Method for producing sulfide solid electrolyte

A novel sulfide solid electrolyte composition with optimized diffraction peak ratios and production methods enhances ionic conductivity and reduces hydrogen sulfide generation, addressing limitations in existing electrolytes for lithium-ion batteries.

JP2024144750AActive Publication Date: 2024-10-11IDEMITSU KOSAN CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024130602
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-05-02
Filing Date
2024-08-07
Publication Date
2024-10-11
Estimated Expiration
2037-08-08

AI Technical Summary

Technical Problem

Existing sulfide solid electrolytes for lithium-ion batteries have limitations in ionic conductivity and are prone to hydrogen sulfide generation due to moisture reaction, necessitating improvements for enhanced performance and safety.

Method used

A novel sulfide solid electrolyte composition containing lithium, phosphorus, sulfur, chlorine, and bromine, with specific diffraction peak ratios and molar ratios, is produced through mechanical stress followed by heat treatment, forming a high ionic conductivity argyrodite crystal structure that minimizes hydrogen sulfide generation.

Benefits of technology

The new electrolyte exhibits higher ionic conductivity and reduced hydrogen sulfide production, improving the safety and efficiency of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144750000013
    Figure 2024144750000013
  • Figure 2024144750000014
    Figure 2024144750000014
  • Figure 2024144750000015
    Figure 2024144750000015
Patent Text Reader

Abstract

To provide a novel method for producing a sulfide solid electrolyte having higher ionic conductivity.SOLUTION: A method for producing a sulfide solid electrolyte containing Argyrodite-type crystal includes: a process of pulverizing and mixing a raw material containing lithium, phosphorus, sulfur, chlorine and bromine with a pulverizer to fabricate an intermediate; and a process of performing heat treatment to the intermediate at 350 to 480°C, where a molar ratio c(Cl / P) of the chlorine to phosphorus and a molar ratio d(Br / P) of the bromine to phosphorus in the raw material satisfy the following formula (1). 1.2<c+d<1.9...(1)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a sulfide solid electrolyte. [Background technology]

[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Among these batteries, lithium-ion batteries have attracted attention because of their high energy density.

[0003] Currently commercially available lithium-ion batteries use electrolytes that contain flammable organic solvents, so they require improvements in structure and materials to prevent short circuits and the installation of safety devices to suppress temperature rises during short circuits.In contrast, lithium-ion batteries, which use a solid electrolyte to create a fully solid-state battery, do not use flammable organic solvents within the battery, so safety devices can be simplified and they are thought to be superior in terms of manufacturing costs and productivity.

[0004] Sulfide solid electrolytes are known as solid electrolytes used in lithium ion batteries. Various crystal structures of sulfide solid electrolytes are known, one of which is the argyrodite-type crystal structure. Patent documents 1 to 5 and non-patent documents 1 to 3 disclose an argyrodite-type crystal structure containing one type of halogen. Non-patent documents 4 and 5 disclose Li 6 P.S. 5 Cl 1-x Br x A solid electrolyte having the composition has been reported, and an argyrodite-type crystal structure containing two types of halogen has been disclosed. Some argyrodite-type crystal structures have high lithium ion conductivity. However, further improvement in ion conductivity is required. In addition, sulfide-based solid electrolytes generally have the problem that they may react with moisture in the air to generate hydrogen sulfide. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2010-540396 [Patent Document 2] International Publication WO2015 / 011937 [Patent Document 3] International Publication WO2015 / 012042 [Patent Document 4] JP 2016-24874 A [Patent Document 5] International Publication WO2016 / 104702 [Non-patent literature]

[0006] [Non-Patent Document 1] Angew.chem Vol.47(2008),No.4,P.755-758 [Non-Patent Document 2] Phys.Status.Solidi Vol.208(2011),No.8,P.1804-1807 [Non-Patent Document 3] Solid State Ionics Vol.221(2012)P.1-5 [Non-Patent Document 4] Abstracts of the 82nd Electrochemical Society Meeting (2015), 2H08 [Non-Patent Document 5] Proceedings of the 94th Annual Meeting of the Chemical Society of Japan, 2014, II, P.474, 1 H2-50 Summary of the Invention [Problem to be solved by the invention]

[0007] One of the objects of the present invention is to provide a novel sulfide solid electrolyte having higher ionic conductivity. Another object of the present invention is to provide a novel sulfide solid electrolyte that suppresses the generation of hydrogen sulfide due to reaction with moisture in the air. [Means for solving the problem]

[0008] According to one embodiment of the present invention, there is provided a novel sulfide solid electrolyte that contains lithium, phosphorus, sulfur, chlorine, and bromine, and has a diffraction peak A at 2θ=25.2±0.5 deg and a diffraction peak B at 2θ=29.7±0.5 deg in powder X-ray diffraction using CuKα radiation, the diffraction peak A and the diffraction peak B satisfy the following formula (A), and the molar ratio c (Cl / P) of chlorine to phosphorus and the molar ratio d (Br / P) of bromine to phosphorus satisfy the following formula (1). 1.2 <c+d<1.9···(1) 0.845 A / S B <1.200···(A) (In the formula, S A indicates the area of ​​the diffraction peak A, and S B indicates the area of ​​the diffraction peak B. According to one embodiment of the present invention, there is provided an electrode mixture containing the above-mentioned sulfide solid electrolyte and an active material. According to one embodiment of the present invention, there is provided a lithium ion battery including at least one of the sulfide solid electrolyte and the electrode mixture. Effect of the Invention

[0009] According to one embodiment of the present invention, a sulfide solid electrolyte having high ionic conductivity can be provided. Moreover, according to one embodiment of the present invention, it is possible to provide a sulfide solid electrolyte in which the amount of hydrogen sulfide generated by reaction with moisture in the air is suppressed. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a plan view of an example of a multi-shaft kneader used in producing a sulfide solid electrolyte, taken along the center of the rotation shaft. [Diagram 2] FIG. 2 is a plan view of a portion of a rotating shaft where a paddle is provided in an example of a multi-shaft kneader used in producing a sulfide solid electrolyte, cut perpendicularly to the rotating shaft. [Diagram 3] ​1 is an X-ray diffraction pattern of the sulfide solid electrolyte obtained in Example 1. [Figure 4] 1 is an X-ray diffraction pattern of the sulfide solid electrolyte obtained in Comparative Example 2. [Diagram 5] FIG. 2 is an explanatory diagram of an apparatus used for evaluating the amount of hydrogen sulfide generated from a sulfide solid electrolyte. [Figure 6] 1 shows the results of a structure analysis of the sulfide solid electrolyte obtained in Example 1 using synchrotron radiation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The sulfide solid electrolyte according to one embodiment of the present invention contains lithium (Li), phosphorus (P), sulfur (S), chlorine (Cl), and bromine (Br) as constituent elements, and is characterized in that, in powder X-ray diffraction using CuKα radiation, it has a diffraction peak A at 2θ=25.2±0.5 deg and a diffraction peak B at 29.7±0.5 deg, and the diffraction peaks A and B satisfy the following formula (A). 0.845 A / S B <1.200···(A) (In the formula, S A is the area of ​​the diffraction peak A, and S B indicates the area of ​​diffraction peak B.)

[0012] Diffraction peak A and diffraction peak B are peaks derived from the argyrodite-type crystal structure. In addition to diffraction peak A and diffraction peak B, the diffraction peak of the argyrodite-type crystal structure may also appear at 2θ=15.3±0.5 deg, 17.7±0.5 deg, 31.1±0.5 deg, 44.9±0.5 deg, or 47.7±0.5 deg, for example. The sulfide solid electrolyte of the present embodiment may have these peaks.

[0013] ​In the present application, the position of the diffraction peak is judged as A±0.5 deg when the median is A, but it is preferable that it is A±0.3 deg. For example, in the case of the above-mentioned diffraction peak at 2θ=25.2±0.5 deg, the median A is 25.2 deg, and it is preferable that it is in the range of 2θ=25.2±0.3 deg. The same applies to the judgment of all other diffraction peak positions in the present application.

[0014] The sulfide solid electrolyte of the present embodiment satisfies the above formula (A), and thus has a higher ionic conductivity than a conventional solid electrolyte containing an argyrodite-type crystal structure. The above formula (A) is expressed by the area ratio of the diffraction peaks (S A / S B ) is larger than that of conventional solid electrolytes containing an argyrodite-type crystal structure. A / S B ) is preferably 0.850 or more and 1.150 or less, and more preferably 0.860 or more and 1.100 or less.

[0015] Area ratio (S A / S B ) is considered to mean that the ratio of halogens (total of Cl and Br) occupying sites in the argyrodite crystal structure is high. In particular, it is estimated that the site occupancy rate of Br is higher than that of the conventional technology. In general, various types of crystalline components and amorphous components are mixed in a sulfide solid electrolyte. A part of Cl and Br input as constituent elements of the sulfide solid electrolyte forms the argyrodite crystal structure, while the other Cl and Br form crystalline structures other than the argyrodite crystal structure and amorphous components. It is also considered that they may be contained in the residual raw materials. In this embodiment, the ratio of halogens occupying sites in the argyrodite crystal structure, in particular the site occupancy rate of Br, is made higher than that of the conventional technology, thereby increasing the area ratio (S A / S B ) and the ionic conductivity of the sulfide solid electrolyte increases.

