Method for manufacturing electrostatic charge image development toner

The use of amorphous polyester resins with specific alcohol and carboxylic acid components in toner production enhances pigment dispersibility, addressing fogging issues and improving image quality in electrophotographic processes.

JP2024144872APending Publication Date: 2024-10-15KAO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023057031
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing toners for electrophotography suffer from issues such as fogging due to low pigment dispersibility and charge amount distribution, which deteriorate image quality, especially at higher speeds.

Method used

A toner production method involving amorphous polyester resins with specific alcohol and carboxylic acid components, combined with colorant particles, is used to enhance pigment dispersibility and reduce surface exposure, thereby suppressing fogging.

Benefits of technology

The method results in improved charge amount distribution and reduced fogging, leading to higher image quality and stability in electrophotographic processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144872000001
    Figure 2024144872000001
  • Figure 2024144872000002
    Figure 2024144872000002
  • Figure 2024144872000003
    Figure 2024144872000003
Patent Text Reader

Abstract

To provide an electrostatic charge image development toner capable of suppressing the occurrence of fog.SOLUTION: A method for manufacturing an electrostatic charge image development toner comprises a step of aggregating and fusing resin particles and colorant particles in an aqueous medium. The resin particles includes an amorphous polyester based resin (A) including a polyester part being a polycondensate between an alcohol component (a) including aliphatic diol having a carbon number of 2 or more and 5 or less and carboxylic acid component (b); the colorant particles includes a colorant and an amorphous polyester based resin (B) including a polyester part being a polycondensate between an alcohol component (c) including aliphatic diol having a carbon number of 2 or more and 5 or less and carboxylic acid component (d); and the mass ratio (the colorant / the amorphous polyester based resin (B)) of the colorant to the amorphous polyester based resin (B) is 55 / 45 or more and 99 / 1 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a toner for developing electrostatic images used in developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like. [Background technology]

[0002] In the field of electrophotography, with the development of electrophotographic systems, there is a demand for the development of electrophotographic toners that can handle higher speeds and higher image quality. As the speed increases, the time it takes for the toner to be transferred to paper also becomes shorter, so toners with excellent charging properties are required. In addition, toners with high coloring power are required to handle higher image quality.

[0003] Patent Document 1 describes a method for producing a toner for developing electrostatic images, the method including: step (1): mixing a polyester resin with a basic aqueous solution to obtain a resin neutralization product; step (2): adding an aqueous medium to the resin neutralization product obtained in step (1) and emulsifying it to obtain a resin particle dispersion; step (3): aggregating the resin particles in the resin particle dispersion obtained in step (2) to obtain aggregated particles; and step (4): fusing the aggregated particles obtained in step (3) to obtain toner particles, for the purpose of providing a method for producing a toner having a narrow particle size distribution and excellent dot reproducibility and charge stability. The method includes the steps of: [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 112488 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the toner obtained by the toner manufacturing method described in Patent Document 1 has room for improvement in terms of suppressing the occurrence of fog. The present invention relates to a toner for developing electrostatic images, which is capable of suppressing the occurrence of fogging. [Means for solving the problem]

[0006] The present inventors have found that by using a toner for developing electrostatic images produced by a method for producing a toner for developing electrostatic images, the method including a step of aggregating and fusing, in an aqueous medium, colorant particles that contain resin particles containing an amorphous polyester resin (A) containing a polyester moiety that is a polycondensation product of a specific alcohol component (a) and a carboxylic acid component (b), and an amorphous polyester resin (B) containing a polyester moiety that is a polycondensation product of a colorant, a specific alcohol component (c) and a carboxylic acid component (d), wherein the mass ratio of the colorant to the amorphous polyester resin (B) is within a specific range. The present invention relates to the following [1] and [2]. [1] A method for producing a toner for developing an electrostatic image, comprising a step of aggregating and fusing resin particles and colorant particles in an aqueous medium, the resin particles contain an amorphous polyester-based resin (A) including a polyester moiety that is a polycondensate of an alcohol component (a) including an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b); the colorant particles contain a colorant and an amorphous polyester-based resin (B) containing a polyester moiety which is a polycondensate of an alcohol component (c) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (d); A method for producing a toner for developing electrostatic images, wherein the mass ratio of the colorant to the amorphous polyester resin (B) (colorant / amorphous polyester resin (B)) is 55 / 45 or more and 99 / 1 or less. [2] A colorant particle dispersion liquid comprising colorant particles containing a colorant and an amorphous polyester resin (B) containing a polyester moiety which is a polycondensate of an alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d), wherein the mass ratio of the colorant to the amorphous polyester resin (B) (colorant / amorphous polyester resin (B)) is 55 / 45 or more and 99 / 1 or less. Effect of the Invention

[0007] According to the present invention, there is provided a toner for developing electrostatic images which can give printed matter with suppressed occurrence of fog. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] [Method of manufacturing toner for developing electrostatic images] The method for producing the toner for developing electrostatic images (hereinafter, also simply referred to as "toner") of the present invention includes a step of aggregating and fusing resin particles and colorant particles in an aqueous medium. The resin particles contain an amorphous polyester resin (A) (hereinafter also simply referred to as "resin (A)") containing a polyester moiety that is a polycondensate of an alcohol component (a) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b). The colorant particles contain a colorant, and an amorphous polyester resin (B) (hereinafter also simply referred to as "resin (B)") containing a polyester moiety that is a polycondensate of an alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d), and the mass ratio of the colorant to the amorphous polyester resin (B) (colorant / amorphous polyester resin (B)) is 55 / 45 or more and 99 / 1 or less. Due to the above-mentioned characteristics, by using the toner of the present invention, it is possible to obtain printed matter in which the occurrence of fog is suppressed.

[0009] The reason why the toner of the present invention can provide printed matter with suppressed fog generation is not clear, but is thought to be as follows. Conventionally, toners containing a colorant and an amorphous polyester resin, which is a polycondensation product of an alcohol component containing an aliphatic diol with 2 to 5 carbon atoms and a carboxylic acid component, have had problems such as poor image quality due to a wide distribution of charge due to low pigment dispersibility and inclusion, resulting in fog and other problems. This is thought to be due to the low affinity between the amorphous polyester and the colorant, and particularly when toners are produced by emulsion polymerization in water, not only is the affinity between the two low, but there is no kneading shear, unlike when producing toners by pulverization, so problems such as pigment aggregation and surface exposure are more pronounced. In the production method of the present invention, resin particles containing a resin (A) containing a polyester moiety that is a polycondensate of an alcohol component (a) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b) as a binder resin, and colorant particles containing a colorant and a resin (B) containing a polyester moiety that is a polycondensate of an alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d) are aggregated and fused in an aqueous medium to obtain a toner for developing electrostatic images that suppresses the occurrence of fog. This is thought to be because in the colorant particles, the resin (B) covers at least a portion of the surface of the colorant, and therefore in the process of aggregating the resin particles and the colorant particles, the high affinity between the resin (A) and the resin (B) makes it easier to finely disperse the colorant particles in the aggregated particles, which not only suppresses exposure of the colorant on the surface of the toner particles obtained by fusing the aggregated particles, but also makes it possible to uniformly incorporate the colorant into the toner particles, resulting in a toner that improves the charge distribution of the toner and suppresses the occurrence of fog. Furthermore, when resin (B) is a composite resin having a styrene-acrylic moiety, the coverage of the colorant by resin (B) is enhanced, which further suppresses exposure of the colorant to the surface of the toner particles and allows the colorant to be more uniformly incorporated into the toner particles. As a result, it is believed that the toner obtained by the production method of the present invention further suppresses the occurrence of fog. The above-mentioned mechanism regarding the effect of the present invention is merely a presumption, and the present invention is not limited thereto.

[0010] The definitions of various terms used in this specification are given below. In the specification, the carboxylic acid component of the polyester resin includes not only the compound itself, but also anhydrides that decompose during the reaction to produce a carboxylic acid, and alkyl esters of each carboxylic acid (alkyl groups having 1 to 3 carbon atoms). Whether a resin is crystalline or amorphous is determined by the crystallinity index. The crystallinity index is defined as the ratio of the softening point of the resin to the maximum endothermic peak temperature (softening point (°C) / maximum endothermic peak temperature (°C)) in the measurement method described in the examples below. A crystalline resin is one with a crystallinity index of 0.6 or more and 1.4 or less. An amorphous resin is one in which no endothermic peak is observed, or, if observed, has a crystallinity index of less than 0.6 or more than 1.4. The crystallinity index can be appropriately adjusted by the types and ratios of raw material monomers, as well as production conditions such as reaction temperature, reaction time, and cooling rate. With respect to hydrocarbon groups, the references "(iso or tertiary)" and "(iso)" in parentheses refer to both the cases with and without the prefixes present; the absence of the prefixes indicates normal. "(Meth)acrylic acid" means at least one selected from acrylic acid and methacrylic acid. The term "(meth)acrylate" refers to at least one selected from acrylate and methacrylate.

[0011] [Resin particles] The resin particles contain an amorphous polyester-based resin (A) containing a polyester moiety which is a polycondensate of an alcohol component (a) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (b) in order to obtain a toner that enhances the dispersibility of colorant particles in toner particles and suppresses the occurrence of fog.

[0012] <Amorphous polyester resin (A) (resin (A))> The resin (A) is a polyester resin which is a polycondensation product of an alcohol component (a) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b), or a composite resin which contains a polyester portion which is a polycondensation product of an alcohol component (a) and a carboxylic acid component (b). Examples of composite resins include urethane-modified polycondensates of an alcohol component (a) and a carboxylic acid component (b), epoxy-modified polycondensates of an alcohol component (a) and a carboxylic acid component (b), and resins in which a polyester portion, which is a polycondensate of an alcohol component (a) and a carboxylic acid component (b), and a styrene-acrylic portion are composited. Among these, the resin (A) is preferably an amorphous polyester resin which is a polycondensation product of an alcohol component (a) and a carboxylic acid component (b).

[0013] The alcohol component (a) contains an aliphatic diol having 2 to 5 carbon atoms. Examples of the aliphatic diol having 2 to 5 carbon atoms include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, 2,3-pentanediol, 2,4-pentanediol, and neopentyl glycol. The aliphatic diol having 2 to 5 carbon atoms is preferably ethylene glycol, 1,2-propanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, and neopentyl glycol, more preferably ethylene glycol, 1,2-propanediol, 2,3-butanediol, and neopentyl glycol, and even more preferably 1,2-propanediol and neopentyl glycol. In order to obtain a toner that suppresses the occurrence of fog, the content of the aliphatic diol having 2 to 5 carbon atoms in the alcohol component (a) is preferably 85 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, and is preferably 100 mol % or less, more preferably 100 mol %.

