Aluminum terminal and aluminum wire with aluminum terminal
The aluminum terminal with a Cu and Sn layer structure, combined with a Ni-containing layer, addresses conductivity and temperature rise issues, enhancing adhesion and reducing resistance for reliable operation.
Patent Information
- Application Number
- JP2023057075
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Aluminum terminals face challenges in ensuring conductivity and preventing temperature rises due to insulating oxide films and poor adhesion of Sn layers, leading to increased resistance and potential fire risks during repeated energization.
The aluminum terminal is designed with a Cu layer of 0.10 μm to 10.00 μm thickness and an Sn layer of 0.50 μm to 20.00 μm thickness, along with a Ni-containing layer of 1.0 μm to 10.0 μm, optimized for crystal grain size and orientation to enhance adhesion and conductivity, reducing the risk of peeling and resistance.
The solution provides excellent conductivity and effectively suppresses temperature rises during repeated energization, ensuring safe and secure operation without ignition.
Smart Images

Figure 2024144903000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aluminum-based terminal and an aluminum-based electric wire with an aluminum-based terminal. [Background technology]
[0002] Usually, copper-based materials such as copper and copper alloys, which have high electrical conductivity, are used for the conductors of electric power distribution cables, but in recent years, aluminum-based materials such as aluminum and aluminum alloys are sometimes used to reduce weight. Aluminum-based terminals are sometimes used for connecting the ends of aluminum-based conductors to prevent dissimilar metal corrosion. An electric circuit is created and a current flows by fastening the plate-shaped connection part of the aluminum-based terminal, which is connected to the aluminum-based conductor, to a connecting member with a bolt or the like.
[0003] However, since an insulating oxide film exists on the surface of the aluminum-based terminal, in order to electrically connect the aluminum-based terminal to the connecting member, it is necessary to apply a certain amount of pressure to destroy the oxide film existing on the surface of the plate-like connecting portion of the aluminum-based terminal and to bring the newly formed aluminum surface of the plate-like connecting portion into contact with the connecting member, but it is difficult to control the pressure, and sufficient electrical connection may not be ensured.
[0004] Therefore, there is a method to ensure conductivity by forming a Sn layer on the surface of the aluminum terminal. However, when a Sn layer is formed on the Ni-P layer formed by normal zincate treatment, peeling of the Sn layer due to poor adhesion causes an increase in resistance at the contact surface with the connecting member of the aluminum terminal and an increase in temperature after repeated current passing through the aluminum terminal, which may cause a fire in the worst case.
[0005] Patent Document 1 also describes a contact portion that comes into direct contact with a mating terminal, which is formed on an Al alloy material, contains Sn as an essential component, and further contains one or more additive elements M selected from Cu, Zn, Co, Ni, and Pd, and a contact portion formed on the alloy layer, which contains Sn. 3 O 2 (OH)2 However, Patent Document 1 does not consider at all the increase in resistance of the aluminum terminal after repeated current flow, and does not sufficiently suppress the increase in temperature of the aluminum terminal after repeated current flow. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-220212 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present disclosure is to provide an aluminum-based terminal and an aluminum-based electric wire with an aluminum-based terminal that have excellent electrical conductivity and can suppress temperature rise after repeated current flow. [Means for solving the problem]
[0008] [1] An aluminum-based terminal comprising: a conductor connection portion for connecting to a conductor; a plate-shaped connection portion having a first principal surface and a second principal surface and for contacting a connection member; a Cu layer having a thickness of 0.10 μm or more and 10.00 μm or less provided on at least one of the first principal surface and the second principal surface; and a Sn layer having a thickness of 0.50 μm or more and 20.00 μm or less provided on the Cu layer. [2] The aluminum-based terminal according to the above [1], further comprising a Ni-containing layer having a thickness of 1.0 μm or more and 10.0 μm or less, provided between the plate-shaped connection portion and the Cu layer. [3] The aluminum-based terminal according to [1] or [2] above, wherein, when crystal orientation analysis is performed by electron backscatter diffraction method on a cross section perpendicular to the longitudinal direction of the plate-like connecting portion, the average crystal grain size of the Cu layer is 3.0 μm or less, and the integration ratios of each of the (100) plane, the (110) plane, and the (111) plane of the Cu layer are 33% or less. [4] An aluminum-based terminal according to any one of [1] to [3] above, wherein, when crystal orientation analysis is performed by electron backscatter diffraction method on a cross section perpendicular to the longitudinal direction of the plate-shaped connecting portion, the proportion of crystal grains in the Sn layer having a grain size smaller than the average grain size of the Cu layer relative to the crystal grains in the Sn layer is 6.0% or less. [5] An aluminum-based electric wire with an aluminum-based terminal, comprising an aluminum-based electric wire connected to the conductor connection portion of the aluminum-based terminal according to any one of the above [1] to [4]. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide an aluminum-based terminal and an aluminum-based electric wire with an aluminum-based terminal that have excellent electrical conductivity and can suppress temperature rise after repeated current passage. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a perspective view showing an example of a configuration of a main part of an aluminum-based terminal according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a plate-shaped connecting portion constituting an aluminum-based terminal of an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing another example of the plate-shaped connecting portion constituting the aluminum-based terminal of the embodiment. [Figure 4] FIG. 4 is a perspective view showing an example of a configuration of a main part of an aluminum-based electric wire with an aluminum-based terminal according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a detailed description will be given based on an embodiment.
[0012] As a result of extensive research, the inventors have discovered that by forming the surface layer of the main surface of the plate-shaped connection part that constitutes an aluminum-based terminal into a predetermined layer structure, when the main surface having the predetermined layer structure is used as a contact surface to connect to a connecting member, it is possible to obtain excellent electrical conductivity and suppress temperature rise after repeated passage of electricity, and have completed the present disclosure based on this finding.
[0013] The aluminum-based terminal of the embodiment includes a conductor connection portion that connects to a conductor, a plate-shaped connection portion having a first main surface and a second main surface and that contacts a connection member, a Cu layer having a thickness of 0.10 μm or more and 10.00 μm or less provided on at least one of the first and second main surfaces, and a Sn layer having a thickness of 0.50 μm or more and 20.00 μm or less provided on the Cu layer.
