIG. 2), and an optically anisotropic layer Y (layer 2 in FIG. 2) in this order can be given as an example, as shown in FIG. 2. In this case, the polarizing plate of the present invention can be obtained by bonding a laminate including the optically anisotropic layer X and the optically anisotropic layer Y to the polarizing film 3 via a pressure-sensitive adhesive layer. In the present invention, when the polarizing film, the optically anisotropic layer X, and the optically anisotropic layer Y are laminated in this order, they are preferably laminated so that the angle between the slow axis (optical axis) of the optically anisotropic layer X constituting the laminate and the absorption axis of the polarizing film is 90±5°.

[0200] In one embodiment of the present invention, when the laminate of the present invention and a polarizing film are laminated, a polarizing plate 21 including a polarizing film 3, an optically anisotropic layer Y (layer 2 in FIG. 3), and an optically anisotropic layer X (layer 1 in FIG. 3) in this order can be given as an example. In this case, the polarizing plate of the present invention can be obtained by bonding a laminate including the optically anisotropic layer Y and the optically anisotropic layer X to the polarizing film 3 via a pressure-sensitive adhesive layer. In the present invention, when the polarizing film, the optically anisotropic layer Y, and the optically anisotropic layer X are laminated in this order, they are preferably laminated so that the angle between the slow axis (optical axis) of the optically anisotropic layer X constituting the laminate and the absorption axis of the polarizing film is 0±5°.

[0201] As the pressure-sensitive adhesive layer for bonding the polarizing film and the optically anisotropic layer X or the optically anisotropic layer Y, the same layer as exemplified as the other layer for bonding the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film can be used.

[0202] The polarizing plate of the present invention may have a structure similar to that of a conventional polarizing plate, or a polarizing film and a retardation film. Examples of such structures include an adhesive layer (sheet) for attaching the polarizing plate to a display element such as a liquid crystal display device, and a protective film used for protecting the surface of a polarizing film or a liquid crystal cured film from scratches and dirt.

[0203] The laminate and polarizing plate of the present invention can be used in various display devices. A display device is a device having a display element, and includes a light-emitting element or a light-emitting device as a light source. Examples of the display device include a liquid crystal display device, an organic electroluminescence (EL) display device, an inorganic electroluminescence (EL) display device, a touch panel display device, an electron emission display device (e.g., a field emission display device (FED) and a surface field emission display device (SED)), electronic paper (a display device using electronic ink or an electrophoretic element, a plasma display device, a projection type display device (e.g., a grating light valve (GLV) display device, a display device having a digital micromirror device (DMD)), and a piezoelectric ceramic display. The liquid crystal display device includes any of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection type liquid crystal display device. In particular, the laminate and the polarizing plate of the present invention can be suitably used in a liquid crystal display device because the effects thereof are easily exhibited, and it is particularly preferable to use them for an IPS (in-plane switching) liquid crystal display device. By using the laminate or the polarizing plate of the present invention, it is possible to easily realize a thin display device and obtain a display device that can exhibit the characteristics of preventing light leakage and color shift when the liquid crystal display device is viewed from an oblique direction during black display. EXAMPLES

[0204] The present invention will now be described in more detail with reference to the following examples. In the examples, "%" and "parts" mean "% by mass" and "parts by mass", respectively, unless otherwise specified.

[0205] 1. Example 1 (1) Preparation of composition for forming horizontal alignment film 5 parts by mass of a photoalignment material (weight average molecular weight: 30,000) having the following structure and 95 parts by mass of cyclopentanone (solvent) were mixed as components, and the resulting mixture was stirred at 80°C for 1 hour to obtain a composition for forming a horizontal alignment film.

[0206] [ka]

[0207] (2) Preparation of polymerizable liquid crystal compounds Polymerizable liquid crystal compound (X1) having the following molecular structure was produced according to the method described in JP 2010-31223 A. Compound (III-1-4) in which k2=4 of polymerizable liquid crystal compound (III-1) was produced according to the method described in JP 2010-270108 A.