[0014] Examples of the alcohol component (a) other than the aliphatic diol having 2 to 5 carbon atoms include alkylene oxide adducts of aromatic diols, aliphatic diols having 6 or more carbon atoms, alicyclic diols, and trihydric or higher polyhydric alcohols. The alkylene oxide adduct of an aromatic diol is preferably represented by the formula (I):

[0015] [ka] (wherein OR and RO are oxyalkylene groups, R each independently represents an ethylene or propylene group, x and y represent the average number of moles of alkylene oxide added and are each positive numbers, and the sum of x and y is 1 or more, preferably 1.5 or more, and 16 or less, preferably 8 or less, and more preferably 4 or less). Examples of the alkylene oxide adduct of bisphenol A represented by formula (I) include a propylene oxide adduct of 2,2-bis(4-hydroxyphenyl)propane, an ethylene oxide adduct of 2,2-bis(4-hydroxyphenyl)propane, etc. One or more of these may be used.

[0016] Examples of the aliphatic diols having 6 or more carbon atoms include 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, and 1,4-butenediol. Examples of alicyclic diols include hydrogenated bisphenol A [2,2-bis(4-hydroxycyclohexyl)propane] and alkylene oxide adducts of hydrogenated bisphenol A having 2 to 4 carbon atoms (average number of moles added: 2 to 12). Examples of trihydric or higher polyhydric alcohols include glycerin, pentaerythritol, trimethylolpropane, and sorbitol. These alcohol components may be used alone or in combination of two or more.

[0017] Examples of the carboxylic acid component (b) include aromatic dicarboxylic acid compounds, aliphatic dicarboxylic acid compounds, and trivalent or higher carboxylic acid compounds. Among these, the carboxylic acid component (b) preferably contains an aromatic dicarboxylic acid compound, from the viewpoint of obtaining a toner that suppresses the occurrence of fog. Examples of the aromatic dicarboxylic acid compound include phthalic acid, isophthalic acid, and terephthalic acid. Among these, at least one selected from terephthalic acid and isophthalic acid is more preferable from the above viewpoint. From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the content of the aromatic dicarboxylic acid compound in the carboxylic acid component (b) is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, and preferably 100 mol % or less.

[0018] Examples of the aliphatic dicarboxylic acid compound include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid which may be substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms, and adipic acid. Examples of succinic acid substituted with an aliphatic hydrocarbon group having 1 to 20 carbon atoms include octyl succinic acid and dodecenyl succinic acid (tetrapropenyl succinic acid). Of these, fumaric acid is preferred. From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the content of the aliphatic dicarboxylic acid compound in the carboxylic acid component (b) is preferably 40 mol % or less, more preferably 30 mol % or less, even more preferably 20 mol % or less, and preferably 0 mol % or more.

[0019] Examples of trivalent or higher carboxylic acid compounds include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, and pyromellitic acid. The alcohol component (a) may appropriately contain a monohydric alcohol, and the carboxylic acid component (b) may appropriately contain a monocarboxylic acid compound.

[0020] The equivalent ratio of the carboxyl groups of the carboxylic acid component (b) to the hydroxyl groups of the alcohol component (a) [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.

[0021] When the resin (A) is a composite resin of a polyester moiety, which is a polycondensation product of an alcohol component (a) and a carboxylic acid component (b), and a styrene-acrylic moiety, the styrene-acrylic moiety is, for example, an addition polymerization product of raw material monomers including a styrene-based compound and a (meth)acrylic compound. Examples of the styrene-based compound include unsubstituted or substituted styrene. Examples of the substituent substituted on styrene include an alkyl group having 1 to 5 carbon atoms, a halogen atom, an alkoxy group having 1 to 5 carbon atoms, a sulfonic acid group, or a salt thereof. Examples of styrene-based compounds include styrene, methylstyrene, α-methylstyrene, β-methylstyrene, tert-butylstyrene, chlorostyrene, chloromethylstyrene, methoxystyrene, styrenesulfonic acid, and salts thereof. Among these, styrene is preferred. In the raw material monomers of the styrene-acrylic portion, the content of the styrene-based compound is preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 15 mass% or more, and preferably 35 mass% or less, more preferably 30 mass% or less, even more preferably 25 mass% or less.

[0022] Examples of (meth)acrylic compounds include (meth)acrylic acid and its esters. Among these, (meth)acrylic acid and alkyl esters of (meth)acrylic acid are preferred. The number of carbon atoms in the alkyl group in the alkyl ester of (meth)acrylic acid is preferably 1 or more, more preferably 4 or more, even more preferably 6 or more, and is preferably 24 or less, more preferably 22 or less, even more preferably 20 or less. Examples of alkyl esters of (meth)acrylic acid include methyl (meth)acrylate, ethyl (meth)acrylate, (iso)propyl (meth)acrylate, (iso- or tertiary)butyl (meth)acrylate, (iso)amyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, (iso)octyl (meth)acrylate, (iso)decyl (meth)acrylate, (iso)dodecyl (meth)acrylate, (iso)palmityl (meth)acrylate, (iso)stearyl (meth)acrylate, (iso)behenyl (meth)acrylate, and the like. Of these, methyl (meth)acrylate and (iso- or tertiary)butyl (meth)acrylate are preferred, and methyl methacrylate and n-butyl acrylate are more preferred.

[0023] In the raw material monomers of the styrene-acrylic portion, the content of the (meth)acrylic compound is preferably 65 mass% or more, more preferably 70 mass% or more, even more preferably 75 mass% or more, and preferably 95 mass% or less, more preferably 90 mass% or less, even more preferably 85 mass% or less. The total amount of the styrene-based compound and the (meth)acrylic compound in the raw material monomer of the styrene-acrylic portion is preferably 80 mass % or more, more preferably 90 mass % or more, even more preferably 95 mass % or more, and even more preferably 100 mass %.

[0024] Examples of raw material monomers other than those mentioned above include olefins such as ethylene, propylene, butadiene, etc.; halovinyls such as vinyl chloride; vinyl esters such as vinyl acetate, vinyl propionate, etc.; vinyl ethers such as methyl vinyl ether; vinylidene halides such as vinylidene chloride; N-vinyl compounds such as N-vinylpyrrolidone; and compounds having at least one functional group selected from a hydroxyl group, a carboxyl group, an epoxy group, a primary amino group, and a secondary amino group, and an addition polymerizable group such as a carbon-carbon unsaturated bond (ethylenically unsaturated bond).

[0025] The composite resin as resin (A) preferably has constitutional units derived from a bireactive monomer bonded to a polyester moiety and a styrene-acrylic moiety via a covalent bond. The bireactive monomer may be a raw material monomer for the styrene-acrylic moiety, and from the viewpoint of reactivity, an addition polymerizable monomer having at least one functional group selected from a hydroxyl group and a carboxy group is preferable, and an addition polymerizable monomer having a carboxy group is more preferable. Examples of the addition polymerizable monomer having a carboxy group include (meth)acrylic acid, fumaric acid, and maleic acid, which are listed as (meth)acrylic compounds. Among these, (meth)acrylic acid is preferred, and acrylic acid is more preferred, from the viewpoint of reactivity in both polycondensation reaction and addition polymerization reaction. When the bireactive monomer is an addition polymerizable monomer having a carboxy group, the amount of the constitutional units derived from the bireactive monomer is preferably 0.5 mol parts or more, more preferably 1 mol parts or more, and preferably 20 mol parts or less, more preferably 10 mol parts or less, and even more preferably 5 mol parts or less, relative to 100 mol parts of the alcohol component in the polyester portion of the composite resin.

[0026] The content of the polyester moiety in the composite resin is preferably 90% by mass or more, more preferably 93% by mass or more, even more preferably 95% by mass or more, and preferably 99% by mass or less, more preferably 98% by mass or less, even more preferably 97% by mass or less, based on the total amount of the polyester moieties and the styrene-acrylic moieties.

[0027] The content of the styrene-acrylic moiety in the composite resin is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 10% by mass or less, more preferably 7% by mass or less, based on the total amount of the polyester moiety and the styrene-acrylic moiety. The bireactive monomer-derived constitutional unit is the styrene-acrylic moiety.

[0028] The amount of the constitutional units derived from the bireactive monomer in the composite resin is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, and preferably 1 mass% or less, more preferably 0.7 mass% or less, and even more preferably 0.5 mass% or less, based on the total amount of the polyester portion and the styrene acrylic portion.

[0029] The mass ratio of the polyester moiety content to the styrene-acrylic moiety content in the composite resin (polyester moiety / styrene-acrylic moiety) is preferably 90 / 10 or more, more preferably 93 / 7 or more, and preferably 99 / 1 or less, more preferably 98 / 2 or less, and even more preferably 97 / 3 or less.

[0030] The amount is calculated based on the ratio of the amounts of the polyester portion, the raw material monomer of the styrene-acrylic portion, the bireactive monomer, and the radical polymerization initiator, and the mass is based on the mass excluding the mass of water generated by polycondensation. When a radical polymerization initiator is used, the mass of the radical polymerization initiator is calculated by including it in the styrene-acrylic portion.

[0031] (Production method of polyester resin (A)) The resin (A) may be produced, for example, by a method including a step A of carrying out a polycondensation reaction of raw material monomers including an alcohol component (a) and a carboxylic acid component (b). When the resin (A) is a composite resin, it may be produced by a method including step A and step B of addition-polymerizing a raw material monomer of a styrene-acrylic moiety and a bireactive monomer. In this case, step B may be performed after step A, step A may be performed after step B, or step A and step B may be performed simultaneously. In step B, a raw material monomer of a styrene-acrylic moiety containing a bireactive monomer is subjected to an addition polymerization reaction, and then raw material monomers containing an alcohol component (a) and a carboxylic acid component (b) are added to the obtained styrene-acrylic moiety, and the polycondensation reaction of step A is further advanced to obtain a composite resin.

[0032] The polycondensation of the alcohol component (a) and the carboxylic acid component (b) can be carried out, for example, in an inert gas atmosphere, in the presence of an esterification catalyst, an esterification promoter, a polymerization inhibitor, etc., as necessary, at a temperature of about 120°C or higher and 250°C or lower. Examples of the esterification catalyst include tin compounds such as dibutyltin oxide and tin(II) di(2-ethylhexanoate), and titanium compounds such as titanium diisopropoxybis(triethanolaminate). Examples of the esterification promoter that can be used together with the esterification catalyst include gallic acid. The amount of the esterification catalyst used is preferably 0.01 parts by mass or more and 10 parts by mass or less based on 100 parts by mass in total of the alcohol component (a) and the carboxylic acid component (b), which are raw material monomers for the resin (A). The amount of the esterification promoter used is preferably 0.001 part by mass or more and 1 part by mass or less based on 100 parts by mass in total of the alcohol component (a) and the carboxylic acid component (b). Furthermore, examples of the polymerization inhibitor include radical polymerization inhibitors such as 4-tert-butylcatechol. When a polymerization inhibitor is used, the amount of the polymerization inhibitor used is preferably 0.001 part by mass or more and 1 part by mass or less based on 100 parts by mass in total of the alcohol component (a) and the carboxylic acid component (b).