[0016] The argyrodite crystal structure is PS4 3- The structure is the main unit structure of the skeleton, and the surrounding sites are occupied by S surrounded by Li and halogens (Cl, Br). From the coordinates of each element in the crystal structure, the area ratio of the X-ray diffraction peak of the crystal structure can be calculated (see XRD Diffraction Handbook, Third Edition, Rigaku Denki Co., Ltd., 2000, pp. 14-15). A typical argyrodite-type crystal structure is represented by the space group F-43M, and is the crystal structure represented by No. 216 in the database of International Tables for Crystallography Volume G: Definition and exchange of crystallographic data (ISBN: 978-1-4020-3138-0). The crystal structure represented by No. 216 includes PS 4 3- There are 4a sites and 4d sites on the periphery of the structure, and elements with a large ionic radius tend to occupy the 4a sites, while elements with a small ionic radius tend to occupy the 4d sites.

[0017] The unit cell of the argyrodite-type crystal structure has a total of eight 4a and 4d sites. The area ratios of the X-ray diffraction peaks were calculated for the case where four Cl atoms and four S atoms are placed at these sites (Case 1), and the case where four Cl atoms, two Br atoms, and two S atoms are placed at these sites (Case 2). As a result, it was found that the area of ​​diffraction peak A (diffraction peak at 2θ=25 deg) is wider in Case 2 than in Case 1, while the change in the area of ​​diffraction peak B (diffraction peak at 2θ=30 deg) is smaller. From the above calculation results, it can be seen that the area ratio (S A / S B ) is expected to become larger.

[0018] In general, the area ratio and intensity ratio of X-ray diffraction peaks are proportional to the number of electrons of the element (see "Guide to X-ray Crystal Analysis", Shokabo Publishing (1983)). Cl and S have roughly the same number of electrons, while Br has more electrons, so it is thought that the site occupancy rate of Br is higher in the crystal diffraction plane corresponding to diffraction peak A. Considering the size of the ionic radius, it can be estimated that the occupancy rate of the 4a site is particularly high.

[0019] An increase in the amount of halogens occupying sites in the argyrodite-type crystal structure means a relative decrease in the amount of S occupying sites in the argyrodite-type crystal structure. Halogens with a valence of -1 have a weaker ability to attract Li than S with a valence of -2. They also attract fewer Li atoms. This reduces the density of Li around the sites and makes Li more mobile, which is thought to increase the ionic conductivity of the argyrodite-type crystal structure.

[0020] In addition, when the halogen is only Cl, the occupancy rate of S is high at the 4a site. By using Br, which has an ionic radius equivalent to that of S, together with Cl, the occupancy rate of Br at the 4a site is high, and as a result, the overall halogen occupancy rate is improved. Even if Cl occupies some of the 4a sites, Cl at the 4a site is unstable and may be desorbed during the heat treatment process. Therefore, it is considered preferable not only to simply increase the halogen occupancy rate, but also to have a halogen with an appropriate ionic radius occupy an appropriate site. In this embodiment, it is presumed that the ionic conductivity is high because two types of halogen (Cl and Br) occupy a large amount and appropriately the sites in the argyrodite crystal structure.

[0021] In addition, this embodiment is characterized in that the molar ratio c of chlorine to phosphorus (Cl / P) and the molar ratio d of bromine to phosphorus (Br / P) satisfy the following formula (1). 1.2 <c+d<1.9···(1) c+d is the molar ratio of chlorine and bromine to phosphorus. By setting it in the above range, the effect of improving the ionic conductivity of the sulfide solid electrolyte is increased. c+d is preferably 1.4 or more and 1.8 or less, and more preferably 1.5 or more and 1.7 or less.

[0022] In the sulfide solid electrolyte according to one embodiment of the present invention, the molar ratio d of bromine to phosphorus (Br / P) is preferably 0.15 or more and 1.6 or less, more preferably 0.2 or more and 1.2 or less, and even more preferably 0.4 or more and 1.0 or less.

[0023] In addition, it is preferable that the molar ratio c (Cl / P) of chlorine to phosphorus and the molar ratio d (Br / P) of bromine to phosphorus satisfy the following formula (2). 0.08 <d / (c+d)<0.8···(2) d / (c+d) is more preferably 0.15 or more and 0.6 or less, and further preferably 0.2 or more and 0.5 or less.

[0024] It is preferable that the molar ratio a of lithium to phosphorus (Li / P), the molar ratio b of sulfur to phosphorus (S / P), the molar ratio c of chlorine to phosphorus (Cl / P), and the molar ratio d of bromine to phosphorus (Br / P) satisfy the following formulas (3) to (5). 5.0≦a≦7.5 (3) 6.5≦a+c+d≦7.5 (4) 0.5≦a b ≦1.5 (5) (Wherein, b>0, c>0, and d>0 are satisfied.) By satisfying the above formulae (3) to (5), an argyrodite-type crystal structure is easily formed.

[0025] In the above formula (3), 5.0≦a≦6.8 is preferable, and 5.2≦a≦6.6 is more preferable. The above formula (4) preferably satisfies 6.6≦a+c+d≦7.4, and more preferably satisfies 6.7≦a+c+d≦7.3. The above formula (5) preferably satisfies 0.6≦ab≦1.3, and more preferably satisfies 0.7≦ab≦1.3.

[0026] The sulfide solid electrolyte according to the present embodiment may contain, in addition to the above Li, P, S, Cl, and Br, Si, Ge, Sn, Pb, B, Al, Ga, As, Sb, Bi, O, Se, Te, etc., within a range that does not impair the effects of the present invention. Also, it may be substantially composed of only Li, P, S, Cl, and Br. "Substantially composed of only Li, P, S, Cl, and Br" means that the sulfide solid electrolyte has only Li, P, S, Cl, and Br as constituent elements, excluding inevitable impurities.

[0027] The molar ratios and compositions of the elements described above are not those of the raw materials used in the production, but those of the sulfide solid electrolyte product. The molar ratios of the elements can be controlled, for example, by adjusting the contents of the elements in the raw materials.

[0028] In this application, the molar ratio and composition of each element in the sulfide solid electrolyte are measured by ICP optical emission spectrometry, except in special circumstances such as when the analysis is difficult. The measurement method of ICP optical emission spectrometry is described in the Examples.

[0029] In the sulfide solid electrolyte according to one embodiment of the present invention, in powder X-ray diffraction using CuKα radiation, it is preferable that the sulfide solid electrolyte does not have a lithium halide diffraction peak, or if it has a lithium halide diffraction peak, it satisfies the following formula (B). 0 C / I A <0.08 (B) (In the formula, I C represents the intensity of the lithium halide diffraction peak, and I A represents the intensity of the diffraction peak at 2θ=25.2±0.5 deg.)

[0030] ​The above formula (B) indicates that the amount of lithium halide is relatively small compared to the argyrodite-type crystal structure. The presence of lithium halide indicates that, among all the halogens in the sulfide solid electrolyte, there are halogens that do not occupy sites in the argyrodite-type crystal structure. Intensities of the diffraction peaks of lithium halides I. C When the lithium halide is LiCl, it is the intensity of the diffraction peak appearing in the range of 34.0 deg ≦ 2θ ≦ 35.5 deg. However, when there are two or more diffraction peaks in the range, it is the intensity of the diffraction peak appearing on the highest angle side. When the lithium halide is LiBr, I C is the intensity of the diffraction peak appearing in the range of 32.5 deg ≦ 2θ ≦ 33.9 deg. However, if there are two or more diffraction peaks in that range, it is the intensity of the diffraction peak appearing on the lowest angle side. The reason for this definition is that, in the presence of a novel crystal structure containing a halogen, which will be described later, diffraction peaks appear at 14.4 ± 0.5 deg and 33.8 ± 0.5 deg. Here, if a diffraction peak is observed at 14.4 ± 0.5 deg but only one diffraction peak is observed in the range of 32.5 deg ≦ 2θ ≦ 35.5 deg, it is considered that these diffraction peaks originate from the novel crystal structure containing a halogen, which will be described later. In this case, it is considered that no diffraction peaks of lithium halide appeared. Note that, when diffraction peaks of LiCl and LiBr are observed, I C is the sum of the intensities of these diffraction peaks. Formula (B) is 0 C / I A <0.07 is more preferable, and 0 C / I A It is even more preferred that it is <0.06.

[0031] In addition, in the sulfide solid electrolyte according to one embodiment of the present invention, in powder X-ray diffraction using CuKα radiation, it is preferable that the sulfide solid electrolyte does not have diffraction peaks at 2θ=14.4±0.5 deg and 33.8±0.5 deg, or if it has diffraction peaks, satisfies the following formula (C). 0 D / I​​​A <0.09 (C) (In the formula, I D represents the intensity of the diffraction peak at 2θ = 14.4 ± 0.5 deg, and I A represents the intensity of the diffraction peak at 2θ=25.2±0.5 deg.)