[0208] Polymerizable liquid crystal compound (X1)

[0209] [ka]

[0210] (3) Preparation of polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film A polymerizable liquid crystal compound (X1) and a polymerizable liquid crystal compound LC242 represented by the following formula (LC242): PaliocolorLC242 (registered trademark of BASF) were mixed in a mass ratio of 65:35 to obtain a mixture. 0.1 parts by mass of a leveling agent "BYK-361N" (manufactured by BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one ("Irgacure (registered trademark) 369 (Irg369)" manufactured by BASF Japan Ltd.) were added as a photopolymerization initiator to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 10%. The mixture was stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film.

[0211] LC242: PaliocolorLC242 (registered trademark of BASF)

[0212] [ka]

[0213] (4) Formation of a horizontally aligned liquid crystal cured film After performing corona treatment on a COP film (ZF14-50) manufactured by Zeon Corporation, the composition for forming a horizontal alignment film was applied using a bar coater and dried at 80°C for 1 minute. After that, a polarized UV irradiation device (SPOT CURE SP-9; manufactured by Ushio Inc.) was used to irradiate the film with an integrated light amount of 100 mJ / cm at a wavelength of 313 nm. 2 The film thickness of the obtained horizontal alignment film was measured by an ellipsometer and found to be 200 nm. Next, a polymerizable liquid crystal composition (1) for forming a cured film for horizontal alignment liquid crystal was applied onto the horizontal alignment film, and heated at 120° C. for 60 seconds. After that, ultraviolet light was irradiated from the surface on which the polymerizable liquid crystal composition (1) for forming a cured film for horizontal alignment liquid crystal was applied using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (accumulated light amount at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2) to form an optically anisotropic layer X made of a horizontally aligned liquid crystal cured film. The thickness of the obtained horizontally aligned liquid crystal cured film was measured by an ellipsometer and found to be 1.4 μm.

[0214] <Measurement of phase difference of horizontally aligned liquid crystal cured film> The surface of the horizontally aligned liquid crystal cured film of the laminate consisting of the above-mentioned substrate, horizontal alignment film, and horizontally aligned liquid crystal cured film was subjected to corona treatment, and the laminate was then attached to glass via a 25 μm pressure-sensitive adhesive manufactured by Lintec Corporation. After confirming that the substrate had no phase difference, the obtained laminate consisting of glass, adhesive, horizontally aligned liquid crystal cured film, horizontal alignment film, and substrate was measured for Re(450) and Re(550) of the horizontally aligned liquid crystal cured film using KOBRA-WPR manufactured by Oji Scientific Instruments Co., Ltd., and A=Re(450) / Re(550) was calculated. The results are shown in Table 1.

[0215] (5) Preparation of polymerizable liquid crystal composition (1) for forming vertically aligned liquid crystal cured film The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: PaliocolorLC242 (BASF registered trademark) were mixed in a mass ratio of 70:30 to obtain a mixture. To 100 parts by mass of the obtained mixture, 0.25 parts by mass of a leveling agent "F-556" (DIC Corporation), 1.5 parts by mass of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of a silane coupling agent "KBE-9103" (Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") were added as a photopolymerization initiator. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. This mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film.

[0216] Ionic compound A:

[0217] [ka]

[0218] (6) Formation of vertically aligned liquid crystal cured film After carrying out a corona treatment on the horizontally aligned liquid crystal cured film of the laminate consisting of the substrate, the horizontally aligned film, and the horizontally aligned liquid crystal cured film prepared as described above, the polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, while still heated to 120° C., ultraviolet light was irradiated from the surface coated with the polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ). 2 ) to form an optically anisotropic layer Y made of a vertically aligned liquid crystal cured film, and a laminate was obtained in which the substrate, the horizontal alignment film, the horizontally aligned liquid crystal cured film, and the vertically aligned liquid crystal cured film were laminated adjacent to each other in this order. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and was found to be 1.0 μm.