[0033] A polymerization initiator such as a radical polymerization initiator may be used in the addition polymerization reaction of step B. Examples of the radical polymerization initiator include peroxides such as dibutyl peroxide, persulfates such as sodium persulfate, and azo compounds such as 2,2'-azobis(2,4-dimethylvaleronitrile). When a radical polymerization initiator is used, the amount of the radical polymerization initiator used is preferably 1 part by mass or more and 20 parts by mass or less based on 100 parts by mass of the raw material monomer of the styrene acrylic moiety. When a radical polymerization initiator is used, the temperature of the addition polymerization is preferably 110° C. or higher, more preferably 130° C. or higher, and preferably 230° C. or lower, more preferably 220° C. or lower, and even more preferably 210° C. or lower.

[0034] In the addition polymerization reaction of step B, the styrene acrylic portion may be synthesized without using a polymerization initiator. When a polymerization initiator is not used, the addition polymerization reaction of step B is preferably a bulk polymerization of the raw material monomer of the styrene acrylic portion from the viewpoint that the viscosity of the obtained styrene acrylic portion is not too high and the molecular weight distribution is relatively narrow. For such bulk polymerization, refer to JP 2021-107920 A.

[0035] (Physical properties of polyester resin (A)) The softening point of the resin (A) is preferably 70°C or higher, more preferably 80°C or higher, and even more preferably 90°C or higher from the viewpoint of heat-resistant storage stability, and is preferably 130°C or lower, more preferably 120°C or lower, and even more preferably 110°C or lower from the viewpoint of low-temperature fixability at high speed. The glass transition temperature of the resin (A) is preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 45° C. or higher, from the viewpoint of heat-resistant storage stability, and is preferably 80° C. or lower, more preferably 70° C. or lower, and even more preferably 60° C. or lower, from the viewpoint of low-temperature fixability at high speed.

[0036] The acid value of the resin (A) is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, even more preferably 15 mgKOH / g or more, and is preferably 40 mgKOH / g or less, more preferably 30 mgKOH / g or less, even more preferably 25 mgKOH / g or less. The softening point, glass transition temperature, and acid value of the resin (A) can be appropriately adjusted by the types and amounts of raw material monomers used, as well as production conditions such as reaction temperature, reaction time, and cooling rate, and these values ​​can be determined by the methods described in the examples. When two or more resins (A) are used in combination, the softening point, glass transition temperature and acid value of the mixture thereof preferably fall within the above-mentioned ranges.

[0037] The resin particles may contain an amorphous resin other than the resin (A) and a crystalline resin. Examples of the amorphous resin other than the resin (A) include an amorphous polyester resin other than the resin (A), a styrene acrylic resin, etc. Examples of the crystalline resin include the crystalline polyester resin (C) described below.

[0038] The resin particles contain the amorphous polyester resin (A) in an amount of preferably 90% by mass or more. From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the amount is more preferably 92% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and is preferably 100% by mass or less, even more preferably 100% by mass.

[0039] <Crystalline polyester resin (C) (resin (C))> The resin particles preferably contain a crystalline polyester resin (C) (hereinafter, also simply referred to as "resin (C)"). The resin (C) is a polycondensate of an alcohol component and a carboxylic acid component.

[0040] The alcohol component is preferably an α,ω-aliphatic diol. The α,ω-aliphatic diol preferably has 2 or more carbon atoms, and preferably has 16 or less, more preferably 14 or less, and further preferably 12 or less carbon atoms. Examples of α,ω-aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, etc. Among these, ethylene glycol, 1,6-hexanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred, and ethylene glycol is more preferred.

[0041] The amount of α,ω-aliphatic diol in the alcohol component is preferably 80 mol% or more, more preferably 85 mol% or more, even more preferably 90 mol% or more, even more preferably 95 mol% or more, and is 100 mol% or less, preferably 100 mol%.

[0042] The alcohol component may contain other alcohol components different from the α,ω-aliphatic diol. Examples of the other alcohol components include aliphatic diols other than α,ω-aliphatic diols, such as 1,2-propanediol and neopentyl glycol; aromatic diols, such as alkylene oxide adducts of bisphenol A; and trihydric or higher alcohols, such as glycerin, pentaerythritol, and trimethylolpropane. These alcohol components may be used alone or in combination.

[0043] The carboxylic acid component is preferably an aliphatic dicarboxylic acid, more preferably a straight-chain aliphatic dicarboxylic acid. The aliphatic dicarboxylic acid has preferably 4 or more, more preferably 8 or more, and even more preferably 10 or more carbon atoms, and preferably 14 or less, and more preferably 12 or less. Examples of aliphatic dicarboxylic acids include fumaric acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid. Among these, sebacic acid and dodecanedioic acid are preferred, and sebacic acid is more preferred. These carboxylic acid components may be used alone or in combination.

[0044] The amount of aliphatic dicarboxylic acid in the carboxylic acid component is preferably 80 mol% or more, more preferably 85 mol% or more, even more preferably 90 mol% or more, even more preferably 95 mol% or more, and is 100 mol% or less, even more preferably 100 mol%.

[0045] The carboxylic acid component may contain other carboxylic acid components different from the aliphatic dicarboxylic acid. Examples of other carboxylic acid components include aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid, and polyvalent carboxylic acids having three or more carboxylic acids. These carboxylic acid components may be used alone or in combination.

[0046] The equivalent ratio of the carboxyl groups of the carboxylic acid component to the hydroxyl groups of the alcohol component [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.

[0047] The method for producing the resin (C) may be, for example, the same method as in step A for the resin (A) described above.

[0048] (Physical properties of crystalline polyester resin (C)) From the viewpoint of the storage stability of the toner, the softening point of the resin (C) is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 75° C. or higher, and from the viewpoint of further improving the low-temperature fixing ability, it is preferably 120° C. or lower, more preferably 100° C. or lower, and even more preferably 95° C. or lower. From the viewpoint of the storage stability of the toner, the melting point of the resin (C) is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher, and from the viewpoint of further improving the low-temperature fixing property, it is preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 80°C or lower.

[0049] The acid value of the resin (C) is preferably 5 mgKOH / g or more, more preferably 8 mgKOH / g or more, and preferably 35 mgKOH / g or less, more preferably 25 mgKOH / g or less, and even more preferably 20 mgKOH / g or less. The softening point, melting point and acid value of the resin (C) can be appropriately adjusted by the type and amount of the raw material monomer, as well as production conditions such as reaction temperature, reaction time, cooling rate, etc., and are determined by the method described in the Examples below. When two or more types of resin (C) are used in combination, it is preferable that the softening point, melting point and acid value obtained as a mixture thereof are each within the above-mentioned ranges.

[0050] From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the content of resin (A) in the toner particles is preferably 45% by mass or more, more preferably 50% by mass or more, even more preferably 55% by mass or more, and is preferably 75% by mass or less, more preferably 70% by mass or less, even more preferably 65% ​​by mass or less. From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the content of the resin (C) in the toner particles is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 12% by mass or more, and is preferably 25% by mass or less, more preferably 20% by mass or less, even more preferably 17% by mass or less.

[0051] From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the total content of resin (A) and resin (C) in the toner particles is preferably 60% by mass or more, more preferably 65% ​​by mass or more, even more preferably 70% by mass or more, and is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less.

[0052] The mass ratio of resin (C) to resin (A) in the toner particles [resin (C) / resin (A)] is, from the viewpoint of obtaining a toner that suppresses the occurrence of fog, preferably 0.1 or more, more preferably 0.15 or more, even more preferably 0.2 or more, and is preferably 0.5 or less, more preferably 0.4 or less, even more preferably 0.3 or less.

[0053] <Method of manufacturing resin particles> When the resin particles contain resin (A) and resin (C), the resin particles contain resin (A) and resin (C) in the same or different resin particles. Here, in the following description, the resin particles containing resin (A) and resin (C) in the particles will be described.

[0054] The dispersion of resin particles can be obtained by dispersing the resin (A) and the resin (C) in an aqueous medium. The aqueous medium is preferably one containing water as a main component, and the content of water in the aqueous medium is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and 100% by mass or less, even more preferably 100% by mass, from the viewpoint of improving the dispersion stability of the dispersion liquid of the particles of resin A and from the viewpoint of environmental friendliness. As the water, deionized water or distilled water is preferable. Examples of components other than water that may be contained in the aqueous medium include water-soluble organic solvents such as alkyl alcohols having 1 to 5 carbon atoms; dialkyl ketones having a total of 3 to 5 carbon atoms, such as acetone and methyl ethyl ketone; and cyclic ethers, such as tetrahydrofuran.

[0055] The dispersion can be carried out by a known method, but is preferably carried out by a phase inversion emulsification method, for example, a method in which an aqueous medium is added to an organic solvent solution of a resin or a molten resin to carry out phase inversion emulsification.

[0056] The organic solvent used for phase inversion emulsification is not particularly limited as long as it dissolves the resin. From the viewpoint of ease of removal from the mixed liquid after addition of the aqueous medium, however, ketone-based solvents and acetate-based solvents are preferred, and methyl ethyl ketone is more preferred. It is preferable to add a neutralizing agent to the organic solvent solution. Examples of the neutralizing agent include basic substances. Examples of the basic substance include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and nitrogen-containing basic substances such as ammonia, trimethylamine, and diethanolamine. The degree of neutralization of the resin contained in the resin particles is preferably 10 mol% or more, more preferably 20 mol% or more, even more preferably 30 mol% or more, even more preferably 40 mol% or more, and preferably 100 mol% or less, more preferably 80 mol% or less, even more preferably 70 mol% or less. The degree of neutralization of the resin contained in the resin particles can be calculated by the following formula (1). Degree of neutralization (mol%) = [{weight of neutralizing agent added (g) / equivalent weight of neutralizing agent} / {weighted average acid value of resin constituting resin particle (mgKOH / g) × weight of resin constituting resin particle (g)} / (56 × 1000)] × 100 (1)

[0057] While stirring the organic solvent solution or the molten resin, the aqueous medium is gradually added to cause phase inversion. From the viewpoint of improving the dispersion stability of the resin particles, the temperature of the organic solvent solution when the aqueous medium is added is preferably not less than the glass transition temperature of the resin constituting the resin particles, preferably not less than 60°C, more preferably not less than 70°C, and is preferably not more than 85°C, more preferably not more than 80°C.