[0032] The crystals having diffraction peaks at 2θ=14.4±0.5 deg and 33.8±0.5 deg are new, but are presumed to have a structure that partially contains halogen. The above formula (C) indicates that the new crystal structure is relatively rare compared to the argyrodite-type crystal structure. The presence of the new crystal structure indicates that, among all the halogens in the sulfide solid electrolyte, there are halogens that do not occupy sites in the argyrodite-type crystal structure. Formula (C) is 0 D / I A <0.06, and more preferably 0 C / I D It is preferred that it is <0.05.

[0033] In the sulfide solid electrolyte according to one embodiment of the present invention, the lattice constant of the argyrodite crystal structure is preferably 9.800 Å or more and 9.920 Å or less. The small lattice constant of the argyrodite crystal structure is believed to mean that the crystal structure contains a large amount of chlorine and bromine. If the lattice constant is less than 9,800 Å, it is believed that it becomes difficult for bromine to be incorporated into the crystal structure.

[0034] The lattice constant of the argyrodite-type crystal structure is calculated from the XRD pattern obtained by X-ray diffraction measurement (XRD) by performing a full pattern fitting (WPF) analysis using crystal structure analysis software. The details of the measurement are shown in the Examples.

[0035] In the sulfide solid electrolyte according to one embodiment of the present invention, 31 ​​In P-NMR measurement, it is preferable that the solid electrolyte has peaks at 81.5 to 82.5 ppm (hereinafter referred to as the first region), 83.2 to 84.7 ppm (hereinafter referred to as the second region), 85.2 to 86.7 ppm (hereinafter referred to as the third region), and 87.2 to 89.4 ppm (hereinafter referred to as the fourth region), and the ratio of the sum of the areas of the peaks at 81.5 to 82.5 ppm and the peaks at 83.2 to 84.7 ppm to the total area of ​​all peaks at 78 to 92 ppm is 60% or more. It is presumed that a high ratio of the sum of the areas of the first and second peaks indicates that the sum of the amounts of chlorine and bromine incorporated in the argyrodite crystal structure is large. As a result, the ionic conductivity of the solid electrolyte is high. The peak in the first region is called the first peak (P 1 ) and the peak in the second region is called the second peak (P 2 ) and the peak in the third region is called the third peak (P 3 ) and the peak in the fourth region is called the fourth peak (P 4 ) A region is peaked means that there is a peak having a peak top within the region, or that there is a peak in this region when separated by a nonlinear least squares method.

[0036] The ajirodite-type crystal structure (Li 6 P.S. 5 Cl) is the PS in the crystal. 4 3- The difference in the distribution of free chlorine (Cl) and free sulfur (S) around the structure 31 It has been reported that in the P-NMR spectrum, multiple phosphorus resonance lines with different chemical shifts are observed overlapping (Non-Patent Document 1). Based on these findings, the present inventors have investigated the solid state of ajirodite crystals with different ratios of free halogen and free S. 31 The P-NMR spectra were examined. As a result, the NMR signals observed in the 78-92 ppm region were determined to be those of four types of PS with different distribution states of free sulfur and free halogens around them. 4 3-It was also found that, among the four peaks, when the area ratio of the peak on the high magnetic field side (the sum of the first and second peaks) is high, the ionic conductivity of the solid electrolyte is high. The first and second peaks are due to the structure of PS, where most of the surrounding free elements are Cl and Br. 4 3- On the other hand, the third and fourth peaks are due to the PS structure, where most of the surrounding free elements are S. 4 3- It is presumed that this is due to the structure.

[0037] The sulfide solid electrolyte according to one embodiment of the present invention can be produced by a production method including, for example, a step of producing an intermediate by applying mechanical stress to a mixture of raw materials to cause a reaction, and a step of heat-treating the intermediate to crystallize it.

[0038] The raw materials used are a combination of two or more compounds or simple substances that, as a whole, contain the elements essential to the sulfide solid electrolyte to be produced, that is, lithium, phosphorus, sulfur, chlorine, and bromine.

[0039] Examples of raw materials containing lithium include lithium sulfide (Li 2 S), lithium oxide (Li 2 O), lithium carbonate (Li 2 CO 3 and lithium metal alone. Among these, lithium compounds are preferred, and lithium sulfide is more preferred. The lithium sulfide can be used without any particular limitation, but is preferably high purity lithium sulfide. Lithium sulfide can be produced by the methods described in, for example, JP-A-7-330312, JP-A-9-283156, JP-A-2010-163356, and JP-A-2011-84438. Specifically, lithium hydroxide and hydrogen sulfide are reacted in a hydrocarbon organic solvent at 70° C. to 300° C. to generate lithium hydrosulfide, and then this reaction liquid is dehydrosulfided to synthesize lithium sulfide (JP 2010-163356 A). Alternatively, lithium hydroxide and hydrogen sulfide can be reacted in an aqueous solvent at 10° C. to 100° C. to produce lithium hydrosulfide, and then this reaction liquid can be dehydrosulfided to synthesize lithium sulfide (JP 2011-84438 A).

[0040] Examples of phosphorus-containing raw materials include diphosphorus trisulfide (P 2 S 3 ), diphosphorus pentasulfide (P 2 S 5 ) and other phosphorus sulfides, sodium phosphate (Na 3 PO 4 Among these, phosphorus sulfide is preferred, and diphosphorus pentasulfide (P 2 S 5 The phosphorus compound and phosphorus element can be used without any particular limitation as long as they are industrially produced and commercially available.

[0041] The raw material containing chlorine and / or bromine preferably contains, for example, a halogen compound represented by the following formula (6). M l -X m (6)

[0042] In formula (6), M represents sodium (Na), lithium (Li), boron (B), aluminum (Al), silicon (Si), phosphorus (P), sulfur (S), germanium (Ge), arsenic (As), selenium (Se), tin (Sn), antimony (Sb), tellurium (Te), lead (Pb), bismuth (Bi), or any of these elements bonded to an oxygen element or a sulfur element, and is preferably lithium (Li) or phosphorus (P), and more preferably lithium (Li). X is chlorine (Cl) or bromine (Br). In addition, l is an integer of 1 or 2, and m is an integer of 1 to 10. When m is an integer of 2 to 10, that is, when there are multiple Xs, Xs may be the same or different. For example, SiBrCl 3 In the formula, m is 4 and X is composed of two different elements, Br and Cl.

[0043] Examples of the halogen compound represented by the above formula (6) include NaCl, NaBr, LiCl, LiBr, BCl 3 , BBr 3 , AlBr 3 , AlCl 3 , SiCl 4 , SiCl 3 , Si 2 Cl 6 , SiBr 4 , SiBrCl 3 , SiBr 2 Cl 2 , PCl 3 , PCl 5 , POCl 3 , PBr 3 , POBr 3 , P 2 Cl 4 , SCl 2 , S 2 Cl 2 , S 2 Br 2 , GeCl 4 , GeBr 4 , GeCl 2 , GeBr 2 , AsCl 3 , AsBr 3 , SeCl 2 , SeCl 4 , Se 2 Br 2 , SeBr 4 , SnCl 4 , SnBr 4 , SnCl 2 , SnBr 2 , SbCl 3 , SbBr 3 , SbCl 5 , TeCl 2 , TeCl 4 , TeBr 2 , TeBr 4 , PbCl 4 , PbCl 2 , PbBr 2 , BiCl 3 , BiBr 3 and so on.

[0044] Among them, lithium chloride (LiCl), lithium bromide (LiBr), phosphorus pentachloride (PCl 5 ), phosphorus trichloride (PCl 3 ), phosphorus pentabromide (PBr 5 ) or phosphorus tribromide (PBr 3 Of these, LiCl, LiBr, or PBr 3 is preferred, with LiCl and LiBr being more preferred. The halogen compound may be one of the above compounds alone or two or more of them may be combined to use, i.e., at least one of the above compounds can be used.

[0045] In one embodiment of the present invention, the raw material contains a lithium compound, a phosphorus compound, and a halogen compound, and at least one of the lithium compound and the phosphorus compound preferably contains elemental sulfur. 2 More preferably, the combination of S, phosphorus sulfide, LiCl, and LiBr is used. 2 S and P 2 S 5 A combination of LiCl and LiBr is even more preferred. For example, Li is used as a raw material for sulfide solid electrolytes. 2 S, P 2 S 5 When LiCl and LiBr are used, the molar ratio of the input raw materials is Li 2 S:P 2 S 5 The total of LiCl and LiBr can be 30-60:10-25:15-50.