[0014] Fig. 1 is a perspective view showing an example of a main configuration of an aluminum-based terminal of an embodiment. Fig. 2 is a cross-sectional view showing an example of a plate-shaped connection part constituting the aluminum-based terminal of the embodiment. For convenience, a Cu layer 13 and an Sn layer 14 are omitted in Fig. 1.
[0015] 1 and 2, the aluminum-based terminal 1 includes a plate-shaped connecting portion 10, a conductor wire connecting portion 20, a Cu layer 13, and an Sn layer 14. The base of the aluminum-based terminal 1 including the plate-shaped connecting portion 10 and the conductor wire connecting portion 20 is formed from an aluminum-based material including pure aluminum and an aluminum alloy, for example, A1070.
[0016] The plate-shaped connection part 10 constituting the aluminum-based terminal 1 has a first main surface 11a and a second main surface 11b, and comes into contact with a connection member (not shown). For example, the plate-shaped connection part 10 is provided on one end side of the aluminum-based terminal 1. The conductor wire connection part 20 is a part that connects to a conductor wire 31 of the aluminum-based electric wire 3 as described later. For example, the conductor wire connection part 20 is provided on the other end side of the aluminum-based terminal 1.
[0017] A through hole 12 penetrating from the first main surface 11a to the second main surface 11b facing each other may be provided in the plate-shaped connection portion 10 of the aluminum-based terminal 1. A fastening member (not shown) such as a bolt is inserted into the through hole 12 to mechanically and electrically connect the plate-shaped connection portion 10 of the aluminum-based terminal 1 to a connecting member (not shown).
[0018] A Cu layer 13 is provided on at least one of the first and second main surfaces 11a and 11b of the plate-shaped connection part 10. The Cu layer 13 is, for example, a plating layer. The main surface of the plate-shaped connection part 10 on which the Cu layer 13 is provided is the surface that comes into contact with a connection member (not shown), and is here the first main surface 11a as shown in FIG. 2. For example, the main surface on which the Cu layer 13 is provided (here, the first main surface 11a) is located on the opposite side to the crimping part 21 of the conductor connection part 20, as shown in FIG. 4 described later. The Cu layer 13 may be provided on the second main surface 11b in addition to the first main surface 11a.
[0019] The thickness of the Cu layer 13 is 0.10 μm or more, preferably 0.50 μm or more, and more preferably 1.00 μm or more. When the thickness of the Cu layer 13 is 0.10 μm or more, peeling of the Cu layer 13 and the Sn layer 14 due to insufficient adhesion of the Cu layer 13 to the plate-shaped connection part 10 can be suppressed, and an increase in resistance between the plate-shaped connection part 10 and a connection member (not shown) can be suppressed.
[0020] The thickness of the Cu layer 13 is 10.00 μm or less, preferably 6.00 μm or less, and more preferably 4.00 μm or less. When the thickness of the Cu layer 13 is 10.00 μm or less, Cu, which easily forms compounds, is easily formed. 3 This can suppress the formation of an Sn alloy layer and can suppress an increase in resistance between the plate-shaped connecting portion 10 and the connecting member. Furthermore, it can suppress a decrease in productivity.
[0021] The thickness of the Sn layer 14 provided on the Cu layer 13 is 0.50 μm or more, preferably 3.00 μm or more, and more preferably 5.00 μm or more. When the thickness of the Sn layer 14 is 0.50 μm or more, it is possible to suppress a lack of conductivity of the aluminum-based terminal 1 due to partial absence or excessive non-uniformity of the Sn layer 14 on the Cu layer 13.
[0022] The thickness of the Sn layer 14 is 20.00 μm or less, preferably 16.00 μm or less, and more preferably 12.00 μm or less. When the thickness of the Sn layer 14 is 20.00 μm or less, the contact pressure change and the resistance value variation due to unevenness of the Sn layer 14 can be suppressed. Furthermore, peeling of the Sn layer 14 can be suppressed, and an increase in the resistance between the plate-shaped connection part 10 and a connection member (not shown) can be suppressed. Furthermore, a decrease in productivity can be suppressed.
[0023] 3 is a cross-sectional view showing another example of the plate-shaped connecting portion constituting the aluminum-based terminal of the embodiment. As shown in FIG. 3, the aluminum-based terminal 1 may further include a Ni-containing layer 15 provided between the plate-shaped connecting portion 10 and the Cu layer 13.
[0024] When the aluminum-based terminal 1 is provided with the Ni-containing layer 15, the adhesion between the plate-shaped connection portion 10 and the Cu layer 13 is improved, so that an increase in resistance between the plate-shaped connection portion 10 and the connection member can be suppressed. Furthermore, an increase in temperature after repeated current flow can be suppressed. On the other hand, if the Ni-containing layer 15 is too thick, the torque load applied when the bolt is fastened to the through hole 12 may cause large cracks in the Ni-containing layer 15, and when the aluminum-based terminal 1 is used outdoors, it is exposed to wind and rain, which may cause corrosion and increase the resistance. For example, 2 In the case of an aluminum-based terminal 1 for connecting a thick electric wire such as a conductor wire 11, the recommended tightening torque is large, and therefore cracks tend to occur easily. In addition, when a layer structure similar to the layer structure of the plate-like connection part 10 is also provided in the conductor wire connection part 20 of the aluminum-based terminal 1, when the conductor wire connection part 20 is crimped to form the crimped part 21 in order to manufacture the aluminum-based electric wire 5 with the aluminum-based terminal 5 shown in Fig. 4 described later, large cracks may occur in the crimped part 21 of the conductor wire connection part 20. Therefore, when the aluminum-based electric wire 5 with the aluminum-based terminal 5 is used outdoors, corrosion may occur and the resistance may increase.
[0025] For the above reasons, the lower limit of the thickness of the Ni-containing layer 15 is preferably 1.0 μm or more, more preferably 2.0 μm or more, and the upper limit is preferably 10.0 μm or less, more preferably 6.0 μm or less. The Ni-containing layer 15 is preferably a Ni-P layer or a Ni layer.
[0026] <Metal structure of aluminum terminals> Next, the metal structure of the aluminum-based terminal will be described. When a crystal orientation analysis is performed by electron backscatter diffraction (EBSD) on a cross section of the plate-like connecting part 10 perpendicular to the longitudinal direction of the plate-like connecting part 10, it is preferable that the average crystal grain size of the Cu layer 13 is 3.0 μm or less, and the accumulation ratio of each of the (100) plane, (110) plane, and (111) plane of the Cu layer 13 is 33% or less. The longitudinal direction of the plate-like connecting part 10 is the same direction as the longitudinal direction of the aluminum-based terminal 1.