[0058] After the phase inversion emulsification, if necessary, the organic solvent may be removed from the obtained dispersion by distillation, etc. In this case, the amount of the remaining organic solvent in the dispersion is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably substantially 0% by mass.

[0059] Volume median diameter D of resin particles in dispersion 50 From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the particle size is preferably 0.1 μm or more, more preferably 0.2 μm or more, and is preferably 0.5 μm or less, more preferably 0.4 μm or less. From the viewpoint of obtaining a toner that suppresses the occurrence of fog, the CV value of the resin particles in the dispersion is preferably 10% or more, more preferably 20% or more, and is preferably 40% or less, more preferably 30% or less. Volume median particle size D 50 The CV value is determined by the method described in the Examples below. Resin particles containing either one of resin (A) and resin (C) can also be produced in accordance with the above-mentioned method. 50 The preferred range of the CV value is the same as that described above.

[0060] [Colorant Particles] The colorant particles contain a non-crystalline polyester resin (B) containing a polyester moiety, which is a polycondensate of a colorant, an alcohol component (c) containing an aliphatic diol having 2 to 5 carbon atoms, and a carboxylic acid component (d), from the viewpoint of obtaining a toner that enhances the dispersibility of the colorant particles in the toner particles and suppresses the occurrence of fogging. It is preferable that the colorant in the colorant particles is coated with the non-crystalline polyester resin (B). The phrase "the colorant is coated with the resin (B)" refers to a state in which the resin (B) is adsorbed to the colorant. It is sufficient that at least a part of the surface of the colorant is coated with the resin (B), but it is preferable that the entire colorant is coated with the resin (B). Whether the colorant is coated with the resin (B) can be identified by analyzing the cut surface of the colorant particle. Specifically, it can be identified by analyzing the resin in contact with the colorant on the cut surface.

[0061] <Coloring agent> The colorant used in the present invention includes pigments and dyes, and from the viewpoint of improving the image density of the printed matter, pigments are preferred. Examples of the pigment include a cyan pigment, a yellow pigment, a magenta pigment, and a black pigment. The cyan pigment is preferably a phthalocyanine pigment, more preferably copper phthalocyanine. The yellow pigment is preferably a monoazo pigment, a benzimidazolone pigment, an isoindoline pigment, or a condensed disazo pigment. The magenta pigment is preferably a soluble azo pigment such as a quinacridone pigment or a BONA lake pigment, or an insoluble azo pigment such as a naphthol AS pigment. The black pigment is preferably carbon black. Examples of the dye include acridine dyes, azo dyes, benzoquinone dyes, azine dyes, anthraquinone dyes, indigo dyes, phthalocyanine dyes, aniline black dyes, etc. The colorants may be used alone or in combination of two or more kinds.

[0062] When the colorant is a yellow pigment, the amount of NH structures contained in one molecule of the yellow pigment is preferably 4.0 mmol / g or more, more preferably 5.0 mmol / g or more, even more preferably 7.0 mmol / g or more, and is preferably 15.0 mmol / g or less, more preferably 12.0 mmol / g or less. The amount of NH structures contained in one molecule of the yellow pigment is the value obtained by dividing the total number of -NH- and -NH2 in the yellow pigment by the molecular weight of the pigment.

[0063] From the viewpoint of setting the amount of NH structures in the above range, the yellow pigment is preferably at least one selected from benzimidazolone pigments, isoindoline pigments, and condensed disazo pigments, and more preferably at least one selected from benzimidazolone pigments and isoindoline pigments. An example of a benzimidazolone pigment is CI Pigment Yellow 180 (total number of -NH- and -NH2 in one molecule=6, molecular weight=733, NH group amount=8.2 mmol / g). An example of an isoindoline pigment is CI Pigment Yellow 185 (total number of -NH- and -NH2 in one molecule=4, molecular weight=337, NH group amount=11.9 mmol / g). Examples of condensed disazo pigments include CI Pigment Yellow 93 (total number of -NH- and -NH2 in one molecule=4, molecular weight=937, NH group amount=4.3 mmol / g) and CI Pigment Yellow 95 (total number of -NH- and -NH2 in one molecule=4, molecular weight=917, NH group amount=4.4 mmol / g). The pigment used in the present invention is preferably at least one selected from CI Pigment Yellow 180 and CI Pigment Yellow 185, from the viewpoint of obtaining a toner that suppresses the occurrence of fog.

[0064] <Amorphous polyester resin B (resin (B))> Resin (B) is a polyester resin which is a polycondensation product of an alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d), or a composite resin which contains a polyester portion which is a polycondensation product of an alcohol component (c) and a carboxylic acid component (d). Examples of the composite resin include a urethane-modified polycondensate of an alcohol component (c) and a carboxylic acid component (d), an epoxy-modified polycondensate of an alcohol component (c) and a carboxylic acid component (d), and a resin in which a polyester portion, which is a polycondensate of an alcohol component (c) and a carboxylic acid component (d), and a styrene-acrylic portion are composited. Among these, the resin (B) is preferably a resin in which a polyester moiety, which is a polycondensation product of an alcohol component (c) and a carboxylic acid component (d), and a styrene-acrylic moiety are composited.

[0065] The alcohol component (c) contains an aliphatic diol having 2 to 5 carbon atoms. Examples of the aliphatic diol having 2 to 5 carbon atoms include the same as those exemplified for the alcohol component (a), and from the viewpoint of obtaining a toner that suppresses the occurrence of fog, neopentyl glycol is preferred. In order to obtain a toner that suppresses the occurrence of fog, the content of the aliphatic diol having 2 to 5 carbon atoms in the alcohol component (c) is preferably 85 mol % or more, more preferably 90 mol % or more, even more preferably 95 mol % or more, and is preferably 100 mol % or less, more preferably 100 mol %.

[0066] Examples of the alcohol component (c) other than the aliphatic diol having 2 to 5 carbon atoms include an alkylene oxide adduct of an aromatic diol, an aliphatic diol having 6 or more carbon atoms, an alicyclic diol, and a polyhydric alcohol having a valence of 3 or more. Examples of these alcohol components include the same ones as those exemplified for the alcohol component (a).

[0067] Examples of the carboxylic acid component (d) include aromatic dicarboxylic acid compounds, aliphatic dicarboxylic acid compounds, and trivalent or higher carboxylic acid compounds. Examples of these carboxylic acid components (d) include the same compounds as those exemplified for the carboxylic acid component (b), and from the viewpoint of obtaining a toner that suppresses the occurrence of fog, the carboxylic acid component (d) is preferably an aromatic dicarboxylic acid compound, and more preferably at least one selected from terephthalic acid and isophthalic acid. The content of the aromatic dicarboxylic acid compound in the carboxylic acid component (d) is preferably 90 mol % or more, more preferably 95 mol % or more, and preferably 100 mol % or less, more preferably 100 mol %.

[0068] The equivalent ratio of the carboxyl groups of the carboxylic acid component (d) to the hydroxyl groups of the alcohol component (c) [COOH groups / OH groups] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.

[0069] When the resin (B) is a composite resin of a polyester moiety, which is a polycondensation product of an alcohol component (c) and a carboxylic acid component (d), and a styrene-acrylic moiety, the styrene-acrylic moiety is, for example, an addition polymerization product of raw material monomers including a styrene-based compound and a (meth)acrylic compound. The styrene acrylic moiety of resin (B) is the same as that of resin (A), and the compounds preferred as raw material monomers and the contents of the compounds in the raw material monomers are the same as those shown for resin (A).

[0070] Resin (B) may be produced by the same method as for resin (A), and the reaction conditions etc. are the same as those shown in the production method for resin (A).

[0071] <Method of manufacturing colorant particles> The colorant particles are obtained, for example, by mixing the colorant with the resin (B). There is no particular limitation on the method for producing the dispersion of colorant particles. 50 However, from the viewpoint of improving the adsorption of the resin (B) to the colorant, a method having a step of dissolving the resin (B) in an organic solvent, and then mixing the resin (B) with an aqueous medium to obtain a dispersion liquid, and dispersing the colorant and the dispersion liquid in the presence of the organic solvent to obtain a dispersion liquid of colorant particles.

[0072] After mixing the resin (B) with the organic solvent, the resin (B) may be neutralized. The neutralizing agent used is the same as the neutralizing agent shown in the method for producing resin particles, and sodium hydroxide is preferred. The degree of neutralization of resin (B) is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 75 mol % or more, and preferably 95 mol % or less, more preferably 90 mol % or less, even more preferably 85 mol % or less. The degree of neutralization of the resin (B) can be determined by the formula (1) in the same manner as the degree of neutralization of the resin contained in the resin particles.

[0073] The device used for mixing the resin (B), the organic solvent, and the aqueous medium may be, for example, a mixing / stirring device equipped with an anchor blade, a dispersing blade, or the like. The temperature during mixing is preferably 5°C or higher, more preferably 10°C or higher, even more preferably 15°C or higher, and is preferably 35°C or lower, more preferably 30°C or lower, even more preferably 25°C or lower. The mixing time is preferably 3 minutes or more, more preferably 5 minutes or more, even more preferably 8 minutes or more, and is preferably 30 minutes or less, more preferably 20 minutes or less, even more preferably 15 minutes or less.

[0074] Examples of devices used for dispersion include kneaders such as roll mills and kneaders, homogenizers such as Microfluidizer (manufactured by Microfluidics), and media-type dispersers such as paint shakers and bead mills. One or more of these devices may be used. Among these, media-type dispersers such as bead mills and homogenizers are preferred from the viewpoint of reducing the particle size of the colorant particles. When a homogenizer is used, the treatment pressure is preferably 60 MPa or more, more preferably 100 MPa or more, even more preferably 130 MPa or more, and preferably 270 MPa or less, more preferably 200 MPa or less, even more preferably 180 MPa or less. The number of passes is preferably 5 or more, more preferably 10 or more, and is preferably 30 or less, more preferably 25 or less.

[0075] The colorant particle dispersion is preferably filtered through a wire mesh or the like to remove coarse particles, etc. When titanium oxide is dispersed using a bead mill, the beads and the coarse particles may be removed simultaneously. Furthermore, various additives such as organic solvents, preservatives, and antifungal agents may be added to the dispersion of colorant particles.

[0076] In the colorant particles, the mass ratio of the colorant to the resin (B) (colorant / resin (B)) is 55 / 45 or more, preferably 60 / 40 or more, more preferably 65 / 35 or more, and is 99 / 1 or less, preferably 90 / 10 or less, more preferably 85 / 15 or less, from the viewpoint of obtaining a toner that suppresses the occurrence of fog.

[0077] From the viewpoint of image density of the printed matter, the content of the colorant in the colorant particle dispersion liquid is preferably 2% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and is preferably 45% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less. The solids concentration of the colorant particle dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less.