[0046] In one embodiment of the present invention, the raw material is subjected to a mechanical stress to react and produce an intermediate. Here, "applying mechanical stress" means mechanically applying a shear force, an impact force, or the like. Examples of means for applying mechanical stress include a grinder such as a planetary ball mill, a vibration mill, or a rolling mill, and a kneader. In conventional techniques (e.g., Patent Document 2, etc.), the raw material powder is pulverized and mixed to a degree that allows the crystallinity of the raw material powder to be maintained. On the other hand, in the present embodiment, it is preferable to apply mechanical stress to the raw material to cause a reaction and produce an intermediate containing a glass component. In other words, the raw material powder is pulverized and mixed to a state in which at least a part of the raw material powder cannot maintain its crystallinity due to a mechanical stress stronger than that of the conventional technique. As a result, the PS, which is the basic skeleton of the argyrodite crystal structure, is formed at the intermediate stage. 4 This produces a structure and allows the halogen to be highly dispersed. It is presumed that the halogen highly dispersed in the intermediate is efficiently introduced into sites in the argyrodite-type crystal structure by heat treatment. It is presumed that this is the reason why the sulfide solid electrolyte of the present embodiment exhibits high ionic conductivity. Incidentally, the presence of a broad peak (halo pattern) due to the amorphous component in an XRD measurement can confirm that the intermediate contains a glass (amorphous) component.

[0047] As for the conditions of the grinding and mixing, for example, when a planetary ball mill is used as a grinder, the rotation speed may be several tens to several hundreds of revolutions per minute, and the processing time may be 0.5 to 100 hours. More specifically, in the case of the planetary ball mill (manufactured by Fritsch: model number P-7) used in the examples of the present application, the rotation speed of the planetary ball mill is preferably 350 rpm or more and 400 rpm or less, and more preferably 360 rpm or more and 380 rpm or less. When balls serving as grinding media are used, for example, zirconia balls, their diameter is preferably 0.2 to 20 mm.

[0048] The intermediate produced by grinding and mixing is heat-treated. The heat treatment temperature is preferably 350 to 480°C, more preferably 360 to 460°C, and even more preferably 380 to 450°C. The halogen contained in the argyrodite crystal structure tends to increase when the heat treatment temperature is slightly lower than in the past. This is presumably because a high heat treatment temperature makes it easier for halogen to leave the sites in the argyrodite crystal structure. The atmosphere for the heat treatment is not particularly limited, but is preferably an inert gas atmosphere such as nitrogen, argon, etc., rather than a hydrogen sulfide gas flow. It is presumed that the amount of halogen in the crystal structure can be increased by suppressing the replacement of free halogen in the crystal structure with sulfur, and as a result, the ionic conductivity of the obtained sulfide solid electrolyte is improved.

[0049] When a kneader is used as the means for applying the mechanical stress, the kneader is not particularly limited, but is preferably a multi-shaft kneader having two or more shafts from the viewpoint of ease of manufacture.

[0050] The multi-shaft kneader may, for example, comprise a casing, two or more rotating shafts arranged to penetrate the casing in the longitudinal direction, and provided with paddles (screws) along the axial direction, with a raw material supply port at one end of the casing in the longitudinal direction and a discharge port at the other end, and other configurations are not particularly limited as long as the two or more rotational motions interact with each other to generate mechanical stress. By rotating the two or more rotating shafts provided with paddles of such a multi-shaft kneader, the two or more rotational motions can interact with each other to generate mechanical stress, and it becomes possible to apply the mechanical stress to the raw material moving along the rotating shafts from the supply port to the discharge port, causing it to react.

[0051] A preferred example of a multi-shaft kneader that can be used in one embodiment of the present invention will be described with reference to Figures 1 and 2. Figure 1 is a plan view cut at the center of the rotating shaft of the multi-shaft kneader, and Figure 2 is a plan view cut perpendicular to the rotating shaft, showing a portion of the rotating shaft where the paddles are provided. The multi-shaft kneader shown in Fig. 1 is a twin-shaft kneader equipped with a casing 1 having a supply port 2 at one end and a discharge port 3 at the other end, and two rotating shafts 4a and 4b that penetrate the casing 1 in the longitudinal direction. The rotating shafts 4a and 4b are provided with paddles 5a and 5b, respectively. The raw materials enter the casing 1 from the supply port 2, and are reacted by applying mechanical stress to the paddles 5a and 5b, and the resulting reaction product is discharged from the discharge port 3.

[0052] There is no particular limitation on the number of rotating shafts 4 as long as there are two or more, and in consideration of versatility, the number is preferably 2 to 4, and more preferably 2. Moreover, the rotating shafts 4 are preferably parallel shafts that are parallel to each other. The paddle 5 is provided on a rotating shaft for kneading the raw materials, and is also called a screw. There are no particular limitations on the cross-sectional shape, and examples include a substantially triangular shape with each side of the equilateral triangle uniformly convex in the shape of a circular arc, an elliptical shape, a substantially rectangular shape, and the like, and a shape having a cutout part based on these shapes may also be used.

[0053] When multiple paddles are provided, each paddle may be provided on the rotation shaft at a different angle as shown in Figure 2. In addition, when it is desired to obtain a better kneading effect, the paddles may be of the intermeshing type. The rotation speed of the paddle is not particularly limited, but is preferably 40 to 300 rpm, more preferably 40 to 250 rpm, and even more preferably 40 to 200 rpm.

[0054] The multi-shaft kneader may be equipped with a screw 6 on the supply port 2 side as shown in FIG. 1 in order to smoothly supply the raw materials into the kneader, and may be equipped with a reverse screw 7 on the discharge port 3 side as shown in FIG. 1 in order to prevent the reaction product obtained through the paddle 5 from remaining in the casing. As the multi-shaft kneader, a commercially available kneader can be used, for example, KRC Kneader (manufactured by Kurimoto Iron Works, Ltd.).

[0055] The kneading time of the raw materials may vary depending on the types and composition ratio of elements constituting the sulfide solid electrolyte to be obtained, and the reaction temperature, and may be appropriately adjusted, and is preferably 5 minutes to 50 hours, more preferably 10 minutes to 15 hours, and even more preferably 1 to 12 hours. The kneading temperature of the raw materials varies depending on the type and composition ratio of elements constituting the sulfide solid electrolyte to be obtained, and the reaction time, and may be appropriately adjusted, and is preferably 0°C or higher, more preferably 25°C or higher, even more preferably 100°C or higher, and most preferably 250°C or higher. The higher the temperature, the more likely it is that the argyrodite-type crystal structure will precipitate at the time of kneading. It is considered that the argyrodite-type crystal structure will precipitate more easily if the temperature is 350°C or higher. The upper limit of the kneading temperature is such that the resulting argyrodite-type crystal structure does not decompose, that is, less than 500°C.

[0056] The intermediate product discharged from the discharge port of the multi-shaft kneader may be fed again from the feed port depending on the degree of progress of the reaction, and the reaction may be allowed to proceed further. The degree of progress of the reaction can be grasped by the increase or decrease in the peaks derived from the raw materials of the obtained intermediate product.

[0057] The intermediate obtained by kneading is heat-treated to obtain a sulfide solid electrolyte. The heat treatment temperature is preferably 350 to 480° C., more preferably 360 to 460° C., and even more preferably 380 to 450° C. The atmosphere for the heat treatment is not particularly limited, but is preferably an inert gas atmosphere such as nitrogen or argon, rather than a hydrogen sulfide stream.

[0058] The sulfide solid electrolyte of the present invention can be used for a solid electrolyte layer, a positive electrode, a negative electrode, etc. of a lithium ion secondary battery or the like.

[0059] [Electrode composite material] An electrode mixture according to an embodiment of the present invention includes the sulfide solid electrolyte of the present invention and an active material. Alternatively, the electrode mixture is produced using the sulfide solid electrolyte of the present invention. When a negative electrode active material is used as the active material, the electrode mixture becomes a negative electrode mixture. On the other hand, when a positive electrode active material is used, the electrode mixture becomes a positive electrode mixture.

[0060] ·Negative electrode composite material A negative electrode mixture is obtained by blending a negative electrode active material with the sulfide solid electrolyte of the present invention. As the negative electrode active material, for example, a carbon material, a metal material, etc. can be used. A composite of two or more of these materials can also be used. In addition, negative electrode active materials that will be developed in the future can also be used. In addition, the negative electrode active material preferably has electronic conductivity. Examples of carbon materials include graphite (e.g., artificial graphite), graphite carbon fiber, resin-calcined carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-calcined carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and non-graphitizable carbon. Examples of the metal material include simple metals, alloys, and metal compounds. Examples of the simple metals include metal silicon, metal tin, metal lithium, metal indium, and metal aluminum. Examples of the alloys include alloys containing at least one of silicon, tin, lithium, indium, and aluminum. Examples of the metal compounds include metal oxides. Examples of the metal oxides include silicon oxide, tin oxide, and aluminum oxide.