[0219] <Measurement of phase difference of vertically aligned liquid crystal cured film> The vertically aligned liquid crystal cured film surface of the laminate consisting of the substrate, horizontal alignment film, horizontal alignment liquid crystal cured film, and vertical alignment liquid crystal cured film prepared by the above procedure was subjected to corona treatment, and the laminate was attached to glass via a 25 μm pressure-sensitive adhesive manufactured by Lintec Corporation. After confirming in advance that the substrate had no phase difference, the obtained laminate was measured using KOBRA-WPR manufactured by Oji Scientific Instruments Co., Ltd. by changing the incident angle of light on the sample for measuring optical properties to measure the in-plane phase difference value of the laminate including the vertically aligned liquid crystal cured film and the horizontally aligned liquid crystal cured film, and the phase difference value when tilted 50° from the fast axis center. In addition, the in-plane phase difference value of the laminate consisting of glass, adhesive, horizontally aligned liquid crystal cured film, horizontal alignment film, and substrate, and the phase difference value when tilted 50° from the fast axis center were measured by the same method. Next, the average refractive index at each wavelength for each of the vertically aligned liquid crystal cured film and the horizontally aligned liquid crystal cured film was measured using an ellipsometer M-220 manufactured by JASCO Corporation. The film thickness was also measured using an Optical NanoGauge film thickness meter C12562-01 manufactured by Hamamatsu Photonics K.K. The three-dimensional refractive index was calculated from the in-plane retardation value, the retardation value when tilted 50° to the center of the fast axis, the average refractive index, and the film thickness values, with reference to Oji Measuring Instruments Technical Documents (http: / / www.oji-keisoku.co.jp / products / kobra / reference.html). From the obtained three-dimensional refractive index, the optical properties of the laminate including the vertically aligned liquid crystal cured film and the horizontally aligned liquid crystal cured film, and the horizontally aligned liquid crystal cured film were calculated according to the following formula, and the values ​​of Rth(450) and Rth(550) of the vertically aligned liquid crystal cured film were calculated from the difference between the respective values, and B=Rth(450) / Rth(550) was calculated. The results are shown in Table 1.

[0220] (7) Evaluation of the laminate <Check the black display> A pressure-sensitive adhesive layer and a polarizing film were laminated in this order on the substrate side surface of the laminate produced in Example 1 to form a polarizing plate. At this time, the polarizing film was laminated so that the angle between the absorption axis and the slow axis of the optically anisotropic layer X of the laminate was 90 degrees. The obtained polarizing plate was attached to the viewing side of an i-Pad (registered trademark) (manufactured by Apple Inc.) from which the viewing side polarizing plate had been removed so that the polarizing film was the outermost surface, and light leakage when black was displayed was visually confirmed from a direction of an azimuth angle of 45° and an elevation angle of 45° with respect to the panel surface, and color loss was judged according to the following criteria. The results are shown in Table 1. Evaluation criteria: A: There is almost no coloring when viewed from an oblique angle. B: Slight discoloration is observed when viewed from an oblique angle. C: Strong coloring is observed when viewed from an oblique angle.

[0221] <Confirmation of characteristic changes due to heat> The laminate consisting of the substrate, horizontal alignment film, horizontal alignment liquid crystal cured film, and vertical alignment liquid crystal cured film produced in Example 1 was placed in an oven at 80° C. and left to stand for 30 minutes. When the in-plane retardation value of the laminate that had been subjected to the above treatment was measured, the change in retardation value compared to before heating was 1 nm or less, confirming that the change in characteristics due to heat was small.

[0222] 2. Example 2 Except for the preparation of the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film and the formation of the vertically aligned liquid crystal cured film, a laminate was prepared in the same manner as in Example 1, in which a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, and a vertical alignment liquid crystal cured film were laminated adjacent to each other in this order. Also, in the same manner as in Example 1, a polarizing plate was prepared by laminating a polarizing film on the surface on the substrate side, and the visibility during black display was confirmed. The results are shown in Table 1.

[0223] (1) Preparation of polymerizable liquid crystal composition (2) for forming vertically aligned liquid crystal cured film Polymerizable liquid crystal compound (X1) and polymerizable liquid crystal compound LC242: PaliocolorLC242 (BASF registered trademark) were mixed in a mass ratio of 50:50 to obtain a mixture. 0.25 parts by mass of leveling agent "F-556" (DIC Corporation), 1.5 parts by mass of ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of silane coupling agent "KBE-9103" (Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. This mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film.

