Method for manufacturing spigot protrusion and shell comprising spigot protrusion
By employing a welding method with angled wires and non-energized second material application, the method addresses shape discrepancies in socket protrusion manufacturing, enhancing productivity and precision in forming pipe joints.
Patent Information
- Application Number
- JP2023057019
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
The existing method for manufacturing socket protrusions on pipe joints requires excessive surface cutting to achieve the desired shape, leading to poor productivity due to shape discrepancies between the formed and desired shapes.
A method involving the use of a first welding wire to form a molten part on the outer surface of a tube, followed by applying a second welding material without electricity to create a protrusion through weld build-up, with specific wire angles and positions to achieve a desired asymmetrical trapezoidal cross-section.
This method improves productivity by forming the protrusion in a single rotation, reducing the need for excessive cutting and achieving precise, efficient manufacturing of pipe joints with enhanced productivity.
Smart Images

Figure 2024144868000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a plug protrusion and a tubular body equipped with a plug protrusion, and in particular to a tubular body having a plug at its tip, a method for manufacturing a plug protrusion that forms a plug protrusion that protrudes radially outward from the outer circumferential surface of the plug, and a tubular body equipped with a plug protrusion. [Background technology]
[0002] Conventionally, there are pipes used to transport various fluids, and their joints have an expansion function and a separation prevention function. This type of joint structure is also called an earthquake-resistant pipe joint. For example, as shown in FIG. 8, a protrusion 10 provided on the outer periphery of the insertion port 1 of a pipe P engages with a lock ring 4 fitted into an inner peripheral groove of a socket 2 of another opposing pipe P to exert a separation prevention function. In addition, the protrusion 10 of the insertion port 1 moves a predetermined distance (corresponding to sections A and B in the figure) between the inner back end surface 3 of the socket 2 and the lock ring 4, allowing the pipe to expand and contract in the axial direction. In addition, a rubber ring 5 is provided between the insertion port 1 and the socket 2, ensuring liquid-tightness between the outer periphery surface 1a of the insertion port 1 and the inner surface 2a of the socket 2.
[0003] The protrusion 10 of the insertion port 1 is formed by depositing weld metal, and an example of a document disclosing such a method is Patent Document 1 (JP Patent Publication No. 2022-310). Patent Document 1 discloses a manufacturing method in which a first welding material and a second welding material are used to form a weld on the outer peripheral surface of the insertion port by an arc generated by passing an electric current through the first welding material, and the second welding material is applied to the weld without electric current before the weld hardens, thereby forming the protrusion by weld deposit. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2022-310 Summary of the Invention [Problem to be solved by the invention]
[0005] However, when forming the insertion port protrusion using the manufacturing method described in Patent Document 1, it is necessary to cut the welded bead surface to form it into the finished shape. However, since the shape of the bead surface is different from the shape of the finished product, the amount of cutting is large, resulting in poor productivity.
[0006] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a method for manufacturing an insertion port protrusion that can improve productivity, and a tube body equipped with an insertion port protrusion. [Means for solving the problem]
[0007] A method for manufacturing a spigot protrusion according to one embodiment of the present invention is a method for manufacturing a spigot protrusion in a tubular body having a spigot at its tip, which forms a spigot protrusion that protrudes radially outward from the outer peripheral surface of the spigot, and includes the steps of holding the tubular body horizontally and rotatably around its axis, setting a first welding wire for feeding a first welding material and a second welding wire for feeding a second welding material toward the outer peripheral surface of the tubular body while being inclined toward the spigot from the vertical direction, and forming a molten portion on the outer peripheral surface of the spigot by an arc generated by passing an electric current through the first welding material, and applying a second welding material to the molten portion without passing an electric current through it before the molten portion hardens, thereby forming the protrusion by weld buildup.
[0008] Preferably, in the setting step, an inclination angle of the first welding wire and the second welding wire with respect to the vertical direction is equal to or greater than 10° and equal to or less than 30°.
[0009] Preferably, in the setting step, the first welding wire and the second welding wire are disposed at positions shifted upstream in a rotation direction of the tubular body with respect to a vertical center line.