[0061] The blending ratio of the negative electrode active material and the solid electrolyte is preferably negative electrode active material:solid electrolyte=95 wt%:5 wt% to 5 wt%:95 wt%, more preferably 90 wt%:10 wt% to 10 wt%:90 wt%, and further preferably 85 wt%:15 wt% to 15 wt%:85 wt%. If the content of the negative electrode active material in the negative electrode mixture is too small, the electric capacity will be small. In addition, if the negative electrode active material has electronic conductivity and does not contain a conductive additive or contains only a small amount of conductive additive, it is considered that the electronic conductivity (electron conduction path) in the negative electrode will decrease, the rate characteristics will be lowered, the utilization rate of the negative electrode active material will decrease, and the electric capacity will be lowered. On the other hand, if the content of the negative electrode active material in the negative electrode mixture is too high, it is considered that the ionic conductivity (ionic conduction path) in the negative electrode will decrease, the rate characteristics will be lowered, the utilization rate of the negative electrode active material will decrease, and the electric capacity will be lowered.

[0062] The negative electrode mixture may further contain a conductive assistant. When the electronic conductivity of the negative electrode active material is low, it is preferable to add a conductive assistant. The conductive assistant only needs to have electrical conductivity, and the electronic conductivity is preferably 1×10 3 S / cm or more, more preferably 1×10 5 S / cm or more. Specific examples of the conductive assistant are preferably substances containing at least one element selected from the group consisting of carbon materials, nickel, copper, aluminum, indium, silver, cobalt, magnesium, lithium, chromium, gold, ruthenium, platinum, beryllium, iridium, molybdenum, niobium, osmium, rhodium, tungsten, and zinc, and more preferably simple carbon having high conductivity, carbon materials other than simple carbon, or simple metals, mixtures, or compounds containing nickel, copper, silver, cobalt, magnesium, lithium, ruthenium, gold, platinum, niobium, osmium, or rhodium. Specific examples of the carbon material include carbon black such as Ketjen Black, Acetylene Black, Denka Black, Thermal Black, and Channel Black; graphite, carbon fiber, activated carbon, etc., which can be used alone or in combination of two or more. Among them, acetylene black, Denka Black, and Ketjen Black, which have high electronic conductivity, are preferred.

[0063] When the negative electrode composite material contains a conductive assistant, the content of the conductive assistant in the composite material is preferably 1 to 40 mass %, more preferably 2 to 20 mass %. If the content of the conductive assistant is too small, it is considered that the electronic conductivity of the negative electrode may decrease, resulting in a decrease in rate characteristics, or the utilization rate of the negative electrode active material may decrease, resulting in a decrease in electric capacity. On the other hand, if the content of the conductive assistant is too large, the amount of the negative electrode active material and / or the amount of the solid electrolyte may decrease. It is presumed that the electric capacity decreases when the amount of the negative electrode active material decreases. It is also considered that the ionic conductivity of the negative electrode may decrease, resulting in a decrease in rate characteristics, or the utilization rate of the negative electrode active material may decrease, resulting in a decrease in electric capacity.

[0064] In order to tightly bind the negative electrode active material and the solid electrolyte to each other, a binder may further be included. As the binder, fluorine-containing resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), fluorine rubber, or thermoplastic resins such as polypropylene and polyethylene, ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, natural butyl rubber (NBR), etc. can be used alone or as a mixture of two or more. In addition, aqueous binders such as cellulose-based and aqueous dispersions of styrene butadiene rubber (SBR) can also be used.

[0065] The negative electrode mixture can be produced by mixing a solid electrolyte, a negative electrode active material, and an optional conductive assistant and / or binder. The mixing method is not particularly limited, but for example, dry mixing using a mortar, ball mill, bead mill, jet mill, planetary ball mill, vibration ball mill, sand mill, cutter mill; and wet mixing using a mortar, ball mill, bead mill, planetary ball mill, vibration ball mill, sand mill, film mix after dispersing the raw material in an organic solvent, and then removing the solvent can be applied. Among these, wet mixing is preferred in order not to destroy the negative electrode active material particles.

[0066] Positive electrode mixture A positive electrode mixture is obtained by blending a positive electrode active material with the solid electrolyte of the present invention. The positive electrode active material is a material capable of inserting and extracting lithium ions, and may be any positive electrode active material known in the battery field, or may be any positive electrode active material to be developed in the future.

[0067] Examples of the positive electrode active material include metal oxides, sulfides, etc. Sulfides include metal sulfides and nonmetal sulfides. The metal oxide is, for example, a transition metal oxide. 2 O 5 , V 6 O 13 , LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4, Li(Ni a Co b Mn c )O 2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), LiNi 1-Y Co Y O 2 , LiCo 1-Y Mn Y O 2 , LiNi 1-Y Mn Y O 2 (where 0 ≤ Y < 1), Li(Ni a Co b Mn c )O 4 (0 < a < 2, 0 < b < 2, 0 < c < 2, and a + b + c = 2), LiMn 2-Z Ni Z O 4 , LiMn 2-Z Co Z O 4 (where 0 < Z < 2), LiCoPO 4 , LiFePO 4 , CuO, Li(Ni a Co b Al c )O 2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), etc. can be mentioned. As metal sulfides, titanium sulfide (TiS 2 ), molybdenum sulfide (MoS 2 ), iron sulfide (FeS, FeS 2 ), copper sulfide (CuS), and nickel sulfide (Ni 3 S 2 ) etc. can be mentioned. In addition, as metal oxides, bismuth oxide (Bi 2 O 3 ), bismuth lead oxide (Bi 2 Pb 2 O 5 ) etc. can be mentioned. As non-metal sulfides, organic disulfide compounds, carbon sulfide compounds, etc. can be mentioned. In addition to the above, niobium selenide (NbSe 3 ), metallic indium, and sulfur can also be used as the positive electrode active material.

[0068] The positive electrode mixture may further contain a conductive assistant. The conductive assistant is the same as that in the negative electrode mixture.

[0069] The mixing ratio of the solid electrolyte and the positive electrode active material in the positive electrode mixture, the content of the conductive additive, and the method for producing the positive electrode mixture are the same as those for the negative electrode mixture described above.

[0070] [Lithium-ion battery] A lithium ion battery according to one embodiment of the present invention includes at least one of the sulfide solid electrolyte and electrode mixture of the present invention described above, or is manufactured using at least one of the sulfide solid electrolyte and electrode mixture of the present invention. The structure of the lithium ion battery is not particularly limited, but generally has a structure in which a negative electrode layer, an electrolyte layer, and a positive electrode layer are laminated in this order. Each layer of the lithium ion battery will be described below.

[0071] (1) Negative electrode layer The negative electrode layer is preferably a layer made from the negative electrode mix of the present invention. Alternatively, the negative electrode layer is preferably a layer containing the negative electrode mixture of the present invention. The thickness of the negative electrode layer is preferably from 100 nm to 5 mm, more preferably from 1 μm to 3 mm, and further preferably from 5 μm to 1 mm. The negative electrode layer can be produced by a known method, for example, a coating method or an electrostatic method (electrostatic spray method, electrostatic screen method, etc.).

[0072] (2) Electrolyte layer The electrolyte layer is a layer including or made of a solid electrolyte. The solid electrolyte is not particularly limited, but is preferably the sulfide solid electrolyte of the present invention. The electrolyte layer may be composed of only a solid electrolyte, or may further contain a binder. As the binder, the same binder as that of the negative electrode mixture of the present invention can be used.

[0073] The thickness of the electrolyte layer is preferably 0.001 mm or more and 1 mm or less. The solid electrolyte of the electrolyte layer may be fused. Fusion means that a part of the solid electrolyte particles is dissolved and the dissolved part is integrated with other solid electrolyte particles. The electrolyte layer may be a plate-like body of the solid electrolyte, and the plate-like body may include a case where a part or all of the solid electrolyte particles are dissolved to form a plate-like body. The electrolyte layer can be produced by a known method, for example, a coating method or an electrostatic method (electrostatic spray method, electrostatic screen method, etc.).

[0074] (3) Positive electrode layer The positive electrode layer is a layer containing a positive electrode active material, and is preferably a layer containing the positive electrode mixture of the present invention or a layer produced from the positive electrode mixture of the present invention. The thickness of the positive electrode layer is preferably 0.01 mm or more and 10 mm or less. The positive electrode layer can be produced by a known method, for example, a coating method or an electrostatic method (electrostatic spray method, electrostatic screen method, etc.).

[0075] (4) Current collector The lithium ion battery of this embodiment preferably further includes a current collector. For example, the negative electrode current collector is provided on the side of the negative electrode layer opposite the electrolyte layer side, and the positive electrode current collector is provided on the side of the positive electrode layer opposite the electrolyte layer side. The current collector may be a plate or foil made of copper, magnesium, stainless steel, titanium, iron, cobalt, nickel, zinc, aluminum, germanium, indium, lithium, or an alloy thereof.