[0078] Volume median particle size D of colorant particles 50 From the viewpoint of improving the dispersibility of the colorant particles in the toner particles, the average particle diameter is preferably 0.05 μm or more, more preferably 0.1 μm or more, even more preferably 0.15 μm or more, and is preferably 0.4 μm or less, more preferably 0.3 μm or less, even more preferably 0.25 μm or less. From the viewpoint of improving the dispersibility of the colorant particles in the toner particles, the CV value of the colorant particles is preferably 10% or more, more preferably 20% or more, and is preferably 45% or less, more preferably 40% or less, and even more preferably 35% or less. Volume median particle size D of colorant particles 50 and CV values ​​are measured by the methods in the Examples.

[0079] From the viewpoint of image density of the printed matter, the content of the colorant in the toner particles is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 5% by mass, and is preferably 20% by mass or less, more preferably 17% by mass or less, even more preferably 15% by mass or less.

[0080] [Colorant particle dispersion] The colorant particle dispersion of the present invention includes colorant particles containing a colorant and an amorphous polyester resin (B) containing a polyester moiety that is a polycondensate of an alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d). The mass ratio of the colorant to the amorphous polyester resin (B) in the colorant particles (colorant / amorphous polyester resin (B)) is 55 / 45 or more and 99 / 1 or less. The colorant particle dispersion of the present invention contains colorant particles coated with resin (B), and therefore can prevent aggregation of the colorant and / or colorant particles, and has high storage stability. Therefore, by using the colorant particle dispersion of the present invention in the production of a toner for developing electrostatic images, a toner for developing electrostatic images that suppresses the occurrence of fogging can be obtained with high productivity.

[0081] The aqueous medium contained in the colorant particle dispersion liquid may be the same as the aqueous medium exemplified in the above-mentioned method for producing colorant particles.

[0082] In the colorant particles, the mass ratio of the colorant to the resin (B) (colorant / resin (B)) is 55 / 45 or more, preferably 60 / 40 or more, more preferably 65 / 35 or more, and is 99 / 1 or less, preferably 90 / 10 or less, more preferably 85 / 15 or less, from the viewpoint of obtaining a toner that suppresses the occurrence of fog.

[0083] Content of colorant in colorant particle dispersion, solids concentration of colorant particle dispersion, volume median particle diameter D of colorant particles 50 and the CV value of the colorant particles are in the same range as shown in the above-mentioned method for producing colorant particles.

[0084] [Step of aggregating resin particles and colorant particles] In the step of aggregating the resin particles and the colorant particles, the resin particles containing the amorphous resin and the crystalline resin in the same or different particles and the colorant particles are aggregated in an aqueous medium to obtain aggregated particles 1. Here, it is more preferable to mix a resin particle dispersion containing the resin particles with a colorant particle dispersion containing the colorant particles to aggregate these particles. It is more preferable that the resin particle dispersion and the colorant particle dispersion are an aqueous dispersion of resin particles and an aqueous dispersion of colorant particles, respectively. In the step of aggregating the resin particles and the colorant particles, it is preferable to further aggregate the release agent. The release agent is more preferably a release agent particle dispersion containing release agent particles containing a release agent, and the release agent particle dispersion is more preferably an aqueous dispersion of release agent particles.

[0085] <Release agent> Examples of the release agent include polypropylene wax, polyethylene wax, polypropylene-polyethylene copolymer wax, hydrocarbon waxes such as microcrystalline wax, paraffin wax, Fischer-Tropsch wax, and oxides thereof, ester waxes such as carnauba wax, montan wax, and deacidified waxes thereof, and fatty acid ester wax, fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts. These may be used alone or in combination of two or more.

[0086] The melting point of the release agent is preferably 60° C. or higher, more preferably 70° C. or higher, and preferably 160° C. or lower, more preferably 140° C. or lower, even more preferably 120° C. or lower, and even more preferably 100° C. or lower.

[0087] The content of the release agent in the toner particles is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 5% by mass or more, and preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 12% by mass or less.

[0088] (Release agent particle dispersion) The release agent particle dispersion can be obtained by using a surfactant, but is preferably obtained by mixing the release agent with the resin particles (S) described below. By preparing the release agent particles using the release agent and the resin particles (S), the release agent particles are stabilized by the resin particles (S), and it becomes possible to disperse the release agent in an aqueous medium without using a surfactant. It is considered that the release agent particle dispersion has a structure in which a large number of resin particles (S) are attached to the surface of the release agent particles. The resin constituting the resin particles (S) in which the release agent is dispersed is preferably a polyester resin, and it is more preferable to use a composite resin D having a polyester resin segment and an addition polymerization resin segment. For information on the release agent particle dispersion and composite resin D, see JP 2021-182045 A.

[0089] In the step of aggregating the resin particles and the colorant particles, the aggregation of the resin particles in the aqueous medium may be carried out in the presence of other additives. As the aqueous medium, the aqueous medium shown in the method for producing resin particles can be used, and the preferred ranges are also the same. Examples of other additives include charge control agents, magnetic powders, flow improvers, conductivity adjusters, reinforcing fillers such as fibrous substances, antioxidants, antiaging agents, and cleaning improvers.

[0090] [Surfactant] In the step of aggregating the resin particles and the colorant particles, when the dispersions of the respective particles are mixed to prepare a mixed dispersion, the process may be performed in the presence of a surfactant from the viewpoint of improving the dispersion stability of the resin particles, the release agent particles, the colorant particles, etc. Examples of the surfactant include anionic surfactants such as alkylbenzene sulfonates and alkyl ether sulfates; and nonionic surfactants such as polyoxyethylene alkyl ethers and polyoxyethylene alkenyl ethers.

[0091] When a surfactant is used, the total amount used is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, per 100 parts by mass of the total amount of resin particles.

[0092] <Flocculant> In the step of aggregating the resin particles and the colorant particles, it is preferable to add an aggregating agent in order to efficiently carry out the aggregation. Examples of the flocculant include cationic surfactants such as quaternary salts, organic flocculants such as polyethyleneimine, and inorganic flocculants. Examples of the inorganic flocculant include inorganic metal salts such as sodium sulfate, sodium nitrate, sodium chloride, calcium chloride, and calcium nitrate; inorganic ammonium salts such as ammonium sulfate, ammonium chloride, and ammonium nitrate; and divalent or higher metal complexes. From the viewpoint of improving the coagulation properties and obtaining uniformly coagulated particles 1, inorganic coagulants having a valence of 1 to 5 are preferred, inorganic metal salts having a valence of 1 to 2 and inorganic ammonium salts are more preferred, inorganic ammonium salts are even more preferred, and ammonium sulfate is even more preferred.

[0093] For example, 5 to 50 parts by mass of the aggregating agent is added to a mixed dispersion liquid containing resin particles, colorant particles, and, if necessary, release agent particles at 0° C. or higher and 40° C. or lower, relative to 100 parts by mass of the resin in the resin particles, and the resin particles, colorant particles, and release agent particles are aggregated in an aqueous medium to obtain aggregated particles 1. Furthermore, from the viewpoint of promoting aggregation, it is preferable to increase the temperature of the dispersion liquid after adding the aggregating agent.

[0094] Examples of a method for stopping the aggregation include a method for cooling the dispersion, a method for adding an aggregation terminator, a method for diluting the dispersion, etc. From the viewpoint of reliably preventing unnecessary aggregation, a method for stopping the aggregation by adding an aggregation terminator is preferred.

[0095] <Aggregation stopper> The aggregation terminator is preferably a surfactant, more preferably an anionic surfactant. Examples of the anionic surfactant include alkylbenzenesulfonate, alkyl sulfate, alkyl ether sulfate, polyoxyalkylene alkyl ether sulfate, etc. These may be used alone or in combination. The aggregation terminator may be added in the form of an aqueous solution. The amount of the aggregation terminator added is preferably 1 part by mass or more, more preferably 3 parts by mass or more, per 100 parts by mass of the resin in the resin particles, from the viewpoint of reliably preventing unnecessary aggregation, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, from the viewpoint of reducing residue in the toner.

[0096] Volume median particle size D of aggregate 1 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.

[0097] In the present invention, after the step of aggregating the resin particles and the colorant particles and before the step of fusing, a step of aggregating the shell resin particles may be included in which shell resin particles containing an amorphous resin (preferably an amorphous polyester resin) are attached to the obtained aggregated particles 1 to obtain aggregated particles 2. By including the step of aggregating the shell resin particles, toner particles having a core-shell structure can be obtained. Here, the amorphous resin used in the shell resin particles is preferably an amorphous polyester resin, and may be the above-mentioned amorphous polyester resin (A). The shell resin particles are obtained by the same method as the above-mentioned method for producing the resin particles. Furthermore, when the toner manufacturing method includes a step of aggregating shell resin particles, it is preferable to stop the aggregation in the step when the aggregated particles 2 have grown to an appropriate particle size for toner particles, and a method of stopping the aggregation by adding the above-mentioned aggregation terminator is preferable.

[0098] [Fusion process] In the fusion step, for example, the aggregated particles are fused in an aqueous medium. By fusion, the particles contained in the aggregated particles are fused together to obtain fused particles. In the fusing step, from the viewpoint of improving the fusing property of the aggregated particles and from the viewpoint of obtaining a toner that suppresses the occurrence of fog, the aggregated particles are maintained at a temperature equal to or higher than the glass transition temperature of the resin having the highest glass transition temperature among the resins contained in the aggregated particles. From the viewpoint of improving the fusibility of the aggregated particles and improving the productivity of the toner, the holding temperature when fusing the aggregated particles is preferably at least 5° C. higher than the glass transition temperature of the resin having the highest glass transition temperature among the resins contained in the aggregated particles, more preferably at least 10° C. higher, and even more preferably at least 15° C. higher, and is preferably not more than 40° C. higher, more preferably not more than 30° C. higher, and even more preferably not more than 25° C. higher than the glass transition temperature of the resin. In this case, the time for which the toner is maintained at a temperature equal to or higher than the glass transition temperature of the resin is, from the viewpoint of obtaining a toner that suppresses the occurrence of fog, preferably 1 minute or more, more preferably 10 minutes or more, even more preferably 30 minutes or more, and is preferably 240 minutes or less, more preferably 120 minutes or less, even more preferably 90 minutes or less. It is preferable to maintain the temperature at the above temperature until the desired circularity is achieved.

[0099] The volume median particle size D of the fused particles obtained by fusion 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.

[0100] The circularity of the fused particles obtained by fusion is preferably 0.955 or more, more preferably 0.960 or more, and is preferably 0.990 or less, more preferably 0.985 or less, and further preferably 0.980 or less. The fusion is preferably terminated after the above-mentioned preferred circularity is reached. The circularity is measured by the method described in the Examples.