[0027] Here, "EBSD" is an abbreviation for Electron Backscatter Diffraction, a crystal orientation analysis technique that utilizes reflected electron Kikuchi diffraction that occurs when an aluminum-based terminal, which is the measurement sample, is irradiated with an electron beam inside a scanning electron microscope (SEM).
[0028] In the aluminum-based terminal 1 having such a configuration, the crystal growth of the Sn layer 14 formed on the Cu layer 13 is uniform without bias toward specific crystal grains, so that the adhesion between the Cu layer 13 and the Sn layer 14 is further improved and the plating is less likely to peel off. Furthermore, the resistance when current is applied to the aluminum-based electric wire 5 with the aluminum-based terminal described below can be reduced and the temperature rise in a heat cycle test can be suppressed. Regarding the crystal growth of the Sn layer 14, it is preferable that the average crystal grain size of the Cu layer 13, which is the base of the Sn layer 14, is small because this can suppress the Sn layer 14 from depending on a specific crystal, and the average crystal grain size of the Cu layer is more preferably 2.0 μm or less, and even more preferably 1.1 μm or less.
[0029] In addition, when a crystal orientation analysis is performed by EBSD on a cross section of the plate-like connecting part 10 perpendicular to the longitudinal direction of the plate-like connecting part 10, it is preferable that the ratio of the crystal grains in the Sn layer 14 that are equal to or smaller than the average crystal grain size of the Cu layer 13 to the crystal grains in the Sn layer 14 is 6.0% or less, from the viewpoint of further improving the adhesion between the Cu layer 13 and the Sn layer 14. With such a configuration, the crystal growth in the Sn layer 14 is less dependent on a specific crystal of the Cu layer 13, so that the Sn layer 14 is likely to grow evenly and the adhesion is improved. For this reason, the ratio of the crystal grains in the Sn layer 14 that are equal to or smaller than the average crystal grain size of the Cu layer 13 to the crystal grains in the Sn layer 14 is preferably 6.0% or less, more preferably 2.0% or less.
[0030] Such an aluminum-based terminal 1 is suitable for use as a terminal for electric wires or cables used in devices such as switchboards and data centers.
[0031] Next, a method for manufacturing the aluminum-based terminal 1 will be described.
[0032] First, in the first forging step, the center of a round bar made of an aluminum-based material is compressed by forging to form the conductor wire connection portion 20.
[0033] The first heat treatment step carried out after the first forging step is performed for the purpose of reducing deformation resistance during crimping between the conductor connection portion 20 and the conductor 31 of the aluminum-based electric wire 3 described below. The first heat treatment step is not particularly limited, but is preferably performed at a temperature of 300° C. or higher and 450° C. or lower for 1 hour or higher and 3 hours or lower, because this is an industrially stable heat treatment.
[0034] In the second forging step carried out after the first heat treatment step, the end opposite the conductor wire connection part 20 is forged into a die and compressed, thus forming the plate-shaped connection part 10.
[0035] Also, a third forging step may be performed after the second forging step. In the third forging step, in order to impart a transfer pattern to the main surface of the plate-shaped connecting part 10, the plate-shaped connecting part 10 is forged using a die having an inner surface processed in a pattern shape and different from the die used in the second forging step. Two dies are placed so as to sandwich the plate-shaped connecting part 10, and the plate-shaped connecting part 10 is pressed to form a pattern on the main surface of the plate-shaped connecting part 10.
[0036] Thereafter, a through hole 12 is opened in the plate-like connection portion 10 by punching, and burrs around the through hole 12 are removed to obtain a sample having the plate-like connection portion 10 and the conductor connection portion 20.
[0037] Next, the sample is immersed in an aqueous solution of an alkaline cleaner to perform an alkaline degreasing process to degrease the surface of the sample. The conditions for the alkaline degreasing process are that the concentration of the alkaline cleaner in the aqueous solution is 400 ml / L to 500 ml / L, the liquid temperature is 35°C to 55°C, and the immersion time is 1 minute to 5 minutes.
[0038] In the oxide film removal process carried out after the alkaline degreasing process, the sample is immersed in an etching solution to remove the insulating oxide film present on the surface of the sample. The conditions for the oxide film removal process are that the concentration of the etching solution is 60 ml / L to 100 ml / L, the liquid temperature is 50°C to 70°C, and the immersion time is 1 minute to 5 minutes.
[0039] In the first nitric acid washing step performed after the oxide film removing step, the sample is immersed in a nitric acid aqueous solution to wash the sample with nitric acid. The conditions for the first nitric acid washing step are a liquid temperature of 10° C. to 30° C. and an immersion time of 10 seconds to 50 seconds.
[0040] In the first zincate treatment step carried out after the first nitric acid washing step, the sample is immersed in an aqueous solution of a zinc substitution agent to perform a zincate treatment on the sample. The conditions for the first zincate treatment step are that the concentration of the zinc substitution agent in the aqueous solution is 230 ml / L or more and 330 ml / L or less, the liquid temperature is 10°C or more and 30°C or less, and the immersion time is 10 seconds or more and 50 seconds or less.
[0041] In the second nitric acid washing step performed after the first zincate treatment step, the sample is immersed in an aqueous nitric acid solution to wash the sample with nitric acid. The conditions for the second nitric acid washing step are a liquid temperature of 10°C to 30°C and an immersion time of 30 seconds to 70 seconds.
[0042] In the second zincate treatment step carried out after the second nitric acid washing step, the sample is immersed in an aqueous solution of a zinc substitution agent to perform a zincate treatment on the sample. The conditions for the second zincate treatment step are that the concentration of the zinc substitution agent in the aqueous solution is 230 ml / L or more and 330 ml / L or less, the liquid temperature is 10°C or more and 30°C or less, and the immersion time is 30 seconds or more and 70 seconds or less.