[0010] Preferably, in the setting step, a tip end of the first welding wire is arranged to face an axial center of the tubular body.
[0011] A pipe body with an insertion port protrusion according to one embodiment of the present invention is a pipe body having an insertion port at its tip and an insertion port protrusion that protrudes radially outward from the outer periphery of the insertion port, and is provided with a protrusion formed from weld metal that is provided at the insertion port and protrudes radially outward from the outer periphery of the insertion port, and a penetration portion located on the inner diameter side of the protrusion and in which the base material of the insertion port and the weld metal are fused, the penetration portion having a maximum thickness portion where its thickness is at its maximum, and the axial length from the insertion port side end of the penetration portion to the maximum thickness portion is longer than the axial length from the receiving port side end of the penetration portion to the maximum thickness portion. Effect of the Invention
[0012] According to the method for manufacturing a plug protrusion and a tube provided with a plug protrusion of the present invention, it is possible to improve productivity. [Brief description of the drawings]
[0013] [Figure 1] 4 is a cross-sectional view showing a plug protrusion formed on a pipe according to an embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a perspective view showing the positional relationship between a base material and a welding position during welding. [Diagram 3] FIG. 4 is a cross-sectional view showing the positional relationship between a base material and a welding position during welding. [Figure 4] 1A and 1B are schematic diagrams showing the positional relationship between the base material and the welding position during welding, in which (A) is a diagram seen from the axial direction, and (B) is a schematic diagram seen from a direction perpendicular to the axial direction. [Diagram 5] FIG. 5 is a diagram showing a modified example and corresponds to FIG. 4(A). [Figure 6] 13 is a photograph showing a protrusion after build-up welding has been performed by tilting the first welding wire and the second welding wire toward the insertion port side and setting the inclination angle with respect to the vertical direction to θ3=0°. [Figure 7]Photographs showing the protrusions after welding buildup was performed by tilting the first welding wire and the second welding wire toward the insertion port and changing the inclination angle θ3 with respect to the vertical direction, where (A) is θ3=10°, (B) is θ3=20°, and (C) is θ3=30°. [Figure 8] FIG. 1 is a vertical end view showing a joint in the prior art. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and their description will not be repeated.
[0015] With reference to Figs. 1 to 4 and 8, a tube P having a protrusion 10 on a plug 1 according to an embodiment of the present invention will be described. The main configuration of the tube P is as shown in Fig. 8 used in the description of the conventional example, so its description will be omitted and the following description will focus on the configuration of the plug protrusion 10, which is a feature of this invention. Note that arrow A in Figs. 1 and 4(B) indicates the plug side, which is also referred to as the axial tip side. The opposite direction of arrow A is the socket side, which is also referred to as the axial rear end side. Arrow R in Figs. 2 to 4 indicates the rotation direction of the tube P.
[0016] (About the insertion port protrusion) As shown in Fig. 8, the tube P of this embodiment basically comprises an insertion port 1 provided at the axial tip end and a socket 2 provided at the axial rear end. The insertion port 1 is provided with a protrusion 10 that protrudes radially outward from the outer circumferential surface 1a of the insertion port 1. The protrusion 10 is provided continuously around the entire circumferential circumference of the tube P. This protrusion 10 is also referred to as an "insertion port protrusion."
[0017] As shown in Fig. 1, protrusion 10 is formed by cutting protrusion 100, which is a weld buildup formed from weld metal. A weld buildup (weld bead) is formed on the metallic base material that constitutes insertion port 1, and the portion formed by the weld metal is protrusion 100. In Fig. 1, the shape of protrusion 10 in its completed form is shown by a dashed line.
[0018] The protrusion 100 after the weld buildup has a mountain-like shape in an axial cross-sectional view, and is formed by the bead surface 14. Specifically, the axial cross-sectional shape of the protrusion 100 is an asymmetric trapezoid, with the inclined portion 100a on the insertion side being longer than the inclined portion 100b on the receiving side. Here, the protrusion 100 is said to be made of weld metal, but this does not exclude the possibility that the material constituting the protrusion 100 includes the base material of the insertion port 1 melted in the weld metal.