[0224] (2) Preparation of vertically aligned liquid crystal cured film After a corona treatment was performed on the surface of the horizontally aligned liquid crystal cured film of a laminate consisting of a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film prepared in the same manner as in Example 1, a polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, ultraviolet light was irradiated from the surface coated with the polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ). 2 ) to form an optically anisotropic layer Y made of a vertically aligned liquid crystal cured film. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 1.4 μm. The laminate made of the substrate, horizontal alignment film, horizontal alignment liquid crystal cured film, and vertical alignment liquid crystal cured film was placed in an oven at 80° C. and left to stand for 30 minutes, and the in-plane retardation value of the laminate subjected to the above treatment was measured. The change in retardation value compared to before heating was 1 nm or less, and it was confirmed that the change in characteristics due to heat was small.

[0225] 3. Example 3 Except for the preparation of the polymerizable liquid crystal composition for forming the horizontally aligned liquid crystal cured film and the formation of the horizontally aligned liquid crystal cured film, a laminate was prepared in the same manner as in Example 1, in which a substrate, a horizontally aligned liquid crystal cured film, a horizontally aligned liquid crystal cured film, and a vertically aligned liquid crystal cured film were laminated adjacent to each other in this order. Also, in the same manner as in Example 1, a polarizing plate was prepared by laminating a polarizing film on the surface on the substrate side, and the visibility during black display was confirmed. The results are shown in Table 1.

[0226] (1) Preparation of polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film A polymerizable liquid crystal compound (X1) and polymerizable liquid crystal compound LC242: PaliocolorLC242 (BASF registered trademark) were mixed in a mass ratio of 50:50 to obtain a mixture. 0.1 parts by mass of a leveling agent "BYK-361N" (BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") were added as a photopolymerization initiator to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. The mixture was stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film.

[0227] (2) Formation of a horizontally aligned liquid crystal cured film As in Example 1, a horizontal alignment film was formed on a substrate, and then the polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film was applied onto the horizontal alignment film. The film was heated at 120° C. for 60 seconds, and then ultraviolet light was irradiated from the surface onto which the polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film was applied using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (accumulated light amount at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2 ) to form an optically anisotropic layer X made of a horizontally aligned liquid crystal cured film. The thickness of the obtained horizontally aligned liquid crystal cured film was measured by an ellipsometer and found to be 1.3 μm. A vertically aligned liquid crystal cured film was formed on the horizontally aligned liquid crystal cured film of the laminate consisting of the substrate, horizontally aligned film, and horizontally aligned liquid crystal cured film prepared as described above in the same manner as in Example 1 to obtain a laminate, and a polarizing film was attached to the substrate side to obtain a polarizing plate. The laminate consisting of the substrate, horizontally aligned film, horizontally aligned liquid crystal cured film, and vertically aligned liquid crystal cured film prepared as described above was placed in an oven at 80°C and left to stand for 30 minutes, and the in-plane retardation value of the laminate subjected to the above treatment was measured. It was confirmed that the change in retardation value was 1 nm or less compared to before heating, and that the change in characteristics due to heat was small.

[0228] 4. Example 4 Using the polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film prepared in Example 3, a laminate was prepared by laminating a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film having a thickness of 1.4 μm adjacent to each other in the same manner as in Example 3. Next, using the polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film, a vertically aligned liquid crystal cured film having a thickness of 1.4 μm was formed on the horizontally aligned liquid crystal cured film in the same manner as in Example 2 to obtain a laminate, and a polarizing film was attached to the surface on the substrate side to prepare a polarizing plate, and the visibility during black display was confirmed. The results are shown in Table 1. The laminate consisting of the substrate, horizontally aligned film, horizontally aligned liquid crystal cured film, and vertically aligned liquid crystal cured film produced was placed in an oven at 80° C. and left for 30 minutes, and the in-plane retardation value of the laminate subjected to the above treatment was measured. It was confirmed that the change in retardation value was 1 nm or less compared to before heating, and that the characteristic change due to heat was small.

[0229] 5. Example 5 Except for the preparation of the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film and the formation of the vertically aligned liquid crystal cured film, a laminate was prepared in the same manner as in Example 3, in which a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, and a vertical alignment liquid crystal cured film were laminated adjacent to each other in this order. Also, in the same manner as in Example 3, a polarizing plate was prepared by laminating a polarizing film on the surface on the substrate side, and the visibility during black display was confirmed. The results are shown in Table 1.