[0043] When the aluminum-based terminal 1 does not have the Ni-containing layer 15, an electroless Cu plating process is performed after the second zincate treatment process. In the electroless Cu plating process, the sample is immersed in a plating solution and a Cu layer is formed on the surface of the sample by electroless plating. The conditions for the electroless Cu plating process are a solution temperature of 35°C to 55°C and an immersion time of 1 minute to 120 minutes. The plating solution contains copper sulfate pentahydrate with a concentration of 0.30 mol / dm 3 More than 0.35mol / dm 3 Below, the concentration of trisodium citrate dihydrate is 0.06 mol / dm 3 More than 0.10mol / dm 3 Below, the concentration of sodium hypophosphite is 0.15 mol / dm 3 More than 0.20mol / dm 3 Below, the concentration of boric acid is 0.25 mol / dm 3 More than 0.30mol / dm 3 The following is the result.
[0044] In the electrolytic Sn plating process carried out after the electroless Cu plating process, the sample is immersed in a plating solution and an electric current is passed through it to form a Sn layer on the surface of the Cu layer. The conditions for the electrolytic Sn plating process are: solution temperature of 10°C to 30°C, immersion time of 20 seconds to 30 minutes, and current density of 1 A / dm 2 More than 3A / dm 2The plating solution has a tin sulfate concentration of 80 g / L to 100 g / L, and a sulfuric acid concentration of 50 ml / L to 60 ml / L. A semi-brightener may be added to the plating solution to improve the gloss of the Sn layer. For example, the concentration of the semi-brightener is about 5 ml / L.
[0045] When the aluminum terminal 1 has a Ni-containing layer 15, an electroless Ni plating process is performed after the second zincate treatment process. In the electroless Ni plating process, the sample is immersed in a plating solution to form a Ni-containing layer on the surface of the sample by electroless plating. The conditions for the electroless Ni plating process are a solution temperature of 85°C to 97°C and an immersion time of 1 minute to 120 minutes. The plating solution has a nickel sulfate concentration of 25 g / L to 30 g / L, a sodium hypophosphite concentration of 20 g / L to 25 g / L, a sodium acetate concentration of 5 g / L to 15 g / L, and a sodium citrate concentration of 5 g / L to 15 g / L.
[0046] In the electrolytic Cu plating process carried out after the electroless Ni plating process, the sample is immersed in a plating solution and an electric current is passed through it to form a Cu layer on the surface of the Ni-containing layer. The conditions for the electrolytic Cu plating process are: solution temperature of 10°C to 30°C, immersion time of 5 seconds to 60 minutes, and current density of 0.4 A / dm 2 More than 3.0A / dm 2 The plating solution has a copper sulfate concentration of 150 g / L or more and 200 g / L or less, a sulfuric acid concentration of 40 g / L or more and 50 g / L or less, and a concentrated hydrochloric acid concentration of 0.150 ml / L or more and 0.175 ml / L or less.
[0047] In the Sn electroplating process carried out after the Cu electroplating process, the sample is immersed in a plating solution and a current is passed through it to form a Sn layer on the surface of the Cu layer. The conditions for the Sn electroplating process are: solution temperature of 10°C to 30°C, immersion time of 5 seconds to 30 minutes, and current density of 1 A / dm 2 More than 3A / dm 2The plating solution has a tin sulfate concentration of 80 g / L to 100 g / L, and a sulfuric acid concentration of 50 ml / L to 60 ml / L. A semi-brightener may be added to the plating solution to improve the gloss of the Sn layer. For example, the concentration of the semi-brightener is about 5 ml / L.
[0048] After each of the above steps, washing with water is performed.
[0049] In this manner, the aluminum-based terminal 1 can be obtained.
[0050] Next, an aluminum-based electric wire with an aluminum-based terminal according to an embodiment will be described. The aluminum-based electric wire with an aluminum-based terminal according to an embodiment is formed by connecting an aluminum-based electric wire to the conductor connection portion of the above-mentioned aluminum-based terminal.
[0051] Fig. 4 is a perspective view showing an example of a main configuration of an aluminum-based electric wire with an aluminum-based terminal according to an embodiment, in which the Cu layer 13 and the Sn layer 14 are omitted for the sake of convenience.
[0052] As shown in FIG. 4, an aluminum-based electric wire 5 with an aluminum-based terminal according to an embodiment includes an aluminum-based terminal 1 and an aluminum-based electric wire 3, and a conductor connection portion 20 of the aluminum-based terminal 1 is connected to a conductor 31 of the aluminum-based electric wire 3. The longitudinal direction of the aluminum-based electric wire 5 with an aluminum-based terminal is the same as the longitudinal direction of the aluminum-based terminal 1. The conductor 31 is composed of at least one or more element wires 31a, as shown in FIG. 4, for example. The conductor 31 may be a stranded wire in which a plurality of element wires 31a are stranded together as shown in FIG. 4, a bundled wire in which a plurality of element wires 31a are bundled, or a single element wire 31a. The conductor 31 of the aluminum-based electric wire 3, i.e., the plurality of element wires 31a, is formed from an aluminum-based material including pure aluminum and an aluminum alloy.
[0053] An insulating coating 32 may be provided on the outer periphery of the conductor 31. A sheath 33 may be provided on the outer periphery of the insulating coating 32.
[0054] In FIG. 4 , at one end of an aluminum-based electric wire 3 including a conductor 31, an insulating coating 32, and a sheath 33, the insulating coating 32 covering the outer periphery of the conductor 31 and the sheath 33 covering the outer periphery of the insulating coating 32 are stripped off from the aluminum-based electric wire 3, exposing the conductor 31.
[0055] A tubular conductor connection portion 20 is provided on the other end side of the aluminum-based terminal 1, into which the conductor 31 exposed on one end side of the aluminum-based electric wire 3 is inserted. When the conductor connection portion 20 of the aluminum-based terminal 1 is crimped with the conductor 31 of the aluminum-based electric wire 3 inserted into the conductor connection portion 20 of the aluminum-based terminal 1, a crimping portion 21 is formed at the conductor connection portion 20, and an electric wire 5 with an aluminum-based terminal is obtained. In the crimping portion 21, the conductor 31 of the aluminum-based electric wire 3 is crimped to the conductor connection portion 20 of the aluminum-based terminal 1. The aluminum-based terminal 1 is electrically connected to the aluminum-based electric wire 3 via the crimping portion 21.