[0019] As shown by the dashed line in the figure, the completed protrusion 10 has an asymmetric trapezoidal cross section in the axial direction. Specifically, the protrusion 10 is formed of a cylindrical portion 10d extending in the axial direction, a tapered portion 10c that is connected to the insertion port 1 side of the cylindrical portion 10d and gradually reduces in diameter toward the tip 1b, and a step portion 10b that is provided on the receiving port 2 side of the cylindrical portion 10d and perpendicular to the extension line of the outer circumferential surface 1a. The angle θ1 between the tapered portion 10c of the protrusion 10 and the extension line of the outer circumferential surface 1a is 15° or more and 30° or less, and is 20° or 25° in this embodiment. The radial height of the cylindrical portion 10d from the outer circumferential surface 1a is 2 mm or more and 3 mm or less, and is 2.5 mm in this embodiment.
[0020] A penetration portion 11 is provided on the inner diameter side of the protrusion 100. The shape of the penetration portion 11 is such that it penetrates radially inward from the outer circumferential surface 1a of the insertion port 1. The penetration portion 11 penetrates to a depth t1 on the inner diameter side from the outer circumferential surface 1a of the insertion port 1, and the base material of the insertion port 1 and the weld metal are fused together. The maximum depth t1 of the penetration portion 11 reaches a depth from the outer circumferential surface 1a of the insertion port 1 that is 10% to 80% of the thickness t0 of the base material of the insertion port 1.
[0021] The penetration portion 11 has a maximum thickness portion 15 where the thickness is maximum. An axial length L1 from an insertion port side end 16 (where the penetration portion 11 and the outer peripheral surface 1a on the insertion port 1 side intersect) to the maximum thickness portion 15 is longer than an axial length L2 from a socket side end 17 (where the penetration portion 11 and the outer peripheral surface 1a on the socket 2 side intersect) to the maximum thickness portion 15. Specifically, the axial length L1 is, for example, 1.2 times or more and 2.5 times or less than the axial length L2.
[0022] The melted portion 11 includes an insertion port side region 12 and a socket side region 13. When an intersection 18 is defined as an intersection between a line extending radially outward from the maximum thickness portion 15 and the outer peripheral surface 1a of the tube body P, the insertion port side region 12 is a region surrounded by the insertion port side end 16, the maximum thickness portion 15, and the intersection 18, and the socket side region 13 is a region surrounded by the socket side end 17, the maximum thickness portion 15, and the intersection 18. In this case, the insertion port side region 12 is larger than the cross-sectional area of the socket side region 13. The melted portion 11, like the protrusion 100, has an asymmetrical cross-sectional shape. The depth of maximum thickness portion 15 of melt-in portion 11 (the radial dimension from outer peripheral surface 1a to maximum thickness portion 15) is approximately the same as the maximum height of protrusion 100 (the radial dimension from outer peripheral surface 1a to the top), and is, for example, 0.8 to 1.2 times. Also, angle θ2 of insertion port side region 12 of melt-in portion 11 is approximately the same as angle θ1 between tapered portion 10c of protrusion 10 and an extension line of outer peripheral surface 1a, or the difference therebetween is within 10°.
[0023] The tube P before the protrusion 100 is formed is manufactured by centrifugal casting. In centrifugal casting, a cylindrical mold is placed on rollers that rotate by a driving force, and while rotating the mold around its axis, molten metal is poured into the mold and the molten metal is hardened to form the tube P. The mold is provided with a dam to prevent the poured molten metal from leaking out. After hardening, the tube P is pulled out of the mold. The material of the tube P is adjusted by a specified heat treatment or the like, and then the protrusion 10 of the insertion port 1 is processed.