[0076] The lithium ion battery of this embodiment can be manufactured by laminating and bonding the above-mentioned members. The bonding method can be a method of laminating the members and pressing them together, or a method of pressing them between two rolls (roll to roll), etc. Moreover, the bonding may be performed via an active material having ion conductivity on the bonding surface, or an adhesive material that does not inhibit ion conductivity. The bonding may be performed by heat fusion within a range in which the crystal structure of the solid electrolyte is not changed. The lithium ion battery of the present embodiment can also be manufactured by sequentially forming the above-mentioned components. It can be manufactured by a known method, for example, a coating method or an electrostatic method (electrostatic spray method, electrostatic screen method, etc.). EXAMPLES

[0077] The present invention will now be described in more detail with reference to examples. The evaluation method is as follows. (1) Ionic conductivity and electronic conductivity measurements The sulfide solid electrolyte produced in each example was filled into a tablet press, and a pressure of 407 MPa (press display value 22 MPa) was applied using a mini press to form a compact. Carbon was placed on both sides of the compact as electrodes, and pressure was applied again using the tablet press to produce a compact for measurement (diameter about 10 mm, thickness 0.1 to 0.2 cm). The ionic conductivity of this compact was measured by AC impedance measurement. The ionic conductivity value at 25°C was used. In the method for measuring ionic conductivity used in this example, the ionic conductivity was 1.0×10 -6 When the ionic conductivity is less than S / cm, it is not possible to measure the ionic conductivity accurately, and therefore it is deemed to be unmeasurable. The electronic conductivity of this molded product was measured by DC electrical measurement. The electronic conductivity was measured at 25°C. The electronic conductivity was 1.0×10 -6 If the electrical conductivity is less than S / cm, the electrical conductivity is considered to be unmeasurable.

[0078] (2) X-ray diffraction (XRD) measurement From the sulfide solid electrolyte powder produced in each example, a circular pellet with a diameter of 10 mm and a height of 0.1 to 0.3 cm was molded to prepare a sample. This sample was measured using an airtight holder for XRD without exposing it to air. The 2θ position of the diffraction peak was determined by the centroid method using the XRD analysis program JADE. The powder X-ray diffraction measurement was performed using a Rigaku Corporation SmartLab under the following conditions. Tube voltage: 45kV Tube current: 200mA X-ray wavelength: Cu-Kα ray (1.5418Å) Optical system: Parallel beam method Slit configuration: Soller slit 5°, entrance slit 1mm, receiving slit 1mm Detector: Scintillation counter Measurement range: 2θ=10-60deg Step width, scan speed: 0.02 deg, 1 deg / min

[0079] In the analysis of peak positions to confirm the presence of a crystal structure from the measurement results, the XRD analysis program JADE was used, and the peak positions were obtained by drawing a baseline using a cubic approximation.

[0080] The intensities and areas of the diffraction peaks at 2θ=25.2±0.5 deg (diffraction peak A) and 2θ=29.7±0.5 deg (diffraction peak B) were analyzed by the following procedure, and the area ratio was calculated. In the XRD pattern, the maximum peak position at 2θ = 23 to 27 deg is obtained, and the intensity (height) of the peak top is called the diffraction peak intensity I A The area S of diffraction peak A was calculated by integrating the 41 measured intensities at ±0.4 deg from the maximum peak position. A Similarly, the maximum peak position at 2θ = 28 to 32 deg was obtained, and the integrated value of the measured intensity at 41 points at ±0.4 deg from the maximum peak position was calculated as the area S of diffraction peak B. B S A and S B From the area ratio (S A / S B ) was calculated. Intensities of the diffraction peaks of lithium halides I. C When the lithium halide is LiCl, the peaks at 2θ = 34.0 to 35.5 deg are identified, and the intensity of the peak top is the diffraction peak intensity I CIn addition, when there are two or more peaks in the range, the intensity of the peak identified on the highest angle side is used. In the case of LiBr, the peaks at 2θ=32.5 to 33.9 deg are identified, and the intensity of the peak top is used as the diffraction peak intensity I C In addition, when there are two or more peaks in the range, the intensity of the peak identified on the lowest angle side is used. In addition, the peaks at 2θ = 14.0 to 15.0 deg were identified, and the peak top intensity was calculated as the diffraction peak intensity I D It was decided.

[0081] (3)ICP measurement The sulfide solid electrolyte powder produced in each example was weighed and collected in a vial in an argon atmosphere. An alkaline KOH solution was placed in the vial, and the sample was dissolved while taking care not to collect sulfur, and then appropriately diluted to obtain a measurement solution. This was measured using a Paschen-Runge type ICP-OES device (SPECTRO ARCOS manufactured by SPECTRO) to determine the composition. Calibration curve solutions were prepared using 1000 mg / L standard solutions for ICP measurement for Li, P, and S, and 1000 mg / L standard solutions for ion chromatography for Cl and Br. Two test solutions were prepared for each sample, and five measurements were made for each test solution, and the average value was calculated. The composition was determined by the average of the two test solutions.

[0082] (4) Lattice constant of argyrodite-type crystal structure XRD was measured under the same conditions as in (2) above. The obtained XRD pattern was subjected to full pattern fitting (WPF) analysis using crystal structure analysis software JADE ver. 6 manufactured by MDI Corporation to identify each crystal component contained in the XRD pattern and calculate the lattice constant of each component.

[0083] - Background removal of XRD patterns In the XRD pattern after measurement, signals from the scattered light from the instrument and the airtight holder exist on the low angle side. To remove such signals, a baseline that decays from the low angle side was calculated by three-dimensional approximation according to the XRD pattern.

[0084] Peak component identification For each component contained in the sample, the peak components were identified by overlaying the XRD pattern with a pattern calculated from structural information on the Inorganic Crystal Structure Database (ICSD). Table 1 shows the structural information used.

[0085] [Table 1]

[0086] ·WPF analysis The main parameter settings for the WPF analysis are shown below. X-ray wavelength: Cukα ray (λ=1.54184Å) Fitting parameters: The peak shape was approximated as a symmetric peak. Temperature factors were excluded from the fitting. Li 2 When crystals such as S remain as fine peaks, the fitting may not converge. In such cases, structures other than the argyrodite-type crystal and lithium halide crystal are excluded from the fitting, and the half-width and intensity are manually entered, fitting is performed, and the lattice constant of the argyrodite-type crystal is calculated. For the lattice constant, we confirmed whether the peak position of the crystal structure to be evaluated matched well with the fitting results. For the area ratio, an R value of 10% or less was used as a guideline for the validity of the results. The R value, which is a guideline for the accuracy of the fitting, may be high if there are many unknown peaks or if amorphous peaks remain.

[0087] (5)Solid 31 P-NMR measurement Approximately 60 mg of powder sample was loaded into an NMR sample tube and solid-state analysis was performed using the following equipment and conditions. 31 P-NMR spectra were obtained. Equipment: ECZ400R equipment (manufactured by JEOL Ltd.) Observation kernel: 31 P Observation frequency: 161.944MHz Measurement temperature: room temperature Pulse sequence: Single pulse (uses 90° pulse) 90°Pulse width: 3.8μ Waiting time until next pulse application after FID measurement: 300 s Magic angle rotation speed: 12kHz Number of times: 16 Measurement range: 250ppm~-150ppm solid 31 In the measurement of P-NMR spectra, chemical shifts were determined using an external standard (NH 4 ) 2 HPO 4 (chemical shift 1.33 ppm) was used.

[0088] solid 31 The NMR signals in the range of 78 to 92 ppm in the P-NMR spectrum were separated into Gaussian functions or Pseudo-Voigt functions (linear sum of Gaussian and Lorentzian functions) by the nonlinear least squares method. In addition to the peaks due to the ajirodite-type crystal structure containing chlorine and bromine, the above range also contains peaks due to Li at 88.5 to 90.5 ppm. 7 P.S. 6 The peak due to Li is at 86 to 87.6 ppm. 3 P.S. 4 Therefore, waveform separation was performed using different methods depending on whether these two peaks were observed or not.

[0089] (5-1)Li 7 P.S. 6 and Li 3 P.S. 4 If no peak due to β crystals is observed, The NMR signals in the range of 78 to 92 ppm were separated into four Gaussian functions or Pseudo-Voigt functions (linear sum of Gaussian and Lorentzian functions) in the range of positions and half-widths shown in Table 2 by the nonlinear least squares method. 1 ~S 4 And the sum S all (=S 1 +S 2 +S 3 +S4 ) and the area ratio (%) of each peak was calculated.

[0090] [Table 2]

[0091] (5-2) Li 7 P.S. 6 Or Li 3 P.S. 4 When a peak due to β crystals is observed As shown in Table 3, in addition to the four peaks due to the chlorine-containing ajirodite-type crystal structure, 7 P.S. 6 (Peak I) or Li 3 P.S. 4 Using the peak due to (Peak II), the NMR signals from 78 to 92 ppm were separated using the nonlinear least squares method, and the areas S of the obtained peaks A to C were calculated. 1 ~S 4 and the area of ​​peaks I and II b 1 and b 2 And the sum of them S all+b (=S 1 +S 2 +S 3 +S 4 +b 1 +b 2 ) and the area ratio (%) of each peak was calculated.