[0101] [Post-processing process] A post-treatment process may be performed after the fusion process, and the fused particles are isolated to obtain toner particles. Since the fused particles obtained in the fusion process are present in an aqueous medium, it is preferable to first perform solid-liquid separation. For solid-liquid separation, a suction filtration method or the like is preferably used. It is preferable to wash the solid-liquid separation product. In this case, it is preferable to remove the added surfactant, so that washing with an aqueous medium at a temperature below the cloud point of the surfactant is preferable. It is preferable to wash the product several times. Next, drying is preferably performed. Examples of the drying method include vacuum low-temperature drying, vibration-type fluidized bed drying, spray drying, freeze drying, and flash jet drying.

[0102] [Toner Particles] Volume median particle size of toner particles D 50 is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 7 μm or less.

[0103] The circularity of the toner particles is preferably 0.955 or more, more preferably 0.960 or more, from the viewpoint of obtaining high quality images, and is preferably 0.990 or less, more preferably 0.985 or less, and even more preferably 0.980 or less, from the viewpoint of cleaning properties.

[0104] From the viewpoint of improving the productivity of the toner, the CV value of the toner particles is preferably 10% or more, more preferably 15% or more, and even more preferably 18% or more, and from the viewpoint of obtaining high-quality images, it is preferably 40% or less, more preferably 35% or less, and even more preferably 30% or less. Volume median particle size of toner particles D 50 The CV value can be measured by the method described in the Examples.

[0105] [Toner for developing electrostatic images] The toner for developing electrostatic images of the present invention contains toner particles. The toner particles can be used as they are, but it is preferable to use the toner after adding a fluidizing agent or the like as an external additive to the surface of the toner particles.

[0106] <External additives> In order to improve the fluidity, the toner of the present invention may contain toner particles and an external additive by treating the surface of the toner particles with a property improving agent such as an external additive. Examples of the external additive include inorganic material particles such as silica, alumina, titania, zirconia, tin oxide, and zinc oxide, and organic particles such as resin particles such as melamine resin particles and polytetrafluoroethylene resin particles. These may be used alone or in combination. Among these external additives, silica is preferred, and hydrophobic silica treated with a hydrophobic treatment agent is more preferred.

[0107] Examples of hydrophobic treatment agents include hexamethyldisilazane (HMDS), dimethyldichlorosilane (DMDS), silicone oil, octyltriethoxysilane (OTES), methyltriethoxysilane, and dimethylpolysiloxane. Among these, hexamethyldisilazane is preferred.

[0108] When the toner particles are surface-treated using an external additive, the content of the external additive is, from the viewpoint of the chargeability and fluidity of the toner, preferably 0.1 part by mass or more, more preferably 0.5 part by mass or more, even more preferably 1 part by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, and even more preferably 4 parts by mass or less, relative to 100 parts by mass of the toner particles. Toners are used for developing electrostatic images in electrophotographic printing. The toners can be used, for example, as one-component developers or mixed with a carrier to form two-component developers. EXAMPLES

[0109] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Each property value was measured and evaluated by the following methods. In the notation such as "alkylene oxide (X)", the number X in parentheses means the average number of moles of alkylene oxide added.

[0110] [Measurement method] The properties of the polyester resin, the resin particles, the toner, etc. were measured and evaluated by the following methods.

[0111] [Softening point, crystallinity index, melting point, and glass transition temperature of resin] (1) Softening point Using a flow tester "CFT-500D" (Shimadzu Corporation), 1 g of sample was heated at a temperature increase rate of 6°C / min, while applying a load of 1.96 MPa with the plunger, and extruding the sample from a nozzle with a diameter of 1 mm and a length of 1 mm. The plunger descent amount of the flow tester was plotted against the temperature, and the temperature at which half of the sample flowed out was taken as the softening point. (2) Crystallinity index Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of sample was weighed into an aluminum pan and cooled to 0°C at a rate of 10°C / min. The sample was then left to stand for 1 minute, and then heated to 180°C at a rate of 10°C / min to measure the amount of heat. The temperature of the peak with the largest peak area among the observed endothermic peaks was taken as the endothermic maximum peak temperature (1), and the crystallinity index was calculated by (softening point (°C)) / (endothermic maximum peak temperature (1) (°C)). (3) Melting point and glass transition temperature Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and cooled from that temperature to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, and the amount of heat was measured. Among the endothermic peaks observed, the temperature of the peak with the largest peak area was taken as the maximum endothermic peak temperature (2). In the case of a crystalline resin, this peak temperature was taken as the melting point. In the case of an amorphous resin, when a peak was observed, the temperature of the peak was taken as the glass transition temperature. When no peak was observed but a step was observed, the temperature at the intersection of the tangent showing the maximum slope of the curve at the step and an extension of the baseline on the low temperature side of the step was taken as the glass transition temperature.

[0112] [Acid value of resin] Measurement was performed according to the neutralization titration method described in JIS K 0070:1992, except that the measurement solvent was chloroform.

[0113] [Melting point of release agent] Using a differential scanning calorimeter "Q100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and then cooled from 200°C to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, the amount of heat was measured, and the maximum endothermic peak temperature was taken as the melting point.

[0114] [Volume median particle diameter D of resin particles, colorant particles, and release agent particles 50 and CV value] (1) Measuring device: Laser diffraction type particle size measuring device "LA-920" (manufactured by Horiba Ltd.) (2) Measurement conditions: Put the sample dispersion in a measurement cell, add distilled water, and measure the volume median particle size D at a concentration where the absorbance is in the appropriate range. 50 and the volume average particle diameter Dv were measured. The CV value (coefficient of variation (particle size distribution)) was calculated according to the following formula. CV value (%) = (Standard deviation of particle size distribution / Volume average particle size Dv) x 100

[0115] [Solid Content Concentration of Resin Particle Dispersion, Colorant Particle Dispersion, and Release Agent Particle Dispersion] Using an infrared moisture meter "FD-230" (Kett Electric Laboratory Co., Ltd.), the moisture content (mass%) of 5 g of the measurement sample was measured at a drying temperature of 150°C and measurement mode 96 (monitoring time 2.5 minutes, moisture content fluctuation range 0.05%). The solid content concentration was calculated according to the following formula. Solid concentration (mass%) = 100-moisture (mass%)

[0116] [Volume median particle diameter of agglomerated particles D 50 〕 Volume median particle size of agglomerated particles D 50 was measured as follows: Measuring instrument: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50μm Analysis software: "Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured again, and the volume median particle size D is calculated from the particle size distribution. 50 asked for.

[0117] [Circularity of fused particles] The circularity of the fused particles was measured under the following conditions. Measurement equipment: Flow-type particle image analyzer "FPIA-3000" (Sysmex Corporation) Preparation of dispersion: A dispersion of fused particles was prepared by diluting with deionized water to a solids concentration of 0.001 to 0.05% by mass. Measurement mode: HPF measurement mode

[0118] [Volume median particle size of toner particles D 50 and CV value] Volume median particle size of toner particles D 50 was measured as follows: The measurement device, aperture diameter, analysis software, and electrolyte were determined based on the volume median particle diameter D 50 The same one used in the measurement was used. Dispersion: Polyoxyethylene lauryl ether "EMULGEN (registered trademark) 109P" (manufactured by Kao Corporation, HLB (hydrophile-lipophile balance) = 13.6) was dissolved in the electrolyte to obtain a dispersion with a concentration of 5 mass %. Dispersion conditions: 10 mg of a measurement sample of dried toner particles was added to 5 mL of the dispersion liquid, and dispersed for 1 minute using an ultrasonic disperser. Thereafter, 25 mL of the electrolyte was added, and the mixture was further dispersed for 1 minute using an ultrasonic disperser to prepare a sample dispersion liquid. Measurement conditions: The sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle size of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured again, and the volume median particle size D is calculated from the particle size distribution. 50 and volume average particle size D V asked for. The CV value (%) was calculated according to the following formula. CV value (%) = (Standard deviation of particle size distribution / Volume average particle size D V ) x 100

[0119] [Resin manufacturing] [Production of amorphous polyester resin (A)] Production Example A1 (Production of Resin A-1) The raw material monomers and esterification catalyst of polyester resin other than fumaric acid shown in Table 1 were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C was passed, a stirrer, and a thermocouple. Under a nitrogen atmosphere, the reaction system was held at 180 ° C for 1 hour, then heated from 180 ° C to 230 ° C at 10 ° C / h, and then held at 230 ° C for 5 hours to perform polycondensation. After that, after cooling to 180 ° C, 5 g of fumaric acid and a radical polymerization inhibitor (4-tert-butylcatechol) were added to the reaction system, heated from 180 ° C to 210 ° C at 10 ° C / h, reacted at 210 ° C for 1 hour, and reacted at 210 ° C and 10 kPa until the softening point shown in Table 1 was obtained. The physical properties are shown in Table 1.

[0120] Production Example A2 (Production of Resin A-2) The raw material monomers and esterification catalyst of polyester resin other than isophthalic acid shown in Table 1 were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C was passed, a stirrer, and a thermocouple. Under a nitrogen atmosphere, the reaction system was held at 180 ° C for 1 hour, then heated from 180 ° C to 230 ° C at 10 ° C / h, and then held at 230 ° C for 5 hours to perform polycondensation. After that, it was cooled to 180 ° C, and isophthalic acid was added to the reaction system, heated from 180 ° C to 230 ° C at 10 ° C / h, reacted at 230 ° C for 1 hour, and reacted at 230 ° C to the softening point shown in Table 1 at 230 ° C and 10 kPa to obtain resin A-2. The physical properties are shown in Table 1.

[0121] Comparative Production Example A1 (Production of Resin A-81) The raw material monomers and esterification catalyst of polyester resin other than fumaric acid shown in Table 1 were placed in a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple. The temperature was raised to 235°C under a nitrogen atmosphere, and then held at 235°C for 5 hours to perform polycondensation. After that, after cooling to 180°C, 5g of fumaric acid and a radical polymerization inhibitor (4-tert-butylcatechol) were added to the reaction system, the temperature was raised from 180°C to 210°C at 10°C / h, and the reaction was carried out at 210°C for 1 hour, and the reaction was carried out at 210°C and 10kPa until the softening point shown in Table 1 was reached, and resin A-81 was obtained. The physical properties are shown in Table 1.

[0122] [Table 1]

[0123] [Production of crystalline polyester resin (C)] Manufacturing Example C1 (Manufacturing of Resin C-1) The inside of a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was replaced with nitrogen, and the raw material monomers of the polyester resin shown in Table 2 were added. The reaction system was heated to 135°C while stirring, and then held at 135°C for 3 hours, and then heated from 135°C to 200°C over 10 hours. Then, 10g of tin(II) di(2-ethylhexanoate) was added to the reaction system, and the reaction system was further held at 200°C for 1 hour, after which the pressure in the flask was reduced and the system was held under a reduced pressure of 8kPa for 1 hour to obtain Resin C-1, a crystalline polyester resin. The physical properties are shown in Table 2.