[0056] Here, an example is shown in which the conductor connection part 20 of the aluminum-based terminal 1 has a closed tubular shape, but the shape of the conductor connection part 20 is not limited as long as the conductor connection part 20 can be crimped to the conductor 31 of the aluminum-based electric wire 3. The conductor connection part 20 may have, for example, an open tubular shape.
[0057] Such an aluminum-based electric wire 5 with an aluminum-based terminal is suitably used as a connection member in a switchboard, a data center, or the like.
[0058] Next, a method for producing the aluminum-based electric wire 5 with the aluminum-based terminal will be described.
[0059] First, in the compound insertion step, a compound material (not shown) is applied to the inside of the conductor connection part 20 in order to improve adhesion between the conductor connection part 20 of the aluminum-based terminal 1 and the conductor 31 of the aluminum-based electric wire 3. The compound material is mainly composed of mineral oil and zinc powder, and is used to satisfactorily connect the conductor connection part 20 and the conductor 31. When the compound material is provided inside the conductor connection part 20, it plays a role of ensuring good conductivity of the aluminum-based electric wire 5 with the aluminum-based terminal, destroying the oxide film of the conductor connection part 20 and the oxide film of the conductor 31, waterproofing the crimped part 21, etc.
[0060] In the crimping step carried out after the compound insertion step, the conductor wire 31 is inserted into the conductor wire connection portion 20, and a crimping tool is used to apply force to the conductor wire connection portion 20 from one direction to crimp the conductor wire connection portion 20 and the conductor wire 31 together to form the crimped portion 21. The larger the depression amount of the crimped portion 21, in other words, the greater the pressing force during crimping, the stronger the bond can be between the conductor wire connection portion 20 of the aluminum-based terminal 1 and the conductor wire 31 of the aluminum-based electric wire 3. In this manner, an aluminum-based electric wire 5 with an aluminum-based terminal can be obtained.
[0061] According to the embodiment described above, by forming the surface layer of the main surface of the plate-shaped connection part constituting the aluminum-based terminal into a predetermined layer structure, when the main surface having the predetermined layer structure is used as a contact surface to connect to a connection member, it has excellent conductivity and can suppress temperature rise after repeated current application. In this way, even if current is repeatedly applied to the aluminum-based terminal or the aluminum-based electric wire with the aluminum-based terminal, heat generation can be suppressed, so that it can be used safely and securely without catching fire.
[0062] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. EXAMPLES
[0063] Next, examples and comparative examples will be described, but the present invention is not limited to these examples.
[0064] (Examples 1 to 9, Comparative Examples 2 to 5) In Examples 1 to 6, 9 and Comparative Examples 2 to 5, samples having a plate-shaped connection part and a conductor connection part were manufactured as follows. First, in the first forging step, the center part of a round bar made of pure aluminum was compressed by forging to form a conductor connection part. Next, in order to reduce the deformation resistance when the conductor connection part and the conductor of the aluminum-based electric wire are crimped, a heat treatment was performed at 300°C for 1 hour as a first heat treatment step. Next, in the second forging step, the end part opposite to the conductor connection part was forged into a die and compressed to form a plate-shaped connection part. Next, a through hole was opened in the plate-shaped connection part, and then burrs around the through hole were removed. In this way, a sample having a plate-shaped connection part and a conductor connection part was obtained.
[0065] In Examples 7 to 8, samples having a plate-shaped connection part and a conductor connection part were obtained as follows. First, in the first forging step, the center part of a round bar made of pure aluminum was compressed by forging to form a conductor connection part. Then, in order to reduce the deformation resistance when the conductor connection part and the conductor of the aluminum-based electric wire are crimped, a heat treatment was performed at 300°C for 1 hour as the first heat treatment step. Then, in the second forging step, the end part opposite the conductor connection part was compressed by forging into a die to form a plate-shaped connection part. Then, in the third forging step, two dies were placed so as to sandwich the plate-shaped connection part, and the plate-shaped connection part was pressed to form a pattern on the main surface of the plate-shaped connection part. The formed pattern was four cylinders having a diameter of φ0.8 mm centered on the four corners of a 1.3 mm square square, and another cylinder having a diameter of φ0.8 mm was positioned at the center of the four cylinders, and the height of the five cylinders was 100 μm. Next, a through hole was opened in the plate-like connection portion, and the burrs around the through hole were removed, thus obtaining a sample having a plate-like connection portion and a conductor connection portion.
[0066] Next, a Cu layer and an Sn layer were formed on the surface of the sample, with the thickness and physical properties shown in Table 1. The conditions for each process were as follows:
[0067] First, in the alkaline degreasing step using an aqueous solution of an alkaline cleaner, the sample was immersed in an aqueous solution of an alkaline cleaner, and the concentration of the alkaline cleaner (manufactured by Uemura Kogyo Co., Ltd., AD-68F) in the aqueous solution was 400 ml / L to 500 ml / L, the liquid temperature was 35°C to 55°C, and the immersion time was 1 minute to 5 minutes. Next, in the oxide film removal step using an etching solution, the sample was immersed in an etching solution, and the concentration of the etching solution (manufactured by Uemura Kogyo Co., Ltd., AD-101F) was 60 ml / L to 100 ml / L, the liquid temperature was 50°C to 70°C, and the immersion time was 1 minute to 5 minutes. Next, in the first nitric acid cleaning step using an aqueous solution of nitric acid, the sample was immersed in an aqueous solution of nitric acid, and the temperature of the aqueous solution of nitric acid (67.5% nitric acid, concentration 250 ml / L to 350 ml / L) was 10°C to 30°C, and the immersion time was 10 seconds to 50 seconds. Next, in the first zincate treatment step using an aqueous solution of a zinc substitute, the sample was immersed in the aqueous solution of the zinc substitute, and the concentration of the zinc substitute in the aqueous solution (AZ-301-3X, manufactured by Uemura Kogyo Co., Ltd.) was set to 230 ml / L or more and 330 ml / L or less, the liquid temperature was set to 10°C or more and 30°C or less, and the immersion time was set to 10 seconds or more and 50 seconds or less. Next, in the second nitric acid washing step using an aqueous solution of nitric acid, the sample was immersed in an aqueous solution of nitric acid, and the temperature of the aqueous solution of nitric acid (67.5% nitric acid, concentration 250 ml / L or more and 350 ml / L or less) was set to 10°C or more and 30°C or less, and the immersion time was set to 30 seconds or more and 70 seconds or less. Next, in the second zincate treatment step using an aqueous solution of a zinc substitution agent, the sample was immersed in the aqueous solution of the zinc substitution agent, and the concentration of the zinc substitution agent (AZ-301-3X, manufactured by Uemura Kogyo Co., Ltd.) in the aqueous solution was set to 230 ml / L or more and 330 ml / L or less, the liquid temperature was set to 10°C or more and 30°C or less, and the immersion time was set to 30 seconds or more and 70 seconds or less.