[0230] (1) Preparation of polymerizable liquid crystal composition (3) for forming vertically aligned liquid crystal cured film Polymerizable liquid crystal compound (X1) and polymerizable liquid crystal compound LC242: PaliocolorLC242 (BASF registered trademark) were mixed in a mass ratio of 30:70 to obtain a mixture. 0.25 parts by mass of leveling agent "F-556" (DIC Corporation), 1.5 parts by mass of ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of silane coupling agent "KBE-9103" (Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. This mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (3) for forming a vertically aligned liquid crystal cured film.

[0231] (2) Preparation of vertically aligned liquid crystal cured film Using the polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film prepared in Example 3, a laminate was prepared in the same manner as in Example 3, in which a substrate, a horizontal alignment film, and a horizontally aligned liquid crystal cured film having a thickness of 1.5 μm were laminated adjacent to each other in this order. Next, a corona treatment was performed on the surface of the horizontally aligned liquid crystal cured film, and then a polymerizable liquid crystal composition (3) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.), ultraviolet light was irradiated from the surface coated with the polymerizable liquid crystal composition (3) for forming a vertically aligned liquid crystal cured film (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm ). 2) to form an optically anisotropic layer Y made of a vertically aligned liquid crystal cured film. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 1.3 μm. The laminate made of the substrate, horizontal alignment film, horizontal alignment liquid crystal cured film, and vertical alignment liquid crystal cured film was placed in an oven at 80° C. and left to stand for 30 minutes, and the in-plane retardation value of the laminate subjected to the above treatment was measured. The change in retardation value compared to before heating was 1 nm or less, and it was confirmed that the change in characteristics due to heat was small.

[0232] 6. Example 6 A laminate was prepared in the same manner as in Example 4, except that the preparation of the polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film and the formation of the horizontally aligned liquid crystal cured film were changed as follows. A laminate was prepared by laminating a substrate, a horizontally aligned liquid crystal cured film, a horizontally aligned liquid crystal cured film, and a vertically aligned liquid crystal cured film adjacent to each other in this order. A polarizing plate was also prepared by laminating a polarizing film on the substrate side in the same manner as in Example 4, and the visibility during black display was confirmed. The results are shown in Table 1.

[0233] (1) Preparation of polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film A mixture was obtained by mixing the polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242:PaliocolorLC242 (BASF registered trademark) in a mass ratio of 30:70. 0.1 parts by mass of a leveling agent "BYK-361N" (BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. The mixture was stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film.

[0234] (2) Formation of a horizontally aligned liquid crystal cured film As in Example 4, a horizontal alignment film was formed on a substrate, and then the polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film was applied onto the horizontal alignment film. The film was heated at 120° C. for 60 seconds, and then ultraviolet light was irradiated from the surface onto which the polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film was applied using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (accumulated light amount at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2 ) to form an optically anisotropic layer X made of a horizontally aligned liquid crystal cured film. The thickness of the obtained horizontally aligned liquid crystal cured film was measured by an ellipsometer and found to be 1.1 μm. A vertically aligned liquid crystal cured film having a thickness of 0.9 μm was formed on the horizontally aligned liquid crystal cured film of the laminate made of the substrate, horizontally aligned film, and horizontally aligned liquid crystal cured film, in the same manner as in Example 4, using the polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film to obtain a laminate, and a polarizing plate was obtained by laminating a polarizing film on the surface on the substrate side. The laminate made of the substrate, horizontally aligned film, horizontally aligned liquid crystal cured film, and vertically aligned liquid crystal cured film was placed in an oven at 80° C. and left to stand for 30 minutes, and the in-plane retardation value of the laminate treated as described above was measured. The change in retardation value was 1 nm or less compared to before heating, and it was confirmed that the characteristic change due to heat was small.