[0124] [Table 2]

[0125] [Production of amorphous polyester resin B] Production Example 1 (Production of Styrene Acrylic Part 1) The raw material monomers of the styrene acrylic moiety containing acrylic acid as a bireactive compound shown in Table 3 were heated to 300°C in an autoclave equipped with a stainless steel stirring rod, and the raw material monomers were polymerized under pressurized and heated conditions for 2 hours. The pressure and temperature were returned to normal, and the precipitated styrene acrylic resin was collected to obtain the styrene acrylic moiety 1. The physical properties are shown in Table 3.

[0126] Production Example 2 (Production of Styrene Acrylic Part 2) Styrene acrylic moiety 2 was obtained in the same manner as in the production of styrene acrylic moiety 1, except that the amounts of raw material monomers added were changed as shown in Table 3. The physical properties are shown in Table 3.

[0127] [Table 3]

[0128] Manufacturing Example B1 (Manufacturing of Resin B-1) The raw material monomers, esterification catalyst, and esterification promoter of the polyester moiety shown in Table 4 were placed in a 10L four-neck flask equipped with a thermometer, a stainless steel stirring rod, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C. was passed, and a nitrogen inlet tube. The mixture was held at 180 ° C. for 1 hour in a mantle heater in a nitrogen atmosphere, and then heated from 180 ° C. to 230 ° C. at 10 ° C. / h, and then subjected to a polycondensation reaction at 230 ° C. for 5 hours, and then reacted at 230 ° C. and 8 kPa for 1 hour. After cooling to 210 ° C., styrene acrylic moiety 1 was added and held at 210 ° C. for 4 hours. The pressure was reduced to 8 kPa, and it was confirmed that the softening point of the resin reached the specified softening point shown in Table 4, and the reaction was stopped to obtain resin B-1. The physical properties are shown in Table 4.

[0129] Manufacturing Example B2 (Manufacturing of Resin B-2) Resin B-2 was obtained in the same manner as in Production Example B1, except that the styrene acrylic moiety 1 was changed to the styrene acrylic moiety 2. The physical properties are shown in Table 4.

[0130] Production Example B3 (Production of Amorphous Resin B-3) As shown in Table 4, without using a styrene acrylic portion, the raw material monomer of the polyester portion, the esterification catalyst, and the esterification promoter were placed in a 10L four-neck flask equipped with a thermometer, a stainless steel stirring rod, a dehydration tube equipped with a fractionating tube through which hot water of 98 ° C was passed, and a nitrogen inlet tube, and after holding at 180 ° C for 1 hour in a mantle heater in a nitrogen atmosphere, the temperature was increased from 180 ° C to 220 ° C at 10 ° C / h, and then polycondensation reaction was carried out at 220 ° C for 5 hours, and further reaction was carried out at 220 ° C and 8 kPa until the softening point shown in Table 4 was reached, and resin B-3 was obtained. The physical properties are shown in Table 4.

[0131] [Table 4]

[0132] [Production of Resin Particle Dispersion] Production Example X1 (Production of Resin Particle Dispersion X-1) In a 3 L vessel equipped with a stirrer, reflux condenser, dropping funnel, thermometer, and nitrogen inlet tube, 160 g of resin A-1, 40 g of resin C-1, and 200 g of methyl ethyl ketone were placed and dissolved for 2 hours at 73° C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution so that the degree of neutralization with respect to the acid value of the resin was 60 mol%, and the mixture was stirred for 30 minutes. Next, while maintaining the temperature at 73°C, 700 g of deionized water was added over 50 minutes while stirring at 200 r / min to cause phase inversion emulsification. While maintaining the temperature of the obtained solution at 73°C, methyl ethyl ketone was distilled off under reduced pressure to obtain a dispersion. Thereafter, while continuing to stir, the dispersion was cooled to 30°C, and deionized water was added so that the solid content concentration was 20 mass%, thereby obtaining a resin particle dispersion X-1. The volume median particle diameter D of the resin particles in the obtained resin particle dispersion X-1 was 50 and CV values ​​are shown in Table 5.

[0133] Production Example X2 and Comparative Production Example X1 (Production of Resin Particle Dispersions X-2 and X-81) Resin particle dispersions X-2 and X-81 were obtained in the same manner as in Production Example X1, except that the resin was changed as shown in Table 5. The volume median particle diameter D of the resin particles in the obtained resin particle dispersions was 50 and CV values ​​are shown in Table 5.

[0134] [Table 5]

[0135] [Preparation of Colorant Particle Dispersion] Production Example F1 (Production of Colorant Particle Dispersion F-1) 75 g of resin B-1 and 326 g of methyl ethyl ketone were placed in a 5 L container equipped with a stirrer equipped with a dispersing blade, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen inlet tube, and the resin was dissolved at 20 ° C. 15 g of 5 mass % aqueous sodium hydroxide solution (an amount that results in a neutralization degree of 80 mol % relative to the acid value of resin B-1) was added to the obtained solution, and 1071 g of deionized water was further added, and the mixture was stirred with a dispersing blade at 20 ° C. for 10 minutes. Next, 300 g of yellow pigment "Paliotol Yellow D1155" (CI Pigment Yellow 185 manufactured by BASF) was added, and the mixture was stirred with a dispersing blade at 6400 r / min at 20 ° C. for 2 hours. After that, the mixture was passed through a 200 mesh filter and treated with a homogenizer "Microfluidizer M-110EH" (manufactured by Microfluidics) at a pressure of 150 MPa for 15 passes. While stirring the obtained dispersion, methyl ethyl ketone and a part of the water were distilled off under reduced pressure at 70°C. After cooling, the mixture was passed through a 200 mesh filter, and deionized water was added to the mixture so that the solid content concentration was 20% by mass, to obtain colorant particle dispersion F-1. The volume median particle diameter D of the colorant particles in the obtained colorant particle dispersion F-1 was 50 The viscosity and CV values, as well as the storage stability of colorant particle dispersion F-1 are shown in Table 6. The storage stability of the colorant particle dispersion was evaluated as follows. Volume median particle diameter D of colorant particles in the colorant particle dispersion before storage 50 The colorant particle dispersion was then stored at 45° C. for one month, and the volume median particle diameter D 50 The storage stability was evaluated by the volume median particle diameter D of the colorant particles before storage. 50 Volume median particle size D of colorant particles after storage 50 It is expressed as (particle size after storage / particle size before storage). The closer the value of (particle size after storage / particle size before storage) is to 1, the more excellent the storage stability is.

[0136] Production Examples F2 to F8 and Comparative Production Example F2 (Production of Colorant Particle Dispersions F-2 to F-8 and F-82) Colorant particle dispersions F-2 to F-8 and F-82 were obtained in the same manner as in Production Example F1, except that the types and amounts of colorants and resins used were changed as shown in Table 1. The volume median particle diameter D 50 The CV value and storage stability of the colorant particle dispersion are shown in Table 6.

[0137] Comparative Production Example F1 (Production of Colorant Dispersion F-81) In a 2L container, 150g of yellow pigment "Paliotol Yellow D1155" (CI Pigment Yellow 185, manufactured by BASF), 37.5g of nonionic surfactant "Emulgen B-66" (nonionic surfactant, manufactured by Kao Corporation), and 750g of deionized water were added, and the mixture was stirred at 6400 rpm / min at 20°C for 1 hour using a stirrer "Labo-lution" (manufactured by Primix Corporation) equipped with a dispersing blade. The mixture was then passed through a 200-mesh filter, and treated 15 times at a pressure of 150 MPa using a homogenizer "Microfluidizer M-110EH" (manufactured by Microfluidics). The mixture was then passed through a 200-mesh filter, and deionized water was added so that the solid content concentration was 20% by mass, thereby obtaining a colorant particle dispersion F-81. The volume median particle diameter D of the resin particles in the obtained colorant particle dispersion F-81 was 50 and CV values ​​are shown in Table 6.

[0138] [Table 6] *1: PY-185 refers to the yellow pigment "Paliotol Yellow D1155" (BASF, CI Pigment Yellow 185), which contains 11.9 mmol / g of NH structure in its structure. PY-180 refers to a yellow pigment "Novoperm Yellow HG01" (Clariant Chemicals Co., Ltd., CI Pigment Yellow 180) containing 8.2 mmol / g of NH structures in its structure. PY-155 refers to a yellow pigment "Toner Yellow 3GP-CT" (Clariant Chemicals Co., Ltd., CI Pigment Yellow 155) containing 2.8 mmol / g of NH structure in its structure. Regal-330 refers to carbon black "Regal-330R" (manufactured by Cabot Corporation). *2: B-66 refers to the nonionic surfactant "Polyoxyethylene (15) tribenzyl phenyl ether" (Kao Corporation, Emulgen B-66). *3: Colorant / resin (B) indicates the mass ratio of the colorant to the resin (B), except for the case of Comparative Production Example F1, where it indicates the mass ratio of the colorant to the surfactant. *4: Indicates the particle size of colorant particles after storage at 45°C for one month compared to the particle size of colorant particles before storage (particle size after storage / particle size before storage).

[0139] As shown in Table 6, colorant particle dispersions F1 to F8, in which colorant particles were dispersed using amorphous polyester resin (B) containing a polyester moiety, which is a polycondensation product of alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and carboxylic acid component (d), suppressed aggregation of colorant particles during storage and had excellent storage stability. On the other hand, colorant particle dispersion F81, in which colorant particles are dispersed using a nonionic surfactant, and colorant particle dispersion F82, in which colorant particles are dispersed using an amorphous polyester resin whose alcohol component is an alkylene oxide adduct of bisphenol A, showed more advanced aggregation of colorant particles during storage than colorant particle dispersions F1 to F8.

[0140] [Production of Composite Resin D] Manufacturing Example D1 (Manufacturing of Resin D-1) The inside of a 10L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was replaced with nitrogen, and 4,313g of a propylene oxide (2.2) adduct of bisphenol A, 818g of terephthalic acid, 727g of succinic acid, 30g of tin (II) di(2-ethylhexanoate), and 3.0g of gallic acid were placed in the flask, and the temperature was raised to 235°C while stirring the reaction system under a nitrogen atmosphere. After maintaining the temperature at 235°C for 5 hours, the pressure in the flask was reduced and maintained at 8kPa for 1 hour. After that, the pressure was returned to atmospheric pressure, and the flask was cooled to 160°C. While maintaining the temperature at 160°C, a mixture of 2,756g of styrene, 689g of stearyl methacrylate, 142g of acrylic acid, and 413g of dibutyl peroxide was added dropwise over 1 hour. After that, the temperature was kept at 160° C. for 30 minutes, and then the temperature was raised to 200° C., and the pressure in the flask was further reduced, and the reaction was continued at 8 kPa until the desired softening point was reached, to obtain Resin D-1. The physical properties are shown in Table 7.