[0024] (About welding equipment) Welding apparatus 20 for processing protrusion 100 is shown in Fig. 2 and Fig. 3. This welding apparatus 20 is an apparatus for performing cold tandem (registered trademark) welding, and includes an arc welding torch 23 for supplying a first welding material 21 for arc welding in an energized state, and a welding material supply device 24 for supplying a second welding material 22 in a non-energized state. Arc welding torch 23 and welding material supply device 24 are connected by a connecting member 25 and maintained at a predetermined distance. This predetermined distance can be increased or decreased by adjustment.
[0025] The arc welding torch 23 feeds the first welding material 21 to the tip (welding position) a of the outer peripheral surface 1a of the insertion port 1, which is the base material, by the feeding device 28. The first welding material 21 functions as an electrode for passing a current, and an arc is generated between the first welding material 21 and the base material by passing a welding current supplied from a power source 27 through the first welding material 21. As the first welding material 21, a well-known welding wire, for example, FeNi φ0.8 to 1.6 mm, can be used. In addition, as the first welding material 21, various materials such as well-known solid wire, flux wire, various welding rods, and strip electrodes can be used. In this embodiment, a welding wire is used as the first welding material 21, and is hereinafter referred to as the first welding wire 21.
[0026] The welding material supply device 24 uses a delivery device 26 to deliver the second welding material 22 toward the tip (welding position) b of the outer circumferential surface 1a of the insertion port 1, which is the base material, without passing current through it. As the second welding material 22, for example, FeNi φ0.8 to 1.6 mm can be used. In addition, as the second welding material 22, various materials such as well-known solid wire, flux wire, various welding rods, and strip electrodes can be used. In this embodiment, a welding wire is used as the second welding material 22, and will be referred to as the second welding wire 22 hereinafter.
[0027] (Method of manufacturing the insertion port protrusion) Next, a method for manufacturing the insertion port protrusion 10 according to this embodiment will be described with reference to Figures 2 to 4. In Figures 3 and 4, the vertical direction is indicated by a dashed line.
[0028] First, the tube P is held rotatably around its axis (tube holding step). Specifically, as shown in Fig. 2, the tube P is held horizontally and rotatably around its axis by a gripping device H. Due to the rotation of the tube P, the arc welding torch 23 and the welding material supply device 24 connected by a connecting member 25 move in the rotational direction relative to the insertion port 1 of the tube P, which is the base material.
[0029] Secondly, the tip a of the first welding wire 21 and the tip b of the second welding wire 22 are set toward the outer circumferential surface 1a of the tubular body P (setting step). Conditions for setting the first welding wire 21 and the second welding wire 22 include the inclination angle with respect to the axial direction, the inclination angle with respect to the circumferential direction, and the position in the circumferential direction. Each item will be described below.
[0030] With reference to FIG. 4(B), the inclination angle with respect to the axial direction will be described. The first welding wire 21 and the second welding wire 22 are inclined in the axial direction at approximately the same angle. Specifically, the first welding wire 21 and the second welding wire 22 are inclined toward the insertion port 1 side with respect to the vertical direction and directed toward the outer circumferential surface 1a of the tube body P. In other words, the tips a and b of the wires 21 and 22 are inclined with respect to the axial direction with respect to the rear end side (opposite side of the arrow A). Specifically, the inclination angle θ3 of the first welding wire 21 and the second welding wire 22 in the vertical direction is set to 10° or more and 30° or less. If the inclination angle θ3 is less than 10°, the cross-sectional shape in the axial direction of the protrusion 100 after the weld buildup becomes approximately an isosceles trapezoid (symmetrical), which is different from the shape of the completed protrusion 10. If the inclination angle θ3 exceeds 30°, the cross-sectional shape becomes asymmetrical, but the height is insufficient. By setting the inclination angle θ3 to be between 10° and 30°, the shape of the projection 100 immediately after welding can be made closer to the shape of the finished projection 10. Furthermore, the axial lengths of the penetration portion 11 have the relationship L1>L2 (FIG. 1).