[0235] 7. Example 7 Using the polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film prepared in Example 6, a laminate was prepared by laminating a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film having a thickness of 1.2 μm adjacent to each other in this order, in the same manner as in Example 6. Next, in the same manner as in Example 5, the polymerizable liquid crystal composition (3) for forming a vertically aligned liquid crystal cured film was applied onto the horizontally aligned liquid crystal cured film to form a vertically aligned liquid crystal cured film having a thickness of 1.2 μm to obtain a laminate, and a polarizing film was attached to the surface on the substrate side to prepare a polarizing plate, and the visibility during black display was confirmed. The results are shown in Table 1. The laminate consisting of the substrate, horizontally aligned film, horizontally aligned liquid crystal cured film, and vertically aligned liquid crystal cured film produced was placed in an oven at 80° C. and left for 30 minutes, and the in-plane retardation value of the laminate subjected to the above treatment was measured. It was confirmed that the change in retardation value was 1 nm or less compared to before heating, and that the characteristic change due to heat was small.

[0236] 8. Example 8 In the same manner as in Example 3, a laminate was prepared by laminating a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, and a vertical alignment liquid crystal cured film adjacent to each other in this order. Next, a polarizing film was attached to the surface of the vertical alignment liquid crystal cured film side using an adhesive to form a polarizing plate. At this time, the polarizing film was laminated so that the angle between the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X of the laminate was 0 degrees. The obtained polarizing plate was attached to the viewing side of an i-Pad (registered trademark) (manufactured by Apple Inc.) from which the viewing side polarizing plate had been removed so that the polarizing film was the outermost surface, and light leakage when black was displayed was visually confirmed from a direction of an azimuth angle of 45° and an elevation angle of 45° with respect to the panel surface. The results are shown in Table 1.

[0237] 9. Example 9 In the same manner as in Example 4, a laminate was prepared by laminating a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, and a vertical alignment liquid crystal cured film adjacent to each other in this order. Next, a polarizing film was attached to the surface of the vertical alignment liquid crystal cured film side using an adhesive to form a polarizing plate. At this time, the polarizing film was laminated so that the angle between the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X of the laminate was 0 degrees. The visibility of the obtained polarizing plate during black display was confirmed in the same manner as in Example 8. The results are shown in Table 1.

[0238] 10. Comparative Example 1 A laminate was prepared in the same manner as in Example 3, except that the preparation of the polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film and the formation of the horizontally aligned liquid crystal cured film were changed as follows. A laminate was prepared by laminating a substrate, a horizontally aligned liquid crystal cured film, a horizontally aligned liquid crystal cured film, and a vertically aligned liquid crystal cured film adjacent to each other in this order. A polarizing plate was also prepared by laminating a polarizing film on the substrate side in the same manner as in Example 3, and the visibility during black display was confirmed. The results are shown in Table 1.

[0239] (1) Preparation of polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal cured film To the polymerizable liquid crystal compound (III-1-4), 0.1 parts by mass of a leveling agent "BYK-361N" (manufactured by BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd.'s "Irgacure (registered trademark) 369 (Irg369)") were added as a photopolymerization initiator. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. The mixture was stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal cured film.

[0240] (2) Formation of a horizontally aligned liquid crystal cured film As in Example 4, a horizontal alignment film was formed on a substrate, and then the polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal cured film was applied onto the horizontal alignment film. The film was heated at 120° C. for 60 seconds, and then ultraviolet light was irradiated from the surface onto which the polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal cured film was applied using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) (accumulated light amount at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2 ) to form an optically anisotropic layer X' made of a horizontally aligned liquid crystal cured film. The thickness of the obtained horizontally aligned liquid crystal cured film was measured by an ellipsometer and found to be 0.9 μm. A vertically aligned liquid crystal cured film having a thickness of 1.0 μm was formed on the horizontally aligned liquid crystal cured film of the laminate consisting of the substrate, horizontally aligned film, and horizontally aligned liquid crystal cured film prepared as described above, in the same manner as in Example 3, to obtain a laminate, and a polarizing plate was obtained by laminating a polarizing film to the surface on the substrate side.

[0241] 11. Comparative Example 2 Except for the preparation of the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film and the formation of the vertically aligned liquid crystal cured film, a laminate was prepared in the same manner as in Example 1, in which a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film, and a vertical alignment liquid crystal cured film were laminated adjacent to each other in this order. Also, a polarizing plate was prepared by laminating a polarizing film on the substrate side in the same manner as in Example 3, and the visibility during black display was confirmed. The results are shown in Table 1.