[0141] [Table 7]

[0142] Production Example S1 (Production of Resin Particle Dispersion S-1) 200 g of Resin D-1 and 200 g of methyl ethyl ketone were placed in a 3 L vessel equipped with a stirrer, a reflux condenser, a dropping funnel, a thermometer, and a nitrogen inlet tube, and the resin was dissolved for 2 hours at 73° C. A 5% by mass aqueous solution of sodium hydroxide was added to the resulting solution so that the degree of neutralization was 60 mol% relative to the acid value of Resin D-1, and the mixture was stirred for 30 minutes. Next, while maintaining the temperature at 73°C, 700 g of deionized water was added over 50 minutes while stirring at 280 r / min to cause phase inversion emulsification. While maintaining the temperature at 73°C, the methyl ethyl ketone was distilled off under reduced pressure to obtain an aqueous dispersion. Thereafter, while stirring at 280 r / min, the aqueous dispersion was cooled to 30°C, and deionized water was added so that the solid content concentration was 20 mass%, to obtain a resin particle dispersion S-1. The volume median particle diameter D of the resin particles in the obtained resin particle dispersion S-1 was 50 The particle size was 0.09 μm and the CV value was 23%.

[0143] [Preparation of Release Agent Particle Dispersion] Production Example W1 (Production of Release Agent Particle Dispersion W-1) Into a 1 L beaker were added 120 g of deionized water, 86 g of resin particle dispersion S-1, and 40 g of paraffin wax "HNP-9" (manufactured by Nippon Seiro Co., Ltd., melting point 75°C), and the mixture was melted and stirred while maintaining the temperature at 90-95°C to obtain a molten mixture. The obtained molten mixture was dispersed for 20 minutes using an ultrasonic homogenizer "US-600T" (manufactured by Nippon Seiki Seisakusho Co., Ltd.) while maintaining the temperature at 90 to 95°C, and then cooled to room temperature (20°C). Deionized water was added to the obtained dispersion to adjust the solid content to 20 mass%, thereby obtaining release agent particle dispersion W-1. The volume median particle size of the release agent particles in the obtained release agent particle dispersion W-1 was 0.47 μm, and the CV value was 27%.

[0144] [Toner manufacturing] Example 1 (Production of Toner 1) In a 3 L four-neck flask equipped with a dehydration tube, a stirrer, and a thermocouple, 500 g of resin particle dispersion X-1, 80 g of release agent particle dispersion W-1, 81 g of colorant particle dispersion F-1, and 3.3 g of 15 mass % sodium dodecylbenzenesulfonate aqueous solution "Neopelex G-15" (Kao Corporation, anionic surfactant) were placed and mixed at a temperature of 25° C. Next, while stirring the mixture, a solution obtained by dissolving 43 g of ammonium sulfate in 980 g of deionized water and adding a 4.8 mass % potassium hydroxide aqueous solution to adjust the pH to 8.2 was added dropwise over 10 minutes at 25° C., and the temperature was then raised to 58° C. over 2 hours, and the volume median particle diameter D of the aggregated particles was measured. 50 The temperature was maintained at 58° C. until the particle size reached 6.2 μm, thereby obtaining a dispersion of aggregated particles 1. To the obtained dispersion liquid of aggregated particles 1, 22 g of sodium polyoxyethylene lauryl ether sulfate "EMAL E-27C" (manufactured by Kao Corporation, anionic surfactant, effective concentration 27% by mass) and 1100 g of deionized water were added. Thereafter, the temperature was raised to 78°C over one hour, and the temperature was maintained at 78°C until the circularity reached 0.970, thereby obtaining a dispersion liquid of fused particles in which aggregated particles 1 were fused. The obtained dispersion of fused particles was cooled to 30° C., and the dispersion was suction filtered to separate the solid content, which was then washed with deionized water at 25° C. and suction filtered at 25° C. for 2 hours. The solid content was then vacuum dried at 33° C. for 24 hours using a vacuum constant temperature dryer "DRV622DA" (manufactured by ADVANTEC Corporation) to obtain toner particles. The physical properties of the toner particles are shown in Table 8. 100 parts by mass of toner particles, 2.5 parts by mass of hydrophobic silica "RY50" (manufactured by Nippon Aerosil Co., Ltd., number average particle size: 0.04 μm), and 1.0 part by mass of hydrophobic silica "Cabosil (registered trademark) TS720" (manufactured by Cabot Japan Co., Ltd., number average particle size: 0.012 μm) were placed in a Henschel mixer, stirred, and passed through a 150 mesh sieve to obtain Toner 1. The evaluation results of Toner 1 are shown in Table 8.

[0145] [Toner Evaluation] [Fog on printed matter] The toner was loaded into a commercially available printer "Microline (registered trademark) 5400" (manufactured by Oki Electric Industry Co., Ltd.), and blank printing was performed on high-quality paper "Excellent White Paper A4 Size" (manufactured by Oki Electric Industry Co., Ltd.) in an environment with a temperature of 23°C and humidity of 50% (NN environment), during which the printer was stopped midway through blank printing. The developing unit was removed from the printer, and "Scotch (registered trademark) Mending Tape 810" (manufactured by 3M Japan Ltd., width: 18 mm) was attached onto the photoconductor, and the toner on the photoconductor was peeled off with the tape. The tape peeled off from the photoreceptor and unused tape were attached to high-quality paper "Excellent White Paper A4 Size" (manufactured by Oki Electric Industry Co., Ltd.), and the tape peeled off from the photoreceptor and unused tape were each measured using a colorimeter "SpectroEye" (manufactured by GretagMacbeth, light irradiation conditions: standard light source D50, observation field of view 2°, density standard DINNB, absolute white standard). The color difference (ΔE) between the tape peeled off from the photoreceptor and unused tape was taken as fog. The smaller the fog value, the better the image without fog that can be obtained.

[0146] Examples 2 to 9 and Comparative Examples 1 to 3 (Production of Toners 2 to 9 and Toners 81 to 83) Toners 2 to 9 and toners 81 to 83 were produced in the same manner as in Example 1, except that the types of resin particle dispersion liquid and colorant particle dispersion liquid used were changed as shown in Table 8. The physical properties of the obtained toner particles and the evaluation results of the toners are shown in Table 8.

[0147] [Table 8]

[0148] As shown in Table 8, toners 1 to 9 suppressing the occurrence of fogging were obtained by the manufacturing method of the present invention, which includes a process of aggregating and fusing resin particles containing an amorphous polyester resin (A) containing a polyester moiety that is a polycondensate of an alcohol component (a) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (b), and a process of fusing colorant particles containing an amorphous polyester resin (B) containing a polyester moiety that is a polycondensate of an alcohol component (c) containing an aliphatic diol having 2 to 5 carbon atoms and a carboxylic acid component (d) in an aqueous medium. In addition, toner 1 of Example 1, in which the amorphous polyester resin (B) is a resin complexed with a styrene acrylic moiety, suppressed the occurrence of fogging more than toner 8 of Example 8, which was the same condition as Example 1 except that the amorphous polyester resin (B) was an amorphous polyester resin. This is thought to be because the resin (B) has a styrene acrylic moiety, which enhances the coverage of the colorant by the resin (B) and improves the dispersibility of the colorant in the toner particles, improving the charge distribution of the toner and suppressing the occurrence of fogging more. On the other hand, in the toner 81 of Comparative Example 1, the colorant particles in which the colorant was dispersed by a nonionic surfactant were used, so the colorant was exposed on the surface of the toner particles, and it is considered that the fogging was not sufficiently suppressed. In addition, in the toner 82 of Comparative Example 2, the colorant particles in which the colorant was dispersed by an amorphous polyester resin in which the alcohol component was an alkylene oxide adduct of bisphenol A were used, so the affinity between the resin particles and the colorant particles was low, so the colorant particles were not taken into the toner particles, and it is considered that the occurrence of fogging could not be suppressed. Furthermore, in the toner 83 of Comparative Example 3, the resin particles containing an amorphous polyester resin in which the alcohol component was an alkylene oxide adduct of bisphenol A were used, so the affinity between the resin particles and the colorant particles containing resin (B) was low, so the colorant particles were not taken into the toner particles, and it is considered that the occurrence of fogging could not be suppressed.

Claims

1. A method for producing a toner for developing an electrostatic image, comprising the steps of aggregating and fusing resin particles and colorant particles in an aqueous medium, the resin particles contain an amorphous polyester-based resin (A) including a polyester moiety which is a polycondensate of an alcohol component (a) including an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (b); the colorant particles contain a colorant, and an amorphous polyester-based resin (B) containing a polyester moiety which is a polycondensate of an alcohol component (c) containing an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d); A method for producing a toner for developing electrostatic images, wherein a mass ratio of a colorant to an amorphous polyester resin (B) (colorant / amorphous polyester resin (B)) is 55 / 45 or more and 99 / 1 or less.

2. 2. The method for producing a toner for developing an electrostatic image according to claim 1, wherein the amorphous polyester resin (B) is a resin further comprising a styrene-acrylic moiety compounded therewith.

3. 3. The method for producing a toner for developing an electrostatic image according to claim 2, wherein the composite styrene-acrylic moiety is synthesized without using a polymerization initiator.

4. 4. The method for producing a toner for developing electrostatic images according to claim 1, wherein the colorant is a yellow pigment containing 4 mmol / g or more and 15 mmol / g or less of an NH structure in the structure.

5. 5. The method for producing a toner for developing electrostatic images according to claim 1, wherein the colorant particles are obtained by dispersing the colorant and the amorphous polyester resin (B) in the presence of an organic solvent.

6. 1. A colorant particle dispersion comprising colorant particles containing a colorant and an amorphous polyester resin (B) including a polyester moiety that is a polycondensate of an alcohol component (c) including an aliphatic diol having from 2 to 5 carbon atoms and a carboxylic acid component (d), wherein the mass ratio of the colorant to the amorphous polyester resin (B) (colorant / amorphous polyester resin (B)) is 55 / 45 or more and 99 / 1 or less.

Citation Information

Patent Citations

  • Electrophotographic toner

    JP2007127684A

  • Electrophotographic toner

    JP2007127685A

  • Method for manufacturing toner

    JP2020024263A

  • Binder resin for toners

    JP2021107920A

  • Method for producing toner for electrostatic charge image development

    JP2021113883A