[0031] With reference to Fig. 4(A), the inclination angle with respect to the circumferential direction will be described. The first welding wire 21 is not inclined with respect to the vertical direction, but is made approximately parallel to the vertical direction. The second welding wire 22 is inclined toward the upstream side in the rotation direction with respect to the vertical center line. Specifically, the inclination angle θ4 of the second welding wire 22 with respect to the vertical direction is set to be 35° or more and 55° or less. The upstream side in the rotation direction is the side based on the rotation direction R in which the tube body P rotates, and the right side on the paper of Fig. 4(A) is the upstream side in the rotation direction with respect to the vertical center line, and the left side is the downstream side.
[0032] The circumferential positions will be described with reference to the figure. The first welding wire 21 and the second welding wire 22 are disposed at positions shifted upstream in the rotation direction of the tube P with respect to the vertical center line. Here, the vertical center line is a line that extends in the vertical direction and passes through the axis of the tube P. That is, in the present embodiment, when the tube P rotates in the counterclockwise direction as viewed from the front, the first welding wire 21 and the second welding wire 22 are disposed to the right of the vertical center line.
[0033] If the tip a of the first welding wire 21 and the tip b of the second welding wire 22 are disposed downstream of the vertical center line, there is a risk that the molten metal from the second welding wire 22 will drip when the rotation speed of the tube P is high. However, in the manufacturing method of this embodiment, the tip a of the first welding wire 21 and the tip b of the second welding wire 22 are disposed upstream in the rotation direction. Therefore, even when the rotation speed of the tube P is high, there is no risk that the molten metal from the second welding wire 22 will drip. Therefore, the manufacturing method of this embodiment can also be used for manufacturing methods in which the rotation speed of the tube P is high.
[0034] Moreover, the first welding wire 21 is positioned upstream of the second welding wire 22 in the rotation direction.
[0035] Third, the protrusion 100 is formed by welding buildup (welding buildup process). Specifically, as shown in FIG. 3, a first welding wire 21 and a second welding wire 22 are used, and a molten part W is formed on the outer peripheral surface 1a of the insertion port 1 by an arc generated by energizing the first welding wire 21, and before the molten part W hardens, the second welding wire 22 is applied to the molten part W in a non-energized state. As a result, the protrusion 100 protruding to the outer diameter side is formed on the outer peripheral surface 1a of the insertion port 1 by welding buildup (welding bead). At this time, the second welding wire 22 is in a non-energized state, but is heated by being applied to the molten part W generated by the arc of the first welding wire 21, and the metal of the second welding wire 22 melts and is supplied to the molten part W as a weld metal.
[0036] At the same time, the penetration portion 11, in which the weld metal of the first welding wire 21 and the second welding wire 22 are fused with the base metal of the insertion port 1, is formed at a depth of 10% or more and less than 80% of the thickness t0 of the base metal of the insertion port 1 from the outer peripheral surface 1a of the insertion port 1. Here, it is more preferable that the ratio of the maximum depth t1 of the penetration portion 11 to the thickness t0 of the base metal is 20% or more and less than 60%. If this depth ratio is too low, the strength of the protrusion 10 may be insufficient due to insufficient penetration, and if this depth ratio is too large, the base metal may be penetrated. When setting such a depth ratio, the above-mentioned cold tandem welding method is optimal.
[0037] That is, when forming the protrusion 100 of the insertion port 1 by weld build-up, the amount of weld metal supplied per unit time is increased by using cold tandem welding, and the amount of melting per unit time (welding speed) can be increased. In addition, by adding a non-current-carrying second welding wire 22 to the fusion zone W, the molten pool of the metal material in the fusion zone W can be cooled, making it possible to reduce the penetration depth and prevent the weld metal from dripping. Due to these effects, it is possible to obtain the desired bead shape of the protrusion 100 at the same speed as the conventional welding method using a ring.
[0038] Finally, the protrusion 100 after the weld buildup is cut to form the protrusion 10 in its finished shape (cutting process). Specifically, the bead surface 14 of the protrusion 100 after the weld buildup is cut to form the shape of the protrusion 10 in its finished shape shown by the dashed line in FIG. 1. In FIG. 1, the tip of the protrusion 10 coincides with the tip 1b of the insertion port 1, so the pipe body P is cut along the line shown by the symbol S in the figure, but this cutting can be performed according to the positional relationship between the tip of the protrusion 10 and the tip 1b of the insertion port 1, and is not an essential process. The protrusion 10 can be formed into its finished shape by combining a high-frequency grinder and lathe processing.