[0242] (1) Preparation of polymerizable liquid crystal composition (4) for forming vertically aligned liquid crystal cured film To the polymerizable liquid crystal compound (III-1-4), 0.25 parts by mass of a leveling agent "F-556" (manufactured by DIC Corporation), 1.5 parts by mass of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") were added as a photopolymerization initiator. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. The mixture was stirred at 80 ° C. for 1 hour to obtain a polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film.

[0243] (2) Preparation of vertically aligned liquid crystal cured film Using the polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film prepared in Example 1, a laminate was prepared in the same manner as in Example 3, in which a substrate, a horizontal alignment film, and a horizontally aligned liquid crystal cured film having a thickness of 1.6 μm were laminated adjacent to each other in this order. Next, a corona treatment was performed on the surface of the horizontally aligned liquid crystal cured film, and then a polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.), ultraviolet light was irradiated from the surface coated with the polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm ). 2 ) to form an optically anisotropic layer Y' made of a vertically aligned liquid crystal cured film. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and was found to be 0.8 μm.

[0244] 12. Comparative Example 3 A retardation film (ZEONORFILM, manufactured by Optes Co., Ltd.) made of a cycloolefin resin with a thickness of 32 μm and an in-plane retardation value of 140 nm was used as a substrate, and after a corona treatment was performed on the substrate surface in the same manner as in Comparative Example 2, a polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, ultraviolet light was irradiated from the surface coated with the polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film using a high-pressure mercury lamp (UNICURE VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ). 2 ) to form a vertically aligned liquid crystal cured film, thereby producing a laminate in which an optically anisotropic layer X made of a substrate and an optically anisotropic layer Y' made of a vertically aligned liquid crystal cured film were laminated adjacent to each other in this order. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 0.8 μm. In addition, a polarizing film was attached to the surface on the substrate side to produce a polarizing plate, and the visibility during black display was confirmed. The results are shown in Table 1. In addition, a laminate consisting of a substrate and a vertically aligned liquid crystal cured film was placed in an oven at 80°C and left to stand for 30 minutes, and the in-plane retardation value of the laminate that had been subjected to the above treatment was measured. As a result, the change in retardation value compared to before heating was 2 nm or more, and it was confirmed that the characteristic change due to heat was large.

[0245] 13. Comparative Example 4 Using the polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film prepared in Example 1, a laminate was prepared by laminating a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film having a thickness of 1.1 μm adjacent to each other in this order in the same manner as in Example 1. Next, in the same manner as in Example 1, a polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film was applied onto the horizontally aligned liquid crystal cured film to form a vertically aligned liquid crystal cured film having a thickness of 1.3 μm to obtain a laminate, and a polarizing plate was prepared by laminating a polarizing film on the surface on the substrate side, and the visibility during black display was confirmed. The results are shown in Table 1.

[0246] 14. Example 10 (1) Preparation of polymerizable liquid crystal composition (5) for forming vertically aligned liquid crystal cured film A mixture was obtained by mixing the polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: PaliocolorLC242 (BASF registered trademark) in a mass ratio of 60:40. 0.25 parts by mass of a leveling agent "F-556" (DIC Corporation), 1.5 parts by mass of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of a silane coupling agent "KBE-9103" (Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (BASF Japan Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 parts by mass of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%. This mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (5) for forming a vertically aligned liquid crystal cured film.

[0247] (2) Preparation of vertically aligned liquid crystal cured film A retardation film made of a cycloolefin resin was used as a substrate, and the substrate surface was subjected to a corona treatment in the same manner as in Comparative Example 3. Then, a polymerizable liquid crystal composition (5) for forming a vertically aligned liquid crystal cured film was applied using a bar coater, and the substrate was heated at 120° C. for 60 seconds. Next, a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) was used to irradiate ultraviolet light from the surface coated with the polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film (under a nitrogen atmosphere, accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ). 2 ) to form a vertically aligned liquid crystal cured film, thereby producing a laminate in which an optically anisotropic layer X made of a substrate and an optically anisotropic layer Y' made of a vertically aligned liquid crystal cured film were laminated adjacent to each other in this order. The thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 1.2 μm. In addition, a polarizing film was attached to the surface on the substrate side to produce a polarizing plate, and the visibility during black display was confirmed. The results are shown in Table 1.