[0068] Next, in the electroless Cu plating process, the concentration of copper sulfate pentahydrate is 0.30 mol / dm 3 More than 0.35mol / dm 3 Below, the concentration of trisodium citrate dihydrate is 0.06 mol / dm 3 More than 0.10mol / dm 3 Below, the concentration of sodium hypophosphite is 0.15 mol / dm 3 More than 0.20mol / dm 3Below, the concentration of boric acid is 0.25 mol / dm 3 More than 0.30mol / dm 3 The sample was immersed in a plating solution having a temperature of 35°C to 55°C and an immersion time of 1 minute to 120 minutes. Next, in the electrolytic Sn plating process, the sample was immersed in a plating solution having a tin sulfate concentration of 80 g / L to 100 g / L, a sulfuric acid concentration of 50 ml / L to 60 ml / L, and a semi-brightener concentration of 5 ml / L (UTB 513Y, manufactured by Ishihara Chemical Co., Ltd.), with a temperature of 10°C to 30°C, an immersion time of 20 seconds to 30 minutes, and a current density of 1 A / dm 2 More than 3A / dm 2 The following is the result.
[0069] After each of the above steps, the substrate was washed with water. Thus, an aluminum-based terminal having a Cu layer and a Sn layer was obtained.
[0070] Next, a compound material (Compound A, manufactured by Furukawa Power Systems Co., Ltd.) was applied to the inside of the conductor connection part. Then, an aluminum-based electric wire (cross-sectional area 250 mm 2 A conductor of 10 mm diameter was inserted into the aluminum-based electric wire and a pressure was applied from one direction to the conductor connection part using a crimping tool to crimp the conductor connection part and the aluminum-based conductor wire to form a crimped part. In this way, an aluminum-based electric wire with an aluminum-based terminal was obtained in which the conductor connection part of the aluminum-based terminal and the conductor of the aluminum-based electric wire were electrically connected.
[0071] (Examples 10 to 13, Comparative Examples 1 and 6) As in Example 1, a sample having a plate-shaped connection portion and a conductor wire connection portion was obtained.
[0072] Next, a Ni-containing layer, a Cu layer, and a Sn layer were formed on the surface of the sample, each having the thickness and physical properties shown in Table 1. The conditions for each step were as follows.
[0073] First, in the alkaline degreasing step using an aqueous solution of an alkaline cleaner, the sample was immersed in an aqueous solution of an alkaline cleaner, and the concentration of the alkaline cleaner (manufactured by Uemura Kogyo Co., Ltd., AD-68F) in the aqueous solution was 400 ml / L to 500 ml / L, the liquid temperature was 35°C to 55°C, and the immersion time was 1 minute to 5 minutes. Next, in the oxide film removal step using an etching solution, the sample was immersed in an etching solution, and the concentration of the etching solution (manufactured by Uemura Kogyo Co., Ltd., AD-101F) was 60 ml / L to 100 ml / L, the liquid temperature was 50°C to 70°C, and the immersion time was 1 minute to 5 minutes. Next, in the first nitric acid cleaning step using an aqueous solution of nitric acid, the sample was immersed in an aqueous solution of nitric acid, and the temperature of the aqueous solution of nitric acid (67.5% nitric acid, concentration 250 ml / L to 350 ml / L) was 10°C to 30°C, and the immersion time was 10 seconds to 50 seconds. Next, in the first zincate treatment step using an aqueous solution of a zinc substitute, the sample was immersed in the aqueous solution of the zinc substitute, and the concentration of the zinc substitute in the aqueous solution (AZ-301-3X, manufactured by Uemura Kogyo Co., Ltd.) was set to 230 ml / L or more and 330 ml / L or less, the liquid temperature was set to 10°C or more and 30°C or less, and the immersion time was set to 10 seconds or more and 50 seconds or less. Next, in the second nitric acid washing step using an aqueous solution of nitric acid, the sample was immersed in an aqueous solution of nitric acid, and the temperature of the aqueous solution of nitric acid (67.5% nitric acid, concentration 250 ml / L or more and 350 ml / L or less) was set to 10°C or more and 30°C or less, and the immersion time was set to 30 seconds or more and 70 seconds or less. Next, in the second zincate treatment step using an aqueous solution of a zinc substitution agent, the sample was immersed in the aqueous solution of the zinc substitution agent, and the concentration of the zinc substitution agent (AZ-301-3X, manufactured by Uemura Kogyo Co., Ltd.) in the aqueous solution was set to 230 ml / L or more and 330 ml / L or less, the liquid temperature was set to 10°C or more and 30°C or less, and the immersion time was set to 30 seconds or more and 70 seconds or less.
[0074] Next, in the electroless Ni plating process, the sample was immersed in a plating solution having a nickel sulfate concentration of 25 g / L to 30 g / L, a sodium hypophosphite concentration of 20 g / L to 25 g / L, a sodium acetate concentration of 5 g / L to 15 g / L, and a sodium citrate concentration of 5 g / L to 15 g / L, the solution temperature was 85° C. to 97° C., and the immersion time was 1 minute to 120 minutes. Next, in Examples 10 to 13 and Comparative Example 6, an electrolytic Cu plating process was performed. In the electrolytic Cu plating process, the sample is immersed in a plating solution with a copper sulfate concentration of 150 g / L to 200 g / L, a sulfuric acid concentration of 40 g / L to 50 g / L, and a concentrated hydrochloric acid concentration of 0.150 ml / L to 0.175 ml / L. The solution temperature is 10°C to 30°C, the immersion time is 5 seconds to 60 minutes, and the current density is 0.4 A / dm 2 More than 3.0A / dm 2 In the subsequent Sn electrolytic plating process, the sample was immersed in a plating solution with a tin sulfate concentration of 80 g / L to 100 g / L, a sulfuric acid concentration of 50 ml / L to 60 ml / L, and a semi-brightener concentration of 5 ml / L (UTB 513Y, manufactured by Ishihara Chemical Co., Ltd.). The solution temperature was 10°C to 30°C, the immersion time was 5 seconds to 30 minutes, and the current density was 1 A / dm 2 More than 3A / dm 2 The following is the result.