[0039] In the manufacturing method of the insertion port projection 10 of this embodiment, the welding build-up process is performed after the positions and orientations of the first welding wire 21 and the second welding wire 22 are set according to the above-mentioned conditions, so that the shape of the projection 100 immediately after welding can be made close to the completed shape of the projection 10 (the cross-sectional shape is a trapezoid with an asymmetric cross section), and the amount of cutting can be reduced. This makes it possible to form the projection 10 more easily and with higher accuracy, and shorten the manufacturing time while maintaining quality.
[0040] Conventionally, it was necessary to perform multi-layer welding in which the tube is rotated two or more times around the tube axis in order to weld the protrusion in the desired shape, but by setting the first welding wire 21 and the second welding wire 22 under the above-mentioned conditions and performing weld build-up, it is possible to perform "single-layer welding" in which the entire circumference of the protrusion 100 is finished in one rotation around the tube axis. This makes it possible to further shorten the manufacturing time.
[0041] (Other manufacturing methods) A manufacturing method according to another embodiment will be described with reference to FIG. 5. The following manufacturing method is basically the same as the setting conditions of the manufacturing method described above, but the inclination angle of the first welding wire 21 with respect to the circumferential direction is different. In the manufacturing method of the insertion port protrusion 10 described above, the first welding wire 21 is set parallel to the vertical direction, but as shown in FIG. 5, it may be set so as to face the axis of the tube body P at the same position. Specifically, the first welding wire 21 is arranged at an incline so that the extension line of the first welding wire 21 passes through the axis. As a result, the angle in the circumferential direction between the first welding wire 21 and the second welding wire 22 is larger than that in the above-mentioned embodiment. Even when the extension line of the first welding wire 21 is set so as to face the axis of the tube body P, the shape of the protrusion 100 after welding buildup can be made close to the completed shape of the protrusion 10, as in the above-mentioned embodiment.
[0042] (About the experimental example) Next, referring to Fig. 6 and Fig. 7, the shape of the protrusion after weld build-up will be described when the inclination angle θ3 of the axial direction of the first welding wire 21 and the second welding wire 22 with respect to the vertical direction is changed and set. In the experiment of Fig. 6 and Fig. 7, only the inclination angle θ3 of the axial direction of the first welding wire 21 and the second welding wire 22 with respect to the vertical direction is changed, and the other setting conditions are the same. In Fig. 6 and Fig. 7, the shape of the protrusion in the completed shape is shown by a solid line. Note that the left side on the paper is the insertion side, and the right side on the paper is the receiving side.
[0043] Figure 6 is a photograph of the protrusion after weld buildup when the inclination angle θ3 is 0°. As shown in Figure 6, when the inclination angle θ3 is 0°, the shape of the bead surface of the protrusion after weld buildup is a trapezoid that is symmetrical on the left and right. In other words, when the inclination angle θ3 is 0°, the shape of the protrusion of the weld buildup does not match the shape of the completed protrusion.
[0044] Fig. 7(A) is a photograph of a protrusion after welding buildup when the inclination angle θ3 is 10°, Fig. 7(B) is a photograph of a protrusion after welding buildup when the inclination angle θ3 is 20°, and Fig. 7(C) is a photograph of a protrusion after welding buildup when the inclination angle θ3 is 30°. As shown in Figs. 7(A) to (C), when the inclination angle θ3 is 10°, 20°, and 30°, the cross-sectional shapes of both the protrusion and the penetration part are asymmetric. Specifically, it can be seen that the angle between the bead surface and the outer peripheral surface of the left side of the tube after welding buildup is smaller than the angle between the bead surface and the outer peripheral surface of the right side, and the shape of the protrusion after welding buildup is in line with the shape of the completed protrusion.