[0248] 15. Example 11 A retardation film made of a cycloolefin resin was used as a substrate, and a corona treatment was performed on the substrate surface in the same manner as in Comparative Example 3. Next, the polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film was applied onto the corona-treated substrate surface using a bar coater in the same manner as in Example 9, and a vertically aligned liquid crystal cured film having a thickness of 1.3 μm was formed on the substrate to obtain a laminate, and a polarizing film was attached to the substrate side to produce a polarizing plate, and the visibility during black display was confirmed.

[0249] 16. Example 12 A retardation film made of a cycloolefin resin was used as a substrate, and a corona treatment was performed on the substrate surface in the same manner as in Comparative Example 3. Then, a polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film was applied using a bar coater in the same manner as in Example 1 to form a vertically aligned liquid crystal cured film having a thickness of 1.0 μm on the substrate, thereby obtaining a laminate. A polarizing film was attached to the substrate side to produce a polarizing plate, and the visibility during black display was confirmed.

[0250] 17. Example 13 A retardation film made of a cycloolefin resin was used as a substrate, and a corona treatment was performed on the substrate surface in the same manner as in Comparative Example 3. Then, a polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film was applied using a bar coater in the same manner as in Example 1 to form a vertically aligned liquid crystal cured film having a thickness of 1.1 μm on the substrate, thereby obtaining a laminate. A polarizing film was attached to the substrate side to produce a polarizing plate, and the visibility during black display was confirmed.

[0251] [Table 1]

[0252] According to the present invention, it is possible to provide a laminate which is thin and exhibits little change in characteristics due to heat, a polarizing plate including the laminate, and an image display device having these. [Explanation of symbols]

[0253] 1: Optically anisotropic layer X 2: Optically anisotropic layer Y 3: Polarizing film 10: Laminate 20: Polarizing plate 21: Polarizing plate

Claims

1. The optically anisotropic layer X satisfies the following formula (1), and the optically anisotropic layer Y satisfies the following formula (2), A laminate satisfying the following formula (3): 0.960≦A≦1.040 (1) 0.960≦B≦1.040 (2) -1.20≦D / C≦0.60 (3) [In formula (1), A represents the ratio (Re(450) / Re(550)) of the in-plane retardation value (Re(450)) at a wavelength of 450 nm of the optically anisotropic layer X to the in-plane retardation value (Re(550)) at a wavelength of 550 nm. In formula (2), B represents the ratio (Rth(450) / Rth(550)) of the retardation value (Rth(450)) in the thickness direction at a wavelength of 450 nm of the optically anisotropic layer Y to the retardation value (Rth(550)) in the thickness direction at a wavelength of 550 nm. In formula (3), C represents the in-plane retardation value (Re(550)) of the optically anisotropic layer X at a wavelength of 550 nm, and D represents the retardation value (Rth(550)) in the thickness direction at a wavelength of 550 nm of the optically anisotropic layer Y.]

2. 2. The laminate according to claim 1, wherein the optically anisotropic layer X has a thickness of 0.5 μm or more and 5 μm or less.

3. The laminate according to claim 1 , wherein the optically anisotropic layer Y has a thickness of 0.3 μm or more and 5 μm or less.

4. A polarizing plate comprising a polarizing film, the optically anisotropic layer X according to claim 1, and the optically anisotropic layer Y according to claim 1 in this order.

5. A polarizing plate comprising a polarizing film, the optically anisotropic layer Y according to claim 1, and the optically anisotropic layer X according to claim 1, in this order.

6. 5. The polarizing plate according to claim 4, wherein the angle between the absorption axis of said polarizing film and the slow axis of said optically anisotropic layer X is 90±5°.

7. 6. The polarizing plate according to claim 5, wherein the angle between the absorption axis of said polarizing film and the slow axis of said optically anisotropic layer X is 0±5°.

8. An image display comprising the polarizing plate according to any one of claims 4 to 7.

Citation Information

Patent Citations

  • Liquid crystal panel and liquid crystal display

    JP2009139747A