[0075] After each of the above steps, the terminals were washed with water. Thus, in Examples 10 to 13 and Comparative Example 6, aluminum-based terminals including a Ni-containing layer, a Cu layer, and a Sn layer were obtained. In Comparative Example 1, an aluminum-based terminal including a Ni-containing layer and a Sn layer was obtained.
[0076] Subsequently, in the same manner as in Example 1, an aluminum-based electric wire with an aluminum-based terminal was obtained.
[0077] [Measurement and Evaluation] The aluminum-based electric wires with aluminum-based terminals obtained in the above Examples and Comparative Examples were subjected to the following measurements and evaluations. The results are shown in Tables 1 and 2.
[0078] [1] Thickness of each layer The thickness of each layer was measured with reference to JIS H 8501, Section 9. Microscopic cross-section test method. First, the plate-shaped connection part was cut along a direction perpendicular to the longitudinal direction of the aluminum-based electric wire with aluminum-based terminal, passing through the center of the through hole. Next, the cut sample was embedded in resin, wet polished and buffed, and the cut surface of the sample was mirror-finished. Three points on this cut surface, separated by 1 mm or more, were observed at 500x magnification using an optical microscope, and the average thickness of each layer was calculated. In addition, the cut surface of the same sample was subjected to WDX analysis to perform a qualitative analysis of each layer.
[0079] [2] Average grain size of the Cu layer The average crystal grain size of the Cu layer was obtained from the crystal orientation analysis data, which was obtained by continuously measuring the crystal orientation data using an EBSD detector (TSL, OIM5.0 HIKARI) attached to a high-resolution scanning analytical electron microscope (JEOL, JSM-7001FA), and calculating (processing) the measured crystal orientation data using analysis software (TSL, OIM Analysis). The measurement object was the surface of the cross section of the plate-shaped connection part perpendicular to the longitudinal direction of the aluminum-based electric wire with aluminum-based terminal, which was processed with a CP (Cross-Section Polisher). When the thickness of the Cu layer was 5.0 μm or more, the measurement area was 5 μm × 50 μm, and when the thickness of the Cu layer was less than 5.0 μm, the boundaries with other layers and the substrate were avoided, and 90% of the thickness of the Cu layer was the measurement area. The measurement was performed with a step size of 0.1 μm. The average crystal grain size of the Cu layer was calculated by drawing a 50 μm straight line on the obtained IPF image in the film surface direction (parallel to the first and second main surfaces), counting the number of times the line crossed the grain boundary, and dividing 50 μm by the count. However, if the film surface was wavy and it was impossible to draw a 50 μm straight line, multiple straight lines were drawn in a direction parallel to the first and second main surfaces, and the total length was adjusted to 50 μm. Furthermore, this measurement was performed three times (n = 3) with different observation areas, and the average value was calculated to be the average crystal grain size. Note that the above measurement was performed by regarding the boundary where the orientation difference between adjacent measurement points was 15° or more as the grain boundary surface.
[0080] [3] Cu layer density on each side The accumulation ratios were calculated by using the crystal orientation analysis data obtained from the average crystal grain size of the Cu layer [2] above, and the ratios of the area of grains oriented ±15° from the crystal plane (100), crystal plane (110), and crystal plane (111) in the chart-crystal direction to the area of all oriented grains in the cross section were defined as the accumulation ratio of the crystal plane (100), the accumulation ratio of the crystal plane (110), and the accumulation ratio of the crystal plane (111), respectively. Here, the surface observed was the cross section, but the calculations were made by converting each crystal plane into a crystal plane observed in the direction from the first principal plane to the second principal plane in the analysis software.
[0081] [4] Presence ratio The grain size of the Sn layer was calculated by setting the measurement area of the Sn layer in the above-mentioned cross section to 5 μm × 50 μm (when the thickness of the Sn layer is 5.00 μm or more) or 90% of the thickness of the Sn layer × 50 μm (when the thickness of the Sn layer is less than 5.00 μm), drawing a 50 μm straight line in the film surface direction (parallel to the first and second main surfaces) on the obtained IPF image, and calculating the length between the points where the line intersects with the grain boundary. However, if the film surface is wavy and it is not possible to draw a 50 μm straight line, multiple straight lines are drawn in the direction parallel to the first and second main surfaces (total length of multiple straight lines is 50 μm), and the length between the points where the line intersects with the grain boundary is calculated as the grain size. This measurement was performed three times (n = 3) by changing the observation range, and the total length of the crystal grains in the Sn layer that were smaller than the average crystal grain size of the Cu layer was divided by the measured length of the Sn layer, which was 150 μm (the length of a straight line drawn in the Sn layer), to obtain the proportion of crystal grains in the Sn layer that were smaller than the average crystal grain size of the Cu layer relative to the crystal grains in the Sn layer.
[0082] [5] Visual inspection of conductor connections The appearance of the conductor connection part of the aluminum terminal connected to the aluminum electric wire with the aluminum terminal was observed with a microscope to check for the presence or absence of cracks in the conductor connection part, and the following ranking was performed. If a crack exists in the conductor connection part, when the aluminum electric wire with the aluminum terminal is used outdoors, it is exposed to wind and rain, which may cause corrosion and increase the resistance. If a crack with a length of 2 mm or more exists in the conductor connection part, cracks are likely to occur in the plate-like connection part due to the torque load during bolt tightening, which may result in an increase in resistance. Therefore, it is preferable that there are no cracks with a length of 2 mm or more, and it is most preferable that there are no cracks at all.