[0092] [Table 3]

[0093] Manufacturing Example 1 (Lithium sulfide (Li 2 S) Production 200 g of LiOH anhydride (Honjo Chemical Co., Ltd.) dried under inert gas was charged into a 500 mL separable flask equipped with a stirrer. The temperature was raised under a nitrogen stream, and the internal temperature was maintained at 200° C. The nitrogen gas was replaced with hydrogen sulfide gas (Sumitomo Seika Chemicals) at a flow rate of 500 mL / min, and the LiOH anhydride and hydrogen sulfide were reacted. The water generated by the reaction was condensed and collected in a condenser. After 6 hours of reaction, 144 mL of water was collected. The reaction was continued for another 3 hours, but no water was generated. The product powder was collected and the purity and XRD were measured. The purity was 98.5% and the XRD showed Li 2 The peak pattern of S was confirmed.

[0094] Example 1 Li produced in Production Example 1 2 S (purity 98.5%), diphosphorus pentasulfide (P 2 S 5 Lithium chloride (LiCl: manufactured by Sigma-Aldrich, purity 99%) and lithium bromide (LiBr: manufactured by Sigma-Aldrich, purity 99%) were used as starting materials (hereinafter, in all examples, the purity of each starting material is the same). 2 S, P 2 S 5 , the molar ratio of LiCl and LiBr (Li 2 S:P 2 S 5 The raw materials were mixed so that the ratio of lithium sulfide was 1.9:0.5:1.0:0.6. Specifically, 0.447 g, 0.569 g, 0.217 g, and 0.267 g of lithium sulfide were mixed to prepare a raw material mixture.

[0095] The raw material mixture and 30 g of zirconia balls with a diameter of 10 mm were placed in a zirconia pot (45 mL) of a planetary ball mill (Fritsch: Model No. P-7) and completely sealed. The pot was filled with an argon atmosphere. The planetary ball mill was rotated at 370 rpm and processed (mechanical milling) for 15 hours to obtain a glassy powder (intermediate).

[0096] About 1.5 g of the intermediate powder was packed in a Tammann tube (PT2, manufactured by Tokyo Glass Equipment Co., Ltd.) in a glove box under an Ar atmosphere, the mouth of the Tammann tube was sealed with quartz wool, and the tube was sealed in a SUS airtight container to prevent air from entering. The airtight container was then placed in an electric furnace (FUW243PA, manufactured by Advantec Co., Ltd.) and heat-treated. Specifically, the temperature was raised from room temperature to 430°C at a rate of 2.5°C / min (it took about 3 hours to reach 430°C), and the temperature was maintained at 430°C for 8 hours. The mixture was then slowly cooled to obtain a sulfide solid electrolyte.

[0097] The ionic conductivity (σ) of the sulfide solid electrolyte was 13.0 mS / cm. The XRD pattern of the sulfide solid electrolyte is shown in Figure 3. Peaks attributable to the argyrodite crystal structure were observed at 2θ = 15.5, 17.9, 25.4, 29.9, 31.3, 44.9, 47.8, 52.4, and 59.1 deg. The sulfide solid electrolyte was subjected to ICP analysis to measure the molar ratios of each element. As a result, the molar ratio a (Li / P) was 5.35, the molar ratio b (S / P) was 4.33, the molar ratio c (Cl / P) was 1.102, and the molar ratio d (Br / P) was 0.62. The composition of the raw materials and the manufacturing conditions are shown in Table 4. The molar ratio of each element in the raw materials and the molar ratio of each element in the sulfide solid electrolyte are shown in Table 5. The areas, area ratios, and ionic conductivity σ of diffraction peaks A and B in the XRD pattern of the sulfide solid electrolyte are shown in Table 6. The intensities and intensity ratios of the diffraction peaks in the XRD pattern of the sulfide solid electrolyte are shown in Table 7. The lattice constants and 31 The area ratios of the P-NMR peaks are shown in Table 8. [Table 4]

[0098] [Table 5] *X is the sum of Cl and Br.

[0099] [Table 6] In the table, S A is the area of ​​the diffraction peak A (2θ=25.2±0.5 deg), and S B is the area of ​​diffraction peak B (29.7±0.5 deg).

[0100] [Table 7] In the table, I A is the intensity of the diffraction peak A (2θ=25.2±0.5 deg), and I C is the sum of the intensities of the lithium halide diffraction peaks, and I D is the intensity of the diffraction peak D (2θ=14.4±0.5 deg).

[0101] [Table 8]

[0102] Comparative Example 1 The same raw materials as in Example 1 were placed in a Schlenk flask and mixed by shaking by hand. The obtained raw material mixture was heat-treated at 430° C. for 8 hours in the same manner as in Example 1 to obtain a sulfide solid electrolyte. The sulfide solid electrolyte was evaluated in the same manner as in Example 1. The results are shown in Tables 5 to 8. In Comparative Example 1, it is presumed that the mixing of the raw materials before the heat treatment was insufficient, so that the halogen did not disperse even after the heat treatment, resulting in insufficient introduction of the halogen into the sites in the argyrodite crystal structure.

[0103] Example 2 In Example 2, a twin-screw kneader was used to prepare the intermediate body instead of the planetary ball mill used in Example 1. Kneading using the twin-screw kneader was specifically carried out as follows. A feeder (Microfeeder, manufactured by Aisin Nano Technologies Co., Ltd.) and a twin-screw kneading extruder (KRC kneader, paddle diameter φ8 mm, manufactured by Kurimoto Iron Works Co., Ltd.) were placed in the glove box. 3.76 g of LiCl, 4.63 g of LiBr, and 1.0 g of Li 2 7.75g of S and P 2 S5 A mixture of 9.87 g of the above was fed from the feed section at a constant speed by a feeder, and kneaded at a rotation speed of 150 rpm and a temperature of 250°C (measured with a thermometer on the outer surface of the casing of the twin-screw kneading extruder). The powder was discharged from the kneader outlet in about 120 minutes. The discharged powder was returned to the feed section and kneaded again. This operation was repeated five times. The reaction time was about 10 hours in total. The resulting intermediate was heat-treated at 430° C. for 8 hours in the same manner as in Example 1 to obtain a sulfide solid electrolyte. The obtained sulfide solid electrolyte was evaluated in the same manner as in Example 1. The results are shown in Tables 5 to 8. The twin-screw extruder used to mix the raw materials is a device with a very high mixing rate, so it is believed that the constituent elements were highly dispersed in the intermediate, which is likely why the ionic conductivity was improved.

[0104] Examples 3 to 7, Comparative Examples 2 to 4 A sulfide solid electrolyte was produced and evaluated in the same manner as in Example 1, except that the raw material composition was changed as shown in Table 4. The results are shown in Tables 5 to 8. In Comparative Example 2, it is believed that the halogens occupying the sites in the crystal structure were released due to the high heat treatment temperature. Cl in the 4a site and Br in the 4d site are easily released from the sites. The XRD pattern of the sulfide solid electrolyte prepared in Comparative Example 2 is shown in FIG. Based on the presence of lithium halide crystals and new crystals with diffraction peaks at 2θ=14.4±0.5 deg and 33.8±0.5 deg, it is presumed that some of the Cl and Br atoms occupying sites in the argyrodite-type crystal structure have been released to form these crystals. As a result of XRD measurement of the sulfide solid electrolyte obtained in each example, a peak derived from an argyrodite-type crystal structure was observed.

[0105] Examples 8 to 12, Comparative Example 5 Sulfide solid electrolytes were produced and evaluated in the same manner as in Example 1, except that the composition of the raw materials and the production conditions were changed as shown in Table 9. The results are shown in Tables 10 to 12. As a result of XRD measurement of the sulfide solid electrolytes obtained in each example, a peak derived from an argyrodite-type crystal structure was observed.

[0106] [Table 9]

[0107] [Table 10] *X is the sum of Cl and Br.

[0108] [Table 11] In the table, S A is the area of ​​the diffraction peak A (2θ=25.2±0.5 deg), and S B is the area of ​​diffraction peak B (29.7±0.5 deg).

[0109] [Table 12]

[0110] Example 13 Intermediates were produced in the same manner as in Example 1, except that the raw material compositions and production conditions were changed as shown in Table 9. In a glove box under an Ar atmosphere, about 1.5 g of the intermediate powder was packed into a glass tube with a sealing function, and the tip of the glass tube was sealed with a special tool to prevent air from entering. The glass tube was then set in an electric furnace. The special tool was inserted into a joint in the electric furnace and connected to a gas flow tube, and heat treatment was performed while flowing hydrogen sulfide at 0.5 L / min. Specifically, the temperature was raised from room temperature to 500°C at a rate of 3°C / min, and the mixture was held at 500°C for 4 hours. It was then slowly cooled to obtain a sulfide solid electrolyte. The obtained sulfide solid electrolyte was evaluated in the same manner as in Example 1. The results are shown in Tables 10 to 12. The sulfide solid electrolyte obtained in Example 13 also had an electronic conductivity of 10 -6 In addition, the XRD measurement revealed that a peak derived from the argyrodite crystal structure was observed.

[0111] Example 14 In the same manner as in Example 2, kneading was carried out using a twin-screw kneader to prepare an intermediate. Specifically, the kneading using the twin-screw kneader was carried out using 1.447 g of LiCl, 1.779 g of LiBr, and 2 S is 2.980g, and P 2 S 5 An intermediate was obtained in the same manner as in Example 2, except that a mixture of 3.794 g of the above was fed at a constant rate from the feeder through the feeder. The resulting intermediate was heat-treated at 430° C. for 4 hours to obtain a sulfide solid electrolyte.