[0045] Furthermore, as the inclination angle θ3 increases to 10°, 20°, and 30°, the radial dimension of the protrusion after weld buildup decreases. This shows that when the inclination angle θ3 is less than 10°, the shape of the protrusion after weld buildup becomes significantly larger than the shape of the completed protrusion. When the inclination angle θ3 exceeds 30°, it is found that the height is insufficient and it becomes impossible to finish by welding in one layer.
[0046] It was also found that, in all cases where the inclination angle θ3 was 10°, 20°, or 30°, the axial length from the insertion end of the penetration part to the maximum thickness part was longer than the axial length from the socket end of the penetration part to the maximum thickness part. It was also found that, in all cases where the inclination angle θ3 was 10°, 20°, or 30°, the radial dimension from the outer circumferential surface of the tube to the maximum thickness part of the penetration part was almost equal to the radial dimension to the maximum height of the bead surface. This revealed that, if the inclination angle θ3 was 10° or more and 30° or less, the shape of the protrusion after the weld build-up would be such that the axial length from the insertion end of the penetration part to the maximum thickness part would be longer than the axial length from the socket end of the penetration part to the maximum thickness part, and the radial dimension to the maximum thickness part would be almost equal to the radial dimension to the maximum height of the bead surface.
[0047] In this embodiment, the tube P before the projection 10 of the insertion port 1 is formed is manufactured by centrifugal casting, but the manufacturing method of the tube P before the projection 10 is formed may be other than centrifugal casting, for example, a pouring casting method in which molten metal is poured into a mold by gravity and solidified. Also, this invention can be applied to various tubes P as long as the insertion port 1 for forming the projection 10 is made of metal compatible with welding.
[0048] Although the embodiment of the present invention has been described above with reference to the drawings, the present invention is not limited to the illustrated embodiment. Various modifications and variations can be made to the illustrated embodiment within the same scope as the present invention or within an equivalent scope. [Explanation of symbols]
[0049] 1 insertion port, 1a outer peripheral surface, 10 protrusion, 11 penetration portion, 15 maximum thickness portion, 16 insertion port side end portion, 17 socket side end portion, 20 welding device, 21 first welding material (first welding wire), 22 second welding material (second welding wire), 100 protrusion, P pipe body.
Claims
1. A method for manufacturing an insertion port protrusion, which forms an insertion port protrusion that protrudes radially outward from an outer circumferential surface of a tube having an insertion port at a tip, comprising: holding the tube horizontally and rotatably about an axis; setting a first welding wire for feeding a first welding material and a second welding wire for feeding a second welding material toward an outer circumferential surface of the tubular body in a state inclined toward the insertion port side with respect to a vertical direction; a step of forming a molten portion on the outer peripheral surface of the insertion port by an arc generated by passing an electric current through the first welding material, and applying the second welding material to the molten portion without passing an electric current through the second welding material before the molten portion hardens, thereby forming the protrusion by weld build-up.
2. 2. The method for manufacturing a spigot projection according to claim 1, wherein in the setting step, an inclination angle of the first welding wire and the second welding wire with respect to the vertical direction is 10 degrees or more and 30 degrees or less.
3. 3. The method for manufacturing a spigot protrusion according to claim 1, wherein in the setting step, the first welding wire and the second welding wire are positioned at a position shifted upstream in the rotation direction of the tubular body with respect to a vertical center line.
4. The method for manufacturing a spigot projection according to claim 3 , wherein in the setting step, the first welding wire is arranged so as to face an axial center of the tubular body.
5. A tube having an insertion port at a tip and an insertion port protrusion protruding radially outward from an outer periphery of the insertion port, A protrusion formed of weld metal provided at the insertion port and protruding radially outward from an outer circumferential surface of the insertion port; a welded portion located on an inner diameter side of the protrusion and formed by fusing the base material of the insertion hole with the weld metal; The penetration portion has a maximum thickness portion where the thickness is maximum, A tube body having an insertion protrusion, the axial length from the insertion end of the penetration portion to the maximum thickness portion being longer than the axial length from the receiving end of the penetration portion to the maximum thickness portion.
Citation Information
Patent Citations
Pipe body having insertion port, and method of manufacturing the same
JP2022000310A