[0083] Yes: Cracks longer than 2mm were confirmed Microcracks: Cracks less than 2 mm in length were confirmed. None: No cracks were found
[0084] [6] Initial resistance measurement The plate-shaped connection parts of two aluminum-based electric wires with aluminum-based terminals obtained in each Example and Comparative Example (aluminum-based electric wires with a total length of 400 mm, both ends of which had aluminum-based terminals connected) were bolted to a terminal block for aluminum terminals (manufactured by Fuji Denki Kogyo Co., Ltd.) with a torque of about 65 N·m, and the aluminum-based electric wires with aluminum-based terminals, the terminal block, and the aluminum-based electric wires with aluminum-based terminals were arranged in a straight line. The aluminum-based terminal on the side of the aluminum-based electric wire with aluminum-based terminal that was not fastened to the terminal block was clamped with an alligator clip, and the resistance was measured using the four-terminal method. In the resistance measurement, after measuring the resistance, the bolts were loosened once and then fastened again to measure the resistance three times, and the average was calculated.
[0085] [7] Heat cycle test To evaluate the amount of temperature rise during repeated current application, a heat cycle test was performed with reference to the heat cycle test described in "JIS C 2810 General Rules for Electric Wire Connectors for Indoor Wiring - Non-separable Type". The plate-shaped connection parts of the two aluminum-based electric wires with aluminum-based terminals (aluminum-based electric wires with a total length of 2 m each having aluminum-based terminals connected to both ends) obtained in each Example and Comparative Example were bolted to an aluminum terminal terminal block (manufactured by Fuji Electric Industries) with a torque of about 65 N·m, and the aluminum-based electric wires with aluminum-based terminals, the terminal block, and the aluminum-based electric wires with aluminum-based terminals were set in a linear arrangement. In addition, an arbitrary notch was made in the insulating coating part of the center part of the aluminum-based electric wire, a thermocouple was inserted so as to contact the conductor of the aluminum-based electric wire, the temperature of the aluminum-based electric wire was measured, and a current value was set so that the temperature of the aluminum-based electric wire became 105°C. In addition, a thermocouple was soldered to the plate-shaped connection part of the aluminum-based terminal, and the temperature of the aluminum-based terminal was measured. One cycle is defined as one hour of current flow at a set current value followed by one hour of no current flow, and the temperature of the aluminum terminal one hour after the 500th cycle of current flow was measured, compared to the temperature of the aluminum terminal one hour after the 25th cycle of current flow. The smaller the temperature rise, the better, in terms of suppressing heat generation in the aluminum electric wire with aluminum terminal.
[0086] [8] Tape peel test A tape peeling test was carried out in accordance with the plating adhesion test method of JIS H 8504. A cutter was used to make a checkerboard cut at 2 mm intervals on the main surface of the plate-like joint where each layer was formed. Then, the test tape was attached to the cut so that the length of the non-attached part was about 50 mm. When attaching, the tape was pressed strongly with a finger for about 10 seconds, taking care not to create air bubbles between the test tape and the surface of the cut. For the test tape, a test tape (polyester film, acrylic adhesive) conforming to the cellophane adhesive tape of JIS Z 1522 was used. Next, the part not attached to the cut was pinched with the finger, and the test tape was pulled strongly so that it was perpendicular to the main surface of the plate-like joint and instantly peeled off. If any layer was not attached to the adhesive surface of the peeled test tape, it was determined that there was no peeling, and the adhesion of the layer to the surface of the plate-like joint was good. If any layer was found to be attached to the adhesive surface of the peeled test tape, it was judged that peeling had occurred, and that there was poor adhesion of the layer to the surface of the plate-like connecting portion.
[0087] [Table 1]
[0088] [Table 2]
[0089] As shown in Table 1, in the above-mentioned examples, the surface layer of the main surface of the plate-shaped connection part constituting the aluminum-based terminal had a predetermined layer structure, so when the main surface having the predetermined layer structure was used as a contact surface to connect to a connection member, the initial resistance value was low and the temperature rise amount after the heat cycle test could be suppressed. Furthermore, as a result of the tape peeling test, there was no peeling. On the other hand, in the above-mentioned comparative examples, the surface layer of the main surface of the plate-shaped connection part constituting the aluminum-based terminal did not have the predetermined layer structure, so at least one of a low initial resistance value and suppression of the temperature rise amount after the heat cycle test could not be achieved. [Explanation of symbols]
[0090] 1 Aluminum terminal 3. Aluminum-based electric wires 5. Aluminum-based electric wire with aluminum-based terminal 10 Plate-shaped connection part 11a 1st main surface 11b 2nd principal surface 12 Through hole 13 Cu layer 14 Sn layer 15 Ni-containing layer 20 Conductor connection 21 Crimping section 31 Conductor 31a Bare wire 32 Insulating coating 33 Sheath
Claims
1. A conductor connection portion for connecting to the conductor; a plate-shaped connection portion having a first main surface and a second main surface and in contact with the connection member; a Cu layer provided on at least one of the first and second main surfaces and having a thickness of 0.10 μm or more and 10.00 μm or less; a Sn layer having a thickness of 0.50 μm or more and 20.00 μm or less provided on the Cu layer; An aluminum-based terminal comprising:
2. 2. The aluminum-based terminal according to claim 1, further comprising a Ni-containing layer provided between said plate-like connection portion and said Cu layer, said Ni-containing layer having a thickness of 1.0 μm or more and 10.0 μm or less.
3. 2. The aluminum-based terminal according to claim 1, wherein, when a crystal orientation analysis is performed by electron backscatter diffraction method on a cross section perpendicular to the longitudinal direction of the plate-shaped connection portion, the average crystal grain size of the Cu layer is 3.0 μm or less, and the integration rate of each of the (100) plane, the (110) plane, and the (111) plane of the Cu layer is 33% or less.
4. 2. The aluminum-based terminal according to claim 1, wherein, when a crystal orientation analysis is performed using electron backscatter diffraction method on a cross section perpendicular to the longitudinal direction of the plate-shaped connection portion, the proportion of crystal grains in the Sn layer having an average crystal grain size smaller than that of the Cu layer relative to the crystal grains in the Sn layer is 6.0% or less.
5. An aluminum-based electric wire with an aluminum-based terminal, comprising an aluminum-based electric wire connected to the conductor connection portion of the aluminum-based terminal according to any one of claims 1 to 4.
Citation Information
Patent Citations
Manufacture of copper plated aluminum terminal
JP1981003694A
JP1992059071U
Connector terminal, and material for connector terminal
JP2014063662A
Surface treatment material
JP2018009203A
Aluminum wire with aluminum crimp terminal
JP2022100544A