[0112] The evaluation results of the obtained sulfide solid electrolyte are shown in Tables 10 to 12. The sulfide solid electrolyte obtained in Example 14 has an electronic conductivity of 10 -6 In addition, the XRD measurement revealed that a peak derived from the argyrodite crystal structure was observed.

[0113] Example 15 A sulfide solid electrolyte was prepared and evaluated in the same manner as in Example 14, except that the preparation conditions were changed as shown in Table 9. The results are shown in Tables 10 to 12. The sulfide solid electrolyte obtained in Example 15 has an electronic conductivity of 10 -6 In addition, the XRD measurement revealed that a peak derived from the argyrodite crystal structure was observed.

[0114] [Amount of hydrogen sulfide generated by sulfide solid electrolyte] The amounts of hydrogen sulfide generated from the sulfide solid electrolytes produced in Example 10 and Comparative Example 4 were evaluated using the apparatus shown in Fig. 5. This apparatus is configured by connecting, in this order, a flask 1 for humidifying air, a flask 2 equipped with a thermometer / hygrometer 6 for measuring the temperature and humidity of the humidified air, a Schlenk flask 3 into which a measurement sample 4 is placed, and a hydrogen sulfide meter 7 for measuring the concentration of hydrogen sulfide contained in the air through tubes. The evaluation procedure is as follows. In a nitrogen glove box with a dew point of -80°C, the sample was thoroughly crushed in a mortar to prepare a powder sample, which was then weighed out at about 0.1 g and placed in a 100 ml Schlenk flask 3 and sealed (number 4 in Figure 5). Next, air was flowed into flask 1 at 500 mL / min. The flow rate of air was measured by a flowmeter 5. Air was passed through water in flask 1 to be humidified. Next, the humidified air was flowed into flask 2, and the temperature and humidity of the air were measured. The temperature of the air immediately after the start of the flow was 25°C, and the humidity was 80 to 90%. Then, the humidified air was flowed into Schlenk flask 3 and contacted with the measurement sample 4. The humidified air that had flowed through Schlenk flask 3 was passed through a hydrogen sulfide measuring instrument 7 (Model 3000RS manufactured by AMI Co., Ltd.) to measure the amount of hydrogen sulfide contained in the humidified air. The measurement time was from immediately after the air flow to one hour after the flow. The amount of hydrogen sulfide was recorded at 15-second intervals. The amount of hydrogen sulfide generated per gram of sample (mg / g) was calculated from the sum of the amounts of hydrogen sulfide observed over two hours, and the results were 26 mg / g for the sulfide solid electrolyte of Example 10 and 64 mg / g for the sulfide solid electrolyte of Comparative Example 4.

[0115] [Lithium-ion battery] Using the sulfide solid electrolytes obtained in Example 13 and Comparative Example 1, lithium ion batteries were manufactured and their rate characteristics were evaluated.

[0116] (A) Lithium-ion battery manufacturing 50 mg of the sulfide solid electrolyte obtained in Example 13 or Comparative Example 1 was placed in a stainless steel mold having a diameter of 10 mm, flattened to make the thickness of the electrolyte layer uniform, and then pressure-molded by applying a pressure of 185 MPa from the upper surface of the electrolyte layer using a hydraulic press. Li as the positive electrode active material 4 Ti 5 O 12 Coat LiNi 0.8 Co 0.15 Al 0.05 O 2 The sulfide solid electrolyte obtained in Example 13 or Comparative Example 1 was mixed in a ratio of 70:30 by weight to form a positive electrode material, and 15 mg of the positive electrode material was poured onto the upper surface of the electrolyte layer and flattened so that the thickness of the positive electrode layer was uniform. After that, a pressure of 407 MPa was applied to the upper surface of the positive electrode layer using a hydraulic press to form a pressure mold. The graphite powder, which is the negative electrode active material, and the sulfide solid electrolyte obtained in Example 13 or Comparative Example 1 were mixed in a ratio of 60:40 by weight to prepare a negative electrode material. 12 mg of the negative electrode material was placed on the surface of the electrolyte layer opposite to the positive electrode layer and flattened to make the thickness of the negative electrode layer uniform, and then a pressure of 555 MPa was applied from the top surface of the negative electrode layer using a hydraulic press to form a pressure mold, thereby producing lithium ion batteries with a three-layer structure of a positive electrode, a solid electrolyte layer, and a negative electrode.

[0117] (B) Rate characteristic test The lithium ion battery manufactured in (A) above was left in a thermostatic chamber set at 25°C for 12 hours and then evaluated. In the first cycle, it was charged to 4.2V at 0.1C (0.189mA), discharged to 3.1V at 0.1C (0.189mA), and in the second to tenth cycles, it was charged to 4.2V at 0.5C (0.945mA), and discharged to 3.1V at 0.5C (0.945mA). The capacity at the tenth cycle was measured. Using a battery manufactured separately using the same sample, the capacity at the tenth cycle when charging and discharging at 0.1C for 1 to 10 cycles was measured. The ratio of the capacity when charging and discharging at 0.5C to the capacity when charging and discharging at 0.1C was used as the evaluation value of the rate characteristic. The rate characteristic of the lithium ion battery using the sulfide solid electrolyte of Example 13 was 73%. In the lithium ion battery using the sulfide solid electrolyte of Comparative Example 1, it was 50%.

[0118] [Evaluation example] A structural analysis was carried out using synchrotron radiation and neutrons on the sulfide solid electrolyte obtained in Example 1. Specifically, X-ray diffraction using synchrotron radiation was carried out at BL19B2 of SPring-8. A sample sealed in a glass capillary was measured. CeO 2 The measurement data was corrected using a standard sample, and a Rietveld analysis was performed based on the structural model of the argyrodite crystal. Neutron diffraction measurements were performed at BL20 at J-PARC. In neutron diffraction, Rietveld structural analysis can be used to calculate the occupancy of each site, distinguishing between S and Cl at the 4a and 4d sites. The occupancy, or abundance ratio, of the 4a and 4d sites was calculated from a structural model that satisfied both the synchrotron radiation X-ray diffraction and neutron diffraction data. Figure 6 shows the results of structural analysis using synchrotron radiation. It can be seen that there is little difference between the measured data and the analytical data, and that the fitting is highly consistent. From the analytical results, it can be seen that with regard to halogen site selectivity, chlorine (Cl) tends to occupy the 4d site, and bromine (Br) tends to occupy the 4a site.

[0119] Although some embodiments and / or examples of the present invention have been described in detail above, those skilled in the art can easily make many modifications to these exemplary embodiments and / or examples without substantially departing from the novel teachings and advantages of the present invention, and therefore many such modifications are within the scope of the present invention. The contents of the Japanese application specification which is the basis for the Paris priority of this application are incorporated herein in their entirety by reference.

Claims

1. A step of crushing and mixing a raw material containing lithium, phosphorus, sulfur, chlorine, and bromine in a crusher to prepare an intermediate; heat-treating the intermediate at 350 to 480°C; a molar ratio c (Cl / P) of chlorine to phosphorus and a molar ratio d (Br / P) of bromine to phosphorus in the raw material satisfy the following formula (1): 1.2<c+d<1.9...(1)

2. 2. The method according to claim 1, wherein the molar ratio of bromine to phosphorus, d(Br / P), is 0.15 or more and 1.6 or less.

3. The method according to claim 1 or 2, wherein the molar ratio c (Cl / P) of chlorine to phosphorus and the molar ratio d (Br / P) of bromine to phosphorus satisfy the following formula (2): 0.08<d / (c+d)<0.8...(2)

4. The method according to any one of claims 1 to 3, wherein a molar ratio a of lithium to phosphorus (Li / P), a molar ratio b of sulfur to phosphorus (S / P), a molar ratio c of chlorine to phosphorus (Cl / P), and a molar ratio d of bromine to phosphorus (Br / P) satisfy the following formulas (3) to (5): 5.0≦a≦7.5 ... (3) 6.5≦a+c+d≦7.5...(4) 0.5≦a−b≦1.5 (5) (Wherein, b>0, c>0, and d>0 are satisfied.)

5. The method according to any one of claims 1 to 4, wherein c+d in formula (1) is 1.4 or more and 1.8 or less.

6. The method according to any one of claims 1 to 5, wherein the heat treatment temperature is 360 to 460°C.

7. The method according to any one of claims 1 to 6, wherein the heat treatment is performed in an inert gas atmosphere.

Citation Information

Patent Citations

  • Solid sulfide electrolyte material, solid-state lithium battery, and method for manufacturing solid sulfide electrolyte material

    JP2013016423A

  • Positive electrode mixture

    JP2014011033A

  • Solid electrolyte compact, process of manufacturing the same, and all solid battery

    JP2014093260A

  • Negative electrode mixture, electrode, and lithium ion battery

    JP2015002054A

  • Sulfide solid electrolyte material, battery and method for producing sulfide solid electrolyte material